How to smelt oxide ores
The use of plant-derived reducing agents like starch in the smelting of nickel oxide ore addresses issues of non-uniform reduction and high costs by producing high-quality ferronickel with controlled drying and reduction processes, enhancing yield and reducing environmental impact.
Patent Information
- Application Number
- JP2020195444
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-25
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-11-25
AI Technical Summary
Existing smelting methods for nickel oxide ore face challenges in producing high-quality metals with uniform reduction reactions, leading to non-uniform metal distribution, low yield, and high manufacturing costs, while also posing environmental concerns due to the use of fossil fuels.
A smelting method using a plant-derived reducing agent, such as starch, to mix with nickel oxide ore, followed by drying at controlled temperatures and oxygen concentrations, and reducing the mixture in a mobile hearth furnace to produce high-quality ferronickel.
The method enhances the quality and uniformity of the reduced metal products, reduces environmental impact, and lowers production costs by utilizing renewable and cost-effective reducing agents.
Smart Images

Figure 0007552289000006 
Figure 0007552289000007 
Figure 0007552289000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a smelting method for producing a reduced product such as ferronickel by reducing and heating pellets produced from an oxide ore such as nickel oxide ore and a reducing agent at high temperatures in a reduction furnace. [Background technology]
[0002] Known methods for smelting nickel oxide ore called limonite or saprolite include a dry smelting method in which nickel matte is produced by roasting together with sulfur using a smelting furnace, a dry smelting method in which nickel matte is produced by reducing the ore with a carbonaceous reducing agent using a rotary kiln or a moving hearth furnace, and an autoclave in which a sulfurizing agent is added to the leachate obtained by leaching nickel and cobalt with sulfuric acid to produce a mixed sulfide.
[0003] Among the various smelting methods described above, when nickel oxide ore is smelted by reduction together with a carbon source, first, a pretreatment is performed to turn the raw material ore into agglomerates, slurry, etc. Specifically, when turning nickel oxide ore into agglomerates, that is, turning it from a powder or fine particle state into agglomerates, the nickel oxide ore is generally mixed with a binder, a reducing agent, etc., and then subjected to moisture adjustment, etc., before being charged into an agglomeration machine to turn it into agglomerates (referring to pellets, briquettes, etc.) of about 10 mm to 30 mm, for example.
[0004] The lumps need to have a certain degree of breathability to "evaporate" the moisture contained therein. Furthermore, if reduction does not proceed uniformly within the lumps, the composition of the resulting reduced product will be non-uniform, leading to problems such as metal dispersion or uneven distribution, so it is important to mix the mixture uniformly and to maintain as uniform a temperature as possible during the reduction treatment of the lumps.
[0005] In addition, it is also important to coarsen the ferronickel produced by reduction. This is because if the produced ferronickel has a fine size of, for example, several tens of μm to several hundreds of μm, it becomes difficult to separate it from the slag produced at the same time, and the recovery rate (yield) of ferronickel is significantly reduced. For this reason, a process for coarsening the ferronickel after reduction is necessary.
[0006] In addition, how to keep smelting costs as low as possible is also an important technical issue, and there is a demand for continuous processing that can be operated in compact facilities.
[0007] For example, Patent Document 1 discloses a method for producing granular metals in which agglomerates containing a metal oxide and a carbonaceous reducing agent are supplied onto the hearth of a moving-bed type reducing melting furnace, heated, and the metal oxide is reduced and melted, in which agglomerates having an average diameter of 19.5 mm to 32 mm are supplied onto the hearth and heated so as to have a laying density of 0.5 to 0.8, where the laying density is the relative value of the projected area ratio of the agglomerates onto the hearth to the maximum projected area ratio of the agglomerates onto the hearth when the distance between the agglomerates is 0. In this method, it is described that the productivity of granular metallic iron can be increased by controlling both the laying density and the average diameter of the agglomerates.
[0008] However, the method disclosed in Patent Document 1 is a technique for controlling the reaction occurring outside the agglomerates, and does not focus on controlling the reaction occurring inside the agglomerates, which is the most important factor in the reduction reaction. On the other hand, there has been a demand for obtaining higher quality metal (metal, alloy) by controlling the reaction occurring inside the agglomerates to increase the reaction efficiency and promote the reduction reaction more uniformly.
