Manufacturing method of rough wire rod
The method of supplying harder additive elements as wire rods and softer elements as lumps during continuous casting and rolling stabilizes the concentration of additives in rough drawn wires, ensuring consistent properties.
Patent Information
- Application Number
- JP2021036809
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-09
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2041-03-09
AI Technical Summary
The challenge of stabilizing the concentration of additive elements in rough drawn wires made of cast alloys, particularly when multiple types of additives are used, as they may deform or have unstable feeding speeds, leading to inconsistent properties in the final product.
A manufacturing method involving continuous casting and rolling, where a harder additive element is supplied as a wire rod and a softer additive element as lumps, ensuring stable concentration by adjusting flow rates and intermittent supply of the lumps to maintain consistent additive element distribution.
Stabilizes the concentration of multiple additive elements in the rough drawn wire, resulting in consistent properties such as tensile strength and conductivity.
Smart Images

Figure 0007552448000003 
Figure 0007552448000004 
Figure 0007552448000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a wire rod. [Background technology]
[0002] As a method for continuously casting a casting alloy that is a raw material for wire rods, two types of additives may be added to a base metal (see, for example, Patent Documents 1, 2, and 3). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-20085 A [Patent Document 2] Japanese Patent Application Publication No. 11-277184 [Patent Document 3] JP 2007-217792 A Summary of the Invention [Problem to be solved by the invention]
[0004] When supplying an additive element to a molten metal, from the viewpoint of stabilizing the concentration of the additive element, a method of continuously feeding a wire made of the additive element formed into a wire shape into the molten metal is preferable. However, depending on the type of additive element, it may be difficult to form the wire into a wire shape. Or, even if it is possible to form the wire into a wire shape, if the wire is soft, the wire may deform during supply to the molten metal, causing the supply rate of the wire into the molten metal to be unstable. In this case, the concentration of the additive element in the rough wire produced by continuous casting is unstable.
[0005] Therefore, an object of the present invention is to provide a technique capable of stabilizing the concentrations of additive elements in a wire rod made of a cast alloy containing two or more types of additive elements. [Means for solving the problem]
[0006] One embodiment of a method for manufacturing a rough wire rod is a method for manufacturing a rough wire rod obtained by continuous casting and rolling, and includes the steps of: (a) obtaining a molten metal made of a base material; (b) continuously supplying a first additive element to the molten metal as a wire rod; (c) intermittently supplying a second additive element different from the first additive element as a lump to the molten metal before or after step (b); and (d) continuously casting the molten metal in which the first additive element and the second additive element are mixed in a mold to form a cast material. Effect of the Invention
[0007] According to a representative embodiment of the present invention, it is possible to stabilize the concentrations of additive elements in a wire rod made of a cast alloy containing two or more types of additive elements. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is an explanatory diagram showing a configuration example of a manufacturing apparatus for a wire rod according to an embodiment; [Diagram 2] 2 is a perspective view showing an example of the shape of an ingot supplied from the ingot supply part shown in FIG. 1 to the molten metal. FIG. [Diagram 3] FIG. 3 is a cross-sectional view showing a cut surface of the block shown in FIG. 2. [Figure 4] FIG. 2 is an explanatory diagram showing a modified example of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.
[0010] <Example of wire rod manufacturing equipment configuration> FIG. 1 is an explanatory diagram showing an example of the configuration of a manufacturing apparatus for a wire rod according to the present embodiment. A wire rod 80 manufactured in this embodiment is made of a cast alloy having copper as a base material and including additive elements contained in the base material. The wire rod 80 is further drawn depending on the application, and is used for applications such as conductors used in electric wires and cables. A method and apparatus for manufacturing a wire rod 80, which is a copper wire rod made of a cast alloy having copper as a base material, will be described below.
[0011] 1, a wire rod manufacturing apparatus 100 of this embodiment includes a melting furnace 10, a holding furnace 20, a tundish 30, an additive element supplying section 40, a mold 50, a rolling section 60, and a winding section 70. The melting furnace 10 and the holding furnace 20, and the holding furnace 20 and the tundish 30 are connected by transfer troughs 11. A spout 31 is connected to the tundish 30, and molten metal stored in the tundish 30 is supplied into the mold 50 via the spout 31.
