Production method of high-homogeneity high-toughness S355MLO maritime work steel thick plate

Through low-carbon composition design and strong rolling process, combined with smelting and continuous casting, the low toughness and stability of the thick plate of offshore steel under low temperature conditions of -50℃ is solved, and high homogeneity and high toughness are achieved. The production of steel thick plates improves performance stability and pass rate, and has excellent welding performance.

CN118979189APending Publication Date: 2024-11-19NANJING IRON & STEEL CO LTD
View PDF 0 Cites 6 Cited by

Patent Information

Application Number
CN202411048760.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The low toughness and stability of existing marine steel thick plates under low temperature conditions of -50℃ lead to low product qualification rate, especially when the thickness increases, it is difficult to ensure uniformity of performance.

Method used

Using low-carbon component design, low-temperature heating and strong controlled rolling technology, the center segregation is improved through smelting process optimization, continuous casting cooling and dynamic pressure process, and combined with top-bottom complex blowing furnace, LF refining and RH vacuum process, the chemical composition of the steel plate is controlled and The rolling process improves the structural uniformity and grain size of the thick plate, thereby improving the low-temperature impact performance of -50℃.

Benefits of technology

It effectively improves the full thickness of the marine steel thick plate -50℃ low-temperature toughness and performance stability, improves the product's pass rate, and has excellent welding performance to meet the technical needs of complex service environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses a production method of a high-homogeneity high-toughness S355MLO marine steel thick plate. The steel plate comprises the following chemical components in percentage by mass: 0.03 to 0.07 percent of C, 0.15 to 0.35 percent of Si, 1.45 to 1.65 percent of Mn, less than or equal to 0.015 percent of P, less than or equal to 0.005 percent of S, 0.025 to 0.045 percent of Alt, 0.025 to 0.040 percent of Nb, 0.25 to 0.50 percent of Ni, 0.10 to 0.25 percent of Cr, less than or equal to 50ppm of N and less than or equal to 2ppm of H. The impurity elements comprise less than or equal to 0.020% of As, less than or equal to 0.010% of Sb, less than or equal to 0.020% of Sn, less than or equal to 0.010% of Pb, less than or equal to 0.010% of Bi, less than or equal to 0.0025% of Ca, less than or equal to The method has the advantages that the low-temperature toughness, the stability and the qualified rate of the total thickness at the temperature of-50 DEG C are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of iron and steel metallurgy, and in particular relates to a method for producing a high-homogeneity and high-toughness S355MLO marine engineering steel thick plate. Background Art

[0002] Offshore steel thick plates are widely used in the construction of oil and gas production platforms. Due to the complex service environment requirements, the materials are usually required to have low-temperature toughness, high uniformity, excellent welding performance and other technical requirements. Generally speaking, for thick plates below 80mm, the core penetration can be increased, the grains can be refined, and the performance uniformity can be improved through low-carbon equivalent design and rolling process optimization; but for thick plates above 80mm, it is difficult to effectively ensure the core penetration when the compression ratio is constant. How to ensure that the thickness increases while improving the uniformity of the performance in the thickness direction becomes the key to the TMCP thick plate process.

[0003] As the technical requirements for offshore service conditions become increasingly higher, higher technical requirements are put forward for offshore steel materials themselves. The impact toughness is adjusted from the original -40℃ impact to -50℃, and requirements are put forward from the near surface, 1 / 4 position to the core of the steel plate, and the performance uniformity of the thick plate is demanding. The patent with application number CN202211408508.6 discloses an extra-thick S355MLO steel plate for fixed offshore structures and its production method. High-quality continuous casting billets are obtained through innovative low-manganese components + smelting methods, and 100~120mm extra-thick S355MLO steel plates are produced by rolling and heat treatment methods. The low-temperature toughness of the near surface + 1 / 2 position at -40℃ is good. The patent with application number CN202211587741.5 discloses a TMCP process extra-thick steel plate and its production method, which adopts composition design, two-fire low-temperature rolling, relaxation and strong cooling process to accurately control the phase change structure after rolling, forming a fine multiphase structure to refine the original austenite grains, and the low-temperature -40℃ impact toughness at the 1 / 4 position and the core position reaches more than 100J, and the continuous casting billet is used to produce a high-toughness steel plate with a low-temperature impact requirement of more than -40℃. In addition, the patent with application number CN202410168048.7 discloses a thick specification high-toughness marine engineering structural steel and a preparation method. Through the design of an economic component system, matching heating and controlling the rolling cooling process, the thick specification high-strength and high-toughness marine engineering wind power steel plate is stably produced, and the -40℃ low-temperature impact toughness and section shrinkage rate of the core are improved.