[0009] In addition, the method of using a specific diameter as the agglomerates as described in Patent Document 1 has a low yield when producing agglomerates because it is necessary to remove those that do not have the specific diameter. In addition, the method described in Patent Document 1 has a low productivity because it is necessary to adjust the spread density of the agglomerates to 0.5 to 0.8 and it is not possible to stack the agglomerates. For these reasons, the method described in Patent Document 1 has a high manufacturing cost.
[0010] As described above, the technology for producing metals and alloys by mixing and reducing oxide ores has many challenges in terms of increasing productivity, reducing production costs, and improving the quality of the metals. Furthermore, the amount of fossil fuels such as coal that can be used is limited, and after being used for reduction, they release CO into the environment. 2 There are also environmental issues, such as an increase in [Prior art documents] [Patent documents]
[0011] [Patent Document 1] JP 2011-256414 A Summary of the Invention [Problem to be solved by the invention]
[0012] The present invention aims to provide a method for smelting oxide ores in which a mixture containing an oxide ore, such as nickel oxide ore, is reduced to produce a metal, which can improve the grade of the resulting metal and efficiently produce a high-quality metal. [Means for solving the problem]
[0013] The present inventors have conducted extensive research to solve the above-mentioned problems, and as a result, have found that the above-mentioned problems can be solved by using a reducing agent containing a plant-derived reducing agent as a reducing agent in the mixing step, and subjecting the mixture to a drying treatment in advance in an atmosphere having an oxygen concentration of a predetermined concentration or less when subjecting the mixture to a reduction treatment, thereby completing the present invention.
[0014] (1) The first aspect of the present invention is a method for producing a mixture containing an oxide ore and a reducing agent, The method for smelting oxide ores includes a drying step of subjecting the mixture to a drying treatment, and a reducing step of subjecting the mixture that has undergone the drying step to a reduction treatment, in which a reducing agent containing a plant-derived reducing agent is used as the reducing agent in the mixing step, and in which the mixture is dried at a drying temperature of 100°C or higher and 500°C or lower in an atmosphere having an oxygen concentration of 3.0% by volume or lower in the drying step.
[0015] (2) A second aspect of the present invention is a method for smelting an oxide ore according to the first aspect of the present invention, wherein the plant-derived reducing agent is starch.
[0016] (3) A third aspect of the present invention is a method for smelting an oxide ore according to the first or second aspect of the present invention, wherein the content of the reducing agent in the mixture is 20% by mass or more and 80% by mass or less relative to 100% by mass of a chemical equivalent required for reducing the oxide ore.
[0017] (4) A fourth aspect of the present invention is a method for smelting an oxide ore according to any one of the first to third aspects of the present invention, wherein the oxide ore is a nickel oxide ore, and in the reduction step, a mixture containing the nickel oxide ore is subjected to a reduction treatment to produce ferronickel. Effect of the Invention
[0018] According to the method for smelting oxide ore of the present invention, high-quality metal can be efficiently produced. [Brief description of the drawings]
[0019] [Figure 1]FIG. 1 is a process diagram showing an example of the flow of a method for smelting nickel oxide ore. [Diagram 2] FIG. 1 is a diagram (plan view) showing a configuration example of a reducing furnace (rotary hearth furnace). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Specific embodiments of the present invention will be described in detail below. Note that the present invention is not limited to the following embodiments, and various modifications are possible without departing from the gist of the present invention.
[0021] 1. Overview of the Invention The present invention relates to a method for smelting an oxide ore, for example, nickel oxide ore, which is a raw material, and produces a metal as a reduced product by mixing the oxide ore with a reducing agent and reducing the resulting mixture. For example, when nickel oxide ore is used as the raw material ore, ferro-nickel metal, an alloy of iron and nickel, is produced as the reduced product.
[0022] Specifically, the method for smelting an oxide ore according to the present invention is characterized in that a reducing agent containing a plant-derived reducing agent is used as a reducing agent to be mixed with the raw oxide ore, and when subjecting the mixture to a reduction treatment, the mixture is previously subjected to a drying treatment at a drying temperature of 100°C or higher and 500°C or lower in an atmosphere with an oxygen concentration of 3.0% by volume or lower.
