Optical Fiber

By controlling chlorine concentration and refractive index differences in the optical fiber core, the issue of air bubbles is mitigated, improving yield and productivity while maintaining low loss and signal quality.

JP7552297B2Active Publication Date: 2024-09-18SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020197047
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-27
Filing Date
2020-11-27
Publication Date
2024-09-18
Estimated Expiration
2040-11-27

AI Technical Summary

Technical Problem

Optical fibers with chlorine-containing cores face issues of air bubbles remaining in the center, leading to increased transmission loss and reduced mechanical reliability, which negatively impact yield and productivity.

Method used

The optical fiber design includes a core with a controlled chlorine concentration range (10,000 ppm to 50,000 ppm) and a specific refractive index difference, suppressing bubble formation by managing chlorine concentration on the glass pipe's inner surface during manufacturing.

Benefits of technology

This approach reduces bubble-related defects, enhancing yield and productivity while maintaining low transmission loss and improving optical signal-to-noise ratio.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552297000002
    Figure 0007552297000002
  • Figure 0007552297000004
    Figure 0007552297000004
  • Figure 0007552297000003
    Figure 0007552297000003
Patent Text Reader

Abstract

To provide an optical fiber capable of suppressing a decrease in yield and productivity.SOLUTION: The optical fiber includes: a core 10 that is a center part 11 in which the diameter is equal to or more than 0.5 μm and is equal to or less than 4 μm, has the center part 11 including a central axis, and is made of silica glass; and a clad that surrounds the core 10 and is made of silica glass. The core 10 contains chlorine, the average chlorine concentration of the core 10 is equal to or more than 10,000 ppm and is equal to or less than 50,000 ppm, and a difference of the average chlorine concentration of the core 10 from the average chlorine concentration of the center part 11 is equal to or more than 4,500 ppm and is equal to or less than 13,500 ppm.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to optical fibers. [Background technology]

[0002] In an optical fiber whose core contains 1.0% or more chlorine by mass fraction, low transmission loss is more likely to be obtained even at a high drawing speed than an optical fiber whose core is made of silica glass without any additives and whose cladding is doped with fluorine. In an optical fiber whose core is made of silica glass without any additives and whose cladding is doped with fluorine, the stress applied to the core region during drawing is tensile stress. This makes it difficult for structural relaxation of the glass to occur. Therefore, in order to reduce transmission loss, it is necessary to reduce the drawing speed and the drawing tension. In contrast, in an optical fiber whose core is doped with 1.0% or more chlorine by mass fraction, the stress applied to the core region during drawing is compressive stress. This allows for a sufficient margin to be secured for increasing the drawing tension and accelerating the drawing speed.

[0003] Patent Document 1 discloses a single optical mode optical fiber whose core contains chlorine at a mass fraction of 1.5% or more. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-526601 A Summary of the Invention [Problem to be solved by the invention]

[0005] As a method for forming a core glass rod containing 1.0% or more chlorine by mass fraction, there is a method in which a glass pipe containing 1.0% or more chlorine by mass fraction is formed by OVD (Outside Vapor Deposition), MCVD (Modified Chemical Vapor Deposition), or PCVD (Plasma Chemical Vapor Deposition), and then the opening of the glass pipe is closed by a collapse method to form a core glass rod. However, the core glass rod formed by this method is prone to have bubbles remaining in the center.

[0006] These bubbles remain in the center of the core of the preform even after the core glass rod is made into a preform. Furthermore, these bubbles remain in the center of the core of the optical fiber even after the preform (preform) is made into a fiber through a drawing process, leading to an increase in transmission loss or a decrease in mechanical reliability. For this reason, the part where the bubbles remain is removed as a defective part. In other words, even if the productivity in the drawing process is improved by increasing the drawing speed by adding chlorine to the core, there is a problem that the productivity cannot be improved overall because there are many defective parts in the optical fiber and the yield is low.

