Rigid substrate and its manufacturing method, as well as supporting substrate for semiconductor and auxiliary plate for polishing pad
A rigid substrate with a photocurable adhesive layer and resin film layers addresses the issues of debris and rigidity in glass epoxy substrates, offering high rigidity and minimal warpage for semiconductor and polishing pad applications.
Patent Information
- Application Number
- JP2020150421
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-08
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-09-08
AI Technical Summary
Glass epoxy substrates generate cutting debris during processing, leading to contamination, while resin substrates without glass fibers lack the rigidity and flatness required for semiconductor applications and polishing pads.
A rigid substrate composed of a photocurable adhesive layer and resin film layers, with a thickness of 500 μm or more, and a storage modulus of 1.0×10^9 Pa, that suppresses cutting debris and warping, providing rigidity comparable to glass epoxy substrates.
The solution achieves high rigidity and minimal warpage, making it suitable for semiconductor substrates and polishing pads without generating cutting debris, and maintaining flatness.
Smart Images

Figure 0007552168000003 
Figure 0007552168000002 
Figure 0007552168000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a rigid substrate used, for example, in printed circuit boards or reinforcing plates for polishing pads, and more particularly to a rigid substrate usable as an alternative to glass epoxy substrates. [Background technology]
[0002] Glass epoxy substrates, which are made by impregnating glass fibers with epoxy resin and then heat-curing them, are highly rigid and do not easily warp even though they are thin. Therefore, they are widely used, for example, as support substrates in semiconductor packages, reinforcing plates for polishing pads, and processed products such as electrical and electronic components (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2010-209126 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, glass epoxy substrates have a problem in that glass fibers are easily scattered as cutting shavings during cutting, and the cutting shavings adhere to the substrate, causing contamination. For example, when a semiconductor substrate using a glass epoxy substrate is divided into individual pieces by dicing, or when a through hole is formed in a glass epoxy substrate for use as a reinforcing plate for a polishing pad, the scattered glass fiber cutting shavings adhere to the surface of a semiconductor wafer or a polishing pad, causing contamination.
[0005] On the other hand, if a resin substrate that does not contain glass fibers is used, the generation of cutting debris as described above is eliminated, but there is a problem that a single-layer resin substrate is unlikely to achieve the same rigidity as a glass epoxy substrate of the same thickness.
[0006] By the way, there is a method for increasing the rigidity of a laminate in which a pair of resin layers are bonded together via a cured layer of the photocurable adhesive by using a photocurable adhesive, in addition to the hardness of the resin layer, by using the hardness of the cured layer. However, when a resin substrate is produced by this method, there is a problem that when the photocurable adhesive is cured during the production process, the curing reaction proceeds rapidly, causing curing shrinkage, and causing a large warp in the entire resin substrate. Therefore, there is a problem that the resin substrate produced by the above method is not suitable for applications requiring high flatness, such as semiconductor substrates and polishing pads.
[0007] In addition, in the case of a resin substrate bonded via a cured product layer of a thermosetting adhesive or a pressure-sensitive adhesive layer not containing glass fibers, it is difficult to sufficiently increase the rigidity of the resin substrate compared to a cured product layer of a photocurable adhesive. In addition, in the process of heat-curing the thermosetting adhesive layer interposed between a pair of resin layers at a high temperature, the time required for curing is long and an excessive load is applied, so that the resin substrate is easily damaged.
[0008] The present invention has been made in consideration of the above-mentioned circumstances, and provides a rigid substrate having high rigidity comparable to that of a glass epoxy substrate, little warping, and less cutting debris during cutting, a method for manufacturing the same, and a support substrate for semiconductors and an auxiliary plate for polishing pads. [Means for solving the problem]
[0009] The present invention relates to an adhesive composition having at least an adhesive layer A1, a resin film layer B1 disposed on one main surface of the adhesive layer A1, and a resin film layer B2 disposed on the other main surface of the adhesive layer, the adhesive layer A1 having a total thickness of 500 μm or more, the adhesive layer A1 being formed of a cured product of an adhesive composition containing at least a photocurable resin having a polymerizable functional group other than a polymerizable unsaturated double bond, a thermoplastic resin having a polymerizable functional group other than a polymerizable unsaturated double bond, and a photopolymerization initiator, the adhesive layer A1 having a thickness of 100 μm or more, and a storage modulus (E') at 25° C. of the adhesive layer A1 measured at a frequency of 1.0 Hz. 25 ) is 1.0 × 10 9The present invention provides a rigid substrate having a surface tension of 50 Pa or more, and wherein the resin film layer B1 and the resin film layer B2 each have a thickness of 50 μm or more.
[0010] The present invention also relates to an adhesive composition having an adhesive layer A1, a resin film layer B1 disposed on one main surface of the adhesive layer A1, and a resin film layer B2 disposed on the other main surface of the adhesive layer, and an intermediate layer C and an adhesive layer A2 are disposed between the adhesive layer A1 and the resin film layer B2, in this order from the adhesive layer A1 side, and a total thickness of 500 μm or more, the adhesive layer A1 and the adhesive layer A2 are each formed of a cured product of an adhesive composition containing at least a photocurable resin having a polymerizable functional group other than a polymerizable unsaturated double bond, a thermoplastic resin having a polymerizable functional group other than a polymerizable unsaturated double bond, and a photopolymerization initiator, the adhesive layer A1 and the adhesive layer A2 each have a thickness of 50 μm or more, and the sum of the thicknesses of the adhesive layer A1 and the adhesive layer A2 is 100 μm, and the adhesive layer A1 and the adhesive layer A2 have a storage modulus (E') at 25° C. measured at a frequency of 1.0 Hz. 25 ) are 1.0×10 9 The present invention provides a rigid substrate having a surface tension of 50 Pa or more, and wherein the resin film layer B1 and the resin film layer B2 each have a thickness of 50 μm or more. Effect of the Invention
[0011] According to the present invention, it is possible to provide a rigid substrate having high rigidity, small warpage, and little generation of cutting swarf during cutting. In particular, the rigid substrate of the present invention has the same thickness and rigidity as a glass epoxy substrate, but has small warpage and little generation of cutting swarf during cutting, and is therefore particularly suitable as an alternative substrate to a glass epoxy substrate. [Brief description of the drawings]
[0012] [Figure 1] 1 is a schematic cross-sectional view showing an example of a rigid substrate of the present invention. [Diagram 2] 1 is a schematic cross-sectional view showing an example of a rigid substrate of the present invention. [Diagram 3]FIG. 2 is a schematic diagram illustrating a stiffness test method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The rigid substrate of the present invention is roughly divided into two aspects. A first embodiment of the rigid substrate of the present invention (hereinafter, may be referred to as a rigid substrate of the first embodiment) has at least an adhesive layer A1, a resin film layer B1 arranged on one main surface of the adhesive layer A1, and a resin film layer B2 arranged on the other main surface of the adhesive layer, and has a total thickness of 500 μm or more, the adhesive layer A1 is formed of a cured product of an adhesive composition containing at least a photocurable resin having a polymerizable functional group other than a polymerizable unsaturated double bond, a thermoplastic resin having a polymerizable functional group other than a polymerizable unsaturated double bond, and a photopolymerization initiator, the adhesive layer A1 has a thickness of 100 μm or more, and the adhesive layer A1 has a storage modulus (E') at 25° C. measured at a frequency of 1.0 Hz. 25 ) is 1.0 × 10 9 Pa or more, and the resin film layer B1 and the resin film layer B2 each have a thickness of 50 μm or more.
[0014] A second embodiment of the rigid substrate of the present invention (hereinafter, sometimes referred to as a rigid substrate of the second embodiment) has an adhesive layer A1, a resin film layer B1 arranged on one main surface of the adhesive layer A1, and a resin film layer B2 arranged on the other main surface of the adhesive layer, and has an intermediate layer C and an adhesive layer A2 in this order from the adhesive layer A1 side between the adhesive layer A1 and the resin film layer B2, and has a total thickness of 500 μm or more, and the adhesive layers A1 and A2 are each laminated. The adhesive composition is formed of a cured product of an adhesive composition containing at least a photocurable resin having a polymerizable functional group other than a polymerizable unsaturated double bond, a thermoplastic resin having a polymerizable functional group other than a polymerizable unsaturated double bond, and a photopolymerization initiator, the adhesive layer A1 and the adhesive layer A2 each have a thickness of 50 μm or more, and the sum of the thicknesses of the adhesive layer A1 and the adhesive layer A2 is 100 μm, and the storage modulus (E') at 25° C. measured at a frequency of 1.0 Hz of the adhesive layer A1 and the adhesive layer A2 is 1.0 μm or more. 25) are 1.0×10 9 Pa or more, and the resin film layer B1 and the resin film layer B2 each have a thickness of 50 μm or more.
[0015] In both the first and second aspects of the rigid substrate of the present invention, a pair of resin film layers B1 and B2 are bonded together via an adhesive layer formed of a cured product of a predetermined adhesive composition, and the total thickness of the rigid substrate and the thickness of the resin film, as well as the total thickness and storage modulus of the adhesive layer formed of the cured product of the predetermined adhesive composition, are each equal to or greater than a predetermined value, so that the rigid substrate can have a rigidity comparable to that of a glass epoxy substrate. In addition, since each component constituting the rigid substrate of the present invention does not contain glass fiber, the generation of cutting waste can be suppressed. Furthermore, since the adhesive layer is formed of a cured product of a predetermined adhesive composition, the occurrence of warping of the entire rigid substrate due to cure shrinkage is suppressed, so that the rigid substrate of the present invention can have small warping and high flatness.
[0016] In the present invention, a rigid substrate refers to a substrate that is not easily deformed even when subjected to bending or folding forces, and specifically refers to a substrate having a distance L measured by the rigidity test method described below of less than 45 mm. In particular, the distance L is preferably 25 mm or less, and more preferably 15 mm or less, because it can have the same rigidity as a glass epoxy substrate of the same thickness, and can have rigidity more suitable as a substitute for a glass epoxy substrate.
[0017] In the stiffness test method, first, an evaluation sample S having a rectangular surface with a length of 100 mm in the longitudinal direction X and a length of 20 mm in the lateral direction Y is cut out from the measurement object, and as illustrated in Fig. 3, a region of 10 mm in the longitudinal direction from one end A of a pair of ends A and B located in the longitudinal direction X of the evaluation sample S is fixed, and the position of the other end B of the evaluation sample S before the load is applied is set as a reference O. A load W of 5 g is applied to the end B of the evaluation sample S, and the position of the end B of the evaluation sample S in the vertical direction (load direction) Z after the end B is left to stand for 5 seconds is set as a position P, and the distance L from the reference O before the load to the position P of the end B of the evaluation sample after the load is measured.
[0018] The rigid substrate of the present invention will be described below for each embodiment. In the following description, the adhesive layer A1 in the first embodiment and the adhesive layers A1 and A2 in the second embodiment are collectively referred to as "adhesive layer" or "adhesive layer A", and the layer formed by the adhesive composition before curing may be referred to as the adhesive composition layer. The layer obtained by curing the adhesive composition layer corresponds to the adhesive layer in the rigid substrate of the present invention (i.e., the adhesive composition layer is a precursor of the adhesive layer before curing). In addition, the resin film layers B1 and B2 may be collectively referred to as "resin film layer" or "resin film layer B" in the description. Furthermore, the resin film layers B1, B2, the intermediate layer in the second embodiment, and other members directly bonded to the adhesive layer A1 and / or the adhesive layer A2 may be referred to as "adherend".
[0019] I. First embodiment of rigid board FIG. 1 is a schematic cross-sectional view showing an example of a rigid substrate of the first embodiment. The rigid substrate 10 of the first embodiment shown in FIG. 1 has at least an adhesive layer A1 (reference number 1 in FIG. 1), a resin film layer B1 (reference number 2 in FIG. 1) arranged on one main surface of the adhesive layer A1 (reference number 1 in FIG. 1), and a resin film layer B2 (reference number 3 in FIG. 1) arranged on the other main surface of the adhesive layer A1, and has a total thickness (reference number T in FIG. 1) of 500 μm or more. In addition, the adhesive layer A1 is formed of a cured product of an adhesive composition containing at least a photocurable resin having a polymerizable functional group other than a polymerizable unsaturated double bond, a thermoplastic resin having a polymerizable functional group other than a polymerizable unsaturated double bond, and a photopolymerization initiator, and the thickness of the adhesive layer A1 (reference number T in FIG. 1) is 500 μm or more. A1 ) is 100 μm or more, and the storage modulus (E') of the adhesive layer A1 at 25° C. measured at a frequency of 1.0 Hz is 25 ) is 1.0 × 10 9 In addition, the thickness of the resin film layer B1 and the resin film layer B2 (reference symbol T B1 and T B2 ) are each 50 μm or more.
[0020] The rigid substrate of the first embodiment has a structure in which a pair of resin films B1 and B2 are bonded via an adhesive layer A1 formed of a cured product of a predetermined adhesive composition, and the total thickness of the rigid substrate, the thickness of the resin films B1 and B2, the thickness of the adhesive layer A1, and the storage elastic modulus of the adhesive layer A1 are each equal to or greater than a predetermined value, so that the rigid substrate has a rigidity comparable to that of a glass epoxy substrate. By providing the above-mentioned characteristics, the rigid substrate of the present invention can be a substrate that is less likely to warp and less likely to produce cutting waste during cutting.
[0021] The rigid substrate of the first embodiment has a total thickness of 500 μm or more, so that it can exhibit rigidity sufficient to replace a glass epoxy substrate. In particular, the total thickness of the rigid substrate of the first embodiment is preferably 600 μm or more, more preferably 700 μm or more, and even more preferably 800 μm or more, in order to provide the rigid substrate with sufficient rigidity. Furthermore, the total thickness of the rigid substrate of the first embodiment is preferably 3000 μm or less, more preferably 2000 μm or less, and even more preferably 1500 μm or less, as this is within the appropriate thickness range for replacing general glass epoxy substrates and other rigid substrates.
[0022] Hereinafter, the rigid board of the first embodiment will be described with respect to each of its constituent members.
[0023] [1] Adhesive layer A1 The adhesive layer A1 in the rigid substrate of the first embodiment is a layer formed of a cured product of an adhesive composition containing at least a photocurable resin having a polymerizable functional group other than a polymerizable unsaturated double bond, a thermoplastic resin having a polymerizable functional group other than a polymerizable unsaturated double bond, and a photopolymerization initiator. The adhesive layer A1 has a thickness of 100 μm or more, and the storage modulus (E′) at 25° C. measured at a frequency of 1.0 Hz of the adhesive layer A1 is 100 μm or more. 25 ) is 1.0 × 10 9 Pa or more.
[0024] (1) Adhesive composition The adhesive composition includes at least a photocurable resin having a polymerizable functional group other than a polymerizable unsaturated double bond, a thermoplastic resin having a polymerizable functional group other than a polymerizable unsaturated double bond, and a photopolymerization initiator. The adhesive composition is cured by irradiation with active energy rays and has a storage modulus (E') at 25°C. 25 ) can form a cured product having a predetermined value or more.
[0025] Since the adhesive composition contains a predetermined composition, when the adhesive composition is irradiated with active energy rays, the polymerizable functional groups of the photocurable resin (A) and the thermoplastic resin (B) are activated, and curing begins in a state of enhanced reactivity. At this time, the polymerizable functional groups of the photocurable resin (A) and the thermoplastic resin (B) are polymerizable functional groups other than polymerizable unsaturated double bonds, so that unlike a radical polymerization reaction such as a photocurable adhesive containing a polymerizable compound having a polymerizable unsaturated double bond in the polymerizable functional group, a rapid curing reaction after irradiation with active energy rays is suppressed and the curing reaction proceeds gradually. That is, unlike a photocurable adhesive that causes a radical polymerization reaction, the adhesive composition is a delayed curing type adhesive composition. This makes it possible to suppress the occurrence of warping of the adhesive layer due to the curing shrinkage caused by the rapid curing reaction of the adhesive composition, and to obtain a rigid substrate with high flatness. Each component contained in the adhesive composition will be described below.
[0026] <Photocurable resin (A)> The adhesive composition contains a photocurable resin (A) having a polymerizable functional group other than a polymerizable unsaturated double bond. The photocurable resin (A) has a polymerizable functional group other than a polymerizable unsaturated double bond, which initiates polymerization by irradiation with active energy rays, and the polymerization proceeds even in a dark reaction or at a low temperature, so that the adhesive composition layer can be bonded to an adherend without being restricted by the light transmittance or heat resistance of the adherend.