[0023] According to this method, the quality of the obtained metal can be improved by carrying out a reduction treatment on a mixture containing a predetermined amount of a plant-derived reducing agent as the reducing agent.
[0024] 2. Nickel oxide ore smelting method Hereinafter, as a specific embodiment of the present invention (hereinafter referred to as "the present embodiment"), a smelting method will be described as an example in which nickel oxide ore is used as a raw ore, and the nickel (nickel oxide) and iron (iron oxide) contained in the nickel oxide ore are metallized by reducing the nickel oxide ore to produce an iron-nickel alloy (ferronickel).
[0025] Specifically, as shown in FIG. 1, the method for smelting nickel oxide ore according to the present embodiment includes a mixing step S1 for obtaining a mixture containing an oxide ore and a reducing agent, an agglomerating step S2 for forming the obtained mixture into a predetermined shape to form an agglomerate, a drying step S3 for drying the obtained agglomerate, a reduction step S4 for subjecting the agglomerate (mixture) to a reduction treatment, and a recovery step S5 for recovering metal from the obtained reduced product (mixture).
[0026] <2-1. Mixing process> In the mixing step S1, nickel oxide ore and a reducing agent are mixed to obtain a mixture. Specifically, in the mixing step S1, a reducing agent is first added to nickel oxide ore, which is a raw material ore, and mixed, and then powders of iron ore, flux components, binders, etc., having a particle size of about 0.2 mm to 0.8 mm, are added as optional additives and mixed to obtain a mixture. The mixing process can be performed using a mixer, etc.
[0027] The nickel oxide ore as the raw material ore is not particularly limited, but limonite ore, saprolite ore, etc. can be used. Nickel oxide ore is a mixture of nickel oxide (NiO) and iron oxide (Fe 2 O 3 ) and at least
[0028] Here, a reducing agent containing a plant-derived reducing agent is used as a reducing agent that is mixed with nickel oxide ore to form a mixture in the mixing step S1. Examples of plant-derived reducing agents include organic reducing agents derived from plants that have the function of reducing oxide ores, and charcoal or bamboo charcoal obtained by carbonizing wood or bamboo derived from plants. In addition, waste materials or food waste containing these may also be used.
[0029] By subjecting a mixture containing a plant-derived reducing agent to a reduction treatment, the quality of the resulting metal can be improved.
[0030] Furthermore, plant-derived reducing agents are generally cheaper than fossil fuels such as coal, and are easily renewable. Also, unlike fossil fuels, plant-derived reducing agents have no risk of depletion. Furthermore, when considering the entire process from production to consumption as a plant-derived reducing agent, there is no greenhouse gas CO 2 It is a reducing agent with little environmental impact, as it does not increase the amount of
[0031] Although the use of a refined plant-derived organic reducing agent can efficiently and stably increase the quality of the resulting metal, unrefined plant-derived reducing agents or waste materials or food waste containing plant-derived organic reducing agents may also be used. This can reduce costs and also the environmental load. In this case, it is preferable to control the proportion of the plant-derived reducing agent and the moisture content within an acceptable range.
[0032] The plant-derived reducing agent is preferably an organic reducing agent derived from a plant. Since the plant-derived organic reducing agent is a compound (including a monomer, oligomer, and polymer) consisting of carbon, hydrogen, and oxygen, when the organic reducing agent in the mixture is heated in the drying step S3 or the reduction step S4 described later, the hydrogen and oxygen constituting the organic reducing agent are converted to H 2 As O is produced and removed, the remaining carbon constituting the organic reducing agent remains uniformly in the mixture. Then, in the reduction step S4 described below, the uniformly remaining carbon makes it possible to uniformly reduce the oxide ore, and the grade of the obtained metal can be efficiently and stably improved.
[0033] Examples of organic reducing agents derived from plants include starch, oil, wheat flour, cellulose, sucrose, lactose, glucose (α-glucose), fructose, etc. Among these, starch is particularly preferred. Starch is, for example, a polymer of α-glucose as represented by the following formula (1).
[0034] [ka]
[0035] Starch is a polymer made up of carbon, hydrogen, and oxygen, so it is easy to mix evenly into a mixture. Furthermore, starch has the property of increasing viscosity when it absorbs water, so it also functions as a binder, making it easy to mold the mixture.