[0007] Therefore, an object of the present invention is to provide an optical fiber capable of suppressing a decrease in yield and productivity. [Means for solving the problem]

[0008] An optical fiber according to one embodiment of the present disclosure comprises a core made of silica glass having a center portion (a portion having a diameter of 0.5 μm or more and 4 μm or less) including a central axis, and a cladding surrounding the core and made of silica glass, wherein the core contains chlorine, the average chlorine concentration of the core is 10,000 ppm or more and 50,000 ppm or less, and the difference between the average chlorine concentration of the core and the average chlorine concentration of the center portion is 4,500 ppm or more and 13,500 ppm or less.

[0009] An optical fiber according to another embodiment of the present disclosure includes a core having a central portion (a portion having a diameter of 0.5 μm or more and 4 μm or less) including a central axis, and a cladding surrounding the core, the core containing chlorine, the average chlorine concentration of the core being 10000 ppm or more and 50000 ppm or less, the relative refractive index difference of the average refractive index of the core when the average refractive index of the cladding at a wavelength of 1550 nm is taken as a reference being 0.25% or more and 0.40% or less, the core diameter being 8.5 μm or more and 13.5 μm or less, and the relative refractive index difference of the average refractive index of the core when the refractive index of pure silica at a wavelength of 1550 nm is taken as a reference being Δn plus When the refractive index of the pure silica at a wavelength of 1550 nm is used as the reference, the relative refractive index difference of the minimum refractive index at the center is Δdip, and Δn plus -Δdip is equal to or greater than 0.05% and equal to or less than 0.15%. Effect of the Invention

[0010] According to the present disclosure, it is possible to provide an optical fiber capable of suppressing a decrease in yield and productivity. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a cross-sectional view of an optical fiber according to an embodiment. [Diagram 2] FIG. 2 is a graph showing a schematic refractive index profile of the optical fiber of FIG. [Diagram 3] FIG. 3 is a graph showing the relationship between the ratio of the effective cross-sectional area to the cable cutoff wavelength and the bending loss. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] [Description of the embodiments of the present disclosure] First, the embodiments of the present disclosure will be listed and described. An optical fiber according to one embodiment includes a core made of silica glass having a central portion (a portion having a diameter of 0.5 μm or more and 4 μm or less) including a central axis, and a cladding made of silica glass surrounding the core, the core containing chlorine, the average chlorine concentration of the core being 10000 ppm or more and 50000 ppm or less, and the difference between the average chlorine concentration of the core and the average chlorine concentration of the central portion being 4500 ppm or more and 13500 ppm or less. Here, the chlorine concentration is expressed as a mass fraction (the ratio of the mass of chlorine contained in the object to the total mass of the object).

[0013] In the optical fiber according to the above embodiment, when the core glass pipe is solidified to form a core glass rod, the chlorine concentration on the inner surface of the glass pipe can be kept low, so that the generation of bubbles due to chlorine on the inner surface can be suppressed. Therefore, the generation of bubbles in the center of the core of the optical fiber can be suppressed. As a result, the decrease in the yield and productivity of the optical fiber can be suppressed.

[0014] The relative refractive index difference of the average refractive index of the core when the average refractive index of the cladding at a wavelength of 1550 nm is taken as a reference may be 0.25% or more and 0.40% or less, and the diameter of the core may be 8.5 μm or more and 13.5 μm or less. This makes it possible to suppress the increase in excess loss and connection loss due to macrobends and microbends. In order to realize the above relative refractive index difference, it is desirable that the core does not contain germanium, and does not contain fluorine or the concentration of fluorine is suppressed to a lower level than that of chlorine. In addition, it is preferable that the cladding is formed of pure silica glass or silica glass doped with fluorine.

[0015] The relative refractive index difference of the average refractive index of the core when the refractive index of pure silica at a wavelength of 1550 nm is taken as the standard is Δn plus When the refractive index of the pure silica at a wavelength of 1550 nm is used as the reference, the relative refractive index difference of the minimum refractive index at the center is Δdip, and Δn plus-Δdip may be 0.05% or more and 0.15% or less. In this case, the difference between the average chlorine concentration in the core and the average chlorine concentration in the center portion is easily set to 4500 ppm or more and 13500 ppm or less.

