Sheet-like precursor for forming noise suppression layer, noise suppression sheet, and method for suppressing noise

A sheet-like precursor with specific filler and resin composition forms a noise suppression layer that addresses flexibility and low-frequency noise suppression issues, ensuring effective noise reduction across complex surfaces.

JP7552060B2Active Publication Date: 2024-09-18TOYO INK MFG CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020068116
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-18
Filing Date
2020-04-06
Publication Date
2024-09-18
Estimated Expiration
2040-04-06

AI Technical Summary

Technical Problem

Conventional noise suppression sheets lack flexibility and extensibility to follow the unevenness of resin molded products, leading to cracks and insufficient low-frequency noise suppression performance below 1 MHz.

Method used

A sheet-like precursor containing 25% by mass or more of conductive filler, magnetic filler, and a binder resin, with specific properties to form a noise suppression layer that has a volume resistivity of 1.0×10^-5 Ω·m or less, a magnetic permeability μ' of 20 or more at 1 MHz, and an elongation rate of 10 to 600%, enabling effective noise suppression.

Benefits of technology

The noise suppression sheet achieves good followability to complex shapes and high suppression ability against low-frequency noise of 1 MHz or less, maintaining flexibility and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552060000002
    Figure 0007552060000002
  • Figure 0007552060000004
    Figure 0007552060000004
  • Figure 0007552060000003
    Figure 0007552060000003
Patent Text Reader

Abstract

To provide a noise suppressing sheet including a noise suppressing layer having high ability to suppress a low-frequency noise of 1 MHz or below, and capable of achieving good followability to a noise source or the like, which has a complicated geometry in concave / convex shape.SOLUTION: A sheet-like precursor for noise suppressing layer formation comprises a conductive filler of 25 wt% or more, a magnetic filler and a binder resin. A noise suppressing sheet is arranged by forming the sheet-like precursor for noise suppressing layer formation on a sheet-like substrate. The noise suppressing sheet comprises a noise suppressing layer having a volume resistance of 1.0×10-5 Ωm or less, a relative magnetic permeability μ' of 20 or larger at 1 MHz, and an elongation of 10 to 600%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sheet-like precursor used for forming a suppression layer for suppressing noise at 1 MHz or less, a noise suppression sheet having a noise suppression layer formed from the precursor, and a method for suppressing noise by using the noise suppression sheet. [Background technology]

[0002] In recent years, there has been a strong demand for measures against low-frequency noise generated by wireless communication devices such as power control units mounted on electric vehicles, etc., and AF / FM radios, etc. One method of noise countermeasure is to cover the noise source or the area or parts to be protected with electromagnetic shielding material, and conventionally, the effects of low-frequency noise have been suppressed by using a metal case. Patent Document 1 discloses a mechanism for suppressing low-frequency noise leakage by using magnetic properties and high-frequency noise leakage by using a shielding composition made by mixing a conductive filler and a magnetic filler in a thermoplastic or thermosetting resin. Patent Document 2 discloses a magnetism suppressing sheet in which a metal foil formed by plating and a resin paste containing a magnetic filler are laminated together. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Special Publication No. 2019-500742 [Patent Document 2] JP 2015-220259 A Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, the weight of automobile bodies has been reduced to improve fuel efficiency, and the replacement of conventional metal housings with resin molded products has been considered. In order to impart the noise suppression function of metal housings to resin molded products, attempts have been made to provide a noise suppression layer on the surface, but there have been issues in achieving both the conformability of the sheet used for noise suppression to resin molded products with complex uneven shapes and the low-frequency noise suppression performance. For example, conventional noise suppression sheets such as those disclosed in Patent Documents 1 and 2 lack flexibility and extensibility to conform to the irregularities of molded products, resulting in the problem of cracks occurring due to their inability to conform to the irregularities (hereafter, abbreviated to "conformity"). In addition, they lack the ability to suppress noise in the 1 MHz or lower band, and there is a problem that this is further reduced when the sheets are made to conform to irregularities (hereafter, abbreviated to "low-frequency shielding").

[0005] In other words, an object of the present invention is to provide a noise suppression sheet that has a noise suppression layer that can achieve good conformability to the complex uneven shapes of noise sources and components to be protected from noise, and that has high suppression capability for low-frequency noise of 1 MHz or less. [Means for solving the problem]

[0006] As a result of extensive investigations, the present inventors have found that the problems of the present invention can be solved in the following aspect, and have thus completed the present invention. That is, the present invention relates to a sheet-like precursor for forming a noise suppression layer capable of suppressing noise of 1 MHz or less, which contains 25 mass % or more of a conductive filler, a magnetic filler, and a binder resin. The present invention further provides a noise suppression sheet having a noise suppression layer formed on a sheet-like substrate from the sheet-like precursor for forming a noise suppression layer, the noise suppression layer having a volume resistivity of 1.0×10 -5 The noise suppression sheet has a magnetic permeability μ´ of 20 or more at 1 MHz and an elongation of 10 to 600%. Effect of the Invention

[0007] The noise suppression sheet of the present invention can achieve good conformability to the complex uneven shapes of noise sources and components to be protected from noise, and has a noise suppression layer with high suppression capability for low-frequency noise of 1 MHz or less, thereby achieving a remarkable noise suppression effect. [Brief description of the drawings]

[0008] [Figure 1] Average orientation angle diagram [Diagram 2] Cross-sectional observation image of the noise suppression layer of Example 1 [Diagram 3] Cross-sectional view explaining tracking ability DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] An example of an embodiment to which the present invention is applied will be described below. The numerical values ​​specified in this specification are values ​​obtained by the method disclosed in the embodiment or example. The numerical values ​​"A to B" specified in this specification refer to a range that satisfies numerical value A and a value greater than numerical value A, and numerical value B and a value smaller than numerical value B. In addition, the "sheet" in this specification includes not only "sheet" as defined in JIS, but also "film". In order to clarify the explanation, the following description and drawings are appropriately simplified. In addition, the same element members are indicated by the same reference numerals even in different embodiments. Unless otherwise noted, the various components appearing in this specification may be used independently, either alone or in combination of two or more types.