[0027] The photocurable resin (A) may be any one having a polymerizable functional group other than a polymerizable unsaturated double bond, and may be a photopolymerizable compound having a polymerizable functional group other than a radically polymerizable unsaturated double bond. Among them, photocationically polymerizable compounds and / or photoanionically polymerizable compounds are preferred. In other words, it is preferred that the photocurable resin (A) has a photocationically polymerizable functional group and / or a photoanionically polymerizable functional group as a polymerizable functional group other than a polymerizable unsaturated double bond. Photopolymerizable compounds having a photocationically polymerizable functional group and / or a photoanionically polymerizable functional group are less susceptible to inhibition by oxygen when curing the adhesive composition layer, and the reaction is more likely to proceed continuously even after irradiation with active energy rays, so that the adherend and the adhesive layer can be bonded without being limited by the light transmittance or heat resistance of the adherend. In particular, photocationically polymerizable compounds are more preferred because they can form an adhesive layer that has excellent reactivity and high adhesion after irradiation with active energy rays. The photopolymerizable compound having a polymerizable functional group other than the above-mentioned polymerizable unsaturated double bond may be used alone or in combination of two or more kinds.
[0028] The photocationically polymerizable compound is not particularly limited as long as it has one or more photocationically polymerizable functional groups in one molecule. The photocationically polymerizable compound is preferably one having one or more photocationically polymerizable functional groups such as epoxy groups, oxetanyl groups, hydroxyl groups, vinyl ether groups, episulfide groups, ethyleneimine groups, and oxazoline groups in one molecule. Among them, the photocationically polymerizable compound is more preferably one having an epoxy group or an oxetanyl group in order to obtain high curability and bondability after curing.
[0029] As the photocationically polymerizable compound having an epoxy group, a compound having one or more epoxy groups in one molecule can be used. Specifically, bisphenol A type epoxy resin, bisphenol F type epoxy resin, biphenyl type epoxy resin, tetramethylbiphenyl type epoxy resin, polyhydroxynaphthalene type epoxy resin, isocyanate-modified epoxy resin, 10-(2,5-dihydroxyphenyl)-9,10-dihydro Examples of epoxy resins that can be used include 9-oxa-10-phosphaphenanthrene-10-oxide modified epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, hexanediol type epoxy resins, triphenylmethane type epoxy resins, tetraphenylethane type epoxy resins, dicyclopentadiene-phenol addition reaction type epoxy resins, phenol aralkyl type epoxy resins, naphthol novolac type epoxy resins, naphthol aralkyl type epoxy resins, naphthol-phenol co-condensed novolac type epoxy resins, naphthol-cresol co-condensed novolac type epoxy resins, aromatic hydrocarbon formaldehyde resin modified phenolic resin type epoxy resins, biphenyl modified novolac type epoxy resins, trimethylolpropane type epoxy resins, alicyclic epoxy resins, acrylic resins having epoxy groups, polyurethane resins having epoxy groups, polyester resins having epoxy groups, and flexible epoxy resins.
[0030] Among them, it is preferable to use at least one of an alicyclic epoxy resin and a polyfunctional aliphatic epoxy resin, and it is more preferable to use an alicyclic epoxy resin, which has excellent photocationic polymerization properties and therefore excellent curing properties, and by curing the adhesive composition, an adhesive layer having high rigidity and small warping and dimensional deformation can be obtained.
[0031] Furthermore, the epoxy resin may be a modified one. Examples of the modified one include CTBN (terminal carboxyl group-containing butadiene-acrylonitrile rubber) modified epoxy resins; epoxy resins in which various rubbers such as acrylic rubber, NBR, SBR, butyl rubber, or isoprene rubber are dispersed in the resin; epoxy resins modified with the above-mentioned liquid rubbers; epoxy resins to which various resins such as acrylic, urethane, urea, polyester, and styrene are added; chelate-modified epoxy resins; and polyol-modified epoxy resins. By including a modified epoxy resin, the adhesive strength of the adhesive layer can be improved, and the flexibility of the adhesive composition layer can also be improved.
[0032] On the other hand, examples of the photocationically polymerizable compound having an oxetanyl group include oxetane compounds such as 1,4-bis[(3-ethyl-3-oxetanylmethoxy)methyl]benzene, 1,4-bis[(3-methyl-3-oxetanylmethoxy)methyl]benzene, 3-methyl-3-glycidyloxetane, 3-ethyl-3-glycidyloxetane, 3-methyl-3-hydroxymethyloxetane, 3-ethyl-3-hydroxymethyloxetane, and di{1-ethyl(3-oxetanyl)}methyl ether.
[0033] The adhesive composition preferably uses, as the photocurable resin (A), a photocurable resin (a1) having a temperature (Tg-tan δ) at which the loss tangent after curing is at a maximum value of 100° C. or more. This is because the heat cycle resistance of the adhesive layer, which is the cured product of the adhesive composition, is improved, and warping and deformation can be suppressed. In particular, the photocurable resin (a1) preferably has a temperature at which the loss tangent after curing is at a maximum value of 105° C. or more, 110° C. or more, or 115° C. or more, and the temperature is preferably 250° C. or less, more preferably 230° C. or less, or 200° C. or less. The temperature (Tg-tan δ) at which the loss tangent after curing of the photocurable resin (a1) is at a maximum value is a value measured at a frequency of 1.0 Hz using a dynamic viscoelasticity measuring device (manufactured by Rheometrics, product name: RSA-II) for a cured product obtained by curing an epoxy resin alone.
[0034] Examples of the photocurable resin (a1) having a temperature (Tg-tan δ) of 100° C. or higher at which the loss tangent after curing is at a maximum value include epoxy resins that are solid at room temperature (hereinafter referred to as room temperature solid epoxy resins). Here, room temperature refers to 25° C.
[0035] Specific examples of room temperature solid epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, biphenyl type epoxy resins, tetramethylbiphenyl type epoxy resins, polyhydroxynaphthalene type epoxy resins, isocyanate modified epoxy resins, 10-(2,5-dihydroxyphenyl)-9,10-dihydro 9-oxa-10-phosphaphenanthrene-10-oxide modified epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, hexanediol type epoxy resins, triphenylmethane type epoxy resins, tetraphenylethane type epoxy resins, dicyclopentadiene-phenol addition reaction type epoxy resins, phenol aralkyl type epoxy resins, naphthol novolac type epoxy resins, naphthol aralkyl type epoxy resins, naphthol-phenol co-condensed novolac type epoxy resins, naphthol-cresol co-condensed novolac type epoxy resins, aromatic hydrocarbon formaldehyde resin modified phenol resin type epoxy resins, biphenyl modified novolac type epoxy resins, and the like.
[0036] The adhesive composition preferably contains at least one or more epoxy resins that are solid at room temperature as the photocurable resin (A), and more preferably contains one or more epoxy resins that are solid at room temperature and one or more epoxy resins that are liquid at room temperature (hereinafter referred to as room temperature liquid epoxy resins). By using a combination of an epoxy resin that is solid at room temperature and an epoxy resin that is liquid at room temperature as the photocurable resin (A), the adhesive composition layer is more likely to exhibit appropriate adhesion for a certain period of time before and after irradiation with active energy rays when curing the adhesive composition layer, and can be easily attached to an adherend.
[0037] Specific examples of room temperature liquid epoxy resins include trimethylolpropane type epoxy resins, alicyclic epoxy resins, acrylic resins having epoxy groups, polyurethane resins having epoxy groups, and polyester resins having epoxy groups.
[0038] When the photocurable resin (A) is an epoxy resin, the ratio of the epoxy resin solid at room temperature to the total amount of epoxy resin is preferably within the range of 20% by mass to 80% by mass, more preferably within the range of 30% by mass to 70% by mass, more preferably within the range of 35% by mass to 65% by mass, and even more preferably within the range of 40% by mass to 65% by mass. By setting the ratio of the epoxy resin solid at room temperature to the total amount of epoxy resin within the above range, an adhesive layer with high heat resistance can be obtained, and the curing reaction of the adhesive composition can be completed in a relatively short time. The ratio of the epoxy resin solid at room temperature to the total amount of epoxy resin can be calculated by the following formula.
[0039] Proportion of epoxy resin that is solid at room temperature in the total amount of epoxy resin = {Content of epoxy resin that is solid at room temperature [parts by mass] / (Content of epoxy resin that is solid at room temperature [parts by mass] + Epoxy resin that is liquid at room temperature [parts by mass])} x 100 [mass %]
[0040] The content of the photocurable resin (A) is preferably within the range of 10% by mass to 84% by mass, preferably within the range of 20% by mass to 70% by mass, preferably within the range of 25% by mass to 65% by mass, preferably within the range of 30% by mass to 60% by mass, and preferably within the range of 30% by mass to 50% by mass. By setting the content of the photocurable resin (A) within the above range, it is possible to obtain an adhesive layer that has high adhesion to the adherend and is firmly bonded to the adherend. If the content of the photocurable resin (A) is more than the above range, the adhesive composition layer and the adhesive layer may have poor shape retention, and if it is less than the above range, the heat resistance of the adhesive layer may be reduced.
[0041] The photocurable resin (A) preferably has a weight average molecular weight in the range of 100 to 5000, more preferably in the range of 150 to 3000, and even more preferably in the range of 200 to 2500. This is because the shape retention and follow-up adhesion of the adhesive composition layer and the adhesive layer to the adherend surface can be improved. If the weight average molecular weight of the photocurable resin (A) is too small, the cohesive force may be insufficient, and the adhesive composition may bleed over time, which may lead to poor handling. On the other hand, if the weight average molecular weight of the photocurable resin (A) is too large, the compatibility with the thermoplastic resin (B) may decrease, making it difficult for the reaction to proceed.
[0042] The weight average molecular weight of the photocurable resin (A) is a value measured under the following conditions by gel permeation chromatography (GPC) in terms of polystyrene. (conditions) Resin sample solution: 0.4% by mass in tetrahydrofuran (THF) solution Measuring device model: HLC-8220GPC (manufactured by Tosoh Corporation) Column: TSKgel (Tosoh Corporation) Eluent: Tetrahydrofuran (THF)
[0043] <Thermoplastic resin (B)> The adhesive composition contains a thermoplastic resin (B) having a polymerizable functional group other than a polymerizable unsaturated double bond, which allows the adhesive composition to react with the photocurable resin (A), suppressing a rapid curing reaction after irradiation with active energy rays and allowing the curing reaction to proceed gradually, thereby forming an adhesive layer with little warping or deformation.
[0044] The content of the thermoplastic resin (B) is preferably within a range of 15% by mass to 50% by mass, more preferably within a range of 25% by mass to 50% by mass, even more preferably within a range of 25% by mass to 45% by mass, even more preferably within a range of 30% by mass to 45% by mass, and particularly preferably within a range of 34% by mass to 45% by mass, based on the total solid content of the adhesive composition. This is because an adhesive layer having high shape retention and heat resistance and high adhesion and conformability to the adherend is obtained.
[0045] Furthermore, the ratio of the content of the thermoplastic resin (B) to the total content of the photocurable resin (A) and the thermoplastic resin (B) is preferably within the range of 25% to 68% by mass, more preferably within the range of 25% to 60% by mass, 30% to 60% by mass, 30% to 55% by mass, 30% to 50% by mass, or 35% to 50% by mass, because this results in an adhesive layer with high adhesion to the adherend.
[0046] The proportion of the content of the thermoplastic resin (B) in the total content of the photocurable resin (A) and the thermoplastic resin (B) can be calculated by the following formula.
[0047] The ratio of the content of thermoplastic resin (B) to the total content of photocurable resin (A) and thermoplastic resin (B) = {content of thermoplastic resin (B) [parts by mass] / (content of thermoplastic resin (A) [parts by mass] + content of thermoplastic resin (B) [parts by mass])} x 100 [% by mass]
[0048] The thermoplastic resin (B) preferably has at least one group selected from the group consisting of an isocyanate group, a hydroxyl group, an oxetanyl group, and an epoxy group as a polymerizable functional group other than the polymerizable unsaturated double bond. By using the thermoplastic resin (B) having at least one polymerizable functional group selected from the above group, it becomes possible to react with the photocurable resin (A) and suppress a rapid curing reaction after irradiation with active energy rays, and it becomes possible to gradually progress the curing reaction, so that an adhesive layer with little warping or deformation can be formed.
[0049] Examples of the thermoplastic resin (B) include polyester resin, polyurethane resin, acrylic resin, polyvinyl acetal resin, and epoxy resin (thermoplastic epoxy resin), each of which has a polymerizable functional group other than a polymerizable unsaturated double bond. These thermoplastic resins may be homopolymers or copolymers. These thermoplastic resins may be used alone or in combination of two or more.
[0050] Among them, the adhesive composition preferably contains, as the thermoplastic resin (B), one or more resins selected from the group consisting of polyurethane resins, acrylic resins, and epoxy resins, each having a polymerizable functional group other than a polymerizable unsaturated double bond, and more preferably contains at least one or more polyurethane resins having a polymerizable functional group other than a polymerizable unsaturated double bond. By using a polyurethane resin having a polymerizable functional group other than a polymerizable unsaturated double bond as the thermoplastic resin (B), the rapid curing reaction of the adhesive composition after irradiation with active energy rays is suppressed, so that the curing reaction can be allowed to proceed gradually, and an adhesive layer with little warping or deformation can be formed.
[0051] In addition, the polyurethane resin having a polymerizable functional group other than a polymerizable unsaturated double bond is preferably crystalline, because the adhesive composition contains a crystalline polyurethane resin having a polymerizable functional group other than a polymerizable unsaturated double bond, which makes it easier to maintain the adhesive composition layer in a sheet shape, resulting in an adhesive layer with excellent shape retention.
[0052] The polyurethane resin having a polymerizable functional group other than a polymerizable unsaturated double bond is preferably a polyurethane resin (B') having at least one selected from the group consisting of an isocyanate group, a hydroxyl group, an oxetanyl group, and an epoxy group, and among these, a polyurethane resin (B') having a hydroxyl group is preferred.
[0053] As the polyurethane resin (B') having an isocyanate group, for example, a polyurethane resin (B'1) having an isocyanate group obtained by reacting a polyol (b'1) with a polyisocyanate (b'2) can be used. As the polyurethane resin (B') having a hydroxyl group, for example, a polyurethane resin (B'2) having a hydroxyl group obtained by reacting a polyol (b'1) with a polyisocyanate (b'2) can be used.
[0054] The polyol (b'1) preferably has a number average molecular weight in the range of 500 to 5000, and more preferably has a number average molecular weight in the range of 1000 to 3000 in order to obtain an adhesive layer excellent in shape retention, coating workability, initial cohesive strength, etc. The number average molecular weight is a value measured under the following conditions.
[0055] The number average molecular weight was measured by gel permeation chromatography (GPC) using polystyrene standards under the following conditions. (conditions) Resin sample solution: 0.4% by mass in tetrahydrofuran (THF) solution Measuring device model: HLC-8220GPC (manufactured by Tosoh Corporation) Column: TSKgel (Tosoh Corporation) Eluent: Tetrahydrofuran (THF)
[0056] As such a polyol (b'1), for example, at least one member selected from the group consisting of polyester polyols, polycarbonate polyols, and polyether polyols can be suitably used.
[0057] Among them, it is preferable to use one or more polyols selected from the group consisting of polyester polyols and polycarbonate polyols as the polyol (b'1), it is preferable to use at least one or more polyester polyols, and it is preferable to use one or more polyester polyols and one or more polycarbonate polyols. This is because the adhesive composition layer has high shape stability and improved follow-up adhesion to the adherend surface, resulting in an adhesive layer with excellent shape retention and follow-up adhesion to the adherend.
[0058] The total amount of polyols selected from the group consisting of polycarbonate polyols and polyester polyols used as polyol (b'1) is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, and more preferably 50 parts by mass or more, based on 100 parts by mass of the polyol (b'1). This is because the conformability and adhesion to the adherend surface can be further improved. In addition, the adhesive composition layer exhibits a level of adhesion that allows attachment at room temperature, so that the rigid substrate of the present invention can be easily manufactured.
[0059] When the polycarbonate polyol and the polyester polyol are used in combination as the polyol (b'1), the mass ratio of the polycarbonate polyol and the polyester polyol (polycarbonate polyol / polyester polyol) is preferably in the range of 0.4 to 7.0, and more preferably in the range of 1.0 to 2.0. This is because a polyurethane resin having a loss tangent value within a desired range can be obtained. In addition, the adhesive layer has high conformability to the adherend surface, and the adhesive composition layer has good handleability when forming the adhesive layer.