[0016] An optical fiber according to another embodiment includes a core having a central portion (a portion having a diameter of 0.5 μm or more and 4 μm or less) including a central axis, and a cladding surrounding the core, the core containing chlorine, the average chlorine concentration of the core being 10000 ppm or more and 50000 ppm or less, the relative refractive index difference of the average refractive index of the core when the average refractive index of the cladding at a wavelength of 1550 nm is taken as a reference being 0.25% or more and 0.40% or less, the core diameter being 8.5 μm or more and 13.5 μm or less, and the relative refractive index difference of the average refractive index of the core when the refractive index of pure silica at a wavelength of 1550 nm is taken as a reference being Δn plus When the refractive index of the pure silica at a wavelength of 1550 nm is used as the reference, the relative refractive index difference of the minimum refractive index at the center is Δdip, and Δn plus -Δdip is equal to or greater than 0.05% and equal to or less than 0.15%.

[0017] In the optical fiber according to the above embodiment, the difference between the average chlorine concentration in the core and the average chlorine concentration in the center can be easily set to 4500 ppm or more and 13500 ppm or less. Therefore, when forming a core glass rod, it is easy to suppress the generation of chlorine bubbles on the inner surface of the glass pipe. Therefore, it is possible to suppress the generation of bubbles in the center of the core of the optical fiber. As a result, it is easy to suppress the decrease in yield and productivity of the optical fiber.

[0018] The cladding may contain fluorine. In this case, even if the chlorine concentration in the core is low, the relative refractive index difference of the average refractive index of the core when the average refractive index of the cladding at a wavelength of 1550 nm is taken as the reference can be 0.25% or more. Therefore, light in the fundamental mode can be confined.

[0019] The mode field diameter of the optical fiber at a wavelength of 1310 nm is 8.6 μm or more and 13.0 μm or less, and the effective area of ​​the optical fiber at a wavelength of 1550 nm is 70 μm or less. 2More than 130μm 2 The cable cutoff wavelength of the optical fiber may be 1530 nm or less, which can improve the optical signal-to-noise ratio of the optical communication system. In addition, it can be interconnected with optical fibers conforming to the widely used ITU-T G.654 recommendation.

[0020] The mode field diameter of the optical fiber at a wavelength of 1310 nm is 8.6 μm or more and 11.0 μm or less, and the effective area of ​​the optical fiber at a wavelength of 1550 nm is 70 μm 2 More than 115μm 2 The cable cutoff wavelength of the optical fiber may be 1260 nm or less. This also improves the optical signal-to-noise ratio of the optical communication system. In addition, it can be interconnected with optical fibers conforming to the widely used ITU-T G.652 recommendation.

[0021] The transmission loss of the optical fiber at a wavelength of 1550 nm may be not less than 0.15 dB / km and not more than 0.18 dB / km, and the transmission loss of the optical fiber at a wavelength of 1310 nm may be not less than 0.24 dB / km and not more than 0.40 dB / km.

[0022] The optical fiber may further include a coating resin layer surrounding the clad and made of an acrylate resin, the coating resin layer having a diameter of 190 μm or more and less than 255 μm. In this case, microvent loss can be suppressed.

[0023] The optical fiber may further include a coating resin layer surrounding the clad and made of an acrylate resin, the coating resin layer having a diameter of 190 μm or more and less than 210 μm. In this case, microvent loss can also be suppressed.

[0024] [Details of the embodiment of the present disclosure] Specific examples of the optical fiber of the present disclosure will be described below with reference to the drawings. Note that the present invention is not limited to these examples, but is indicated by the claims, and is intended to include all modifications within the meaning and scope equivalent to the claims. In the description of the drawings, the same elements are given the same reference numerals, and duplicate descriptions will be omitted.