[0010] (Sheet-shaped precursor for forming noise suppression layer) The sheet-like precursor for forming a noise suppression layer (hereinafter also referred to as the sheet-like precursor) of the present invention contains 25 mass % or more of a conductive filler, a magnetic filler, and a binder resin.

[0011] [Conductive filler] In the present invention, the conductive filler imparts a desired volume resistivity to the noise suppression layer constituting the noise suppression layer-forming sheet described below. The content of the conductive filler in 100% by mass of the sheet-shaped precursor (which is also 100% by mass of the noise suppression layer described below) must be 25% by mass, preferably 25 to 70% by mass, and more preferably 30 to 65% by mass. By setting the content in the above range, the desired volume resistivity value is easily obtained.

[0012] Examples of the conductive filler include metal powders such as gold, silver, copper, and nickel, alloy powders such as solder, and core-shell particles of silver-coated copper powder, gold-coated copper powder, silver-coated nickel powder, and gold-coated nickel powder. From the viewpoint of obtaining an excellent volume resistivity, conductive fillers containing gold, silver, and copper are preferred. From the viewpoint of cost, silver-coated copper powder is preferred. The content of silver in silver-coated copper is preferably 6 to 20 mass% in 100 mass% of the total of silver and copper, more preferably 8 to 17 mass%, and even more preferably 10 to 15 mass%. In the case of core-shell particles, the coverage of the coating layer with respect to the core part is preferably 60% or more, more preferably 70% or more, and even more preferably 80% or more on average. The core part may be nonmetallic, but from the viewpoint of conductivity, a conductive substance is preferred, and metal particles are more preferred. The conductive filler can be used alone or in combination of two or more kinds.

[0013] The conductive filler may be in the form of flake particles, dendritic particles, plate-like particles, grape-like particles, or spherical particles, with flake particles and dendritic particles being preferred, and flake particles being more preferred. By making the conductive filler in the form of a flake, the elongation rate of the noise suppression layer can be increased to 10% or more, and the reduction in the number of contact points between the conductive fillers even after expansion and contraction can be suppressed, making it possible to maintain a good volume resistivity.

[0014] Average particle size of flake particles D 50 (a) is preferably 4 to 20 μm. By making the average particle size 4 to 20 μm, it is possible to adjust the average orientation angle of the conductive filler to 10° to 40°, and the volume resistivity can be improved, which is preferable. Nano-sized conductive fillers may be mixed into the flake particles. By mixing nano-sized particles, intermetallic bonds are formed during heat and pressure bonding by utilizing the melting point drop phenomenon of nanoparticles, which has the effect of improving shielding properties.

[0015] Average particle diameter D 50 can be measured by laser diffraction / scattering method. Specifically, for example, it is a value obtained by measuring each conductive fine particle with a tornado dry powder sample module using a laser diffraction / scattering particle size distribution analyzer LS 13 320 (manufactured by Beckman Coulter), and is the average particle diameter of the particle diameter at which the integrated value of the particles is 50%. The refractive index is set to 1.6 for the measurement.

[0016] The average thickness of the flake-like conductive filler is preferably 0.01 to 1.5 μm, and more preferably 0.05 to 1.0 μm. By setting the average thickness of the conductive filler within the above range, the conductive filler can be appropriately oriented in the thickness direction in the noise suppression layer, thereby reducing the volume resistivity.

[0017] The thickness of the conductive filler was determined by measuring approximately 10 to 20 different particles based on an image of a cross section of a noise suppression sheet cut perpendicularly to the thickness direction and magnifying it 1,000 to 2,000 times with a laser microscope (Keyence, VK-X100), and calculating the average value.

[0018] As the conductive filler, it is preferable to use flake particles, but flake particles may be used in combination with particles of other shapes. The particle shapes to be used in combination are not particularly limited, but particles selected from the group consisting of dendritic particles, fibrous particles, needle particles, and spherical particles are preferred. The particles to be used in combination may be used alone or in combination. When used in combination, examples include a combination of flake particles and dendritic particles, a combination of flake particles, dendritic particles and spherical particles, and a combination of flake particles and spherical particles. Among these, from the viewpoint of increasing noise suppression ability and increasing elongation, it is more preferable to use flake particles alone or a combination of flake particles and dendritic particles.

[0019] The tap density of the conductive filler is 0.2 to 4.0 g / cm, which provides a high volume occupancy rate in the noise suppression layer. 3 is preferable, and 0.25 to 3.0 g / cm 3 is more preferred.

[0020] [Magnetic filler] In the present invention, the magnetic filler imparts a desired relative magnetic permeability μ' to the noise suppression layer. There are soft magnetic and hard magnetic magnetic fillers, and the soft magnetic fillers are preferred in that they can achieve a high relative magnetic permeability μ'. Examples of soft magnetic materials include metal-based soft magnetic materials such as crystalline metal magnetic materials, amorphous metal magnetic materials, and nanocrystalline metal magnetic materials. As the crystalline metal magnetic material, it is preferable to use one selected from the group consisting of Fe, Co, Ni, FeSi alloys, FeNi alloys, FeSiAl alloys, and FeSiCr alloys. Examples of the metal-based soft magnetic materials include ferrite-based materials such as MnZn ferrite, MgZn ferrite, MnMg ferrite, CuZn ferrite, MgMnSr ferrite, and NiZn ferrite. These magnetic fillers can be used alone or in combination of two or more.

[0021] The shape of the magnetic filler is preferably flake-like to obtain a high relative magnetic permeability μ´, and the average particle diameter D 50 (b) is preferably 20 to 70 μm, more preferably 25 to 65 μm. 50 If the thickness is less than 20 μm, it is difficult to obtain a sufficient relative magnetic permeability μ', and if the thickness is more than 70 μm, it becomes difficult to form the sheet, and the relative magnetic permeability μ' decreases.

[0022] Average particle size of magnetic filler D 50 (b) can be measured in the same manner as for the conductive filler. Metal-plated magnetic fillers are also preferred. The metal used for plating is preferably one with high electrical conductivity, and more preferably, for example, gold, silver, copper, or nickel. By plating the surface of the magnetic filler with the above metal, the number of contact points between the metal-plated magnetic fillers or between the metal-plated magnetic fillers and the conductive filler increases, and the volume resistance value of the noise suppression layer can be more effectively improved.