[0036] Furthermore, since starch has an established purification method and it is easy to obtain starch with high purity and small variation in composition, the use of a reducing agent containing starch makes it possible to efficiently and stably increase the quality of the obtained metal.
[0037] Examples of starch include corn starch, wheat starch, rice starch, bean starch, potato starch, sweet potato starch, tapioca starch, potato starch, bracken starch, kudzu starch, and the like.
[0038] The content of the plant-derived reducing agent is preferably 50 mass% or more of the total amount of reducing agent contained in the mixture, preferably 70 mass% or more, and more preferably 90 mass% or more, and it is most preferable that the reducing agent contained in the mixture consists only of plant-derived reducing agent (i.e., the content of the plant-derived reducing agent is 100 mass% of the total amount of reducing agent contained in the mixture).
[0039] It is preferable that the reducing agent has a particle size and particle size distribution similar to those of the nickel oxide ore, which is the raw material ore described above. The similar particle size and particle size distribution are preferable because they facilitate uniform mixing and the reduction reaction occurs uniformly.
[0040] The amount of the reducing agent mixed is preferably 80% by mass or less, and more preferably 65.0% by mass or less, when the amount of the reducing agent necessary to reduce the nickel oxide and iron oxide constituting the nickel oxide ore without excess or deficiency is taken as 100% by mass. The lower limit of the amount of the reducing agent mixed is not particularly limited, but is preferably 20.0% by mass or more, and more preferably 23.0% by mass or more, relative to 100% by mass of the total value of the chemical equivalents.
[0041] The amount of reducing agent required to reduce nickel oxide and iron oxide without excess or deficiency can be rephrased as the total value of the chemical equivalent required to reduce all of the nickel oxide to nickel metal and the chemical equivalent required to reduce the iron oxide to iron metal (hereinafter also referred to as the "total value of chemical equivalents").
[0042] Examples of the iron ore that can be used as an optional additive include iron ore with an iron content of about 50 mass% or more, and hematite obtained by wet smelting of nickel oxide ore. Examples of the flux component include calcium oxide, calcium hydroxide, calcium carbonate, and silicon dioxide. Examples of the binder include bentonite, polysaccharides, resins, water glass, and dehydrated cake.
[0043] In mixing, kneading may be performed simultaneously or after mixing to improve the mixing property. Kneading can be performed using a batch kneader such as a Brabender, a Banbury mixer, a Henschel mixer, a helical rotor, a roll, a single-shaft kneader, a twin-shaft kneader, or the like. By kneading the mixture, a shear force is applied to the mixture, and the aggregation of the reducing agent and raw material powder can be broken down to mix uniformly, and the adhesion of each particle can be improved and voids can be reduced. This makes it easier for the reduction reaction to occur in the mixture and allows the reaction to occur uniformly, thereby shortening the reaction time of the reduction reaction. In addition, the variation in quality can be suppressed.
[0044] Also, after mixing, or after mixing and kneading, the mixture may be extruded using an extruder. This applies pressure (shear force) to the mixture, which breaks down agglomerations of the reducing agent, raw material powder, etc., making the mixture more uniformly mixed. Furthermore, voids within the mixture can be reduced. As a result, the reduction reaction of the mixture is more likely to occur uniformly in the reduction step S2 described below, the quality of the resulting metal can be improved, and high-quality metal can be produced.
[0045] The extruder is preferably one that can knead and mold the mixture under high pressure and high shear force, and examples of such extruders include a single screw extruder and a twin screw extruder. In particular, an extruder equipped with a twin screw extruder is preferable. By kneading the mixture under high pressure and high shear force, it is possible to break up the agglomerations of the mixture of raw material powders, and it is possible to effectively knead the mixture, and it is also possible to increase the strength of the mixture. Furthermore, by using an extruder equipped with a twin screw extruder, it is possible to obtain the mixture while maintaining a continuous high productivity.
[0046] In the mixing step S1, the raw material powder containing nickel oxide ore is mixed uniformly to obtain a mixture. Table 1 below shows an example of the composition (mass%) of some of the raw material powders mixed in the mixing step S1, but the composition of the raw material powder is not limited to this.