[0025] According to the findings of the present inventors, when a glass pipe containing 1.0% (10,000 ppm) or more of chlorine is collapsed to form a solid body, chlorine bubbles (meaning bubbles containing chlorine and its compounds) are generated on the inner surface of the glass pipe. This phenomenon occurs when the chlorine concentration on the inner surface of the glass pipe is high. That is, when a glass pipe containing a high concentration of chlorine even on the inner surface is heated, chlorine bubbles are generated on the inner surface, and the generated chlorine bubbles remain in the center of the core glass rod after collapse. Therefore, the chlorine concentration on the inner surface of the glass pipe is reduced to suppress the generation of chlorine bubbles.

[0026] A method for reducing the chlorine concentration on the inner surface of a glass pipe is described below. In the MCVD and PCVD methods, the concentration of the chlorine source gas flowing when depositing glass is adjusted. The chlorine concentration on the inner surface of the glass pipe can be reduced by lowering the concentration of chlorine gas when depositing the area that will become the center after collapse.

[0027] In the OVD method, the chlorine concentration on the inner surface of the glass pipe body can be reduced by adding chlorine to the soot pipe, sufficiently baking it, and then collapsing it. In addition, when depositing soot on a starting rod in the OVD method, the soot may be deposited so that the bulk density of the part near the inner surface of the pipe is large.

[0028] Fig. 1 is a cross-sectional view of an optical fiber according to an embodiment. As shown in Fig. 1, the optical fiber 1 of this embodiment includes a glass fiber 2 and a coating resin layer 3 surrounding the glass fiber 2. The glass fiber 2 includes a core 10 and a cladding 20 surrounding the core 10. The cross-sectional view of Fig. 1 represents a cross section perpendicular to the central axis C of the optical fiber 1.

[0029] The core 10 has a central portion 11 including a central axis C, and an outer core portion 12 surrounding the central portion 11. The diameter (outer diameter) 2a of the core 10 is, for example, 8.5 μm or more and 13.5 μm or less. The diameter 2a may be, for example, 8.5 μm or more and 12.5 μm or less, or 8.5 μm or more and 11.5 μm or less. The definition of the central portion 11 will be described later. The diameter (outer diameter) of the outer core portion 12 is, for example, equal to the diameter 2a.

[0030] The core 10 is made of silica glass. The core 10 contains chlorine, and the average chlorine concentration of the core 10 is 10,000 ppm or more and 50,000 ppm or less. Here, the average chlorine concentration of the core 10 refers to the average chlorine concentration in the entire core 10 including the central portion 11 and the outer core portion 12. The average chlorine concentration of the central portion 11 is lower than the average chlorine concentration of the core 10. The difference between the average chlorine concentration of the core 10 and the average chlorine concentration of the central portion 11 is 4,500 ppm or more and 13,500 ppm or less. This difference may be, for example, 7,200 ppm or more and 13,500 ppm or less.

[0031] The diameter (outer diameter) of the cladding 20 is, for example, 124 μm or more and 126 μm or less. The diameter of the cladding 20 is, for example, 125 μm. The diameter of the cladding 20 is, for example, equal to the diameter (outer diameter) of the glass fiber 2. The cladding 20 is made of silica glass. The cladding 20 may contain fluorine, and the average fluorine concentration of the cladding 20 is, for example, 0 ppm or more and 8000 ppm or less.

[0032] In particular, in the region outside the radius of 30 μm, the concentration of halogens including chlorine and fluorine may be 1000 ppm or less, thereby relatively lowering the viscosity of the inner region including the core, and preventing an increase in transmission loss and a decrease in optical confinement strength due to residual drawing tension in the core.