[0004] However, the above patent proposes optimization of composition and rolling process, and the low-temperature impact is -40°C. The impact positions involve near the surface, 1 / 4 position and core, with the focus on the core. The -50°C low-temperature impact problem of the full thickness of the thick plate is not involved. Summary of the invention

[0005] The purpose of the present invention is to solve the problems of insufficient low-temperature toughness at -50°C, poor stability and low product qualification rate of existing marine steel thick plates, and to provide a method for producing high-homogeneity and high-toughness S355MLO marine steel thick plates. The impact performance of the thick plates is improved by controlling the internal quality and rolling process, and the uniformity of the impact performance of the thick plates is improved by controlling the structure and grain size of the thick plates, thereby effectively improving the performance qualification rate of TMCP thick plates, and the method is suitable for the production of TMCP marine steel thick plates.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions: A method for producing a high-homogeneity and high-toughness S355MLO marine steel thick plate. The chemical composition of the steel plate and its mass percentage content include: C: 0.03-0.07%, Si: 0.15-0.35%, Mn: 1.45-1.65%, P≤0.015%, S≤0.005%, Alt: 0.025-0.045%, Nb: 0.025-0.040%, Ni: 0.25-0.50%, Cr: 0.10-0.25%, N≤50ppm, H≤2ppm; wherein the impurity elements include: As≤0.020%, Sb≤0.010%, Sn≤0.020%, Pb≤0.010%, Bi≤0.010%, Ca≤0.0025%, B≤0.0005%, and the rest are Fe and unavoidable impurities.

[0007] Furthermore, the thickness of the steel plate is 80-120 mm, and the mechanical properties meet R eH ≥355Mpa, R m It is 470~630Mpa, A≥22%, yield strength ratio≤0.93%, -50℃ lateral impact values ​​include: near surface ≥150J, 1 / 2 and 1 / 4 ≥200J, section shrinkage ≥40%, 5% time-effect strain impact value ≥150J.

[0008] Furthermore, the method for producing high-homogeneity and high-toughness S355MLO marine steel thick plates includes a smelting process, a heating process and a rolling process that cooperate with each other. In the smelting process, a top and bottom combined blowing converter + LF refining + RH vacuum + continuous casting process is adopted; the oxygen of the converter steel is controlled to be ≤500ppm, the LF refining furnace produces white slag, and the calcium-aluminum ratio is controlled to be 1.6~1.8 to improve the purity of the molten steel; continuous casting uses 460mm billet, cooling adopts a strong cooling system, and the dynamic reduction is controlled at 13~15mm to improve center segregation.

[0009] Furthermore, in the heating process, the ingot cooling time is ≥72h, and a continuous furnace is used for segmented heating, with a total heating time of 9-13min / cm, a soaking section for 60-80min, and a soaking temperature of 1070-1100°C to prevent excessive growth of surface grains.

[0010] Furthermore, in the rolling process, rough rolling is performed 7 to 11 times, the intermediate billet thickness is 130 to 180 mm, and the total reduction rate of the last three rough rolling times is ≥30%; finishing rolling is performed 7 to 9 times, the reduction rate of the first finishing rolling time is ≥10%, the starting rolling temperature is 740 to 780°C, and the final cooling temperature is 400 to 450°C.

[0011] Furthermore, the chemical composition of the steel plate and its mass percentage include: C: 0.052%, Si: 0.30%, Mn: 1.47%, P: 0.012%, S: 0.002%, Alt: 0.034%, Ni: 0.35%, Nb: 0.031%, Cr: 0.12%, N: 0.0040%, H: 0.00015%, and the rest are Fe and unavoidable impurities.