[0060] As the polyester polyol, for example, those obtained by an esterification reaction between polyol (b'1a) and polycarboxylic acid, polyesters obtained by a ring-opening polymerization reaction of a cyclic ester compound such as ε-caprolactone, and copolymer polyesters thereof can be used.
[0061] Examples of the polyol (b'1a) that can be used to prepare the above polyester polyol include low molecular weight polyols. Specifically, aliphatic alkylene glycols such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, diethylene glycol, neopentyl glycol, and 1,3-butanediol, each having a molecular weight of about 50 to 300, and cyclohexanedimethanol can be used.
[0062] In addition, examples of the polyol (b'1a) that can be used to prepare the polyester polyol include aromatic polyols. By using an aromatic polyol, the rigidity of the polyurethane resin (B') can be improved, and it is possible to suppress the bonding displacement and deformation of the adhesive layer over time. Specific examples of aromatic polyols include hydroquinone, resorcinol, dihydroxyphenyl, naphthalenediol, dihydroxydiphenyl ether, bisphenol F, bisphenol A, adducts of bisphenol A with alkylene oxides such as ethylene oxide and propylene oxide (diethoxylated bisphenol A, etc.), p-xylylene glycol, m-xylylene glycol, o-xylylene glycol, 4,4'-bishydroxymethylbiphenyl, 4,2'-bishydroxymethylbiphenyl, 2,2'-bishydroxymethylbiphenyl, 4,3'-bishydroxymethylbiphenyl, 3,3'-bishydroxymethylbiphenyl, 3,2'-bishydroxymethylbiphenyl, phenol novolac, cresol novolac, 1,4-benzenedimethanol, 1,3-benzenedimethanol, 1,2-benzenedimethanol, 4,4'-naphthalenedimethanol, 3,4'-naphthalenedimethanol, and modified compounds thereof.
[0063] Examples of the polycarboxylic acid that can be used in the preparation of the polyester polyol include aliphatic dicarboxylic acids such as succinic acid, adipic acid, sebacic acid, and dodecanedicarboxylic acid; aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, and naphthalenedicarboxylic acid; and anhydrides or esters thereof.
[0064] The polyester polyol is preferably one or more selected from the group consisting of aromatic polyester polyols and aliphatic polyester polyols, and preferably contains both an aromatic polyester polyol and an aliphatic polyester polyol.
[0065] Among the aliphatic polyester polyols, linear aliphatic polyester polyols are preferred. This is because a polyurethane resin (B') having a loss tangent value within a desired range can be obtained, and an adhesive layer having higher conformability and adhesion to the adherend surface can be formed. In addition, the adhesive composition layer has good handleability when forming the adhesive layer. The linear aliphatic polyester polyol refers to a polyester polyol having no alkyl group in the side chain.
[0066] Examples of the aliphatic polyester polyol include those obtained by reacting the aliphatic alkylene glycol with an aliphatic dicarboxylic acid. For example, it is preferable to use an aliphatic polyester polyol obtained by an esterification reaction of 1,6-hexanediol with adipic acid, or an aliphatic polyester polyol obtained by reacting 1,6-hexanediol with dodecanedioic acid.
[0067] In addition, it is preferable to use an aromatic polyester polyol as the polyester polyol. This is because it can improve the rigidity of the polyurethane resin (B') and can suppress the bonding displacement, warping, and deformation of the adhesive layer over time. The aromatic polyester polyol can be obtained by reacting the above-mentioned aromatic polyol with an aliphatic or aromatic dicarboxylic acid, and for example, an aromatic polyester polyol obtained by reacting an ethylene oxide adduct of bisphenol A with phthalic acid and adipic acid is preferably used.
[0068] The polyester polyol preferably has a number average molecular weight in the range of 1000 to 5000. This is because a polyurethane resin (B') having a loss tangent value within the desired range can be obtained, the adhesive layer has high conformability to the adherend surface, and the adhesive composition layer has good handleability when the adhesive layer is formed.
[0069] In particular, when a polyester polyol obtained by reacting an aliphatic diol such as 1,2-ethanediol or 1,4-butanediol with adipic acid is used as the polyester polyol, it is preferable to use one having a number average molecular weight in the range of 1100 to 2900. When a polyester polyol obtained by reacting 1,6-hexanediol with adipic acid is used, it is preferable to use one having a number average molecular weight in the range of 1100 to 5000. When a polyester polyol obtained by reacting 1,6-hexanediol with sebacic acid is used, it is preferable to use one having a number average molecular weight in the range of 1000 to 5000.
[0070] The polyester polyol is preferably used in the range of 10% by mass to 50% by mass, and more preferably 20% by mass to 40% by mass, based on the total amount of the polyol (b'1), because this increases the conformability of the adhesive layer to the adherend surface and allows the adhesive composition layer to maintain a level of adhesion that allows application at room temperature.
[0071] The polycarbonate polyol may be, for example, one obtained by reacting a carbonate ester and / or phosgene with a low molecular weight polyol. As the carbonate ester, for example, methyl carbonate, dimethyl carbonate, ethyl carbonate, diethyl carbonate, cyclocarbonate, diphenyl carbonate, etc. may be used.
[0072] Examples of low molecular weight polyols that can react with the above carbonate esters and phosgene include ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, 1,2-propanediol, 1,3-propanediol, dipropylene glycol, tripropylene glycol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 1,5-pentanediol, 1,5-hexanediol, 1,6-hexanediol, 2,5-hexanediol, 1,7-heptanediol, 1,8- Octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 2-methyl-1,3-propanediol, neopentyl glycol, 2-butyl-2-ethyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 2-ethyl-1,3-hexanediol, 2-methyl-1,8-octanediol, 1,4-cyclohexanedimethanol, hydroquinone, resorcinol, bisphenol A, bisphenol F, 4,4'-biphenol, and the like can be used.
[0073] As the polycarbonate polyol, it is preferable to use an aliphatic polycarbonate polyol or an alicyclic polycarbonate polyol.
[0074] As the aliphatic polycarbonate polyol, it is preferable to use one obtained by reacting a dialkyl carbonate with one or more polyols selected from the group consisting of 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, and 1,6-hexanediol, because the adhesive composition layer containing the polyurethane resin (B') can have adhesion that allows application at room temperature.
[0075] As the alicyclic polycarbonate polyol, it is preferable to use one obtained by reacting, for example, a dialkyl carbonate with a polyol containing one or more selected from the group consisting of cyclohexanedimethanol and its derivatives, because the adhesive composition layer containing the polyurethane resin (B') can have adhesion that allows application at room temperature and excellent initial cohesion.
[0076] The polycarbonate polyol preferably has a number average molecular weight in the range of 500 to 5000, and more preferably in the range of 800 to 3000. This is because a polyurethane resin (B') having a loss tangent value within a desired range can be obtained, the adhesive layer has high conformability to the adherend surface, and the adhesive composition layer has good handleability when forming the adhesive layer.
[0077] The polycarbonate polyol is preferably used in the range of 20% by mass to 80% by mass, more preferably 30% by mass to 70% by mass, and more preferably 40% by mass to 50% by mass, based on the total amount of the polyol (b'1). This is because the adhesive composition layer containing the polyurethane resin (B') can exhibit adhesion that allows attachment at room temperature, and the adhesive layer has improved conformability to the adherend surface.
[0078] Examples of polyether polyols include those obtained by addition polymerization of alkylene oxide using one or more compounds having two or more active hydrogen atoms as an initiator.
[0079] Examples of the initiator that can be used include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, trimethylene glycol, 1,3-butanediol, 1,4-butanediol, 1,6-hexanediol, bisphenol A, glycerin, trimethylolethane, and trimethylolpropane.
[0080] As the alkylene oxide, for example, ethylene oxide, propylene oxide, butylene oxide, styrene oxide, epichlorohydrin, tetrahydrofuran, etc. can be used.
[0081] As the polyether polyol, it is preferable to use an aliphatic polyether polyol or a polyether polyol having an alicyclic structure.
[0082] As the polyether polyol, polytetramethylene glycol obtained by ring-opening polymerization of tetrahydrofuran, polytetramethylene glycol derivative obtained by reacting tetrahydrofuran with alkyl-substituted tetrahydrofuran, polytetramethylene glycol derivative obtained by copolymerizing neopentyl glycol with tetrahydrofuran, etc. can be used. Among them, as the polyether polyol, it is preferable to use polytetramethylene glycol (PTMG) and polytetramethylene glycol derivative (PTXG). This is because the adhesive composition layer can exhibit adhesion at room temperature and the physical properties such as durability of the adhesive layer can be improved.
[0083] In addition to the above, other polyols may be used as the polyol (b'1). Examples of the other polyols include acrylic polyols.
[0084] As the polyisocyanate (b'2) to be reacted with the polyol (b'1), an alicyclic polyisocyanate, an aliphatic polyisocyanate, an aromatic polyisocyanate, etc. can be used, and it is preferable to use an alicyclic polyisocyanate.
[0085] Examples of the alicyclic polyisocyanate include isophorone diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, 4,4'-dicyclohexylmethane diisocyanate, 2,4- and / or 2,6-methylcyclohexane diisocyanate, cyclohexylene diisocyanate, methylcyclohexylene diisocyanate, bis(2-isocyanatoethyl)-4-cyclohexylene-1,2-dicarboxylate, and 2,5- and / or 2,6-norbornane diisocyanate, dimer acid diisocyanate, and bicycloheptane triisocyanate, which may be used alone or in combination of two or more.
[0086] Among the above-mentioned alicyclic polyisocyanates, it is preferable to use 4,4'-dicyclohexylmethane diisocyanate (HMDI), isophorone diisocyanate (IPDI), and 1,3-bis(isocyanatomethyl)cyclohexane (BICH), because these isocyanates have good reactivity with the above-mentioned polyol (b'1), and can form an adhesive layer having excellent heat resistance and the like by curing the adhesive composition containing the polyurethane resin (B').
[0087] As a method for preparing the polyurethane resin (B') by reacting the polyol (b'1) with the polyisocyanate (b'2), for example, the polyol (b'1) charged in a reaction vessel is heated under normal or reduced pressure conditions to remove moisture, and then the polyisocyanate (b'2) is supplied all at once or in portions and reacted.
[0088] The reaction of the polyol (b'1) with the polyisocyanate (b'2) is preferably carried out in such a manner that the equivalent ratio of the isocyanate groups in the polyisocyanate (b'2) to the hydroxyl groups in the polyol (b'1) (referred to as the [NCO / OH equivalent ratio]) is in the range of 1.1 to 20.0, more preferably in the range of 1.1 to 13.0, even more preferably in the range of 1.1 to 5.0, and particularly preferably in the range of 1.5 to 3.0.
[0089] The reaction conditions (temperature, time, etc.) between the polyol (b'1) and the polyisocyanate (b'2) may be appropriately set taking into consideration various conditions such as safety, quality, and cost, and are not particularly limited. For example, the reaction temperature is preferably in the range of 70 to 120°C, and the reaction time is preferably in the range of 30 minutes to 5 hours.
[0090] When reacting the polyol (b'1) with the polyisocyanate (b'2), a catalyst such as a tertiary amine catalyst or an organometallic catalyst may be used as necessary.
[0091] The reaction may be carried out in a solvent-free environment or in the presence of an organic solvent. The organic solvent may be, for example, an ester solvent such as methyl acetate, ethyl acetate, propyl acetate, or butyl acetate; a ketone solvent such as acetone, methyl ethyl ketone, methyl butyl ketone, or cyclohexanone; an ether ester solvent such as methyl cellosolve acetate or butyl cellosolve acetate; an aromatic hydrocarbon solvent such as toluene or xylene; or an amide solvent such as dimethylformamide or dimethylacetamide, either alone or in combination. The organic solvent may be removed during or after the production of the polyurethane resin (B') by a suitable method such as heating under reduced pressure or drying at normal pressure.
[0092] Examples of the polyurethane resin (B') having an oxetanyl group or an epoxy group include 1) a polyurethane (B'1) having an isocyanate group; 2) a monomer (B") having a functional group (b"1) capable of reacting with an isocyanate group, an oxetanyl group or an epoxy group, and a polymerizable functional group (b"2) other than one or more polymerizable unsaturated double bonds; It is possible to use a polyurethane resin (B'3) obtained by reacting the following:
[0093] As the functional group (b''1) capable of reacting with the isocyanate group, for example, a hydroxyl group, an amino group, a carboxyl group, a mercapto group, etc. can be used, and among these, it is preferable to use a hydroxyl group or an amino group.
[0094] The polymerizable functional group (b''2) other than the above-mentioned polymerizable unsaturated double bond refers to a functional group other than a so-called radically polymerizable functional group, such as a functional group having cationic polymerizability or a functional group having anionic polymerizability, and examples of such a functional group include an epoxy group, an oxetanyl group, and an ethylene sulfide group.
[0095] The monomer (B″) is not particularly limited as long as it has a functional group (b″1) and a polymerizable functional group (b″2), and examples thereof include 3-ethyl-3-(4-hydroxybutyl)oxymethyl-oxetane, 3-hydroxymethyl-3-ethyloxetane, 2-hydroxymethyloxetane, and 3-hydroxyoxetane.
[0096] The monomer (B") is preferably used in an amount of 5 to 20 parts by mass, and more preferably 5 to 15 parts by mass, per 100 parts by mass of the polyurethane resin (B'1).
[0097] More specifically, the monomer (B") can be used in an amount capable of supplying functional groups reactive with the isocyanate groups, preferably more than 50 mol % and not more than 100 mol %, more preferably 60 mol % to 100 mol %, and even more preferably 80 mol % to 100 mol %, based on the number of moles of isocyanate groups in the polyurethane resin (B'1). This makes it possible to obtain a polyurethane resin that is excellent in shape retention, mechanical strength, durability (particularly hydrolysis resistance), conformability to the adherend surface, and the like.
[0098] When reacting the polyurethane resin (B'1) with the monomer (B"), a urethanization catalyst can be used as necessary. The urethanization catalyst can be added as appropriate at any stage of the urethanization reaction. The urethanization reaction is preferably carried out until the isocyanate group content (%) becomes substantially constant. As the urethanization catalyst, for example, nitrogen-containing compounds such as triethylamine, triethylenediamine, N-methylmorpholine, etc.; organic metal salts such as potassium acetate, zinc stearate, stannous octoate, etc.; and organic metal compounds such as dibutyltin dilaurate, etc. can be used.
[0099] In addition, as the thermoplastic epoxy resin having a polymerizable functional group other than a polymerizable unsaturated double bond, a polymer or copolymer of epoxy compounds having a straight-chain structure, or a copolymer of an epoxy compound and a monomer polymerizable with this epoxy compound having a straight-chain structure may be used.Specific examples include bisphenol A type epoxy resin, bisphenol fluorene type epoxy resin, cresol novolac type epoxy resin, phenol novolac type epoxy resin, cyclic aliphatic type epoxy resin, long-chain aliphatic type epoxy resin, glycidyl ester type epoxy resin, and glycidyl amine type epoxy resin, among which bisphenol A type epoxy resin and bisphenol fluorene type epoxy resin are preferred.
[0100] The adhesive composition preferably contains, as the thermoplastic resin (B), a polyester urethane resin having a hydroxyl group, which is a reaction product of a polyol including a polyester polyol and a polyisocyanate. This is because delayed curing properties can be exhibited. In addition, the polyester urethane resin having a hydroxyl group is preferably a crystalline polyester urethane resin having a hydroxyl group, in terms of excellent delayed curing properties and sheet shape retention.
[0101] Whether the polyurethane or polyester urethane contained in the adhesive composition is crystalline can be confirmed by detecting the melting point as a peak in DSC measurement (differential scanning calorimetry).
[0102] The above thermoplastic resin (B) has a loss tangent (tanδ) at a frequency of 1.0 Hz and a temperature of 40°C before curing. 40 ) is preferably 3 or less, more preferably 0.001 to 2.0, even more preferably 0.001 to 1.0, and even more preferably 0.001 to 0.9. By setting the loss tangent at a frequency of 1.0 Hz and a temperature of 40°C before curing of the thermoplastic resin (B) within the above range, it is possible to suppress changes in the thickness and shape of the adhesive layer.