[0047] [Table 1]
[0048] <2-2. Agglomeration process> In the agglomeration step S2, the mixture is molded into a predetermined shape to form lumps (pellets). The agglomeration step is not an essential step, but molding the mixture into a predetermined shape can improve the ease of handling. The shape of the lumps (pellets) may be any shape that can be stacked on the hearth of the reduction furnace, and is preferably, for example, a spherical, rectangular, cubic, cylindrical, or other shape. Molding the mixture into such a shape makes it easier to mold the mixture, and therefore the cost of molding can be reduced. In addition, since the molded shape is not complicated, the occurrence of pellets with molding defects can be reduced.
[0049] In the agglomeration step S2, for example, the mixture can be molded using a pellet molding device. The pellet molding device is not particularly limited, but is preferably one that can knead and mold the mixture under high pressure and high shear force. By kneading the mixture under high pressure and high shear, it is possible to break up the agglomerations of the raw material powder mixture, to effectively knead the mixture, and to increase the strength of the resulting pellets.
[0050] It is also possible to form the powder using a briquette press. The appropriate equipment can be selected in consideration of the equipment, pellet strength, yield, etc.
[0051] <2-3. Drying process> In the drying step S3, the aggregates obtained in the agglomerating step S2 are dried. When the mixture is mixed with a large amount of water in the kneading in the mixing step S1 or the agglomerating step S2 or in the molding of the aggregates, the moisture content of the atmospheric gas in the reduction furnace can be reduced by subjecting the aggregates (mixture) to a drying treatment.
[0052] In addition, when a reducing agent containing starch is used, when the lump is dried and the starch in the lump is heated, at least some of the hydrogen and oxygen that compose the starch are converted to H 2 O is generated and escapes. By drying the aggregates obtained in the agglomeration step S2, it is possible to prevent the aggregates from collapsing, which makes it difficult to remove them from the reduction furnace. In addition, it is possible to more effectively reduce the amount of moisture contained in the atmospheric gas in the reduction furnace, and it is possible to more effectively suppress the oxidation of the metal contained in the aggregates.
[0053] However, because plant-derived reducing agents are relatively susceptible to decomposition and oxidization, the mixture may burn if a large amount of oxygen is present during drying. This makes it impossible to carry out the reduction treatment properly in the reduction step described below, and causes a decrease in the quality of the resulting metal.
[0054] Therefore, when the mixture is subjected to a reduction treatment, the mixture is dried in advance at a drying temperature of 100°C or higher and 500°C or lower in an atmosphere with an oxygen concentration of 3.0% by volume or lower. This prevents the mixture from burning due to the presence of oxygen during drying, and makes it possible to appropriately perform the reduction treatment in the reduction step described below while maintaining the mixture ratio of the oxide ore and the reducing agent at a desired ratio.
[0055] If the drying temperature is less than 100°C, the drying will not be sufficient and it will not be possible to prevent the collapse of the lumps. Furthermore, it will not be possible to reduce the amount of moisture contained in the atmospheric gas in the reduction furnace, making it impossible to suppress the oxidation of the metal. If the drying temperature is more than 500°C, a reduction process will be performed in the drying process, and the reduction process described below will not be performed properly, which will cause a decrease in the quality of the resulting metal.
[0056] In particular, when using a reducing agent containing starch, at least some of the hydrogen and oxygen that compose the starch must be converted to H 2 This generates O which cannot escape, resulting in a decrease in metal grade.
[0057] The drying temperature is preferably 200° C. or higher, and more preferably 250° C. or higher. The drying temperature is preferably 490° C. or lower. The oxygen concentration is preferably 2.8% by volume or lower.
[0058] The method for drying the aggregates is not particularly limited as long as the mixture is dried at a drying temperature of 100°C to 500°C in an atmosphere with an oxygen concentration of 3.0% by volume or less, and conventionally known means can be used, such as a method of keeping the aggregates at a drying temperature of 100°C to 500°C or a method of blowing hot air at a predetermined drying temperature onto the mixture to dry it. By such a drying process, for example, the solid content of the aggregates is about 70% by mass and the moisture content is about 30% by mass. Note that the temperature of the mixture itself during this drying process is preferably less than 100°C, which can prevent the mixture from bursting due to bumping of moisture.