[0033] The coating resin layer 3 has a primary resin layer 31 surrounding the clad 20 and a secondary resin layer 32 surrounding the primary resin layer 31. The diameter (outer diameter) of the coating resin layer 3 may be 190 μm or more and less than 255 μm, or may be 190 μm or more and less than 210 μm. The thickness of the coating resin layer 3 is, for example, 30 μm or more and 68 μm or less. The diameter (outer diameter) of the primary resin layer 31 is, for example, 150 μm or more and 210 μm or less. The thickness of the primary resin layer 31 is, for example, 10 μm or more and 45 μm or less. The diameter (outer diameter) of the secondary resin layer 32 is, for example, equal to the diameter of the coating resin layer 3. The thickness of the secondary resin layer 32 is, for example, 20 μm or more and 35 μm or less.

[0034] The primary resin layer 31 and the secondary resin layer 32 are made of a cured product of an ultraviolet-curable resin composition. That is, the coating resin layer 3 contains a cured product of an ultraviolet-curable resin composition. The ultraviolet-curable resin composition used for the primary resin layer 31 and the secondary resin layer 32 is, for example, urethane acrylate. After applying these resin compositions to the glass fiber 2, ultraviolet rays are irradiated to cure the resin composition, thereby forming the primary resin layer 31 and the secondary resin layer 32.

[0035] The mode field diameter (hereinafter, "MFD") of the optical fiber 1 at a wavelength of 1310 nm is 8.6 μm or more and 13.0 μm or less. The MFD may be, for example, 8.6 μm or more and 12.5 μm or less, 8.6 μm or more and 11.0 μm or less, or 8.6 μm or more and 9.5 μm or less.

[0036] The effective area (Aeff) of the optical fiber 1 at a wavelength of 1550 nm is 70 μm 2 More than 130μm2 Aeff is, for example, 70 μm or less. 2 More than 120μm 2 It may be less than 70 μm 2 More than 115μm 2 It may be less than 70 μm 2 More than 110μm 2 It may be less than 70 μm 2 More than 100μm 2 Aeff may be 75 μm or less. 2 More than 105μm 2 It may be the following.

[0037] The cable cutoff wavelength (hereinafter, "λcc") of the optical fiber 1 is 1530 nm or less. In this case, single-mode optical communication is possible in the C band (1530 nm or more and 1565 nm or less). The λcc of the optical fiber 1 may be, for example, 1260 nm or less. In this case, single-mode optical communication is possible even in the 1.3 μm band.

[0038] The transmission loss of the optical fiber 1 at a wavelength of 1550 nm is 0.15 dB / km or more and 0.18 dB / km or less, and may be 0.15 dB / km or more and less than 0.18 dB / km. The transmission loss of the optical fiber 1 at a wavelength of 1310 nm is 0.24 dB / km or more and 0.40 dB / km or less.

[0039] Fig. 2 is a graph showing a schematic of the refractive index profile of the optical fiber shown in Fig. 1. The horizontal axis indicates the radial position r, and the vertical axis indicates the refractive index n at a wavelength of 1550 nm. The radial position of the central axis C (see Fig. 1) is 0 (r=0). Here, the refractive index n has a correlation with the chlorine concentration.

[0040] As shown in FIG. 2, the average refractive index n 1 is the average refractive index n of the entire cladding 20 (see FIG. 1) at a wavelength of 1550 nm. 2 The average refractive index n of the cladding 20 at a wavelength of 1550 nm is higher than 2 The average refractive index of the core 10 based on n1 The relative refractive index difference Δn of (n 1 -n 2 ) / n 1 Δn is defined as 0.25% or more and 0.40% or less. Δn may be 0.25% or more and 0.38% or less, or may be 0.28% or more and 0.37% or less.

[0041] The portion corresponding to the central portion 11 (see FIG. 1) is a recessed portion in which the refractive index decreases toward the central axis C (see FIG. 1). In the recessed portion, the chlorine concentration also decreases toward the central axis C. The portion corresponding to the outer core portion 12 (see FIG. 1) surrounds the recessed portion. The minimum refractive index n 3 is the refractive index n of pure silica at a wavelength of 1550 nm 0 Higher than the average refractive index n 1 is the refractive index n 0 and the minimum refractive index n 3 Higher than.