[0012] The manufacturing method of the wire rod in this embodiment includes a step of melting copper, which is the base material of the cast alloy constituting the wire rod 80 (base material melting step). This base material melting step is performed in a melting furnace 10 shown in FIG. 1. The molten copper metal melted in the melting furnace 10 is transferred to a holding furnace 20 via a transfer trough 11. In the holding furnace 20, the molten metal is stored while maintaining the molten state. The molten metal stored in the holding furnace 20 is transferred sequentially to a tundish 30 via the transfer trough 11.
[0013] In the tundish 30, foreign objects (inclusions) present in the molten metal are removed (foreign object removal process). For example, foreign objects may be removed by scooping up the foreign objects floating on the surface of the molten metal. Note that while FIG. 1 shows an example in which the holding furnace 20 and the tundish 30 are connected via a transfer trough 11, as a modified example, a container called a ladle (not shown) may be interposed between the holding furnace 20 and the tundish 30. In this case, the removal of foreign objects may also be performed in the ladle.
[0014] The manufacturing method of the wire rod of this embodiment includes a step of supplying molten metal accumulated in a tundish 30 to a mold 50 (molten metal supplying step). In the molten metal supplying step, for example, molten copper accumulated in the tundish 30 is supplied to the mold 50 through a spout (nozzle) 31. The mold 50 has a circular shape in a side view and a casting wheel 51 that rotates around the center of the circle as the rotation axis. Fig. 1 shows a schematic direction r1 of rotation of the casting wheel 51.
[0015] A groove (not shown) is formed on the periphery of the casting ring 51 along the circumferential direction of the casting ring 51. A casting belt 53 is disposed on the periphery of the casting ring 51 so as to face the groove of the casting ring 51. The groove of the casting ring 51 functions as a mold for casting molten metal. The casting belt 53 is disposed at a position facing the groove, thereby preventing the metal from dropping out of the mold 50 during casting. The molten metal is supplied from the spout 31 into the groove of the mold 50. The metal supplied into the groove is rapidly cooled through the casting ring 51, and a casting material 81 is obtained that is shaped into the shape of the mold 50, i.e., the shape of the groove.
[0016] The manufacturing method of the wire rod of this embodiment includes a step of supplying two or more kinds of additive elements to the molten metal (additive element adding step). The additive elements to be supplied to the molten copper, which is the base material of the wire rod 80, are supplied from an additive element supplying section 40 to the molten metal at a position on the path from the holding furnace 20 to the mold 50. FIG. 1 shows, as an example, an example in which two kinds of additive elements are supplied to the molten metal in a transfer trough 11 connecting the holding furnace 20 and the tundish 30. However, the position at which the additive elements are supplied is not limited to the example shown in FIG. 1, and for example, the additive elements may be supplied in the tundish 30 or directly to the mold 50. The method of supplying the additive elements will be described later in detail.
[0017] The manufacturing method of the wire rod of this embodiment includes a step (casting step) of casting molten metal to which an additive element has been added in a mold 50. As shown in Fig. 1, a casting wheel 51 of the mold 50 rotates along a rotation direction r1. The molten metal containing the additive element supplied into the mold 50 is cast in a region surrounded by the casting wheel 51 and the casting belt 53, and a cast material 81 that is an alloy of the base metal and the additive element is obtained.
[0018] The manufacturing method of the wire rod of the present embodiment includes a step (rolling step) of rolling the obtained cast material 81 to form the wire rod 80. In the rolling step, for example, the cast material 81 is gradually rolled using a plurality of rollers (not shown) provided in the rolling section 60 shown in FIG. 1 to obtain a rolled material rolled into a wire rod such as the wire rod 80. The obtained rolled material is subjected to a surface cleaning treatment such as removal of surface oxides, to obtain the wire rod 80.