[0059] This drying step may be carried out outside a reduction furnace, which will be described later, or the lumps may be placed in a reduction furnace, which will be described later, and the drying process may be carried out in the reduction furnace.
[0060] Here, when drying lumps having a particularly large volume, it is acceptable for the lumps to have cracks or cracks before and after drying. When the volume of the lumps is large, they melt and shrink during reduction, which often results in cracks or cracks. However, when the volume of the lumps is large, the effect of the increase in surface area caused by the cracks or cracks is small, and therefore it is unlikely that a major problem will occur. Therefore, it is acceptable for the lumps before reduction to have cracks or cracks.
[0061] The drying process may be carried out continuously at one time or in several separate steps. By carrying out the drying process in several separate steps, the mixture can be more effectively prevented from bursting. When the drying process is carried out in several separate steps, the drying temperature for the second and subsequent steps is preferably 150°C or higher and 400°C or lower. Drying within this range makes it possible to dry the mixture without causing the reduction reaction to proceed.
[0062] An example of the composition (parts by mass) of the solid content in the aggregates (mixture) after drying treatment is shown in the following Table 2. Note that the composition of the aggregates (mixture) is not limited to this.
[0063] [Table 2]
[0064] <2-4. Reduction process> In the reduction step S4, the lumps (mixture) obtained in the drying step are subjected to a reduction treatment. Specifically, the lumps (mixture) obtained are charged into a reduction furnace, and the mixture is subjected to a heating reduction treatment. The heating reduction treatment in the reduction step S2 causes a smelting reaction (reduction reaction) to proceed based on the reducing agent in the mixture, and ferronickel metal (hereinafter simply referred to as "metal") and ferronickel slag (hereinafter simply referred to as "slag") are generated separately in the mixture.
[0065] In the heat reduction process, for example, in a short time of about one minute, nickel oxide and iron oxide in the mixture are first reduced and metalized to ferronickel near the surface of the mixture where the reduction reaction is likely to proceed, forming a shell. Meanwhile, in the shell, the slag components gradually melt as the shell forms, forming liquid slag. As a result, metal and slag are generated separately in the mixture.
[0066] After about 10 minutes of treatment, the excess reducing agent that is not involved in the reduction reaction is absorbed into the metal, lowering its melting point and causing the metal to become liquid.
[0067] In this case, the quality of the obtained metal can be improved by subjecting the mixture containing a plant-derived reducing agent as the reducing agent to a reduction treatment.
[0068] Furthermore, in the reduction step described above, the mixture is dried at a drying temperature of 100°C or higher and 500°C or lower in an atmosphere with an oxygen concentration of 3.0% by volume or lower, thereby preventing the mixture from burning due to the presence of oxygen during drying. This makes it possible to appropriately carry out the reduction process while maintaining the mixture ratio of the oxide ore and the reducing agent at a desired ratio.
[0069] In addition, when a plant-derived organic reducing agent is used as the plant-derived reducing agent, there is a possibility that it may burn during the heat reduction treatment. Therefore, it is preferable to perform the reduction treatment on the mixture containing the plant-derived organic reducing agent in an atmosphere with a low oxygen concentration. For example, the reduction treatment is preferably performed in an atmosphere with an oxygen concentration of 3.0% by volume or less, and more preferably in an atmosphere with an oxygen concentration of 1.0% by volume or less. The reduction treatment may also be performed in an inert gas atmosphere such as nitrogen or argon.
[0070] In addition, when using a reducing agent containing a plant-derived organic reducing agent, when the organic reducing agent in the mixture is heated, the hydrogen and oxygen that compose the organic reducing agent are converted to H2 As O is produced and released, the remaining carbon remains in the mixture. As a result, the remaining carbon acts as a reducing agent to uniformly reduce the ore.
[0071] The temperature in the reduction treatment (reduction temperature) is not particularly limited, but is preferably in the range of 1200°C to 1450°C, and more preferably in the range of 1300°C to 1400°C. By carrying out reduction within such a temperature range, the reduction reaction can be caused to occur uniformly, and ferronickel with reduced quality variation can be produced. Moreover, by carrying out reduction at a reduction temperature more preferably in the range of 1300°C to 1400°C, the desired reduction reaction can be caused to occur in a relatively short time.