[0042] The refractive index n of pure silica at a wavelength of 1550 nm 0 The average refractive index of the core 10 based on n 1 The relative refractive index difference Δn plus , (n 1 -n 0 ) / n 0 The refractive index of pure silica at a wavelength of 1550 nm is defined as n 0 The minimum refractive index n of the central portion 11 when 3 The relative refractive index difference Δdip of (n 3 -n 0 ) / n 0 The depth of the refractive index of the depression is defined as Δn plus It is expressed as -Δdip.

[0043] Δn plus -Δdip is 0.05% or more and 0.15% or less. When the difference between the average chlorine concentration of the core 10 and the average chlorine concentration of the center portion 11 is 4500 ppm or more and 13500 ppm or less, Δn plus -Δdip falls within this range. Δn plus-Δdip may be 0.08% or more and 0.15% or less. When the difference between the average chlorine concentration of the core 10 and the average chlorine concentration of the center portion 11 is 7200 ppm or more and 13500 ppm or less, Δn plus -Δdip falls within this range.

[0044] The diameter of the center portion 11 is the effective diameter (diameter) of the recessed portion 2r dip The effective diameter of the recess 2r corresponds to dip is the refractive index n of pure silica at a wavelength of 1550 nm 0 The relative refractive index difference of the recessed portion when the refractive index is based on (Δdip+Δn plus ) / 2. That is, when the optical fiber 1 is viewed in a cross section perpendicular to the central axis C, the central portion 11 is the inner portion of a circle whose chlorine concentration is an intermediate value between the average chlorine concentration in the core 10 and the minimum chlorine concentration in the central portion 11, and the diameter of the circle is the diameter of the central portion 11.

[0045] Effective diameter 2r dip (i.e., the diameter of the central portion 11) is 0.5 μm or more and 4 μm or less. dip It may be 0.8 μm or more and 3 μm or less, or 1 μm or more and 2.5 μm or less.

[0046] As described above, in the optical fiber 1, the difference between the average chlorine concentration in the core 10 and the average chlorine concentration in the central portion 11 of the core 10 is 4500 ppm or more and 13500 ppm or less. Therefore, when forming a core glass rod, it is possible to suppress the generation of chlorine bubbles on the inner surface of the glass pipe. Since it is possible to suppress the generation of bubbles in the central portion of the glass core rod, it is also possible to suppress the generation of bubbles in the central portion of the core part of the preform. Therefore, it is possible to suppress the generation of bubbles in the central portion 11 of the optical fiber 1 obtained by drawing the preform. As a result, it is possible to suppress a decrease in the yield and productivity of the optical fiber 1.

[0047] Refractive index depth of the recess Δn plus −Δdip is 0.05% or more and 0.15% or less. Therefore, the difference between the average chlorine concentration of the core 10 and the average chlorine concentration of the central portion 11 can be easily set to 4500 ppm or more and 13500 ppm or less.

[0048] The cladding 20 contains fluorine. In this case, even if the chlorine concentration in the core 10 is low, the average refractive index n 2 The average refractive index of the core 10 based on n 1 The relative refractive index difference Δn can be set to 0.25% or more. Therefore, light in the fundamental mode can be confined.

[0049] The MFD at a wavelength of 1310 nm is 8.6 μm or more and 13.0 μm or less, and the Aeff at a wavelength of 1550 nm is 70 μm 2 More than 130μm 2 The MFD may be 8.6 μm or more and 11.0 μm or less, and the Aeff is 70 μm or less. 2 More than 115μm 2 or less, and λcc may be 1260 nm or less. In the optical fiber 1, Aeff can be increased, and therefore the optical signal-to-noise ratio of the optical communication system can be improved.