[0103] In addition, the thermoplastic resin (B) has a loss tangent (tanδ) at a frequency of 1.0 Hz and a temperature of 60° C. before curing. 60 ) is preferably 1 or more, more preferably 1.2 to 20, further preferably 1.3 to 15, and even more preferably 1.5 to 15. By setting the loss tangent of the thermoplastic resin (B) at a frequency of 1.0 Hz and a temperature of 60°C within the above range, excellent conformability to the adherend is achieved.
[0104] The loss tangent of the thermoplastic resin (B) at each temperature (40°C, 60°C) at a frequency of 1.0 Hz is determined by molding the thermoplastic resin (B) before curing to a thickness of 1 mm, molding and cutting into a circle having a diameter of 8 mm to prepare a test piece, and using a dynamic viscoelasticity tester (manufactured by Rheometrics, Inc., product name: Ares 2KSTD), sandwiching the test piece between parallel disks, which are the measurement section of the tester, and measuring the storage modulus (G') and loss modulus (G") at each temperature at a frequency of 1.0 Hz, and dividing the loss modulus (G") by the storage modulus (G') to give a value (G" / G').
[0105] The loss tangent (tan δ) of the thermoplastic resin (B) at each temperature can be adjusted, for example, when a urethane resin is used as the thermoplastic resin (B), by appropriately selecting the composition of the polyol and polyisocyanate constituting the urethane resin, the number average molecular weight thereof, and the like.
[0106] The melting point of the thermoplastic resin (B) is preferably in the range of 30° C. to 120° C., more preferably in the range of 35° C. to 100° C., and more preferably in the range of 40° C. to 80° C. By using a thermoplastic resin (B) having a melting point within the above range, the conformability of the adhesive layer to the adherend can be improved, and the shape of the adhesive composition layer becomes more stable, improving handleability.
[0107] The melting point of the thermoplastic resin (B) refers to the temperature at which the maximum exothermic peak (exothermic peak top) is observed when the temperature is increased from 20°C to 150°C at a heating rate of 10°C / min using differential scanning calorimetry (DSC), held for 1 minute, cooled to -10°C at a cooling rate of 10°C / min, held for 10 minutes, and then measured again at a heating rate of 10°C / min.
[0108] The weight average molecular weight of the thermoplastic resin (B) is preferably within the range of 5500 to 2000000, more preferably within the range of 5500 to 1000000, and more preferably within the range of 5500 to 800000. By setting the weight average molecular weight of the thermoplastic resin (B) within the above range, the adhesive layer can have high conformal adhesion to the adherend. In addition, the shape of the adhesive composition layer becomes more stable, improving the handleability. If the weight average molecular weight of the thermoplastic resin (B) is too small, the adhesive composition may have insufficient cohesive force, resulting in poor handleability, such as bleeding. On the other hand, if the weight average molecular weight of the thermoplastic resin (B) is too large, the compatibility with the photocurable resin (A) may decrease, making it difficult to proceed with the reaction.
[0109] The weight average molecular weight was measured by gel permeation chromatography (GPC) using polystyrene standards under the following conditions. (conditions) Resin sample solution: 0.4% by mass in tetrahydrofuran (THF) solution Measuring device model: HLC-8220GPC (manufactured by Tosoh Corporation) Column: TSKgel (Tosoh Corporation) Eluent: Tetrahydrofuran (THF)
[0110] <Photopolymerization initiator (C)> The adhesive composition contains one or more photopolymerization initiators (C), which promotes the reaction after irradiation with active energy rays and improves the bonding strength of the adhesive layer. In addition, the adhesive composition contains a photopolymerization initiator (C) that is activated by light and whose reaction proceeds, so that the reaction continues to proceed even after the irradiation with active energy rays is stopped, and therefore a good delayed curing reaction can be obtained, and the occurrence of warping or deformation of the adhesive layer due to a rapid curing reaction can be suppressed.
[0111] The photopolymerization initiator (C) is not particularly limited as long as it is activated by light. The photopolymerization initiator (C) can be, for example, a photoradical polymerization initiator, a photocationic polymerization initiator, or a photoanionic polymerization initiator. Among them, at least one of a photocationic polymerization initiator and a photoanionic polymerization initiator is preferred, and a photocationic polymerization initiator is more preferred because it can suitably adjust the polymerization reaction.
[0112] The photocationic polymerization initiator is not particularly limited as long as it can induce the ring-opening reaction of the cationic polymerizable functional group by the light of the wavelength used.Among them, a compound that induces the ring-opening reaction of the cationic polymerizable functional group by the light of the wavelength of 300nm to 370nm and is inactive in the wavelength region of more than 370nm is preferably used.As such a photocationic polymerization initiator, for example, onium salts such as aromatic diazonium salt, aromatic iodonium salt, aromatic sulfonium salt, etc. can be mentioned.
[0113] Specific examples of onium salts include OPTOMER SP-150, OPTOMER SP-170, OPTOMER SP-171 (all manufactured by ADEKA Corporation), UVE-1014 (manufactured by General Electronics Corporation), OMNICAT250, OMNICAT270 (all manufactured by IGM Resin Corporation), IRGACURE290 (manufactured by BASF Corporation), SAN-AID SI-60L, SAN-AID SI-80L, SAN-AID SI-100L (all manufactured by Sanshin Chemical Industry Co., Ltd.), CPI-100P, CPI-101A, CPI-200K (all manufactured by San-Apro Ltd.), and the like.
[0114] The cationic photopolymerization initiator may be used alone or in combination of two or more. Furthermore, the adhesive composition layer may be cured in multiple stages by using a plurality of cationic photopolymerization initiators having different effective active wavelengths.
[0115] The above-mentioned cationic photopolymerization initiator may be used in combination with a sensitizer such as anthracene-based or thioxanthone-based sensitizer, if necessary.
[0116] The photopolymerization initiator (C) is preferably contained in the range of 0.001% by mass to 30% by mass, more preferably 0.01% by mass to 20% by mass, and even more preferably 0.1% by mass to 10% by mass, based on the total solid content of the adhesive composition. By setting the amount of the photopolymerization initiator (C) in the adhesive composition within the above range, the curing reaction after irradiation with active energy rays proceeds slowly, and an adhesive layer exhibiting sufficient bonding properties and rigidity can be formed.
[0117] <Other ingredients (D)> The adhesive composition may contain other components (D) as necessary in addition to the above-mentioned photocurable resin (A), thermoplastic resin (B), and photopolymerization initiator (C).
[0118] By including a pressure-sensitive adhesive resin as the other component (D), the adhesive composition can provide an adhesive composition layer that exhibits good room temperature lamination properties and can form an adhesive layer that has high conformability and adhesion to the adherend.
[0119] The weight average molecular weight of the adhesive resin is preferably within a range of 2000 to 2,000,000, more preferably within a range of 5,000 to 1,000,000, and even more preferably within a range of 5,000 to 800,000. The weight average molecular weight of the adhesive resin can be measured by the same method as that for the weight average molecular weight of the thermoplastic resin (B) described above.
[0120] Examples of the adhesive resin include polyester, polyurethane, poly(meth)acrylate, polyvinyl acetal, etc. These adhesive resins may be homopolymers or copolymers. These adhesive resins may be used alone or in combination of two or more.
[0121] The adhesive resin preferably has a glass transition temperature in the range of −30° C. to 20° C., more preferably in the range of −25° C. to 10° C. By including an adhesive resin having a glass transition temperature within the above range, the adhesive composition layer can exhibit good adhesion and elasticity at room temperature, and an adhesive layer can be formed that exhibits good adhesion to the adherend and high bonding strength.
[0122] The glass transition temperature can be calculated, for example, by using a dynamic viscoelasticity tester (manufactured by Rheometrics, product name: Ares 2KSTD) to sandwich a test piece of an adhesive resin between parallel disks, which are the measuring part of the tester, and measuring the storage modulus (G') and loss modulus (G") at a frequency of 1.0 Hz, and by dividing the loss modulus (G") by the storage modulus (G'), the loss tangent (tan δ) can be calculated as the maximum value (G" / G').
[0123] The adhesive resin may have a functional group that can react with a crosslinking agent or with a functional group contained in the photocurable resin (A) or the thermoplastic resin (B). This is because the adhesive resin can be crosslinked. Examples of the functional group include a hydroxyl group, a carboxyl group, an epoxy group, and an amino group, and it is preferable to select the functional group appropriately within a range that does not inhibit the polymerization reaction of the photocurable resin (A) and the thermoplastic resin (B).
[0124] The adhesive resin is preferably contained in a range of 0.1 to 100 parts by mass, more preferably 1 to 50 parts by mass, and even more preferably 5 to 30 parts by mass relative to the total amount (100 parts by mass) of the adhesive composition. By making the adhesive resin blend ratio within the above range, the adhesive composition can be improved in lamination property at room temperature and in bonding property of the adhesive layer.
[0125] The adhesive composition may contain, as other component (D), inorganic fillers such as metal particles and silica particles, organic fillers, thermally expandable particles, silane coupling agents, phosphoric acid additives, acrylate additives, etc. The adhesive composition may also contain a photocurable silane coupling agent capable of reacting with the photocurable resin (A) and the thermoplastic resin (B), etc.
[0126] The adhesive composition may contain, as other components (D), for example, softeners, stabilizers, adhesion promoters, leveling agents, defoamers, plasticizers, tackifier resins, fibers, antioxidants, hydrolysis inhibitors, thickeners, colorants such as pigments, fillers, tackifier resins, etc. It is preferable that the adhesive composition does not contain glass fibers.
[0127] <Physical properties of adhesive composition> The adhesive composition preferably has a melting point of 25°C or higher, preferably 30°C or higher, preferably 35°C or higher, and preferably 40°C or higher. The melting point is preferably 120°C or lower, preferably 90°C or lower, preferably 85°C or lower, and preferably 60°C or lower. More specifically, the melting point of the adhesive composition can be preferably within the range of 30°C to 120°C, 30°C to 90°C, or 40°C to 85°C. By setting the melting point of the adhesive composition within the above range, an adhesive layer having high follow-up adhesion to the adherend can be formed. In addition, in the manufacturing process of the rigid substrate of the present invention, the shape stability and handleability of the adhesive composition layer are improved. The melting point of the adhesive composition refers to the temperature at which the maximum exothermic peak (exothermic peak top) is observed when the adhesive composition is heated using differential scanning calorimetry (DSC) at a heating rate of 10°C / min from 20°C to 150°C, held for 1 minute, then cooled to -10°C at a cooling rate of 10°C / min, held for 10 minutes, and then measured again at a heating rate of 10°C / min.
[0128] The adhesive layer composition has a loss tangent (tanδ) at 23°C. 23) is preferably less than 3.0, more preferably 1.5 or less, even more preferably 1.0 or less, and particularly preferably 0.8 or less. 23 ) can be 0.01 or more, preferably 0.1 or more. This is because an adhesive layer of a constant thickness can be formed. Also, in the manufacturing process of the rigid substrate of the present invention, the thickness of the adhesive composition layer can be kept constant, resulting in good handleability. The loss tangent of the adhesive composition can be adjusted by appropriately selecting the composition of the photocurable resin, thermoplastic resin, and other components contained in the adhesive layer, their number average molecular weights, and the like.
[0129] The loss tangent (tanδ) of the adhesive composition at 23°C 23 ) is a circular adhesive composition layer having a thickness of 1 mm and a diameter of 8 mm formed using the adhesive composition, which is used as a test piece, and using a dynamic viscoelasticity tester (manufactured by Rheometrics, product name: Ares 2KSTD), the test piece is sandwiched between parallel disks which are the measurement section of the tester, and the storage modulus (G') and loss modulus (G") are measured at temperatures of 0 to 150°C and at a frequency of 1 Hz, and the loss modulus (G") at 23°C is divided by the storage modulus (G') at 23°C to obtain the loss tangent (tan δ) at 23°C (G" / G').
[0130] (2) Adhesive layer A1 In the rigid substrate of the first embodiment, the adhesive layer A1 is formed of the cured product of the adhesive composition described above and has a thickness of 100 μm or more. The adhesive layer A1 also has a storage modulus (E′ 25 ) is 1.0 × 10 9 It is difficult for the resin film layer alone to exhibit the desired rigidity, so in the rigid substrate of the first embodiment to be bonded to the resin film layers B1 and B2, the thickness and storage modulus (E' 25 ) is a predetermined value or more, high rigidity can be imparted when the resin film layers B1 and B2 are laminated on both sides of the adhesive layer A1.
[0131] The thickness of the adhesive layer A1 may be 100 μm or more, preferably 110 μm or more, more preferably 120 μm or more, and more preferably 130 μm or more in terms of sufficient adhesion between the resin film layers B1 and B2 and the adhesive layer A1. The thickness of the adhesive layer A1 is determined according to the total thickness of the rigid substrate, but is preferably 2900 μm or less, more preferably 2000 μm or less, and even more preferably 1000 μm or less. This is because the first embodiment rigid substrate can be made to have an appropriate thickness range when replacing a glass epoxy substrate or other substrates. When one adhesive layer A1 is made of a multilayer structure, the thickness of one adhesive layer A1 refers to the thickness of the entire multilayer structure.
[0132] The storage modulus (E') of the adhesive layer A1 at 25°C measured at a frequency of 1.0 Hz 25 ) is 1.0 × 10 9 Pa or more, but above all, 1.1×10 9 Pa or more, and 1.5×10 9 More preferably, the pressure is 2.0×10 Pa or more. 9 It is more preferable that the E' of the adhesive layer A1 is equal to or larger than E'Pa in order to provide a rigid substrate with high rigidity. 25 is 5.0 x 10 11 Pa or less, and 1.0×10 11 More preferably, the surface tension is 8.0×10 Pa or less. 9 It is particularly preferable that the pressure is 0.1 Pa or less.
[0133] The storage modulus (E') of the adhesive layer A1 at 25°C measured at a frequency of 1.0 Hz 25) is a value measured using a dynamic viscoelasticity measuring device (manufactured by Rheometrics, product name: RSA-II) at a frequency of 1.0 Hz and a temperature of 25°C. The above-mentioned adhesive composition is applied to a release film to form an adhesive composition layer having a thickness of 150 µm, and the adhesive composition layer is subjected to irradiation with an electric current of about 100 mW / cm using an electrodeless lamp (Fusion Lamp H bulb). 2 The adhesive composition layer is cured by irradiating it with ultraviolet light of intensity of 100 nm for 60 seconds, and then left for 30 minutes at 23°C and 50% RH to produce an adhesive layer A1. Measurements are performed using a sample prepared by punching out the adhesive layer A1 using a dumbbell cutter into the shape of a JIS K 7127 type 5 test piece.
[0134] The storage elastic modulus (E') of the adhesive layer A1 25 ) can be adjusted, for example, by varying the amounts of the photocurable resin (A), thermoplastic resin (B), and photopolymerization initiator (C) in the above-mentioned adhesive composition, and the conditions for irradiating the adhesive composition layer, which is the precursor of the adhesive layer A1, with active energy rays.
[0135] The thickness of the adhesive layer A1 in the total thickness of the rigid substrate of the first embodiment is preferably within a range of 20% to 90%, more preferably within a range of 30% to 85%, and even more preferably within a range of 50% to 80%. By setting the thickness of the adhesive layer A1 in the total thickness of the rigid substrate of the first embodiment within the above range, high rigidity can be imparted to the rigid substrate.
[0136] [2] Resin film layers B1 and B2 The resin film layer B1 is a layer disposed on one main surface of the adhesive layer A1, and the resin film layer B2 is a layer disposed on the other main surface of the adhesive layer A1. The resin film layer B1 and the resin film layer B2 each have a thickness of 50 μm or more.
[0137] The resin film layers B1 and B2 each have flexibility. The flexibility of the resin film layers B1 and B2 allows them to be bonded to the adhesive layer A in the manufacture of the rigid substrate of the present invention. The term "flexible" means that the layer can be repeatedly bent or folded, and more specifically, that the distance L measured by the above-mentioned rigidity test method is 45 mm or more.
[0138] As long as the resin film layers B1 and B2 each have a thickness within a predetermined range, they may be the same film, or may be films different in material, thickness, physical properties, etc. Furthermore, as long as the resin film layers B1 and B2 each have a thickness equal to or greater than a predetermined value, the thickness of the resin film layer B1 and the thickness of the resin film layer B2 may be the same or different.