[0072] The time for the reduction treatment (treatment time) is set according to the temperature of the reduction furnace, but is preferably 10 minutes or more, and more preferably 15 minutes or more. On the other hand, the upper limit of the time for the reduction heat treatment may be 50 minutes or less, or 40 minutes or less, from the viewpoint of suppressing an increase in production costs.
[0073] The heat required for reduction, calculated by multiplying the reduction temperature (°C) by the reduction time (min), is preferably in the range of 20,000 (°C x min) to 40,000 (°C x min). This allows efficient production of high-quality metal.
[0074] The reduction furnace may be a fixed hearth, but it is preferable to use a moving hearth furnace. By using a moving hearth furnace as such a reduction furnace, the mixture can be treated more efficiently. In addition, by using a moving hearth furnace, the reduction reaction proceeds continuously and the reaction can be completed in one facility, and the treatment temperature can be controlled more accurately than when the treatment in each step is performed using separate furnaces. Furthermore, the heat loss between each treatment is reduced, making it possible to operate more efficiently. Below, the configuration of a rotary hearth furnace as an example of a moving hearth furnace is explained using FIG. 2.
[0075] FIG. 2 is a diagram (plan view) showing an example of the configuration of a rotary hearth furnace with a rotating hearth. As shown in FIG. 2, a rotary hearth furnace 2 that is circular and divided into a plurality of processing chambers 20a to 20d can be used. In the rotary hearth furnace 2, each process is performed in each region while rotating in a predetermined direction. In this rotary hearth furnace, the processing temperature in each region can be adjusted by controlling the time (moving time, rotating time) when passing through each region, and the mixture 1 is smelted every time the rotary hearth furnace rotates once. Here, the rotary hearth furnace 2 may be provided with a preheating chamber outside the furnace. In addition, the rotary hearth furnace 2 may be provided with a cooling chamber outside the furnace. The moving hearth furnace may be a roller hearth kiln or the like.
[0076] The heating means of the reduction furnace is not particularly limited, and may be a burner or may be one using electricity or the like. A burner is preferable because it can effectively perform a heating and reducing treatment on the mixture in a short time. When a reduction furnace having a burner is used, for example, LPG, LNG, coal, coke, pulverized coal, or the like is used as the fuel. The cost of these fuels is very low, and the equipment costs and maintenance costs can be kept significantly lower than those of an electric furnace or the like.
[0077] <2-5. Recovery process> In the recovery step S5, the metal is recovered from the reduced product obtained in the reduction step S4. Specifically, the reduced product (mixture) containing a metal phase and a slag phase obtained by the thermal reduction treatment is cooled, and if necessary, pulverized to form a powder, and the metal (metal powder particles) is separated and recovered.
[0078] Methods for separating the metal phase and the slag phase from the mixture of the metal phase and the slag phase obtained as a solid include, for example, sieving to remove unnecessary materials, as well as separation by specific gravity or magnetic force.
[0079] Furthermore, the obtained metal phase and slag phase have poor wettability and can be easily separated. For example, by dropping the large mixture obtained by the reduction step S4 described above from a predetermined drop or by applying a predetermined vibration during sieving, the metal phase and slag phase can be easily separated from the mixture.
[0080] By separating the metal phase from the slag phase in this manner, the metal phase is recovered. EXAMPLES
[0081] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.
[0082] [Mixing process] For each sample, nickel oxide ore as raw ore, iron ore, silica sand and limestone as flux components, and a reducing agent were mixed in a mixer while adding an appropriate amount of water to obtain a mixture. As the reducing agent, a plant-derived reducing agent (starch) or pulverized coal (coal) was used to reduce nickel oxide and iron oxide (Fe 2 O 3 ) were contained in the amounts shown in Table 4 relative to the required chemical equivalent of 100 mass %.
[0083] [Clumping process] Next, the mixture obtained for each sample was formed into a sphere using a pelletizer to obtain a lump (sample) having a diameter of 15±0.3 mm.
[0084] [Drying process] Next, the aggregates obtained in the agglomeration step were subjected to a drying treatment under the conditions shown in Table 3 so that the solid content was about 70% by mass and the moisture content was about 30% by mass. The drying time was 2 hours for each.