[0023] The tap density of the magnetic filler is set to 0.2 to 4.0 g / cm from the viewpoint of obtaining a high volume occupancy rate in the noise suppression layer and improving the relative permeability. 3 is preferable, and 0.25 to 3.0 g / cm 3 is more preferred.

[0024] The content of the magnetic filler in 100% by mass of the sheet-shaped precursor (which is also 100% by mass of the noise suppression layer described below) is preferably 20 to 65% by mass, and more preferably 30 to 50% by mass. By setting it in this range, the desired relative magnetic permeability μ' can be easily obtained.

[0025] In order to achieve both high relative magnetic permeability by the magnetic filler and low resistance by the conductive filler, it is preferable that the orientation degrees of the two fillers are different. 50 (a) Average particle size of magnetic filler D 50 The ratio of (b) (hereinafter sometimes abbreviated as [(b) / (a)]), i.e., [(b) / (a)], is preferably 3 to 15, more preferably 4 to 14, and even more preferably 6 to 13. When [(b) / (a)] is 3 or more, the sizes of the two fillers differ appropriately, which makes it easier for a difference in orientation between the two fillers in the noise suppression layer to occur, and each filler can be appropriately oriented. The orientation in the noise suppression layer will be described later.

[0026] The average thickness of the magnetic filler is preferably 0.5 to 5 μm, more preferably 1 to 3 μm. By setting the average thickness of the magnetic filler within the above range, orientation in the planar direction can be suppressed and the relative permeability can be improved.

[0027] The thickness of the flake-like magnetic filler is determined by measuring approximately 10 to 20 different particles based on an image of a cross section obtained by cutting the noise suppression layer perpendicularly from the thickness direction and magnifying it 1,000 to 2,000 times with a laser microscope (Keyence Corporation, VK-X100), and calculating the average value.

[0028] [Binder resin] The binder resin used in the present invention is preferably a thermosetting resin or a thermoplastic resin, and a thermoplastic resin and a thermosetting resin may be used in combination.

[0029] The thermosetting resin is a resin having a plurality of crosslinkable reactive functional groups, and examples of the reactive functional groups include a hydroxyl group, a phenolic hydroxyl group, a carboxyl group, an amino group, an epoxy group, an oxetanyl group, an oxazoline group, an oxazine group, an aziridine group, a thiol group, an isocyanate group, a blocked isocyanate group, a silanol group, etc. Among these, it is preferable to have a carboxyl group. Examples of thermosetting resins having reactive functional groups include acrylic resins, maleic acid resins, polybutadiene resins, polyester resins, condensation type polyester resins, addition type polyester resins, melamine resins, polyurethane resins, polyurethane urea resins, epoxy resins, oxetane resins, phenoxy resins, polyimide resins, polyamide resins, phenolic resins, alkyd resins, amino resins, polylactic acid resins, oxazoline resins, benzoxazine resins, silicone resins, fluororesins, etc. Among these, polyurethane resins, polyurethane urea resins, epoxy resins, addition type polyester resins, polyimide resins, polyamide resins, and polyamideimide resins are preferred from the viewpoints of followability and volume resistivity. The thermosetting resins can be used alone or in combination of two or more kinds.

[0030] Examples of the thermoplastic resin include polyolefin resins, vinyl resins, styrene-acrylic resins, diene resins, terpene resins, petroleum resins, cellulose resins, polyamide resins, polyurethane resins, polyester resins, polycarbonate resins, polyimide resins, and fluororesins, which do not have the curable functional group.

[0031] The polyolefin resin is preferably a homopolymer or copolymer of ethylene, propylene, an α-olefin compound, etc. Specific examples include polyethylene propylene rubber, an olefin thermoplastic elastomer, an α-olefin polymer, etc. The vinyl resin is preferably a polymer obtained by polymerization of a vinyl ester such as vinyl acetate, or a copolymer of a vinyl ester and an olefin compound such as ethylene. Specific examples include ethylene-vinyl acetate copolymer and partially saponified polyvinyl alcohol. The styrene-acrylic resin is preferably a homopolymer or copolymer made of styrene, (meth)acrylonitrile, acrylamides, (meth)acrylic acid esters, maleimides, etc. Specific examples include syndiotactic polystyrene, polyacrylonitrile, acrylic copolymers, ethylene-methyl methacrylate copolymers, etc. The diene resin is preferably a homopolymer or copolymer of a conjugated diene compound such as butadiene or isoprene, or a hydrogenated product thereof. Specific examples include styrene-butadiene rubber and styrene-isoprene block copolymer. The terpene resin is preferably a polymer made of terpenes or a hydrogenated product thereof. Specific examples include aromatic modified terpene resin, terpene phenol resin, and hydrogenated terpene resin. The petroleum resin is preferably a dicyclopentadiene type petroleum resin or a hydrogenated petroleum resin. The cellulose resin is preferably a cellulose acetate butyrate resin. The polycarbonate resin is preferably a bisphenol A polycarbonate. The polyimide resin is preferably a thermoplastic polyimide, a polyamide-imide resin, or a polyamic acid type polyimide resin. The thermosetting resins can be used alone or in combination of two or more kinds.

[0032] The mass average molecular weight of the binder resin used is preferably 20,000 to 200,000, and more preferably 25,000 to 180,000. When the mass average molecular weight is 20,000 to 200,000, the desired volume resistivity, relative magnetic permeability μ' and elongation can be achieved at the same time. The mass average molecular weight (Mw) can be measured using GPC (gel permeation chromatography) ("HPC-8020" manufactured by Tosoh Corporation).

[0033] A curing agent may also be added. The curing agent has a plurality of functional groups capable of reacting with the reactive functional groups in the thermosetting resin. The curing agent is preferably an epoxy compound, an acid anhydride group-containing compound, an isocyanate compound, an aziridine compound, a dicyandiamide, an amine compound such as an aromatic diamine, or a phenol compound such as a phenol novolac resin. The curing agent can be used alone or in combination of two or more kinds.

[0034] The sheet-like precursor may further contain a dispersant, a colorant, a flame retardant, an inorganic additive, a lubricant, an antiblocking agent, a silane coupling agent, and the like.