[0050] The transmission loss of the optical fiber 1 at a wavelength of 1550 nm is not less than 0.15 dB / km and not more than 0.18 dB / km, and the transmission loss of the optical fiber 1 at a wavelength of 1310 nm is not less than 0.24 dB / km and not more than 0.40 dB / km.

[0051] The diameter of the coating resin layer 3 is 190 μm or more and less than 255 μm. The diameter of the coating resin layer 3 may be 190 μm or more and less than 210 μm. When the diameter of the coating resin layer 3 becomes smaller (the coating resin layer 3 becomes thinner), the microbending loss increases. In the optical fiber 1, if the diameter of the coating resin layer 3 is within this range, the microbending loss can be suppressed. EXAMPLES

[0052] The present disclosure will be described in more detail below by showing the results of evaluation tests using examples and comparative examples according to the present disclosure. Note that the present disclosure is not limited to these examples.

[0053] Table 1 shows the results of measuring the optical characteristics of the optical fibers according to the comparative example and the examples. In the comparative examples 1 and 2, the chlorine concentration on the inner surface of the glass pipe was not reduced. In the examples 1 to 5, the chlorine concentration on the inner surface of the glass pipe was reduced. The number of bubbles in the preform in Table 1 indicates the number of bubbles formed at the center of the preform (the portion where the center of the glass core rod is solidified) in the longitudinal region of the preform corresponding to 1000 km of an optical fiber having an outer diameter of 125 μm. The bending loss indicates the loss at a wavelength of 1550 nm when the optical fiber is wound 10 times around a mandrel having a diameter of 30 mm.

[0054] [Table 1]

[0055] As shown in Table 1, in the comparative example, the number of bubbles in the base material is 5 or more, and the transmission loss is 0.18 dB / km. In contrast, in the examples, the number of bubbles in the base material is suppressed to 1 or less, and the transmission loss is suppressed to less than 0.18 dB / km. In the comparative example, many tiny chlorine bubbles that cannot be confirmed by the naked eye remain in the center of the base material, and it is believed that these act as scatterers and worsen the transmission loss. In contrast, in the examples, the chlorine concentration on the inner surface of the glass pipe body is reduced to suppress the generation of tiny chlorine bubbles, and as a result, it is believed that the deterioration of the transmission loss is suppressed.

[0056] Fig. 3 is a graph showing the relationship between the ratio of Aeff to λcc, Aeff / λcc, and bending loss. As shown in Fig. 3, the relationship between Aeff / λcc and bending loss is different between the embodiment and the comparative example. That is, when compared at the same Aeff / λcc, the embodiment has a lower bending loss than the comparative example. This is considered to be due to the effect of reducing the chlorine concentration on the inner surface of the glass pipe body and lowering the chlorine concentration in the center of the glass core rod, which creates a recess in the refractive index of the optical fiber finally obtained by spinning the optical fiber preform.

[0057] When compared at the same Aeff / λcc, the bending loss of the Example is lower than that of the Comparative Example, which means that for the same bending loss and the same λcc, the Example can have a larger Aeff than the Comparative Example. In other words, the optical signal-to-noise ratio can be improved in the optical communication system using the optical fiber of the Example, compared to the optical communication system using the optical fiber of the Comparative Example.

[0058] In addition, when compared at the same Aeff / λcc, the bending loss of the examples is lower than that of the comparative examples, so that the microbending loss, which is a concern as it increases when the diameter of the coating resin layer is reduced (the coating resin layer is made thinner), can be suppressed. [Explanation of symbols]

[0059] 1...optical fiber, 2...glass fiber, 3...coating resin layer, 10...core, 11...center portion, 12...outer core portion, 20...clad, 31...primary resin layer, 32...secondary resin layer, C...center axis.