[0139] The thickness of the resin film layers B1 and B2 is 50 μm or more. This is because the rigidity exhibited by the resin film layer B in addition to the rigidity exhibited by the adhesive layer A1 results in a rigid substrate with high rigidity. Also, by each of the resin films B1 and B2 having a thickness of a predetermined value or more, when the rigid substrate of the present invention is manufactured, wrinkles are less likely to occur when the adhesive layer is bonded to the resin film layer, and the rigid substrate has excellent flatness and surface smoothness. Among them, the thickness of the resin film layers B1 and B2 is preferably 60 μm or more, more preferably 70 μm or more, and more preferably 80 μm or more. This is because the rigidity exhibited by the resin film layer B is further increased, resulting in a rigid substrate with higher rigidity. Also, when the rigid substrate of the present invention is manufactured, wrinkles are less likely to occur when the adhesive layer A1 is bonded to the resin film layer A1, the surface smoothness can be increased, and the workability during manufacturing is excellent, which is more preferable. On the other hand, the thicknesses of the resin film layers B1 and B2 are each determined according to the total thickness of the rigid substrate, and are preferably 2850 μm or less, more preferably 1000 μm or less, and more preferably 300 μm or less, because this allows the rigid substrate of the present invention to be within an appropriate thickness range so as to be able to replace general-purpose substrates such as glass epoxy substrates. When one resin film layer B is a film having a multilayer structure, the thickness of one resin film layer B refers to the overall thickness of the film having a multilayer structure.
[0140] The resin film layer B may be a transparent resin film having light transmittance, or may be an opaque resin film having no light transmittance. At least one of the resin film layer B1 and the resin film layer B2 is preferably a transparent resin film, since it is easy to transmit active energy rays, and when the rigid substrate of the present invention is manufactured, the adhesive composition layer is irradiated with sufficient active energy rays to form a sufficiently cured adhesive layer, resulting in a rigid substrate with higher rigidity. In addition, when both the resin film layer B1 and the resin film layer B2 are transparent resin films, the rigid substrate of the present invention can be made a transparent substrate by making other layers such as the adhesive layer transparent, and it can be applied as a substitute for a substrate that requires transparency. The transparent resin film preferably has a light transmittance of 80% or more at a wavelength of 200 nm to 780 nm, and more preferably 90% or more.
[0141] The resin film may be any resin film that does not contain glass fibers, and examples thereof include resin films made of resins such as polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyvinyl chloride, polyimide (PI), polyester, polycarbonate, polystyrene, polylactic acid, cycloolefin polymer (COP), cycloolefin copolymer (COC), polyvinyl alcohol, triacetyl cellulose, and acrylonitrile-butadiene-styrene (ABS). Among these, the resin film layer B1 and the resin film layer B2 are preferably transparent resin films independently selected from the group consisting of polyethylene terephthalate film, polyethylene film, and polycarbonate film. These resin films are preferred because they easily transmit active energy rays, and when the rigid substrate of the present invention is produced, the adhesive composition layer is irradiated with sufficient active energy rays to form a sufficiently cured adhesive layer, resulting in a rigid substrate with higher rigidity. In particular, in the manufacture of the rigid substrate of the present invention, a polyethylene terephthalate film is preferred because it provides good workability when bonded to the adhesive composition layer, which is the precursor of the adhesive layer, and also results in a rigid substrate with high surface smoothness.
[0142] The resin film layer B may contain additives such as organic pigments, inorganic pigments, stabilizers, etc., and may contain components that reduce the ultraviolet transmittance, such as ultraviolet absorbers, plasticizers, etc. The surface of the resin film may be subjected to various treatments, such as antistatic treatment, easy-adhesion treatment, etc.
[0143] The resin film layer B may be a film having a single layer structure or a film having a multilayer structure.
[0144] The resin film layer B may be colorless or colored.
[0145] The resin film layer B may have high or low heat resistance. A resin film having low heat resistance is, for example, a resin film having a melting point of 200° C. or less, and among these, a resin film having a melting point of 180° C. or less can be preferably used. The lower limit of the melting point of the resin film layer B is not particularly limited, but from the viewpoint of suppressing the occurrence of warping of the resin film layer B and the rigid substrate due to heat, the melting point of the resin film layer B is preferably 80° C. or more, and more preferably 90° C. or more.
[0146] The melting point of resin film layer B refers to the temperature at which the maximum exothermic peak (exothermic peak top) is observed when a differential scanning calorimetry (DSC) method is used to increase the temperature from 20°C to 150°C at a heating rate of 10°C / min, hold the temperature for 1 minute, then cool to -10°C at a cooling rate of 10°C / min, hold the temperature for 10 minutes, and then measure again at a heating rate of 10°C / min.
[0147] The resin film layer B has a storage modulus (E' 25 ) is 1.1 × 10 9 Pa or more, and 1.5×10 9 More preferably, the pressure is 2.0×10 Pa or more. 9 It is more preferable that the E' of the resin film layer B is equal to or higher than E'. 25By setting E' of the adhesive layer A1 in the above range, the rigid substrate of the present invention can exhibit higher rigidity. 25 is 5.0 x 10 11 Pa or less, and 1.0×10 11 More preferably, the surface tension is 8.0×10 Pa or less. 9 It is more preferable that the pressure is less than or equal to Pa from the viewpoint of ease of cutting the rigid substrate.
[0148] Storage modulus (E') of resin film layer B at 25°C measured at a frequency of 1.0 Hz 25 ) is a value measured using a dynamic viscoelasticity measuring device (manufactured by Rheometrics, product name: RSA-II) at a frequency of 1.0 Hz and a temperature of 25°C. For the measurement, the resin film layer B1 was punched out using a dumbbell cutter into the shape of a JIS K 7127 type 5 test piece.
[0149] [3] Other The rigid substrate of the first embodiment has a structure in which a resin film layer B1 is directly bonded to one surface of an adhesive layer A1, and a resin film layer B2 is directly bonded to the other surface of the adhesive layer A1. That is, one surface of the adhesive layer A1 contacts with the resin film layer B1, and the other surface of the adhesive layer A1 contacts with the resin film layer B2.
[0150] [4] Manufacturing method of rigid board according to the first embodiment The method for producing the rigid substrate of the first embodiment is not particularly limited, but it can be produced, for example, by using the first or second example described below.
[0151] (1) First Example A first example of the manufacturing method for the rigid substrate of the first embodiment is a manufacturing method comprising, in this order, step 1 of forming a laminate by bonding a resin film layer B1 and a resin film layer B2 to both main surfaces of an adhesive composition layer a1 containing at least a photocurable resin having a polymerizable functional group other than a polymerizable unsaturated double bond, a thermoplastic resin having a polymerizable functional group other than a polymerizable unsaturated double bond, and a photopolymerization initiator, and step 2 of irradiating the adhesive composition layer a1 with active energy rays from at least one of the resin film layer B1 side and the resin film layer B2 side of the laminate to form an adhesive layer A1 formed by curing the adhesive composition layer a1.
[0152] In the first example, since the adhesive composition layer a1 before the active energy ray irradiation exhibits pressure-sensitive adhesive strength (adhesive strength), the adhesive composition layer a1 and the resin film layers B1 and B2 can be bonded together before the active energy ray irradiation. In addition, the resin film layers B1 and B2 can be re-attached or aligned until the curing reaction of the adhesive composition layer a1 is completed, and the curing reaction of the adhesive composition layer a1 is completed to become the adhesive layer A1, so that the resin film layers B1 and B2 can be firmly bonded via the adhesive layer A1. Furthermore, since a delayed curing adhesive composition is used, even if the laminate is first formed and then irradiated with active energy rays, warping or deformation due to curing shrinkage or the like is unlikely to occur, and a rigid substrate with excellent smoothness can be produced.
[0153] In step 1, an adhesive sheet having an adhesive composition layer a1 formed thereon by applying the adhesive composition to a release liner in advance may be prepared, the release liner of the adhesive sheet may be removed, and the resin film layer B1 and the resin film layer B2 may be laminated to both main surfaces of the adhesive composition layer a1 to form a laminate. Alternatively, the adhesive composition may be directly applied to one surface of the resin film layer B1 to form the adhesive composition layer a1, and the resin film layer B2 may be laminated to the surface of the adhesive composition layer a1 opposite to the resin film layer B1 to form a laminate.
[0154] In step 1, the adhesive composition layer a1 and the resin film layer B are preferably bonded together at a pressure in the range of 0.1 kPa to 3000 KPa, more preferably at a pressure in the range of 0.5 kPa to 1000 kPa, and even more preferably at a pressure in the range of 1.0 kPa to 500 kPa.
[0155] The time for pressure bonding at the above pressure is preferably within a range of 0.1 seconds to 10 minutes, more preferably within a range of 0.3 seconds to 5 minutes, and even more preferably within a range of 0.5 seconds to 3 minutes. By setting the pressure bonding force and pressure bonding time within the above ranges, it is possible to apply sufficient pressure to bond the resin film layer B and the adhesive composition layer a1 together while preventing damage to the resin film layer B, and to obtain high bonding strength.
[0156] In step 1, the adhesive composition layer a1 and the resin film layer B can be laminated at room temperature, but may be laminated while heating, and are preferably laminated at a temperature in the range of 5° C. to 100° C., more preferably at a temperature in the range of 10° C. to 70° C., and even more preferably at a temperature in the range of 20° C. to 40° C. By setting the lamination temperature within the above range, it is possible to prevent thermal deterioration of the resin film layer B while sufficiently adhering to the adhesive composition layer a1, and to obtain high bonding strength.
[0157] In step 2, since the adhesive composition layer a1 is irradiated with active energy rays through the resin film, at least one of the resin film layers B1 and B2 is preferably a transparent resin film. In addition, the active energy rays may be irradiated from the resin film layer B1 side, from the resin film layer B2 side, or from both the resin film layers B1 and B2.
[0158] The active energy ray used in step 2 is not particularly limited, but it is preferable to use ultraviolet rays. In order to efficiently carry out the curing reaction, ultraviolet rays may be irradiated under an inert gas atmosphere such as nitrogen gas, or may be irradiated under an air atmosphere. When ultraviolet rays are used as the active energy ray, examples of the light source include a low-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, an electrodeless lamp (fusion lamp), a chemical lamp, a black light lamp, a mercury-xenon lamp, a short arc lamp, a helium-cadmium laser, an argon laser, sunlight, and an LED. Among them, an LED is preferable because it generates less heat during irradiation and can suppress thermal deterioration of the resin film layer B. As the irradiation device for the active energy ray, in addition to the above, a germicidal lamp, a carbon arc, a xenon lamp, a metal halide lamp, a scanning type, a curtain type electron beam accelerator, and the like can be used.
[0159] The irradiation intensity of the active energy rays is not particularly limited as long as the adhesive composition layer a1 can undergo a curing reaction to form an adhesive layer A1 exhibiting predetermined physical properties, and is preferably 10 mW / cm 2 ~1000mW / cm 2 Preferably in the range of 10 mW / cm 2 ~800mW / cm 2 More preferably, the range is 50 mW / cm 2 ~400mW / cm 2 By adjusting the irradiation intensity within the above range, the heat generated upon irradiation with active energy rays can be reduced, so that thermal deterioration of the resin film layer B can be suppressed and the cure rate of the adhesive composition after irradiation with active energy rays can be adjusted.
[0160] The irradiation time of the active energy rays is preferably within a range of 1 to 60 seconds, more preferably within a range of 5 to 50 seconds, and even more preferably within a range of 10 to 40 seconds. By adjusting the irradiation time within the above range, the heat generated upon irradiation with active energy rays can be reduced, so that thermal deterioration of the resin film layer B can be suppressed, and the rigidity of the adhesive composition after irradiation with active energy rays can be adjusted.
[0161] The active energy rays may be irradiated at once, or may be irradiated in portions to facilitate adjustment of the curing rate of the adhesive composition. When irradiating the active energy rays in portions, for example, irradiation for 1 minute may be divided into two portions, and irradiation for 30 seconds may be performed twice.
[0162] Step 2 is preferably carried out in a room temperature environment. In addition, an aging treatment may be performed by exposing the laminate after irradiating the active energy rays to a desired temperature environment for a desired time. The environmental temperature is preferably in the range of 20°C to 80°C, more preferably in the range of 20°C to 60°C, and more preferably in the range of 20°C to 40°C. In this case, the time of exposure to the above-mentioned environmental temperature is preferably 60 minutes to 1 week, more preferably 120 minutes to 3 days, and more preferably 180 minutes to 2 days. This is because the adhesive composition layer a1 can be sufficiently cured while preventing thermal damage to the resin film layer B, and the resin film layer B1 and the resin film layer B2 can be firmly bonded via the adhesive layer A1 formed by the cured product of the adhesive composition. In addition, when exposed to an environmental temperature higher than room temperature, the time until the curing reaction is completed can be further shortened.
[0163] (2) Second Example Furthermore, a second example of the manufacturing method for the rigid substrate of the first embodiment is a manufacturing method having, in this order, step 1 of forming an adhesive composition layer a1 containing at least a photocurable resin having a polymerizable functional group other than a polymerizable unsaturated double bond, a thermoplastic resin having a polymerizable functional group other than a polymerizable unsaturated double bond, and a photopolymerization initiator on one surface of a resin film layer B1 to obtain a laminate; step 2 of irradiating the adhesive composition layer a1 of the laminate with active energy rays; and step 3 of laminating a resin film layer B2 to the surface of the adhesive composition layer a1 opposite to the resin film layer B1 before the curing reaction of the adhesive composition layer a1 after the irradiation with active energy rays is completed, thereby forming an adhesive layer A1 formed by curing the adhesive composition layer a1.
[0164] In the second example, the adhesive composition layer a1 before the active energy ray irradiation exhibits pressure-sensitive adhesive strength (adhesive strength), so the adhesive composition layer a1 and the resin film layer B1 can be bonded together before the active energy ray irradiation. In addition, the adhesive composition layer a1 is irradiated with active energy rays before the resin film layer B2 is bonded. However, the adhesive composition layer a1 after the active energy ray irradiation undergoes a slow curing reaction, and exhibits pressure-sensitive adhesive strength (adhesive strength) for a certain period of time after irradiation. Therefore, the resin film layer B2 can be bonded together before the curing reaction of the adhesive composition layer a1 is completed, making it possible to re-attach the adhesive composition layer a1, and suppressing the occurrence of warping due to curing shrinkage. Furthermore, the curing reaction of the adhesive composition layer a1 is completed to become the adhesive layer A1, so that the resin film layers B1 and B2 can be firmly bonded together via the adhesive layer A1.
[0165] In step 1, the method of forming the laminate may involve directly applying the adhesive composition to the surface of the resin film layer B1 to form the adhesive composition layer a1, or may involve applying the adhesive composition to a release liner to prepare an adhesive sheet to form the adhesive composition layer a1, and then laminating the resin film layer B1 to the adhesive composition layer a1 of the adhesive sheet. The conditions for laminating the adhesive composition layer a1 and the resin film layer B1 can be the same as those described in step 1 of the above-mentioned first example.
[0166] In step 2, the active energy rays may be irradiated from the resin film layer B1 side of the laminate, or from the adhesive composition layer a1 side of the laminate. In the former case, a transparent resin film is used as the resin film layer B1. In the latter case, the resin film layer B1 may be a transparent resin film, or may be an opaque or low light transmittance resin film.
[0167] The conditions for irradiation with active energy rays in step 2 can be the same as those described in the first example above, and therefore a description thereof will be omitted here.
[0168] In step 3, the time from irradiation with active energy rays to laminating the adhesive composition layer a1 with the resin film layer B2 is preferably less than 10 minutes, more preferably within the range of 1 second to 8 minutes, more preferably within the range of 2 seconds to 6 minutes, and even more preferably within the range of 2 seconds to 5 minutes. This is because the adhesive composition layer a1 and the resin film layer B2 can be laminated together due to the pressure-sensitive adhesiveness (tackiness) of the adhesive composition layer a1 before the curing reaction of the adhesive composition layer a1 is completed.
[0169] In step 3, the pressure bonding temperature when laminating the resin film layer B2 to the adhesive composition layer a1 is preferably 100° C. or lower, more preferably in the range of 20° C. to 100° C., further preferably in the range of 40° C. to 90° C., and even more preferably in the range of 50° C. to 85° C. The adhesive composition layer a1 and the resin film layer B2 can be sufficiently adhered and laminated while suppressing thermal damage to the resin film layer B.