[0035] Examples of dispersants include phosphate ester surfactants and long-chain alkyl fatty acids. Examples of colorants include organic pigments, carbon black, ultramarine, red iron oxide, zinc oxide, titanium oxide, graphite, etc. Among these, by including a black colorant, print visibility is improved when printing on the sheet. Examples of the flame retardant include a halogen-containing flame retardant, a phosphorus-containing flame retardant, a nitrogen-containing flame retardant, and an inorganic flame retardant. Examples of the inorganic additives include glass fiber, silica, talc, and ceramics. Examples of the lubricant include fatty acid esters, hydrocarbon resins, paraffin, higher fatty acids, fatty acid amides, fatty alcohols, metal soaps, and modified silicones. Examples of the anti-blocking agent include calcium carbonate, silica, polymethylsilsesquioxane, and aluminum silicate.

[0036] <Method of manufacturing sheet-shaped precursor> The sheet-like precursor of the present invention is obtained by mixing and stirring a binder resin, a conductive filler, and a magnetic filler to obtain a resin composition, and coating the resin composition on a first sheet-like substrate. Examples of the first sheet-like substrate include a release film and various plastic films. The sheet-like precursor of the present invention is preferably produced using the first sheet-like substrate, but the sheet-like precursor itself can also be isolated by peeling off the first sheet-like substrate.

[0037] For stirring, a known stirring device can be used, and a Dispermat, a homogenizer, or the like is preferable. For coating, known coating methods such as gravure coating, kiss coating, die coating, lip coating, comma coating, blade coating, roll coating, knife coating, spray coating, bar coating, spin coating, and dip coating can be used. During coating, a drying step may be provided as necessary. For the drying, known drying devices such as a hot air dryer and an infrared heater can be used.

[0038] The release film can use a substrate such as paper or plastic, and may be a sheet having a known release treatment applied to one side of the substrate, or a film having a weak adhesive layer formed thereon instead of the release treatment.

[0039] The thickness of the sheet-shaped precursor can be appropriately designed depending on the application, but is preferably about 50 μm to 1000 μm, and more preferably about 100 μm to 600 μm. If it is 50 μm or more, the noise suppression ability is sufficient, and if it is 1000 μm or less, the flexibility and the ability to follow the adherend are more excellent.

[0040] The sheet-like precursor of the present invention is preferably provided in a state in which at least one side is directly covered with a release film, and may further include other layers between the sheet-like precursor and the release film. Examples of the other layers include layers having hard coat properties, thermal conductivity, heat insulation, water vapor barrier properties, oxygen barrier properties, low dielectric constant, high dielectric constant, low dielectric loss tangent, high dielectric loss tangent, heat resistance, etc.

[0041] (Noise suppression sheet) Next, the noise suppression sheet of the present invention will be described. The noise suppression sheet of the present invention has a sheet-like substrate and a noise suppression layer formed from the above-mentioned sheet-like precursor, and the noise suppression layer has a volume resistivity of 1.0×10 -5 The magnetic resistance is Ω·m or less, the relative permeability μ´ at 1 MHz is 20 or more, and the elongation is 10 to 600%. By setting the magnetic resistance within these ranges, low-frequency noise, particularly at 1 MHz or less, can be significantly suppressed. The sheet-like substrate needs to cover at least one surface of the noise suppression layer.

[0042] For example, when a sheet-like precursor is formed using a release film as a first sheet-like substrate, the side of the sheet-like precursor that is not in contact with the first sheet-like substrate can be covered with a second sheet-like substrate and subjected to a pressure treatment to produce a noise suppression sheet in which both sides of the noise suppression layer are covered with the sheet-like substrate. When a release film is used as the first sheet-like substrate and a film other than a release film is used as the second sheet-like substrate, the first sheet-like substrate is peeled off to produce a noise suppression sheet in which one side of the noise suppression layer is covered with the second sheet-like substrate, and the noise suppression sheet can be attached to a noise source member or the like using an adhesive or the like. The noise suppression layer itself can also serve as an adhesive layer. In this case, the noise suppression layer can be attached to the noise source member or the like, or the second sheet-like substrate can be attached to the noise source member or the like. When a release film is also used as the second sheet-like substrate, the release film on one side can be peeled off, the noise suppression layer and the noise source component or the like can be attached using an adhesive or the like, and then the release film on the other side can be peeled off.

[0043] Alternatively, when a sheet-like precursor is formed using a film "other" than the release film as the first sheet-like substrate, the surface of the sheet-like precursor not in contact with the first sheet-like substrate can be covered with a release film as the second sheet-like substrate and pressure-treated to produce a noise suppression sheet in which both sides are covered with the sheet-like substrate. Then, the noise suppression sheet obtained by peeling off the second sheet-like substrate can be attached to a noise source member or the like using an adhesive or the like. The noise suppression layer itself can also serve as an adhesive layer. In this case, the noise suppression layer can be attached to the noise source member or the like, or the first sheet-like substrate can be attached to the noise source member or the like.

[0044] Examples of the method for the pressure treatment include the use of a heat pressing device such as a pressure type heat pressing device, a transfer molding device, a compression molding device, or a vacuum / pressure molding device. For example, the pressing can be performed by plate pressing or roll pressing, and is preferably performed while heating. The heating temperature is preferably 23 to 200° C., and more preferably 50 to 160° C. If the temperature exceeds 200° C., the sheet-shaped precursor may be destroyed. The pressure is preferably 1 to 10 MPa, more preferably 2 to 8 MPa. By setting the heating temperature and pressure within the above ranges, the average orientation angle of the magnetic filler described below can be preferably set to 10° or less. More specifically, the noise suppression sheet of the present invention can be obtained by applying pressure at 90° C., 2 MPa, and for 5 minutes.

[0045] The thickness of the noise suppression layer can be appropriately designed depending on the application, but is preferably about 50 μm to 1000 μm, and more preferably about 100 μm to 600 μm. If it is 50 μm or more, the noise suppression ability is sufficient, and if it is 1000 μm or less, the conformability when attached to a noise source member or the like is excellent.