Claims

1. a core made of silica glass having a central portion with a diameter of 0.5 μm or more and 4 μm or less, the central portion including a central axis; a cladding surrounding the core and made of silica glass; the core comprises chlorine; the average chlorine concentration of the central portion is lower than the average chlorine concentration of the core; The average chlorine concentration of the core is 10,000 ppm or more and 50,000 ppm or less, a difference between an average chlorine concentration of the core and an average chlorine concentration of the center portion is 4500 ppm or more and 13500 ppm or less; In the central portion, the refractive index decreases toward the central axis, The diameter of the central portion is the diameter at a position having a chlorine concentration that is an intermediate value between the average chlorine concentration of the core and the minimum chlorine concentration of the central portion. Optical fiber.

2. a relative refractive index difference of the average refractive index of the core relative to the average refractive index of the cladding at a wavelength of 1550 nm is 0.25% or more and 0.40% or less; The diameter of the core is 8.5 μm or more and 13.5 μm or less.

2. The optical fiber of claim 1.

3. The relative refractive index difference of the average refractive index of the core when the refractive index of pure silica at a wavelength of 1550 nm is taken as the reference is Δn plus When the relative refractive index difference of the minimum refractive index of the central portion when the refractive index of pure silica at a wavelength of 1550 nm is taken as a reference, Δdip is plus -Δdip is 0.05% or more and 0.15% or less; The optical fiber of claim 2.

4. a core having a center portion with a diameter of 0.5 μm or more and 4 μm or less, the center portion including a central axis; a cladding surrounding the core; the core comprises chlorine; The average chlorine concentration of the core is 10,000 ppm or more and 50,000 ppm or less, a relative refractive index difference of the average refractive index of the core relative to the average refractive index of the cladding at a wavelength of 1550 nm is 0.25% or more and 0.40% or less; The diameter of the core is 8.5 μm or more and 13.5 μm or less, The relative refractive index difference of the average refractive index of the core when the refractive index of pure silica at a wavelength of 1550 nm is taken as the reference is Δn plus When the relative refractive index difference of the minimum refractive index of the central portion when the refractive index of pure silica at a wavelength of 1550 nm is taken as a reference, Δdip is plus -Δdip is 0.05% or more and 0.15% or less, In the central portion, the refractive index decreases toward the central axis, The diameter of the central portion is the diameter at a position having a chlorine concentration that is an intermediate value between the average chlorine concentration of the core and the minimum chlorine concentration of the central portion. Optical fiber.

5. The cladding comprises fluorine. The optical fiber according to any one of claims 1 to 4.

6. The mode field diameter of the optical fiber at a wavelength of 1310 nm is 8.6 μm or more and 13.0 μm or less, The effective area of ​​the optical fiber at a wavelength of 1550 nm is 70 μm 2 More than 130 μm 2 is as follows: The cable cutoff wavelength of the optical fiber is 1530 nm or less. The optical fiber according to any one of claims 1 to 5.

7. The mode field diameter of the optical fiber at a wavelength of 1310 nm is 8.6 μm or more and 11.0 μm or less, The effective area of ​​the optical fiber at a wavelength of 1550 nm is 70 μm 2 115 μm or more 2 is as follows: The cable cutoff wavelength of the optical fiber is 1260 nm or less. The optical fiber according to any one of claims 1 to 5.

8. The transmission loss of the optical fiber at a wavelength of 1550 nm is 0.15 dB / km or more and 0.18 dB / km or less, The transmission loss of the optical fiber at a wavelength of 1310 nm is 0.24 dB / km or more and 0.40 dB / km or less. The optical fiber according to any one of claims 1 to 7.

9. The clad is surrounded by a coating resin layer made of an acrylate resin. The diameter of the coating resin layer is 190 μm or more and less than 255 μm. The optical fiber according to any one of claims 1 to 8.

10. The clad is surrounded by a coating resin layer made of an acrylate resin. The diameter of the coating resin layer is 190 μm or more and less than 210 μm. The optical fiber according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Optical fiber and optical fiber preform

    JP2015105199A

  • Optical fiber

    JP2016200830A

  • Optical fiber

    JP2017076053A

  • Low attenuation optical fiber with high chlorine content

    JP2017526601A

  • Optical fiber

    JP2018081328A