[0012] Furthermore, the method for producing the high-homogeneity and high-toughness S355MLO marine steel thick plate comprises: (1) In the smelting process, the smelting and continuous casting processes are used to ensure high purity and internal quality of molten steel. The top and bottom combined blowing converter + LF refining + RH vacuum + continuous casting process is adopted. The oxygen of the converter steel is 490ppm, the LF refining furnace produces white slag, and the calcium-aluminum ratio is controlled at 1.7. 460mm billet is used for continuous casting, and a strong cooling secondary cooling system is adopted. The dynamic reduction is controlled at 13mm, and the main reduction sections are in sections 6 and 7 to improve the center segregation. (2) In the heating process, the billet cooling time is ≥72h, and continuous furnace is used for segmented heating. The total heating time is 12min / cm, the soaking section is kept warm for 70min, and the soaking temperature is 1080℃ to prevent excessive growth of surface grains; (3) In the rolling process, the thickness of the rolled steel plate is 100 mm, the width is 3000 mm, the rough rolling is 11 passes, the intermediate billet thickness is 155 mm, and the total reduction rate of the last three rough rolling passes is 33%; the finishing rolling is 6 passes, the reduction rate of the first finishing rolling pass is 12%, the starting rolling temperature is 745°C, and the final cooling temperature is 405°C.

[0013] Furthermore, the chemical composition of the steel plate and its mass percentage include: C: 0.045%, Si: 0.25%, Mn: 1.58%, P: 0.010%, S: 0.001%, Alt: 0.032%, Ni: 0.42%, Nb: 0.033%, Cr: 0.13%, N: 0.0039%, H: 0.00010%, and the rest are Fe and unavoidable impurities.

[0014] Furthermore, the method for producing the high-homogeneity and high-toughness S355MLO marine steel thick plate comprises: (1) In the smelting process, the smelting and continuous casting processes are used to ensure high purity and internal quality of molten steel. The top and bottom combined blowing converter + LF refining + RH vacuum + continuous casting process is adopted. The oxygen content of the converter steel is 485ppm, and the LF refining furnace produces white slag, and the calcium-aluminum ratio is controlled at 1.65. 460mm billet is used for continuous casting, and a strong cooling secondary cooling system is adopted. The dynamic reduction is controlled at 14mm, and the main reduction sections are in sections 6 and 7 to improve the center segregation. (2) In the heating process, the billet cooling time is ≥72h, and continuous furnace heating is adopted. The total heating time is 13min / cm, the soaking section is kept warm for 72min, and the soaking temperature is 1075℃ to prevent excessive growth of surface grains. (3) In the rolling process, the thickness of the rolled steel plate is 120 mm, the width is 3000 mm, the rough rolling is 11 passes, the intermediate billet thickness is 145 mm, and the total reduction rate of the last three rough rolling passes is 32%; the finishing rolling is 8 passes, the reduction rate of the first finishing rolling pass is 11%, the starting rolling temperature is 745°C, and the final cooling temperature is 420°C.

[0015] In the technical solution of the present invention, low-carbon component design, low-temperature heating and strong controlled rolling processes are adopted, continuous casting cooling and dynamic pressing processes are optimized, center segregation is improved, large pressing and strong controlled rolling processes are utilized to improve the penetration of the core of the thick plate, and low-temperature heating is used to improve the surface organization, thereby achieving high-homogeneity and high-toughness thick plate organization control, and achieving -50°C low-temperature toughness improvement of the entire thickness of the thick plate, effectively improving the performance stability and qualified rate of the marine steel thick plate, the product meets the -50°C impact performance near the surface, 1 / 4 position and the core, has excellent welding performance, and the product can meet the technical requirements of marine steel in special, low-temperature and complex service environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a microstructure photo of the 120 mm thick S355MLO offshore steel near the surface 2 mm in this embodiment; Figure 2 This is a photo of the 1 / 4 position structure of the 120 mm thick S355MLO marine steel of this embodiment; Figure 3 This is a photo of the core structure of the 120 mm thick S355MLO marine steel in this embodiment; Figure 4 This is the mechanical properties table of 100 mm thick S355MLO marine steel in Example 1; Figure 5 This is a table of mechanical properties of 120 mm thick S355MLO marine steel in Example 2. DETAILED DESCRIPTION Example 1

[0017] To make the present invention more clear, a method for producing a high-homogeneity and high-toughness S355MLO marine steel thick plate of the present invention is further described below in conjunction with the accompanying drawings. The specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.