[0046] <Volume resistance value> The volume resistance of the noise suppression layer is 1.0×10 -5 Ω m or less, 5.0×10 -6 Ω·m or less is preferable, and 1.0×10 -6 Ω·m or less is more preferable. 1.0×10 ー5 A significant noise suppression effect is observed in the noise region below 1 MHz, with the Ω·m being the boundary. By controlling the conductive filler content and pressure treatment conditions of the sheet precursor, the volume resistivity can be increased to 1.0×10 -5 It is possible to make the volume resistivity Ω·m or less. For example, the content of the conductive filler is 25 mass % or more, preferably 25 to 70 mass %, and more preferably 30 to 65 mass %. By setting it in the above range, it is easy to obtain a desired volume resistivity value.

[0047] <Relative permeability> The noise suppression layer has a relative permeability μ' at 1 MHz of 20 or more, preferably 30 or more, more preferably 40 or more, and even more preferably 50 or more. With a relative permeability μ' of 20 as the boundary, a significant suppression effect is exhibited in the noise region below 1 MHz. The relative permeability in the present invention is the ratio of the permeability μ of the object to be measured, that is, in this case the noise suppression layer, to the permeability μ0 in a vacuum, and is the real part of the complex permeability μ, a dimensionless value. By controlling the type and content of the magnetic filler used and the pressure treatment conditions of the sheet-shaped precursor, it is possible to make the relative permeability μ' 20 or more, and as mentioned above, it is preferable to use a flake-shaped metallic soft magnetic material as a magnetic filler that can exhibit a high relative permeability μ'. The content of the magnetic filler is preferably 20 to 65% by mass, and more preferably 30 to 50% by mass, relative to 100% by mass of the noise suppression layer. By setting the content within this range, the desired relative magnetic permeability μ' is easily obtained.

[0048] <Growth rate> The noise suppression layer in the noise suppression sheet of the present invention has an elongation percentage of 10 to 600%, preferably 10 to 500%, and more preferably 10 to 400%. By setting the elongation rate of the noise suppression layer to 10 to 600%, the ability to conform to noise source components can be improved, and noise suppression of 1 MHz or less can be achieved even when the noise source components have a complex uneven shape. In the present invention, for example, when a noise suppression layer having a length of 10 cm becomes 11 cm, the elongation rate is 10%, and when it becomes 20 cm, the elongation rate is 10%. 1 The answer is 00%.

[0049] <Average orientation angle> In the noise suppression layer of the noise suppression sheet of the present invention, the magnetic filler contained in the noise suppression layer preferably has an average orientation angle of 10° or less, and the conductive filler preferably has an average orientation angle of 10° to 40°.

[0050] A higher relative magnetic permeability can be obtained by setting the average orientation angle of the magnetic filler to 10° or less. In order to set the average orientation angle to 10° or less, pressure treatment of the sheet-shaped precursor is effective.

[0051] On the other hand, in order to achieve high conductivity, it is preferable that the conductive filler has many contact points. However, when the conductive filler is in a flake shape, if the average orientation angle is less than 10°, the number of contact points decreases, making it difficult to obtain high conductivity. Also, if the average orientation angle is greater than 40°, it may affect the orientation of the surrounding magnetic filler, resulting in a decrease in relative permeability. In order to set the average orientation angle of the conductive filler to 10° to 40°, the pressure treatment of the sheet-shaped precursor and the average particle diameter D of the magnetic filler as described above are required. 50(a) Average particle diameter D of conductive filler 50 It is preferable that there is a difference between (a) and (b), and the ratio [(b) / (a)] is 3-15. Average particle size of both fillers D 50 If the average particle diameter D is close to the average particle diameter D, the fillers will follow each other's orientation when pressure treatment is applied, so the orientation angles within the sheet will be almost equal and the average orientation degree will be 10° or less, making it difficult to obtain high conductivity. 50 If the orientations of the magnetic filler particles are significantly different from each other, the two fillers have difficulty in following each other's orientation, and the small conductive fillers are mainly present randomly in the noise suppression layer, which may hinder the orientation of the magnetic filler. As a result, the average orientation degree of the magnetic filler exceeds 10°, and the relative permeability μ' is likely to decrease.

[0052] The average orientation angle in the present invention will be described. The average orientation angle is measured by first pressing a sheet-like precursor sandwiched between a first sheet-like substrate and a second sheet-like substrate to form a noise suppression sheet having a noise suppression layer, and then exposing a cross section of the noise suppression sheet. The cut surface is then observed under an electron microscope to obtain a cross-sectional image of the noise suppression sheet. The surface of the first or second sheet-like substrate in the image is set as a horizontal plane, and angles formed with the horizontal plane set at 0° and the major axis directions of various fillers are measured, and the average value of about 20 measured values ​​is taken as the average orientation angle.

[0053] The method of measuring the angle will be described in more detail with reference to FIG. 1. FIG. 1 is a schematic diagram of a cross-sectional image of a noise suppression sheet in which a noise suppression layer is provided on a sheet-like substrate. The average orientation angle of filler A is 20° when the interface between the noise suppression layer and the sheet-like substrate is taken as the horizontal plane and the inclination of filler A from this is calculated. On the other hand, the average orientation angle of filler B is 160°. In the present application, the average orientation angle of a filler exceeding 90° is calculated by subtracting the angle from 180°. Therefore, the average orientation angle of filler B is 180°-160°=20°.

[0054] The noise suppression sheet of the present invention may further include other layers in addition to the noise suppression layer, such as a pressure-sensitive adhesive layer (a pressure-sensitive adhesive layer) or an adhesive layer (a non-pressure-sensitive adhesive layer). For example, a sheet-like precursor is provided on a first sheet-like substrate other than the release film, and a separate adhesive sheet having an adhesive layer provided between two release films is prepared. The release film on one side of the adhesive sheet is peeled off and the exposed adhesive layer is attached to the noise suppression layer in the sheet-like precursor to form a layered structure of [first sheet-like substrate other than the release film / sheet-like precursor / adhesive layer / release film]. Then, pressure treatment is applied to turn the sheet-like precursor into a noise suppression layer, and the noise suppression sheet can be provided as a noise suppression sheet with an adhesive layer having a layered structure of [first sheet-like substrate other than the release film / noise suppression layer / adhesive layer / release film]. Alternatively, an intermediate laminate having a layered structure of [first sheet-like substrate other than the release film / sheet-like precursor / second sheet-like substrate which is a release film] can be pressure-treated to form the sheet-like precursor into a noise suppression layer, and then the second sheet-like substrate which is a release film can be peeled off and an adhesive layer can be laminated on the noise suppression layer to provide a noise suppression sheet with an adhesive layer having a layered structure of [first sheet-like substrate other than the release film / noise suppression layer / adhesive layer / release film]. Furthermore, when a release film is used as the first sheet-like substrate, it is also possible to provide a noise suppression sheet having a laminated structure of [release film / noise suppression layer / adhesive layer / release film].