[0085] [Reduction process] Next, the lumps (samples) obtained in the drying process were each charged into a reduction furnace under a nitrogen atmosphere substantially free of oxygen. The temperature condition during charging into the reduction furnace was 500±20°C.
[0086] Next, the mixture pellets were subjected to a reducing heat treatment at the temperature and for the time shown in Table 4. After the reducing treatment, the pellets were quickly cooled to room temperature in a nitrogen atmosphere, and then taken out into the air.
[0087] Here, the lump is charged into the reduction furnace by first adding ash (mainly composed of SiO 2 The other components are Al 2 O 3 The experiment was carried out by spreading a layer of silica gel (containing small amounts of oxides such as MgO) on the surface and placing the block on top of it.
[0088] [Recovery process] After the reduction heat treatment, each reduced material (sample) was crushed by wet processing, and the metal was recovered by magnetic separation. The nickel metallization rate and the nickel content in the metal were analyzed and calculated using an ICP emission spectrometer (SHIMAZU S-8100 model).
[0089] The nickel metallization rate, nickel content in the metal, and nickel metal recovery rate were calculated using the following formulas (1), (2), and (3). Nickel metallization rate = mass of nickel in metal / (mass of all nickel in reduced material) × 100 (%) (1) Nickel content in metal = mass of nickel in metal / (total mass of nickel and iron in metal) × 100 (%) (2) Nickel metal recovery rate = amount of nickel recovered / (amount of ore input × nickel content in ore) × 100 (3)
[0090] Table 4 below shows the nickel metallization rate, nickel content in the metal, and nickel metal recovery rate for each sample.
[0091] [Table 3]
[0092] [Table 4]
[0093] As shown in the results of Tables 3 and 4, in Examples 1 to 15, in which a reducing agent containing a plant-derived reducing agent was used as the reducing agent and the mixture was dried at a drying temperature of 100°C to 500°C in an atmosphere with an oxygen concentration of 3.0% by volume or less, good results were obtained in terms of the nickel metallization rate and the nickel content in the metal. This shows that the method for smelting oxide ore according to the present invention can efficiently produce high-quality metal.
[0094] On the other hand, in Comparative Example 1, in which the mixture was dried at a drying temperature of over 500°C, and in Comparative Example 2, in which the mixture was dried in an atmosphere with an oxygen concentration of over 3.0% by volume, it was not possible to efficiently produce a high-quality metal. Also, in Reference Examples 1 and 2, in which a reducing agent containing a plant-derived reducing agent was not used as the reducing agent, it was not possible to efficiently produce a high-quality metal. [Explanation of symbols]
[0095] 1 mixture 2 Rotary bed furnace 20a~20d Processing chamber 21 Preheating Room 40 Cooling room
Claims
1. A method for producing a nickel oxide ore, comprising: a drying step of subjecting the mixture to a drying treatment; A reduction step of producing ferronickel by subjecting the mixture that has been subjected to the drying step to a reduction treatment, In the mixing step, a plant-derived organic reducing agent is used as the reducing agent, In the reduction step, a value obtained by multiplying the reduction temperature (° C.) and the reduction time (min.) is 20,000 (° C.×min.) or more and 40,000 (° C.×min.) or less; In the drying step, the mixture is dried at a drying temperature of 280° C. or more and 490° C. or less in an atmosphere having an oxygen concentration of 1.5% by volume or more and 2.8% by volume or less. A method for smelting oxide ores.
2. The plant-derived organic reducing agent is starch; The starch is mixed in the mixture so that the content of the starch in the mixture is 21% by mass or more and 48% by mass or less with respect to 100% by mass of a chemical equivalent necessary for reducing nickel oxide and iron oxide constituting the nickel oxide ore. A method for smelting oxide ore according to claim 1.
Citation Information
Patent Citations
process for the production of iron ore briquettes
DE1123351A
Hydrometallugy of ore containing iron group metal
JP2000008128A
Method for producing reduced metal
JP2003105452A
Self-reducing cold-bonded pellets
JP2007523256A
Production of iron using environment-friendly renewable reducing agents or regenerated reducing agents
JP2009530492A