[0018] In this embodiment, taking 100mmS355MLO thick plate as an example, the chemical composition of the steel plate and its mass percentage include: C: 0.052%, Si: 0.30%, Mn: 1.47%, P: 0.012%, S: 0.002%, Alt: 0.034%, Ni: 0.35%, Nb: 0.031%, Cr: 0.12%, N: 0.0040%, H: 0.00015%, and the rest are Fe and unavoidable impurities.

[0019] The production method specifically includes: (1) According to the above-mentioned composition control, the smelting and continuous casting processes are used to ensure high purity and internal quality of molten steel. The top and bottom combined blowing converter + LF refining + RH vacuum + continuous casting process is adopted; the converter oxygen is 490ppm, the LF refining furnace produces white slag, and the calcium-aluminum ratio is controlled at 1.7; 460mm billet is used for continuous casting, and a strong cooling secondary cooling system is adopted. The dynamic reduction is controlled at 13mm, and the main reduction sections are in sections 6 and 7 to improve center segregation.

[0020] (2) The heating process: the billet cooling time is ≥ 72 hours, continuous furnace segmented heating is adopted, the total heating time is 12 min / cm, the soaking section is kept warm for 70 min, and the soaking temperature is 1080°C to prevent excessive growth of surface grains.

[0021] (3) The rolling process: the thickness of the rolled steel plate is 100 mm, the width is 3000 mm, the rough rolling is 11 passes, the intermediate billet thickness is 155 mm, the total reduction rate of the last three rough rolling passes is 33%; the finishing rolling is 6 passes, the reduction rate of the first finishing rolling pass is 12%, the starting rolling temperature is 745°C, and the final cooling temperature is 405°C.

[0022] The mechanical properties of the 100 mm thick S355MLO marine steel in this example are shown in Figure 4 , the CTOD characteristic values ​​of the parent material welding at -10℃ are 1.216mm, 1.117mm, and 1.123mm respectively. The steel plate is welded, and the -50℃ impact values ​​of the weld joints at different positions are: weld center WM: 128 / 124 / 88, fusion line FL: 199 / 206 / 231, fusion line FL+2mm: 285 / 287 / 242, fusion line FL+5mm: 346 / 341 / 307. The heat affected zone has excellent impact properties. Example 2

[0023] In this embodiment, a 120 mm S355MLO thick plate is taken as an example. The chemical composition of the steel plate and its mass percentage include: C: 0.045%, Si: 0.25%, Mn: 1.58%, P: 0.010%, S: 0.001%, Alt: 0.032%, Ni: 0.42%, Nb: 0.033%, Cr: 0.13%, N: 0.0039%, H: 0.00010%, and the rest are Fe and unavoidable impurities.

[0024] The production method is as follows: (1) According to the above-mentioned composition control, the smelting and continuous casting processes are used to ensure high purity and internal quality of molten steel. The top and bottom combined blowing converter + LF refining + RH vacuum + continuous casting process is adopted; the oxygen content of the converter steel is 485ppm, the LF refining furnace produces white slag, and the calcium-aluminum ratio is controlled at 1.65; 460mm billet is used for continuous casting, and a strong cooling secondary cooling system is adopted. The dynamic reduction is controlled at 14mm, and the main reduction sections are in sections 6 and 7 to improve the center segregation.

[0025] (2) The heating process: the billet cooling time is ≥ 72 hours, continuous furnace segmented heating is adopted, the total heating time is 13 min / cm, the soaking section is kept warm for 72 minutes, and the soaking temperature is 1075°C to prevent excessive growth of surface grains.

[0026] (3) The rolling process is as follows: the thickness of the rolled steel plate is 120 mm, the width is 3000 mm, the rough rolling is performed in 11 passes, the intermediate billet thickness is 145 mm, the total reduction rate of the last three rough rolling passes is 32%, the finishing rolling is performed in 8 passes, the reduction rate of the first finishing rolling pass is 11%, the starting rolling temperature is 745°C, and the final cooling temperature is 420°C.