[0055] The noise suppression sheet of the present invention may be provided with layers having hard coat properties, thermal conductivity, heat insulation, water vapor barrier properties, oxygen barrier properties, low dielectric constant, high dielectric constant, low dielectric tangent, high dielectric tangent, heat resistance, etc. After providing these layers, the sheet-like precursor may be compressed, or these layers may be provided after the sheet-like precursor is compressed.

[0056] The noise suppression sheet of the present invention can be used for any product that requires noise suppression of 1 MHz or less, such as wireless communication devices mounted on automobiles, AM / FM radios, electronic tags, RFID for vehicle management, and smart keys. These articles are often sources of noise of 1 MHz or less, so by covering the components constituting these articles (e.g., a housing, etc.) with the noise suppression sheet of the present invention, the impact of the generated noise on the outside of the article can be suppressed. If a noise suppression sheet provided with an adhesive layer is used, the noise suppression sheet can be attached to the inner and / or outer surface of a housing, etc. Alternatively, the effects of noise can be suppressed by covering an article from which it is desired to eliminate the effects of noise with the noise suppression sheet of the present invention. Furthermore, the noise suppression sheet of the present invention can also be used in the process of manufacturing a housing. For example, a noise suppression sheet having one side covered with a sheet-like substrate can be set in a mold for manufacturing a housing, and a resin for injection molding of the housing can be melt-injected onto the noise suppression layer side to integrally mold the housing and the noise suppression layer. If the sheet-like substrate is a release film, it can be peeled off after integral molding. If the sheet-like substrate is "other" than a release film, the sheet-like substrate is also integrated with the housing via the noise suppression layer. EXAMPLES

[0057] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. Note that the "parts" and "%" below are values ​​based on "mass%". Moreover, Example 8 is to be read as Reference Example 8 for the purpose of conforming to the scope of Claim 1.

[0058] The average particle diameter D of the conductive filler and the magnetic filler 50 The thickness of the conductive filler and the magnetic filler, the acid value of the resin, and the mass average molecular weight of the resin were measured by the following methods.

[0059] <Average particle diameter D 50 Measurements > Average particle diameter D50 The conductive filler and magnetic filler were measured using a laser diffraction / scattering particle size distribution analyzer LS13320 (manufactured by Beckman Coulter) with a Tornado dry powder sample module. The refractive index was set to 1.6.

[0060] <Filler thickness measurement> The thickness of the flake-shaped magnetic filler was determined by embedding a sheet-shaped precursor 2 with a release film (described later) in an embedding resin almost vertically, polishing the surface, and then observing the sheet-shaped precursor from the thickness direction at a magnification of 1000 to 2000 times using a laser microscope (Keyence Corporation, VK-X100), measuring the thicknesses of approximately 10 to 20 different particles in the observation field, and calculating the average value.

[0061] <Acid value measurement> 1 g of thermosetting resin was dissolved in 40 ml of methyl ethyl ketone, and a Kyoto Electronics Co., Ltd. automatic titrator "AT-510" was used with the same company's "APB-510-20B" connected as a burette. Potentiometric titration was performed using a 0.1 mol / L ethanolic KOH solution as the titration reagent, and the mg of KOH per 1 g of resin was calculated.

[0062] <Mass average molecular weight (Mw)> The mass average molecular weight (Mw) was measured using GPC (gel permeation chromatography) ("HPC-8020" manufactured by Tosoh Corporation). GPC is a liquid chromatography that separates and quantifies substances dissolved in a solvent (THF; tetrahydrofuran) based on the difference in their molecular size. The measurement in the present invention was performed using two "LF-604" columns (manufactured by Showa Denko K.K.: GPC column for rapid analysis: 6 mm ID x 150 mm size) connected in series, at a flow rate of 0.6 ml / min and a column temperature of 40°C, and the mass average molecular weight (Mw) was determined in polystyrene equivalent.

[0063] <Synthesis of thermosetting resin> [Synthesis Example 1] In a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, a dropping device, and a nitrogen inlet tube, 414 parts of a diol having a number average molecular weight (hereinafter referred to as "Mn") of 1006 obtained from adipic acid, terephthalic acid, and 3-methyl-1,5-pentanediol, 8 parts of dimethylolbutanoic acid, 145 parts of isophorone diisocyanate, and 40 parts of toluene were charged and reacted for 3 hours at 90 ° C. under a nitrogen atmosphere. 300 parts of toluene were added to this to obtain a solution of a urethane prepolymer having an isocyanate group at the end. Next, 816 parts of the obtained urethane prepolymer solution were added to a mixture of 27 parts of isophorone diamine, 3 parts of di-n-butylamine, 342 parts of 2-propanol, and 576 parts of toluene, and the mixture was reacted at 70 ° C. for 3 hours to obtain a solution of a polyurethane polyurea resin having a mass average molecular weight (hereinafter referred to as "Mw") of 54,000 and an acid value of 5 mgKOH / g. To this were added 144 parts of toluene and 72 parts of 2-propanol to obtain a polyurethane polyurea resin solution with a solid content of 50%.

[0064] [Example 1] The thermosetting resin obtained in Synthesis Example 1 (15.7 parts in terms of solid content), magnetic filler 1 (40 parts), conductive filler 1 (40 parts), dispersant (2 parts), silane coupling agent (2 parts), and aziridine compound (0.3 parts) were charged into a container (all in terms of solid content), and a mixed solvent of toluene:isopropyl alcohol (mass ratio 2:1) was added so that the non-volatile content concentration was 50 mass%, and the mixture was stirred with a disperser for 10 minutes to obtain a magnetic resin composition. Next, the magnetic resin composition was coated onto a release film using a doctor blade to a dry thickness of 30 μm, and then dried in an electric oven at 100° C. for 10 minutes. After that, a release film was placed on top to obtain an intermediate 1 in which both sides of the sheet-like precursor 1 were covered with a release film. Separately, in the same manner as above, an intermediate 2 was prepared for measuring the low frequency shielding property described later, in which a sheet-like precursor 2 having a thickness of 300 μm was provided on a release film.