[0170] In step 3, the adhesive composition layer a1 and the resin film layer B2 are preferably bonded together under a pressure in the range of 0.1 KPa to 3000 KPa, more preferably 0.5 KPa to 1000 KPa, and even more preferably 1.0 KPa to 500 KPa. The pressure bonding time is preferably in the range of 0.1 seconds to 10 minutes, more preferably 0.3 seconds to 5 minutes, and even more preferably 0.5 seconds to 3 minutes. By setting the pressure bonding force and pressure bonding time in step 3 to the above ranges, respectively, the adhesive composition layer a1 and the resin film layer B2 can be bonded together in sufficient contact without damaging the resin film layer B2, and high bonding strength can be obtained.
[0171] Step 3 is preferably carried out in a room temperature environment. In addition, after the adhesive composition layer a1 is pressure-bonded to the resin film layer B2, an aging treatment may be performed in which the adhesive composition layer a1 is exposed to a desired environmental temperature for a desired time. This is because the adhesive composition layer a1 can be sufficiently cured while preventing thermal damage to the resin film layer B, and the resin film layer B1 and the resin film layer B2 can be firmly bonded via the adhesive layer A1 formed by the cured product of the adhesive composition. In addition, when exposed to an environmental temperature higher than room temperature, the time until the curing reaction is completed can be further shortened. The preferred environmental temperature and the time of exposure to the environmental temperature can be the same as the environmental temperature and the environmental temperature of the aging treatment in step 2 in the first example of the manufacturing method.
[0172] II. Second embodiment of rigid board Fig. 2 is a schematic cross-sectional view showing an example of a rigid substrate of the second embodiment. The rigid substrate 20 of the second embodiment shown in Fig. 2 has an adhesive layer A1 (reference number 1 in Fig. 2), a resin film layer B1 (reference number 2 in Fig. 2) arranged on one main surface of the adhesive layer A1, and a resin film layer B2 (reference number 3 in Fig. 2) arranged on the other main surface of the adhesive layer A1, and has an intermediate layer C (reference number 4 in Fig. 2) and an adhesive layer A2 (reference number 5 in Fig. 2) in this order from the adhesive layer A1 side between the adhesive layer A1 and the resin film layer B2, and the total thickness of the rigid substrate 20 (reference number T in Fig. 2) is 500 μm or more. The adhesive layer A1 and the adhesive layer A2 are each formed of a cured product of an adhesive composition containing at least a photocurable resin having a polymerizable functional group other than a polymerizable unsaturated double bond, a thermoplastic resin having a polymerizable functional group other than a polymerizable unsaturated double bond, and a photopolymerization initiator, and the thickness of the adhesive layer A1 and the adhesive layer A2 (represented by the symbol T in FIG. 2) is A1 and T A2 ) is 50 μm or more, and the sum of the thicknesses of the adhesive layers A1 and A2 (T A1 +T A2 ) is 100 μm, and the storage modulus (E') at 25° C. of the adhesive layer A1 and the adhesive layer A2 is measured at a frequency of 1.0 Hz. 25 ) are 1.0×10 9 In addition, the thickness of the resin film layer B1 and the resin film layer B2 (reference symbol T B1 and T B2 ) are 50 μm or more.
[0173] The rigid substrate of the second embodiment can have a rigidity comparable to that of a glass epoxy substrate, has little warping, and is less likely to produce cutting chips during cutting. In addition, the rigid substrate of the second embodiment has an intermediate layer C, which can further increase the rigidity of the entire rigid substrate due to the rigidity of the intermediate layer C. Furthermore, the rigid substrate can be formed by reducing the thickness of the adhesive layer in the rigid substrate, which may be advantageous in terms of thinning the substrate and manufacturing costs.
[0174] The rigid substrate of the second embodiment has a total thickness of 500 μm or more, which allows the rigid substrate to have high rigidity. In particular, the total thickness of the rigid substrate of the second embodiment is preferably 600 μm or more, more preferably 7000 μm or more, and even more preferably 800 μm or more, which allows the rigid substrate to have high rigidity. Furthermore, the total thickness of the rigid substrate of the second embodiment is preferably 3000 μm or less, more preferably 2000 μm or less, and even more preferably 1500 μm or less, since this allows the substrate to be within an appropriate thickness range in order to replace glass epoxy substrates and other substrates.
[0175] Hereinafter, the rigid board according to the second embodiment will be described with respect to each of its constituent members.
[0176] [1] Adhesive layer A1 and adhesive layer A2 The adhesive layers A1 and A2 in the rigid substrate of the second embodiment are each formed of a cured product of an adhesive composition containing at least a photocurable resin having a polymerizable functional group other than a polymerizable unsaturated double bond, a thermoplastic resin having a polymerizable functional group other than a polymerizable unsaturated double bond, and a photopolymerization initiator. The adhesive layers A1 and A2 each have a thickness of 50 μm or more, and the sum of the thicknesses of the adhesive layers A1 and A2 is 100 μm. Furthermore, the storage modulus (E') at 25° C. of the adhesive layers A1 and A2 measured at a frequency of 1.0 Hz is 25 ) are 1.0×10 9 Pa or more,
[0177] (1) Adhesive composition Details of the adhesive composition forming the adhesive layer in the rigid substrate of the second embodiment are the same as those of the adhesive composition described above in the section "I. First embodiment of rigid substrate [1] Adhesive layer A1 (1) Adhesive composition," and therefore will not be described here.
[0178] The adhesive composition forming adhesive layer A1 and the adhesive composition constituting adhesive layer A2 may be the same or different, so long as they contain the above-mentioned components and have the specified physical properties.
[0179] (2) Adhesive layer A1 and adhesive layer A2 In the rigid substrate of the second embodiment, the adhesive layers A1 and A2 are each formed of a cured product of the adhesive composition described above, each having a thickness of 50 μm or more, and the sum of the thicknesses of the adhesive layers A1 and A2 is 100 μm. In addition, the adhesive layers A1 and A2 each have a storage modulus (E') at 25° C. measured at a frequency of 1.0 Hz. 25 ) is 1.0 × 10 9 In the rigid substrate of the second embodiment, the thickness and storage modulus (E' 25 ) being equal to or greater than the predetermined value, the resin film layer B and the intermediate layer C can be bonded with high adhesive strength, and the rigidity of the adhesive layers A1 and A2 can impart high rigidity to the rigid substrate.
[0180] In the rigid substrate of the second embodiment, the thickness of each of the adhesive layers A1 and A2 may be 50 μm or more, but is preferably 100 μm or more, more preferably 110 μm or more, and more preferably 130 μm or more, in order to be able to sufficiently adhere to the resin films B1 and B2 and the intermediate layer and to be firmly bonded. In addition, the thickness of each of the adhesive layers A1 and A2 is preferably 1500 μm or less, more preferably 1000 μm or less, and even more preferably 500 μm or less, in order to be able to give rigidity to the rigid substrate and to make the thickness of the rigid substrate within a range suitable for replacing other substrates such as glass epoxy substrates. The adhesive layers A1 and A2 may have the same thickness as the adhesive layer A1 and the adhesive layer A2, or may be different, as long as they each have a thickness of a predetermined value or more. In addition, when one adhesive layer A1 is made of a multilayer structure, the thickness of one adhesive layer A1 refers to the thickness of the entire multilayer structure. The same applies to the case where the adhesive layer A2 is made of a multilayer structure.
[0181] In the rigid substrate of the second embodiment, the sum of the thicknesses of the adhesive layers A1 and A2 may be 100 μm or more, preferably 110 μm or more, more preferably 120 μm or more, and more preferably 130 μm or more, in order to ensure sufficient adhesion and strong bonding with the resin films B1, B2 and the intermediate layer. The sum of the thicknesses of the adhesive layers A1 and B2 is preferably 1500 μm or less, more preferably 1000 μm or less, and even more preferably 500 μm or less. This is because it is possible to provide high rigidity to the rigid substrate of the second embodiment while keeping the thickness within an appropriate range for replacing glass epoxy substrates and other substrates.
[0182] In the rigid substrate of the second embodiment, the storage modulus (E') of the adhesive layers A1 and A2 at 25°C measured at a frequency of 1.0 Hz 25 ) are 1.0×10 9 Pa or more, but above all, 1.1×10 9 Pa or more, and 1.5×10 9 More preferably, the pressure is 2.0×10 Pa or more. 9 It is more preferable that the E' of the adhesive layers A1 and A2 is equal to or more than E' Pa, since this can impart high rigidity to the rigid substrate of the second embodiment. 25 are 5.0×10 11 Pa or less, and 1.0×10 11 More preferably, the surface tension is 8.0×10 Pa or less. 9 It is more preferable that the elastic modulus is 1 Pa or less, in order to obtain a rigid substrate that has high rigidity and is easy to cut.
[0183] In the rigid substrate of the second embodiment, the storage modulus (E') at 25°C measured at a frequency of 1.0 Hz of the adhesive layers A1 and A2 25 ) are values measured at a frequency of 1.0 Hz and a temperature of 25° C. using a dynamic viscoelasticity measuring device (manufactured by Rheometrics, product name: RSA-II), and the measurement method was the same as that of E' of adhesive layer A1 described in the above section "I. First embodiment of rigid substrate [1] Adhesive layer A1 (1) Adhesive layer A1". 25 The measurement method is the same as that of
[0184] In the rigid substrate of the second embodiment, the storage elastic modulus (E' 25 ) can be adjusted by the amounts of the photocurable resin (A), thermoplastic resin (B), and photopolymerization initiator (C) in the above-mentioned adhesive composition used to form the adhesive layers A1 and A2, respectively, and the conditions for irradiating the adhesive composition layer, which is the precursor of the adhesive layers A1 and A2, with active energy rays.
[0185] The ratio of the sum of the thicknesses of the adhesive layers A1 and A2 to the total thickness of the rigid substrate of the second embodiment is preferably within a range of 20% to 90%, more preferably within a range of 30% to 85%, and even more preferably within a range of 30% to 80%. By making the sum of the thicknesses of the adhesive layers A1 and A2 to the total thickness of the rigid substrate of the second embodiment within the above range, a rigid substrate with high rigidity is obtained by laminating with the resin film layers B1, B2 and the intermediate layer.
[0186] In addition, in the rigid substrate of the second embodiment, the thickness T of the adhesive layer A1 A1 and the thickness T of the adhesive layer A2 A2 The sum of (T A1 +T A2 ) and the thickness T of the resin film layer B1 B1 and the thickness T of the resin film layer B2 B2 The sum of (T B1 +T B2 ) and the ratio [(T A1 +T A2 ) / (T B1 +T B2)] is preferably in the range of 0.3 to 4, more preferably in the range of 0.4 to 3.7, and even more preferably in the range of 0.5 to 3.5. In the rigid substrate of the second embodiment, by setting the ratio of the sum of the thicknesses of the adhesive layers A1 and A2 to the sum of the thicknesses of the resin film layers B1 and B2 within the above range, a rigid substrate having high rigidity can be obtained by covering the outermost layer with the resin film layers B1 and B2, regardless of the type or thickness of the intermediate layer, due to the rigidity exerted by the adhesive layers A1 and A2 and the rigidity exerted by the resin film layers B1 and B2.
[0187] [2] Resin film layers B1 and B2 The resin film layers B1 and B2 in the rigid substrate of the second embodiment each have a thickness of 50 μm or more. This is because the rigidity exhibited by the resin film layer B in addition to the rigidity exhibited by the adhesive layers A1 and A2 and the intermediate layer C results in a rigid substrate with high rigidity. In addition, by each of the resin films B1 and B2 having a thickness of a predetermined value or more, when the rigid substrate of the present invention is manufactured, wrinkles are less likely to occur when the adhesive layers are bonded to the resin film layers, and the rigid substrate has excellent flatness and surface smoothness. Among these, the thicknesses of the resin film layers B1 and B2 are preferably 60 μm or more, more preferably 70 μm or more, and more preferably 80 μm or more. This is because the rigidity exhibited by the resin film layer B is further increased, resulting in a rigid substrate with higher rigidity. In addition, when the rigid substrate of the present invention is manufactured, wrinkles are less likely to occur when the adhesive layers A1 and A2 are bonded to the resin film layers A1 and A2, surface smoothness can be increased, and the rigid substrate has excellent workability during manufacturing, which is more preferable. On the other hand, the thicknesses of the resin film layers B1 and B2 are each determined according to the total thickness of the rigid substrate, and are preferably 2800 μm or less, more preferably 1000 μm or less, and more preferably 300 μm or less, because this allows the rigid substrate of the present invention to be within an appropriate thickness range so as to be able to replace general-purpose substrates such as glass epoxy substrates. When one resin film layer B is a film having a multilayer structure, the thickness of one resin film layer B refers to the overall thickness of the film having a multilayer structure.
[0188] As long as the resin film layers B1 and B2 each have a thickness within a predetermined range, they may be the same film, or may be films different in material, thickness, physical properties, etc. Furthermore, as long as the resin film layers B1 and B2 each have a thickness equal to or greater than a predetermined value, the thickness of the resin film layer B1 and the thickness of the resin film layer B2 may be the same or different.
[0189] Other details regarding the resin film layers B1 and B2 in the rigid substrate of the second embodiment are the same as those described above in the section “I. First embodiment of rigid substrate [2] Resin film layers B1 and B2” and therefore will not be described here.
[0190] [3] Middle layer C The intermediate layer C in the rigid substrate of the second embodiment is a layer disposed between the adhesive layer A1 and the adhesive layer A2. The intermediate layer C may be any layer that does not contain glass fibers, and examples thereof include resin films made of resins such as polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), rigid polyvinyl chloride, polyimide (PI), polyester, polycarbonate, polystyrene, polylactic acid, cycloolefin polymer (COP), cycloolefin copolymer (COC), polyvinyl alcohol, triacetyl cellulose, and acrylonitrile-butadiene-styrene (ABS); bakelite sheets such as paper bakelite and cloth bakelite; decorative sheets and decorative boards such as melamine; mineral boards and mineral sheets such as mica and talc; and the like. Among these, it is preferable that the intermediate layer C is a layer selected from the group consisting of rigid polyvinyl chloride layer, melamine decorative board, paper bakelite layer, cloth bakelite layer, and mica board. These have high rigidity relative to their thickness, and the rigidity of the adhesive layers A1 and A2 and the resin films B1 and B2, as well as the rigidity of the intermediate layer, can impart high rigidity to the entire rigid substrate.
[0191] The thickness of the intermediate layer C is not particularly limited, but is preferably 50 μm or more, more preferably 100 μm or more, and even more preferably 150 μm or more. The thickness of the intermediate layer C is preferably 400 μm or less, more preferably 350 μm or less, and even more preferably 300 μm or less. By setting the thickness of the intermediate layer within the above range, it is possible to provide high rigidity to the rigid substrate while keeping the thickness within an appropriate thickness range that can replace a general-purpose substrate such as a glass epoxy substrate.
[0192] The intermediate layer C has a storage modulus (E' 25 ) is 1.0×10 9 Pa or more, and more preferably 1.5×10 9 Pa or more, and 2.0×10 9 The storage modulus (E') of the intermediate layer C is more preferably 1.0 Pa or more. 25 By setting E' of the intermediate layer C to the value above or more, high rigidity can be imparted to the rigid board. 25 are 5.0×10 11 Pa or less, and 1.0×10 11 More preferably, the surface tension is 8.0×10 Pa or less. 9 It is more preferable that the hardness be 100 Pa or less from the viewpoint of ease of cutting the rigid substrate. Storage modulus (E') of intermediate layer C at 25°C measured at a frequency of 1.0 Hz 25 ) is the storage modulus (E') of the above-mentioned adhesive layer or resin film at 25°C measured at a frequency of 1.0 Hz. 25 ) can be measured in the same manner as described above.
[0193] [4] Other The rigid substrate of the second embodiment has a resin film layer B1, an adhesive layer A1, an intermediate layer C, an adhesive layer A2, and a resin film layer B2 laminated in this order, and it is preferable that the resin film layer B1 and the adhesive layer A1, the adhesive layer A1 and the intermediate layer C, the intermediate layer C and the adhesive layer A2, and the adhesive layer A2 and the resin film layer B2 are adhered to each other.
[0194] The rigid substrate of the second embodiment has at least one set of the intermediate layer C and the adhesive layer A2 between the adhesive layer A1 and the resin film layer B2, but may have two or more sets of the intermediate layer C and the adhesive layer A2. For example, the rigid substrate of the second embodiment having two sets of the intermediate layer C and the adhesive layer A2 may have a layer structure having a resin film layer B1, an adhesive layer A1 in contact with the resin film layer B1, an intermediate layer C1 in contact with the adhesive layer A1, an adhesive layer A2a in contact with the intermediate layer C1, an intermediate layer C2 in contact with the adhesive layer A2a, an adhesive layer A2b in contact with the intermediate layer C2, and a resin film layer B2 in contact with the adhesive layer A2b.