[0027] In this embodiment, the mechanical properties of 120 mm thick S355MLO marine steel are shown in Figure 5 , its full thickness tissue picture is as follows Figure 1 , Figure 2 and Figure 3 As shown in the figure, the CTOD characteristic values ​​of the parent material at -10℃ are 1.160mm, 1.147mm, and 1.122mm respectively. The steel plate is welded, and the -50℃ impact values ​​of the weld joints at different positions are as follows: weld center WM: 146 / 158 / 163, fusion line FL: 195 / 170 / 170, fusion line FL+2mm: 222 / 219 / 209, fusion line FL+5mm: 301 / 329 / 324. The heat affected zone has excellent impact properties.

[0028] The present invention achieves improvement in low-temperature toughness of thick plates at -50°C throughout the entire thickness by controlling internal quality, low-temperature heating and strong controlled rolling processes, effectively improving the performance stability and qualified rate of thick offshore steel plates, and providing technical support for the development and product application of offshore steel for special low-temperature and complex service environments.

[0029] In addition to the above embodiments, the present invention may also have other implementation modes. Any technical solution formed by equivalent replacement or equivalent transformation falls within the protection scope required by the present invention.

Claims

1. A method for producing high-homogeneity and high-toughness S355MLO marine steel thick plate, characterized by: The chemical composition of the steel plate and its mass percentage include: C: 0.03-0.07%, Si: 0.15-0.35%, Mn: 1.45-1.65%, P≤0.015%, S≤0.005%, Alt: 0.025-0.045%, Nb: 0.025-0.040%, Ni: 0.25-0.50%, Cr: 0.10-0.25%, N≤50ppm, H≤2ppm; wherein, impurity elements include: As≤0.020%, Sb≤0.010%, Sn≤0.020%, Pb≤0.010%, Bi≤0.010%, Ca≤0.0025%, B≤0.0005%, and the rest are Fe and unavoidable impurities.

2. The method for producing high-homogeneity and high-toughness S355MLO marine steel thick plate according to claim 1, characterized in that: The thickness of the steel plate is 80-120 mm, and the mechanical properties meet R eH ≥355Mpa, R m It is 470~630Mpa, A≥22%, yield strength ratio≤0.93%, -50℃ lateral impact values ​​include: near surface ≥150J, 1 / 2 and 1 / 4 ≥200J, section shrinkage ≥40%, 5% time-effect strain impact value ≥150J.

3. The method for producing a high-homogeneity and high-toughness S355MLO marine steel thick plate according to claim 1 or 2, characterized in that: The method for producing high-homogeneity and high-toughness S355MLO marine steel thick plates comprises a smelting process, a heating process and a rolling process that cooperate with each other. In the smelting process, a top and bottom combined blowing converter + LF refining + RH vacuum + continuous casting process is adopted; oxygen in the converter is controlled to be ≤500ppm, white slag is produced in the LF refining furnace, the calcium-aluminum ratio is controlled to be 1.6-1.8, and the purity of the molten steel is improved; 460mm billet is used for continuous casting, a strong cooling system is used for cooling, and the dynamic reduction is controlled to be 13-15mm to improve center segregation.

4. The method for producing high-homogeneity and high-toughness S355MLO marine steel thick plate according to claim 3, characterized in that: In the heating process, the billet cooling time is ≥72h, and continuous furnace segmented heating is adopted, with a total heating time of 9-13min / cm, a soaking section insulation time of 60-80min, and a soaking temperature of 1070-1100°C to prevent excessive growth of surface grains.

5. The method for producing high-homogeneity and high-toughness S355MLO marine steel thick plate according to claim 3, characterized in that: In the rolling process, rough rolling is performed for 7 to 11 times, the intermediate billet thickness is 130 to 180 mm, the total reduction rate of the last three rough rolling times is ≥30%, and the finishing rolling is performed for 7 to 9 times, the reduction rate of the first finishing rolling time is ≥10%, the starting rolling temperature is 740 to 780°C, and the final cooling temperature is 400 to 450°C.