[0065] Next, intermediates 1 and 2 were each pressed at 90° C. and 2 MPa for 5 minutes to obtain noise suppression sheets 1 and 2 in which both sides of noise suppression layers 1 and 2 were covered with release films. According to the methods described later, the elongation, volume resistivity, relative magnetic permeability μ', and average orientation angle were determined for noise suppression sheet 1. Additionally, the low-frequency shielding ability of noise suppression sheet 2 was evaluated according to the methods described later.

[0066] [Examples 2 to 10, Comparative Examples 1 to 3] Intermediates 1 and 2 and noise suppression sheets 1 and 2 were obtained in the same manner as in Example 1 except that the types and blending amounts (parts by mass) of the raw materials in Example 1 were changed as shown in Table 1.

[0067] The materials used in the examples are shown below. Magnetic filler 1: Fe-Si-Al soft magnetic particles (average particle size: 45 μm, average thickness: 1.3 μm) manufactured by Sanyo Special Steel Co., Ltd. Magnetic filler 2: Silver-coated Fe-Si-Al alloy (metal-based soft magnetic material in which magnetic filler is coated with 20% Ag by mass) (average particle size: 45 μm, average thickness: 1.3 μm) Magnetic filler 3: Fe-Si-Al soft magnetic particles (magnetic filler 1 with particle size adjusted by sieving) (average particle size: 35 μm, average thickness: 1.3 μm) manufactured by Sanyo Special Steel Co., Ltd. Magnetic filler 4: Fe-Si-Al soft magnetic particles (average particle size: 58 μm, average thickness: 1.3 μm) manufactured by Mate Co., Ltd. Magnetic filler 5: Fe-Si-Al soft magnetic particles (magnetic filler 1 with particle size adjusted by sieving) (average particle size: 79 μm, average thickness: 1.3 μm)

[0068] Conductive filler 1: Flake-shaped silver particles (average particle size: 5.1 μm, average thickness: 0.3 μm) manufactured by Fukuda Metals Co., Ltd. Conductive filler 2: Flake-shaped silver-coated copper particles (average particle size: 10 μm, average thickness: 0.6 μm) manufactured by DOWA Electronics Co., Ltd. Conductive filler 3: Flake-shaped silver particles (average particle size: 19 μm, average thickness: 0.8 μm) manufactured by Fukuda Metals Co., Ltd. Conductive filler 4: Flake-shaped silver particles (average particle size: 26 μm, average thickness: 1.1 μm) manufactured by Fukuda Metals Co., Ltd.

[0069] Dispersant: Phosphate ester dispersant (product name: Disparlon (registered trademark) PW-36, manufactured by Kusumoto Chemical Industries, Ltd.) Silane coupling agent: 3-acryloxypropyltrimethoxysilane (product name: KBM-5103, manufactured by Shin-Etsu Silicones) Aziridine compound: "Chemithite PZ-33" manufactured by Nippon Shokubai Co., Ltd.

[0070] The above-mentioned Examples and Comparative Examples were evaluated according to the following physical property measurements and evaluation criteria. The results are shown in Table 1. In addition, [(b) / (a)] in the table is the average particle diameter D of the conductive filler. 50 (a) Average particle size of magnetic filler D 50 (b) is the ratio [(b) / (a)].

[0071] <Growth rate> A noise suppression sheet 1 measuring 20 mm wide and 60 mm long was prepared, and the release films on both sides were removed to obtain the noise suppression layer 1 as a measurement sample. A tensile test (test speed 50 mm / min) was performed on the measurement sample using a small tabletop tester EZ-TEST (manufactured by Shimadzu Corporation) at a temperature of 25°C and a relative humidity of 50%. The elongation rate (%) of the magnetic resin layer was calculated from the obtained SS curve (stress-strain curve).

[0072] <Follow-up ability> The following description will be given with reference to FIG. The release film on one side of noise suppression sheet 1 (FIG. 3, (1)) was peeled off, and adhesive layer 18 of a separately prepared adhesive sheet was attached to the noise suppression layer to form noise suppression sheet 17, which was then cut to a size of 40 mm wide and 40 mm long. A polyimide film 13 with adhesive, 200 μm thick, 20 mm wide, and 30 mm long, and a stainless steel plate 14, 200 μm thick, 50 mm wide, and 50 mm long, were prepared. The polyimide film 13 and the stainless steel plate 14 simulated a housing having irregularities that are a noise source. An adhesive was applied to the stainless steel plate 14 so that the polyimide film 13 was positioned approximately at the center, and the plate was attached by thermocompression. Next, noise suppression sheet 17' was placed on polyimide film 13 so that the approximate center of polyimide film 13 was located at the approximate center of noise suppression sheet 17' obtained by peeling release film 11' from noise suppression sheet 17, and so that adhesive layer 18 was in contact with polyimide film 13 (FIG. 3, (2)). Noise suppressing sheet 17' was then pressed against the irregularities formed by stainless steel plate 14 and polyimide film 13 under conditions of 90° C., 2 MPa, and 5 minutes, thereby deforming noise suppressing sheet 17' and attaching it to the irregularities. After application, the release film 11 was peeled off (FIG. 3(3)). The state of fracture of the noise suppression layer at the end (step portion) of polyimide film 13 indicated by circular dashed line 16 was evaluated by observing the noise suppression layer with the naked eye and by observing a 50x magnified image using a microscope. ◯: The noise suppression layer was not broken, which was a good result. ×: The noise suppression layer was broken. Not practical.

[0073] <Volume resistance value> (1) Measurement of thickness t A sample measuring 50 mm in width and 50 mm in length was cut out from the noise suppression sheet 1, the release films on both sides were peeled off, and a glass slide, the noise suppression layer 1, and a 50 μm-thick polyimide film (Kapton 300H, Toray DuPont) were bonded using epoxy resin (Petropoxy 154, manufactured by Maruto Co., Ltd.) to obtain a measurement sample with a configuration of [glass slide / noise suppression layer / polyimide film]. The obtained measurement sample was cut from the polyimide film side by ion beam irradiation using a cross-section polisher (SM-09010, manufactured by JEOL Ltd.) The exposed cross section was observed at a magnification of 1000 to 2000 times using a laser microscope (VK-X100, manufactured by Keyence Corporation) to measure the thickness t of the noise suppression layer 1.