[0195] [5] Manufacturing method The method for producing the rigid substrate of the second embodiment is not particularly limited, but it can be produced, for example, by using the first or second example described below.
[0196] (1) First Example The first example of the method for producing the rigid substrate of the second embodiment includes a step 1 of preparing a laminate 1 in which an adhesive composition layer a1 containing at least a photocurable resin having a polymerizable functional group other than a polymerizable unsaturated double bond, a thermoplastic resin having a polymerizable functional group other than a polymerizable unsaturated double bond, and a photopolymerization initiator is disposed on one surface of a resin film layer B1, and a laminate 2 in which an adhesive composition layer a2 containing at least a photocurable resin having a polymerizable functional group other than a polymerizable unsaturated double bond, a thermoplastic resin having a polymerizable functional group other than a polymerizable unsaturated double bond, and a photopolymerization initiator is disposed on one surface of a resin film layer B2; and step 3 of irradiating the adhesive composition layer a1 and the adhesive composition layer a2 with active energy rays from the resin film layer B1 side and the resin film layer B2 side of the laminate 3, respectively, to form adhesive layer A1 and adhesive layer A2, which are formed by curing the adhesive composition layer a1 and the adhesive composition layer a2.
[0197] In the first example, the adhesive composition layers a1 and a2 before the active energy ray irradiation are formed of the above-mentioned adhesive composition, and exhibit pressure-sensitive adhesive strength (adhesive strength), so that the adhesive composition layers a1 and a2 can be bonded to the intermediate layer C before the active energy ray irradiation. In addition, the intermediate layer C can be re-attached or aligned until the curing reaction of the adhesive composition layers a1 and a2 is completed, and the adhesive composition layers a1 and a2 are cured to form the adhesive layers A1 and A2, so that the resin film layers B1 and B2 and the intermediate layer C can be firmly bonded via the adhesive layers A1 and A2. Furthermore, since a delayed curing adhesive composition is used, even if the laminate is first formed and then irradiated with active energy rays, warping or deformation due to curing shrinkage or the like is unlikely to occur, and a rigid substrate with excellent smoothness can be produced.
[0198] In step 1, adhesive sheets having adhesive composition layers a1 and a2 formed thereon may be prepared in advance by applying the adhesive composition to a release liner, and the release liner of the adhesive sheet may be removed, and resin film layers B1 and B2 may be laminated to both main surfaces of the adhesive composition layers a1 and a2, respectively, to form laminates 1 and 2. Alternatively, the adhesive composition may be directly applied to one surface of the resin film layers B1 and B2 to form the adhesive composition layers a1 and a2, thereby forming laminates 1 and 2.
[0199] In step 1, the conditions for bonding the adhesive composition layers a1, a2 to the resin film layers B1, B2 can be the same as the conditions for bonding the adhesive composition layer a1 to the resin film layer B1 described in step 1 of the first example of the method for manufacturing a rigid substrate of the first embodiment described above.
[0200] In step 2, the bonding conditions for bonding the intermediate layer C to the adhesive composition layer a1 of the laminate 1 and the adhesive composition layer a1 of the laminate 2 can be the same as the bonding conditions for the adhesive composition layer and the resin film layer in step 1.
[0201] In step 3, since the adhesive composition layers a1, a1 are irradiated with active energy rays through the resin film layers B1, B2, respectively, it is preferable that both of the resin film layers B1 and B2 are transparent resin films.
[0202] The type and irradiation conditions of the active energy rays used in step 3 can be the same as those described in step 2 of the first example of the method for producing a rigid substrate of the first embodiment above.
[0203] Step 3 is preferably carried out in a room temperature environment, but after irradiation with active energy rays, an aging treatment may be performed in which the laminate is exposed to a desired environmental temperature for a desired time. This is because the adhesive composition layers a1 and a2 can be sufficiently cured while preventing thermal damage to the resin film layer B, and the resin film layer B1 and the resin film layer B2, and the intermediate layer C can be firmly bonded via the adhesive layers A1 and A2 formed by the cured product of the adhesive composition. In addition, when exposed to an environmental temperature higher than room temperature, the time until the curing reaction is completed can be further shortened.
[0204] (2) Second Example A second example of the manufacturing method for the rigid substrate of the second embodiment is a manufacturing method having, in this order, step 1 of preparing a laminate 1 in which an adhesive composition layer a1 is disposed on one surface of a resin film layer B1, and a laminate 2 in which an adhesive composition layer a2 is disposed on one surface of a resin film layer B2; step 2 of irradiating the adhesive composition layer a1 of the laminate 1 and the adhesive composition layer a2 of the laminate 2 with active energy rays, respectively; and step 3 of laminating the intermediate layer C and the laminate 1 so that one surface of the intermediate layer C contacts the adhesive composition layer a1 of the laminate 1 before the curing reaction of the adhesive composition layers a1 and a2 is completed, and laminating the intermediate layer C and the laminate 2 so that the other surface of the intermediate layer C contacts the adhesive composition layer a1 of the laminate 2, thereby forming adhesive layers A1 and A2 formed by curing the adhesive composition layer a1 and the adhesive composition layer a2.
[0205] In the second example, the adhesive composition layers a1 and a2 before the active energy ray irradiation each exhibit pressure-sensitive adhesive strength (adhesive strength), so that the adhesive composition layers a1 and a2 can be bonded to the resin film layers B1 and B2 before the active energy ray irradiation. In addition, the adhesive composition layers a1 and a2 are irradiated with active energy rays before bonding with the intermediate layer C, but the adhesive composition layers a1 and a2 after the active energy ray irradiation have a slow progress of curing reaction, and exhibit pressure-sensitive adhesive strength (adhesive strength) for a certain time after irradiation, so that the intermediate layer C can be bonded before the curing reaction of the adhesive composition layers a1 and a2 is completed. Furthermore, the curing reaction of the adhesive composition layers a1 and a2 is completed to become the adhesive layers A1 and A2, so that the resin film layer B1 and the intermediate layer C, and the resin film layer B2 and the intermediate layer C can be firmly bonded via the adhesive layer A1 and the adhesive layer A2. The conditions for each step in the second example may be the same as those described for each step in the second example of the method for producing a rigid substrate of the first aspect described above.
[0206] III. Rigid board In both the first and second aspects of the rigid substrate of the present invention, components such as the resin film layer and intermediate layer are bonded via an adhesive layer formed from the cured product of the above-mentioned specific adhesive composition, and therefore the rigid substrate has less warping and higher flatness than when bonded via an adhesive layer formed from the cured product of a photocurable adhesive or thermosetting adhesive. Specifically, the flatness of the rigid substrate of the present invention is such that when the rigid substrate cut into a square shape is placed on a horizontal surface, the warpage of each of the four sides of the rigid substrate from the horizontal surface is preferably 2500 μm or less, more preferably 1000 μm or less, and even more preferably 500 μm or less. When the warpage is within the above range, the rigid substrate can be suitably used for applications requiring small warpage and high flatness, such as a support substrate for a semiconductor device or a reinforcing plate for a polishing pad. The position for measuring the warpage of each of the four sides of the rigid substrate is the position furthest from the horizontal surface on each target side when the rigid substrate is placed on a horizontal surface.
[0207] The rigid substrate of the present invention, in both the first and second embodiments, has high rigidity, little warping and high flatness, and generates little cutting debris during cutting, and therefore can be used as a replacement for general-purpose substrates having rigidity. In particular, since it has rigidity equivalent to that of a glass epoxy substrate of the same thickness, it can be suitably used as a replacement for a glass epoxy substrate. Furthermore, specific applications of the rigid substrate of the present invention include applications in which glass epoxy substrates have conventionally been used, such as support substrates (semiconductor substrates) in semiconductor devices and reinforcing plates for polishing pads.
[0208] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and any embodiment that has substantially the same configuration as the technical idea described in the claims of the present disclosure and exhibits similar effects is included in the technical scope of the present disclosure. EXAMPLES
[0209] The present invention will be described more specifically below with reference to examples and comparative examples.
[0210] <Preparation of Thermoplastic Resin (X-1)> A reaction vessel was charged with 51 parts by mass of an aromatic polyester polyol having a number average molecular weight of 1,300 obtained by reacting an ethylene oxide 2-mol adduct of bisphenol A, phthalic acid, and adipic acid, 32 parts by mass of an aliphatic polyester polyol having a number average molecular weight of 3,500 obtained by reacting 1,6-hexanediol and dodecanedioic acid, 7 parts by mass of polypropylene glycol having a number average molecular weight of 1,000, and 2 parts by mass of an ethylene oxide 2-mol adduct of bisphenol A, and the mixture was dehydrated until the moisture content became 0.05% by mass by heating to 100°C under reduced pressure conditions to obtain a mixture.
[0211] Next, the mixture was cooled to 70°C and mixed with 8.0 parts by mass of 4,4'-diphenylmethane diisocyanate, and then heated to 100°C and reacted for 3 hours until the hydroxyl group content became constant, to obtain a polyester polyurethane as a thermoplastic resin (X-1). The polyester polyurethane had a hydroxyl group as a polymerizable functional group.
[0212] <Creating the adhesive sheet (A1-1)> An adhesive solution containing an adhesive composition was obtained by mixing and stirring 40 parts by mass of a thermoplastic resin (X-1), 22 parts by mass of an alicyclic epoxy resin (manufactured by Daicel Corporation, "CEL-2021P"), 35 parts by mass of a cresol novolac type epoxy resin (manufactured by DIC Corporation, "N-685-EXP-S"), 2.5 parts by mass of a sulfonium salt-based photocationic polymerization initiator (manufactured by San-Apro Ltd., "CPI-100P", solid content concentration 50%), and 10.0 parts by mass of hydrophobic silica particles (manufactured by Fuji Silysia Chemical Ltd., "Silohobic 603", average particle size 6.7 μm), and adding methyl ethyl ketone to adjust the non-volatile content to 75% by mass.
[0213] Next, an adhesive solution containing the above adhesive composition was applied to the surface of release liner A (a 50 μm-thick polyethylene terephthalate film with one side released with a silicone compound) using a rod-shaped metal applicator so that the thickness after drying would be 150 μm. The film was then placed in a dryer at 85° C. for 5 minutes to dry and form an adhesive composition layer. The exposed surface of the adhesive composition layer was then bonded to the release-treated surface of release liner B (a 38 μm-thick polyethylene terephthalate film with one side released with a silicone compound) using a hand roller, to obtain an adhesive sheet (A1-1).
[0214] <Preparation of Thermoplastic Resin (X-2)> A reaction vessel was charged with 51 parts by mass of an aromatic polyester polyol having a number average molecular weight of 1,300 obtained by reacting an ethylene oxide 2-mol adduct of bisphenol A, phthalic acid, and adipic acid, 32 parts by mass of an aliphatic polyester polyol having a number average molecular weight of 3,500 obtained by reacting 1,6-hexanediol and dodecanedioic acid, 7 parts by mass of polypropylene glycol having a number average molecular weight of 1,000, and 2 parts by mass of an ethylene oxide 2-mol adduct of bisphenol A, and the mixture was dehydrated until the moisture content became 0.05% by mass by heating to 100°C under reduced pressure conditions to obtain a mixture.
[0215] Next, the mixture was cooled to 70°C and mixed with 8.0 parts by mass of 4,4'-diphenylmethane diisocyanate, and then heated to 100°C and reacted for 3 hours until the hydroxyl group content became constant, to obtain polyester polyurethane as thermoplastic resin (X-2). Note that the polyester polyurethane had hydroxyl groups as polymerizable functional groups.
[0216] <Creating the adhesive sheet (A1-2)> An adhesive solution containing an adhesive composition was obtained by mixing and stirring 43 parts by mass of a thermoplastic resin (X-2), 22 parts by mass of an alicyclic epoxy resin (manufactured by Daicel Corporation, "CEL-2021P"), 35 parts by mass of a cresol novolac type epoxy resin (manufactured by DIC Corporation, "N-685-EXP-S"), 2.5 parts by mass of a sulfonium salt-based photocationic polymerization initiator (manufactured by San-Apro Corporation, "CPI-100P", solid content concentration 50%), and 10.0 parts by mass of hydrophobic silica particles (manufactured by Fuji Silysia Corporation, "Silohobic 603", average particle size 6.7 μm), and adding methyl ethyl ketone to adjust the non-volatile content to 75% by mass. Next, an adhesive solution containing the above adhesive composition was applied to the surface of release liner A (a 50 μm-thick polyethylene terephthalate film with one side released with a silicone compound) using a rod-shaped metal applicator so that the thickness after drying would be 150 μm. The film was then placed in a dryer at 85° C. for 5 minutes to dry and form an adhesive composition layer. The exposed surface of the adhesive composition layer was then bonded to the release-treated surface of release liner B (a 38 μm-thick polyethylene terephthalate film with one side released with a silicone compound) using a hand roller, to obtain an adhesive sheet (A1-2).
[0217] <Preparation of Thermoplastic Resin (X-3)> Add 44.1 mass of polypropylene glycol (number average molecular weight: 2,000) to a reaction vessel. Part 1, 4-cyclohexanedimethanol, 1,6-hexanediol, and dimethyl carbonate The polycarbonate polyol (number average molecular weight 900) obtained by the reaction of 0.2 parts by weight of 2-hydroxyethyl acrylate, 2,6-di-tert-butyl 0.3 parts by mass of p-cresol and 0.05 parts by mass of p-methoxyphenol were added.
[0218] After the temperature inside the reaction vessel was adjusted to 40° C., 14.9 parts by mass of 4,4′-diphenylmethane diisocyanate was added to the reaction vessel.
[0219] Next, 0.1 parts by mass of dioctyltin dineodecane was added to the reaction vessel, and the mixture was stirred for 1 hour. The temperature is raised to 80°C over a period of time, and after confirming that all isocyanate groups have disappeared, the mixture is cooled. By this, a polyurethane having a weight average molecular weight of 35,000 and a polymerizable unsaturated double bond as a polymerizable functional group was obtained as a thermoplastic resin (X-3).
[0220] <Creating adhesive sheet (A1-3)> In a reaction vessel equipped with a stirrer, a reflux condenser, and a thermometer and adjusted to 80°C, 100 parts by mass of the thermoplastic resin (X-3) having a polymerizable unsaturated double bond as a polymerizable functional group and 67 parts by mass of ethyl acetate were supplied and mixed. Next, 0.3 parts by mass of Irgacure 184 (manufactured by BASF Ltd.) and 10.3 parts by mass of dipentaerythritol hexaacrylate were supplied to the mixture and stirred to obtain an adhesive solution containing an adhesive composition. Next, an adhesive solution containing the above adhesive composition was applied to the surface of release liner A (a 50 μm-thick polyethylene terephthalate film with one side released with a silicone compound) using a rod-shaped metal applicator so that the thickness after drying would be 150 μm. The film was then placed in a dryer at 85° C. for 5 minutes to dry and form an adhesive composition layer. The exposed surface of the adhesive composition layer was then bonded to the release-treated surface of release liner B (a 38 μm-thick polyethylene terephthalate film with one side released with a silicone compound) using a hand roller, to obtain an adhesive sheet (A1-3).
[0221] <Creating adhesive sheet (A1-4)> In a reaction vessel equipped with a stirrer, a reflux condenser, a thermometer, a dropping funnel, and a nitrogen gas inlet, 44.9 parts by mass of butyl acrylate, 50 parts by mass of 2-ethylhexyl acrylate, 2 parts by mass of acrylic acid, 3 parts by mass of vinyl acetate, 0.1 parts by mass of 4-hydroxybutyl acrylate, and 0.1 parts by mass of 2,2'-azobisisobutylnitrile as a polymerization initiator were dissolved in 100 parts by mass of ethyl acetate, and polymerized at 70°C for 10 hours, thereby obtaining an acrylic copolymer solution having a weight average molecular weight of 800,000.
[0222] Next, 40 parts by mass of a polymerized rosin ester tackifying resin (Pensel D-160, manufactured by Arakawa Chemical Industries, Ltd., softening point 150 to 160°C) was added to 100 parts by mass of the acrylic copolymer, ethyl acetate was added and mixed, and then 1.1 parts by mass of an isocyanate crosslinking agent (Coronate L-45, manufactured by Nippon Polyurethane Industry Co., Ltd., solids content 45% by mass) was added and stirred for 15 minutes to obtain a pressure-sensitive adhesive solution (X-4).