6. The method for producing high-homogeneity and high-toughness S355MLO marine steel thick plate according to claim 1 or 2, characterized in that: The chemical composition of the steel plate and its mass percentage include: C: 0.052%, Si: 0.30%, Mn: 1.47%, P: 0.012%, S: 0.002%, Alt: 0.034%, Ni: 0.35%, Nb: 0.031%, Cr: 0.12%, N: 0.0040%, H: 0.00015%, and the rest are Fe and unavoidable impurities.

7. The method for producing high-homogeneity and high-toughness S355MLO marine steel thick plate according to claim 6, characterized in that: The method for producing a high-homogeneity and high-toughness S355MLO marine steel thick plate comprises: (1) In the smelting process, the smelting and continuous casting processes are used to ensure high purity and internal quality of molten steel. The top and bottom combined blowing converter + LF refining + RH vacuum + continuous casting process is adopted. The oxygen of the converter steel is 490ppm, the LF refining furnace produces white slag, and the calcium-aluminum ratio is controlled at 1.

7. 460mm billet is used for continuous casting, and a strong cooling secondary cooling system is adopted. The dynamic reduction is controlled at 13mm, and the main reduction sections are in sections 6 and 7 to improve the center segregation. (2) In the heating process, the billet cooling time is ≥72h, and continuous furnace is used for segmented heating. The total heating time is 12min / cm, the soaking section is kept warm for 70min, and the soaking temperature is 1080℃ to prevent excessive growth of surface grains; (3) In the rolling process, the thickness of the rolled steel plate is 100 mm, the width is 3000 mm, the rough rolling is 11 passes, the intermediate billet thickness is 155 mm, and the total reduction rate of the last three rough rolling passes is 33%; the finishing rolling is 6 passes, the reduction rate of the first finishing rolling pass is 12%, the starting rolling temperature is 745°C, and the final cooling temperature is 405°C.

8. The method for producing high-homogeneity and high-toughness S355MLO marine steel thick plate according to claim 1 or 2, characterized in that: The chemical composition of the steel plate and its mass percentage include: C: 0.045%, Si: 0.25%, Mn: 1.58%, P: 0.010%, S: 0.001%, Alt: 0.032%, Ni: 0.42%, Nb: 0.033%, Cr: 0.13%, N: 0.0039%, H: 0.00010%, and the rest are Fe and unavoidable impurities.

9. The method for producing high-homogeneity and high-toughness S355MLO marine steel thick plate according to claim 8, characterized in that: The method for producing a high-homogeneity and high-toughness S355MLO marine steel thick plate comprises: (1) In the smelting process, the smelting and continuous casting processes are used to ensure high purity and internal quality of molten steel. The top and bottom combined blowing converter + LF refining + RH vacuum + continuous casting process is adopted. The oxygen content of the converter steel is 485ppm, and the LF refining furnace produces white slag, and the calcium-aluminum ratio is controlled at 1.

65. 460mm billet is used for continuous casting, and a strong cooling secondary cooling system is adopted. The dynamic reduction is controlled at 14mm, and the main reduction sections are in sections 6 and 7 to improve the center segregation. (2) In the heating process, the billet cooling time is ≥72h, and continuous furnace is used for segmented heating. The total heating time is 13min / cm, the soaking section is kept warm for 72min, and the soaking temperature is 1075℃ to prevent excessive growth of surface grains; (3) In the rolling process, the thickness of the rolled steel plate is 120 mm, the width is 3000 mm, the rough rolling is 11 passes, the intermediate billet thickness is 145 mm, and the total reduction rate of the last three rough rolling passes is 32%; the finishing rolling is 8 passes, the reduction rate of the first finishing rolling pass is 11%, the starting rolling temperature is 745°C, and the final cooling temperature is 420°C.

Citation Information

Cited By

  • Large-thickness high-toughness S355NLO wind power steel plate and production method thereof

    CN119710470A

  • A thick, high-toughness S355NLO wind power steel plate and its production method

    CN119710470B

  • Large-thickness normalized S355G8 + N maritime work steel plate and production method thereof

    CN119736554A

  • High-uniformity extra-thick 420MPa-grade maritime work steel plate for extremely low-temperature environment and manufacturing method thereof

    CN121380741A

  • Thick normalized s355g8+n offshore steel plate and production method therefor

    WO2026152848A1