[0074] (2) Measurement of surface resistance R The release film on one side was peeled off from a noise suppression sheet 1 measuring 50 mm wide and 80 mm long, and the resistance of the noise suppression layer 1 was measured using a four-point probe of Mitsubishi Chemical's Loresta GP in accordance with JIS K7194-1994. The surface resistance value R was calculated by multiplying the measured value by the constant 4.239.

[0075] (3) How to calculate volume resistivity The thickness t (μm) and surface resistance R (mΩ / □) obtained in (1) and (2) above were used to calculate the resistance according to the following formula. Volume resistance = R × t × 10 -9 (Ω m)

[0076] <Relative permeability> The noise suppression sheet 1 was cut into a doughnut shape with an outer diameter of 18 mm and an inner diameter of 5 mm to be used as a measurement sample. The measurement was performed using an impedance analyzer (Agilent Technologies, model number 4294A) and a test jig 16454A (Keysight Technologies). The measurement conditions were a measurement range of 1 kHz to 100 MHz, a sweep type of log, a signal source level of 0.5, and a measurement point of 401. The real part μ´ of the complex permeability was calculated from the obtained value. In the case of Comparative Example 3, which did not contain a magnetic filler, the magnetic permeability was 1.

[0077] <Average orientation angle> In the same manner as in measuring the thickness t of the noise suppression sheet 1, the cross section of the measurement sample was observed, and the interface between the noise suppression layer 1 and the polyimide film was used as the reference plane. The inclinations of any 20 magnetic fillers and any 20 conductive fillers in the noise suppression layer 1 relative to the reference plane were determined, and the average values ​​for each were calculated.

[0078] <Low frequency shielding> The noise suppression sheet 2 having a noise suppression layer 2 with a thickness of 300 μm was used to measure the shielding effect by the KEC method using a magnetic field antenna. Shielding performance at 500kHz ○: 15 dB or more. Very good results. △: 10 dB or more and less than 15 dB. Good result. ×: Less than 10 dB. Not practical. Shielding at 1MHz ○: 15 dB or more. Very good results. △: 10 dB or more and less than 15 dB. Good result. ×: Less than 10 dB. Not practical.

[0079] [Table 1]

[0080] As can be seen from Table 1, the sheet-like precursor for forming a noise suppression layer of the present invention, which contains 25 mass % or more of conductive filler, a magnetic filler, and a binder resin, has a volume resistivity of 1.0×10 -5 It is possible to form a noise suppression sheet having a noise suppression layer with a magnetic permeability of Ω·m or less, a relative magnetic permeability of μ´20 or more at 1 MHz, and an elongation rate of 10 to 600%. As a result, it was confirmed that the noise suppression sheet of the present invention has good conformability to the complex uneven shape of the housing of the noise source, and therefore has high suppression ability for low-frequency noise of 1 MHz or less. [Industrial Applicability]

[0081] The noise suppression sheet of the present invention can be used in general products that require noise suppression of 1 MHz or less. Noise of 1 MHz or less is generated, for example, by wireless communication devices installed in automobiles, and examples of such noise include AM / FM radio noise (522 kHz to 1.7 MHz), RFID for electronic tags and vehicle management (135 kHz), and smart keys (134 kHz). [Explanation of symbols]

[0082] 11, 11' Sheet-shaped substrate 12 Noise suppression layer 17 Noise suppression sheet 18 Adhesive layer 13 Polyimide film 14 Stainless steel plate

Claims

1. A noise suppression sheet having a sheet-like substrate and a noise suppression layer formed from a sheet-like precursor for forming a noise suppression layer, the sheet-like precursor for forming a noise suppression layer contains 25% by mass or more of a conductive filler, 20 to 65% by mass of a magnetic filler, and a binder resin; The magnetic filler is a flake-shaped FeSiAl-based soft magnetic particle having an average thickness of 1 to 3 μm, The conductive filler is flaky silver particles having an average thickness of 0.01 to 1.5 μm or flaky silver-coated copper particles having an average thickness of 0.01 to 1.5 μm, The binder resin is a thermosetting polyurethane urea resin having a mass average molecular weight of 25,000 to 180,000, The noise suppression layer has a volume resistivity of 1.0×10 -5 A noise suppression sheet having a relative magnetic permeability μ' of 20 or more at Ω·m or less and 1 MHz, and an elongation rate of 200 to 600%.

2. 2. The noise suppression sheet according to claim 1, wherein the conductive filler has an average particle size D50(a) of 4 to 20 μm.

3. 3. The noise suppression sheet according to claim 1, wherein the magnetic filler has an average particle size D50(b) of 20 to 70 μm.

4. 4. The noise suppression sheet according to claim 1, wherein the surface of the magnetic filler is coated with gold, silver, copper or nickel.

5. 5. The noise suppression sheet according to claim 2, wherein the ratio [(b) / (a)] of the average particle diameter D50(b) of the magnetic filler to the average particle diameter D50(a) of the conductive filler is 3 to 15.

6. 6. The noise suppression sheet according to claim 1, wherein the conductive filler and the magnetic filler have a tap density of 0.2 to 4.0 g / cm.

7. 7. The noise suppression sheet according to claim 6, wherein in the noise suppression layer, the magnetic filler has an average orientation angle of 10° or less, and the conductive filler has an average orientation angle of 10° to 40°.

8. A method for suppressing noise, comprising covering a noise source member with the noise suppression sheet according to claim 6 or 7.

Citation Information

Patent Citations

  • Magnetism suppression sheet and method of manufacturing the same

    JP2015220259A

  • Sealing film, method for sealing electronic component-mounted substrate, and electronic component-mounted substrate covered with sealing film

    JP2018060990A

  • Conductive composition for low frequency EMI shielding

    JP2019500742A

  • Electromagnetic wave absorption sheet

    WO2018084235A1