[0223] Next, the pressure-sensitive adhesive solution (X-4) was applied to the surface of release liner A (a 50 μm-thick polyethylene terephthalate film with one side released with a silicone compound) using a rod-shaped metal applicator so that the thickness after drying would be 150 μm, and the film was placed in a dryer at 85° C. for 15 minutes to dry and form an adhesive composition layer. The exposed surface of the adhesive composition layer was then bonded to the release-treated surface of release liner B (a 38 μm-thick polyethylene terephthalate film with one side released with a silicone compound) using a hand roller, and the film was left in a 40° C. temperature environment for 2 days to obtain an adhesive sheet (A1-4).
[0224] Example 1 Four adhesive sheets (A1-1) were prepared, the release liners were peeled off, and the four sheets were stacked together to form an adhesive composition layer a1 having a thickness of 600 μm. A transparent polyethylene terephthalate film (E') having a thickness of 100 μm was applied as a resin film layer B1 to one side of the adhesive composition layer a1. 25℃ = approx. 2.0×10 9 A 100 μm-thick transparent polyethylene terephthalate film (E' Pa) was laminated on the other surface of the adhesive composition layer a1 as a resin film layer B2. 25℃ = approx. 2.0×10 9 Pa) were laminated together using a hand roller to form a laminate.
[0225] Next, the laminate was irradiated with about 100 mW / cm using an electrodeless lamp (Fusion Lamp H bulb). 2 After irradiating with ultraviolet light of intensity of 1000 for 60 seconds, the sample was placed at 23°C and 50% RH for 30 minutes to prepare a substrate sample having a layer structure of resin film layer B1 / adhesive layer A1 / resin film layer B2 ( / is the adhesive interface).
[0226] Example 2 A substrate sample was produced in the same manner as in Example 1, except that the adhesive sheet (A1-2) was used instead of the adhesive sheet (A1-1).
[0227] Example 3 The release liner of the adhesive sheet (A1-1) was peeled off, and a 100 μm-thick transparent polyethylene terephthalate film (E' 25℃ = approx. 2.0×10 9 A transparent polyethylene terephthalate film (E'Pa) having a thickness of 200 μm was laminated on the other side of the adhesive composition layer a1 as an intermediate layer C. 25℃ = approx. 2.0×10 9 Next, the release liner of another adhesive sheet (A1-1) was peeled off, and one surface of the exposed adhesive composition layer a2 was bonded to the surface of the intermediate layer C opposite to the surface in contact with the adhesive composition layer a1, and then a 100 μm-thick transparent polyethylene terephthalate film (E' 25℃ = approx. 2.0×10 9 Pa) were laminated to form a laminate.
[0228] Next, the laminate was irradiated with about 100 mW / cm using an electrodeless lamp (Fusion Lamp H bulb). 2 After being exposed to ultraviolet light of intensity of 1000 nm for 60 seconds, the sample was placed at 23°C and 50% RH for 30 minutes to create a substrate sample consisting of a layer structure of resin film layer B1 / adhesive layer A1 / intermediate layer C / adhesive layer A2 / resin film layer B2 ( / represents the adhesive interface).
[0229] Comparative Example 1 The release liner of the adhesive sheet (A1-1) was peeled off, and a 50 μm thick transparent polyethylene terephthalate film was laminated as a resin film layer B1 to one side of the exposed adhesive composition layer a1, and then a 50 μm thick transparent polyethylene terephthalate film was laminated as a resin film layer B2 to the other side of the adhesive composition layer a1 using a hand roller to form a laminate.
[0230] Next, the laminate was irradiated with about 100 mW / cm using an electrodeless lamp (Fusion Lamp H bulb). 2After irradiating with ultraviolet light of intensity of 1000 for 60 seconds, the sample was placed at 23°C and 50% RH for 30 minutes to prepare a substrate sample having a layer structure of resin film layer B1 / adhesive layer A1 / resin film layer B2 ( / is the adhesive interface).
[0231] Comparative Example 2 A substrate sample was produced in the same manner as in Example 1, except that the adhesive sheet (A1-3) was used instead of the adhesive sheet (A1-1).
[0232] Comparative Example 3 A substrate sample was produced in the same manner as in Example 1, except that the adhesive sheet (A1-4) was used instead of the adhesive sheet (A1-1).
[0233] (Reference example) A glass epoxy substrate having a thickness of 800 μm was used as a reference example.
[0234] Evaluation 1: Storage modulus E' of adhesive layer 25℃ > The adhesive composition used in each of the Examples and Comparative Examples was applied to a release film to form an adhesive composition layer having a thickness of 150 μm, and the adhesive composition layer was then subjected to irradiation with approximately 100 mW / cm using an electrodeless lamp (Fusion Lamp H bulb). 2 After irradiating with ultraviolet light of intensity of 100 nm for 60 seconds, the adhesive layer was cured by irradiating with light under conditions of 23°C and 50% RH for 30 minutes to prepare an adhesive layer. The adhesive layer was punched out into the shape of a type 5 test piece of JIS K 7127 using a dumbbell cutter, and the dynamic viscoelasticity of the test piece was measured using a dynamic viscoelasticity measuring device (manufactured by Rheometrics, product name: RSA-II) to measure the storage modulus E' at a frequency of 1.0 Hz and a temperature of 25°C. The measured value was used as the storage modulus (E') at 25°C measured at a frequency of 1.0 Hz of the adhesive layer of the sample in each example and comparative example. 25 ) was decided.
[0235] <Evaluation 2: Presence or absence of warping> The substrate samples prepared in the examples and comparative examples, and the evaluation sample obtained by cutting the glass epoxy substrate of the reference example into a square shape were used, and the evaluation samples were placed on a level desk, and the floating of each of the four sides of the evaluation sample from the horizontal plane was visually observed. The amount of warping (floating distance) of the substrate sample and the glass epoxy substrate from the mounting surface (horizontal plane) was measured according to the following criteria, and the presence or absence of warping was evaluated. The substrate samples prepared in the examples and comparative examples were used after 10 minutes had passed since their preparation. The position for measuring the amount of warping (floating distance) of each side of the evaluation sample was the position on each target side that was furthest from the horizontal plane when the evaluation sample was placed on a horizontal plane. (evaluation) ○: The amount of warping (floating distance) from the horizontal plane on all four sides of the evaluation sample was less than 1 mm △: Of the four sides of the evaluation sample, there was at least one side with a warp (floating distance) from the horizontal plane of 1 mm or more and 2.5 mm or less. ×: Of the four sides of the evaluation sample, at least one side had a warp (floating distance) exceeding 2.5 mm from the horizontal plane.
[0236] <Rating 3: Rigidity> Evaluation samples were prepared by cutting out the substrate samples prepared in the examples and comparative examples, and the glass epoxy substrate of the reference example to a length of 100 mm in the longitudinal direction X and a length of 15 mm in the transverse direction Y, and as shown in FIG. 3, an area of 10 mm from one end A in the longitudinal direction X of the evaluation sample S was fixed, and the position of the other end B of the evaluation sample S before the load was applied was set as a reference O. Next, a load W of 5 g was applied to the fixed end B of the evaluation sample S, and the end B was left stationary for 5 seconds, and then the position P of the end B of the evaluation sample S in the vertical (load) direction Z was measured. The distance L from the position (reference O) of the end B of the evaluation sample S before the load W was applied to the position P of the end B of the evaluation sample S when the load W was applied was calculated, and the rigidity was evaluated according to the following criteria. (evaluation) ○: Distance L is less than 15 mm △: Distance L is 15 mm or more and 45 mm or less ×: Distance L exceeds 45 mm
[0237] <Evaluation 4: Presence or absence of cutting powder during cutting> The substrate samples prepared in the Examples and Comparative Examples, and the glass epoxy substrate of the Reference Example were each cut into a size of 50 mm wide x 60 mm long using a dicing saw (manufactured by Disco Corporation, product name "DAD-522"). The blade used was ZH05-SD4000-N1-70-BB (manufactured by Disco Corporation), and the conditions were a blade height of 90 μm, a blade rotation speed of 40,000 rpm, and a dicing speed of 40 mm / sec. The presence or absence of cutting powder was evaluated according to the following criteria. (evaluation) 〇: No cutting powder was generated or cutting powder was not visually confirmed ×: Cutting powder was generated during cutting.
[0238] The configurations and evaluation results of the examples and comparative examples are shown in the table below.
[0239] [Table 1]
[0240] From Table 1, it can be seen that the composition has a layer structure of resin film layer B1 / adhesive layer A1 / resin film layer B2, the total thickness is a predetermined value or more, the adhesive layer A1 is formed of a cured product of a predetermined adhesive composition, and the thickness and storage modulus (E' 25 ), and the substrate samples of Examples 1 and 2 (rigid substrates of the first aspect of the present invention) in which the thicknesses of the resin film layers B1 and B2 were each equal to or greater than a predetermined value, had rigidity comparable to that of a glass epoxy substrate of the same total thickness, were free from warping, and no cutting powder was observed to be generated during cutting.
[0241] The adhesive layer A1 and the adhesive layer A2 are each formed of a cured product of a predetermined adhesive composition, and the adhesive layers A1 and A2 have a thickness and a storage modulus (E' 25), as well as the substrate sample of Example 3 (rigid substrate of the second aspect of the present invention) in which the thicknesses of the resin film layers B1 and B2 were each equal to or greater than a predetermined value, had rigidity comparable to that of a glass epoxy substrate, was not warped, and no cutting powder was observed during cutting.
[0242] On the other hand, the substrate sample of Comparative Example 1 did not have the same rigidity as the glass epoxy substrate because the resin film layer and the total thickness of the sample did not satisfy the prescribed range. Also, the substrate sample of Comparative Example 2 had an adhesive layer formed from a cured product of a photocurable adhesive (radical curable adhesive) that cures by a radical polymerization reaction, and the substrate sample warped more than a glass epoxy substrate of the same thickness. The substrate sample of Comparative Example 3 had a storage modulus (E' 25 ) did not satisfy the required range, and the same rigidity as that of a glass epoxy board of the same thickness could not be obtained. [Explanation of symbols]
[0243] 1...Adhesive layer A1 2...Resin film layer B1 3...Resin film layer B2 4. Middle class 5…Adhesive layer A2 10, 20...Rigid board
Claims
1. The adhesive film has at least an adhesive layer A1, a resin film layer B1 disposed on one main surface of the adhesive layer A1, and a resin film layer B2 disposed on the other main surface of the adhesive layer, The total thickness is 500 μm or more, The adhesive layer A1 is formed of a cured product of an adhesive composition including at least a photocurable resin having a polymerizable functional group other than a polymerizable unsaturated double bond, a thermoplastic resin having a polymerizable functional group other than a polymerizable unsaturated double bond, and a photopolymerization initiator; The adhesive layer A1 has a thickness of 100 μm or more, and the adhesive layer A1 has a storage modulus (E′) at 25° C. measured at a frequency of 1.0 Hz. 25 ) is 1.0 x 10 9 Pa or more, The resin film layer B1 and the resin film layer B2 each have a thickness of 50 μm or more.
2. 2. The rigid substrate according to claim 1, wherein the ratio of the thickness of said adhesive layer A1 to the total thickness is within a range of 20% to 90%.
3. The adhesive layer A1 has a resin film layer B1 disposed on one main surface of the adhesive layer A1, and a resin film layer B2 disposed on the other main surface of the adhesive layer, an intermediate layer C and an adhesive layer A2 are provided between the adhesive layer A1 and the resin film layer B2 in this order from the adhesive layer A1 side; The total thickness is 500 μm or more, The adhesive layer A1 and the adhesive layer A2 are each formed of a cured product of an adhesive composition including at least a photocurable resin having a polymerizable functional group other than a polymerizable unsaturated double bond, a thermoplastic resin having a polymerizable functional group other than a polymerizable unsaturated double bond, and a photopolymerization initiator; The thickness of each of the adhesive layers A1 and A2 is 50 μm or more, and the sum of the thicknesses of the adhesive layers A1 and A2 is 100 μm or more, The storage modulus (E') of the adhesive layer A1 and the adhesive layer A2 at 25°C measured at a frequency of 1.0 Hz 25 ) are 1.0 × 10 9 Pa or more, The resin film layer B1 and the resin film layer B2 each have a thickness of 50 μm or more.
4. 4. The rigid substrate according to claim 3, wherein the intermediate layer C is a layer selected from the group consisting of a resin film, a bakelite sheet, a decorative sheet, a decorative board, and a mineral sheet.
5. 5. The rigid board according to claim 3, wherein the intermediate layer C is a layer selected from the group consisting of a hard polyvinyl chloride layer, a melamine decorative plate, a paper Bakelite layer, a cloth Bakelite layer, and a mica plate.
6. 6. The rigid substrate according to claim 3, wherein the ratio of the sum of the thicknesses of the adhesive layers A1 and A2 to the total thickness is within a range of 20% to 80%.
7. 7. The rigid substrate according to claim 1, wherein at least one of the resin film layer B1 and the resin film layer B2 is a transparent resin film layer.
8. The resin film layer B1 and the resin film layer B2 are each independently a resin film selected from the group consisting of a polyethylene terephthalate film, a polyethylene film, and a polycarbonate film. A rigid substrate according to any one of claims 1 to 7.
9. The rigid substrate according to any one of claims 1 to 8, wherein when the rigid substrate cut into a rectangle is placed on a horizontal surface, the amount of warping of each of the four sides of the rigid substrate from the horizontal surface is 2500 μm or less.
10. 10. The rigid substrate according to claim 1, which is used as a substitute for a glass epoxy substrate.
11. A semiconductor support substrate using the rigid substrate according to any one of claims 1 to 10.
12. A reinforcing plate for a polishing pad, comprising the rigid substrate according to any one of claims 1 to 10.
13. A method for manufacturing a rigid substrate according to any one of claims 1 to 2 and claims 7 to 10, A step 1 of forming a laminate by bonding a resin film layer B1 and a resin film layer B2 to both main surfaces of an adhesive composition layer a1 containing at least a photocurable resin having a polymerizable functional group other than a polymerizable unsaturated double bond, a thermoplastic resin having a polymerizable functional group other than a polymerizable unsaturated double bond, and a photopolymerization initiator; a step 2 of irradiating the adhesive composition layer a1 with active energy rays from at least one of the resin film layer B1 side and the resin film layer B2 side of the laminate to form an adhesive layer A1 by curing the adhesive composition layer a1; A method for manufacturing a rigid substrate having the above-mentioned steps in this order.
14. A method for manufacturing a rigid substrate according to any one of claims 3 to 10, A step 1 of preparing a laminate 1 in which an adhesive composition layer a1 containing at least a photocurable resin having a polymerizable functional group other than a polymerizable unsaturated double bond, a thermoplastic resin having a polymerizable functional group other than a polymerizable unsaturated double bond, and a photopolymerization initiator is disposed on one surface of a resin film layer B1, and a laminate 2 in which an adhesive composition layer a2 containing at least a photocurable resin having a polymerizable functional group other than a polymerizable unsaturated double bond, a thermoplastic resin having a polymerizable functional group other than a polymerizable unsaturated double bond, and a photopolymerization initiator is disposed on one surface of a resin film layer B2; a step 2 of laminating the intermediate layer C and the laminate 1 such that one surface of the intermediate layer C contacts the adhesive composition layer a1 of the laminate 1, and laminating the intermediate layer C and the laminate 2 such that the other surface of the intermediate layer C contacts the adhesive composition layer a1 of the laminate 2, thereby forming a laminate 3 in which the resin film layer B1, the adhesive composition layer a1, the intermediate layer C, the adhesive composition layer a2, and the resin film layer B2 are laminated in this order; a step 3 of irradiating the adhesive composition layer a1 and the adhesive composition layer a2 with active energy rays from the resin film layer B1 side and the resin film layer B2 side of the laminate 3, respectively, to form an adhesive layer A1 and an adhesive layer A2 formed by curing the adhesive composition layer a1 and the adhesive composition layer a2; A method for manufacturing a rigid substrate having the above-mentioned steps in this order.
Citation Information
Patent Citations
Curable pressure-sensitive adhesive composition, curable pressure-sensitive adhesive sheet, and bonding method of optical or electronic substrate
JP2001247834A
Substrate treatment apparatus
JP2009164346A
Photosetting adhesive composition, polarizing plate and production method of the same, optical member, and liquid crystal display
JP2010209126A
Urethane resin composition, urethane resin molded article and method for producing the same