[0019] The roughly drawn wire 80 obtained through the rolling process is wound onto a reel (not shown) by the winding section 70. The outer diameter of the roughly drawn wire 80 is, for example, not less than 6 mm and not more than 30 mm.
[0020] <Details of the additive element supply process> Next, the details of the additive element supplying process will be described. The rough wire 80 used for the conductor wire etc. is formed by adding various additive elements to the base material in order to improve the function or characteristics when it is made into a conductor wire. The additive elements are supplied into the molten metal constituting the base material. Considering the ease of the work of supplying the additive elements or the layout of the device, a method of supplying the additive elements in the transfer trough 11 or the tundish 30 shown in FIG. 1 is preferable. For example, in the tundish 30, a process of floating and removing foreign matter contained in the molten metal may be performed, so a space is secured above the liquid surface of the molten metal to a degree that the work of removing the foreign matter can be performed. Therefore, if the additive elements are supplied using this space, the work can be performed efficiently. In addition, it is easy to secure the space for arranging the supplying device for the additive elements.
[0021] When casting is performed continuously as in the present embodiment, it is preferable to continuously supply the additive element to the molten metal after adjusting the flow rate of the molten metal and the supply rate of the additive element from the viewpoint of reducing the variation in the content rate of the additive element in the cast alloy constituting the wire rod. As a method for continuously supplying the additive element, a method of continuously supplying a wire rod 43 formed into a wire shape (wire shape) to the molten metal as shown as a wire rod supply section 41 in FIG. 1 is preferable. It is preferable that the wire diameter of the wire rod 43 has small variation. This makes it easier to control the flow rate of the molten metal at the supply location (transport trough 11 in the case of FIG. 1) and the supply rate of the wire rod 43, so that the concentration of the additive element in the wire rod produced by continuous casting can be relatively easily stabilized.
[0022] Depending on the type of additive element, it may be difficult to form the wire into a wire shape. For example, in the case of a soft metal such as indium, it is difficult to form the wire into a wire shape, and even if it can be formed into a wire shape, the wire may be deformed during supply to the molten metal. If the wire is deformed during supply, the supply rate of the wire into the molten metal may not be stable. In this case, the concentration of the additive element in the rough wire produced by continuous casting is not stable. If there is variation in the concentration of the additive element, this causes the properties such as the tensile strength or electrical conductivity of the copper alloy wire produced by drawing the rough wire to be unstable.
[0023] In this embodiment, in the manufacturing process of the wire rod made of the cast alloy to which two or more kinds of additive elements are added, the additive element supply unit 40 uses both the supply of the wire rod 43 supplied from the wire rod supply unit 41 to the molten metal and the supply of the lump (ingot) 44 supplied from the lump supply unit (ingot supply unit) 42 to the molten metal. In other words, the manufacturing method of the wire rod of this embodiment includes a step (first adding step) of continuously supplying a first additive element (such as tin which is harder than indium (has a large Brinell hardness (HB) value)) as the wire rod 43 to the molten metal to add the first additive element to the base material constituting the molten metal, and a step (second adding step) of intermittently adding a second additive element (such as a metal such as indium which is less hard (has a small Brinell hardness (HB) value) than the first additive element made of metal made of tin) as the lump 44 to the molten metal to add the second additive element to the base material constituting the molten metal. The second additive element is, for example, a metal having a Brinell hardness value of 0.1HB or more and 1.0HB or less. For example, indium (In) is used as such a metal. The first additive element is, for example, a metal having a Brinell hardness value greater than that of the metal constituting the second additive element. The first additive element is, for example, a metal having a Brinell hardness value greater than 1.0HB. For example, tin (Sn), aluminum (Al), magnesium (Mg), titanium (Ti), nickel (Ni), iron (Fe), zinc (Zn), zirconium (Zr), silver (Ag), etc. are used as such a metal. The Brinell hardness can be measured, for example, by a Brinell hardness tester.
[0024] In this way, in the manufacturing process of rough wire made of a cast alloy to which two or more types of additive elements have been added, a second addition step in which an additive element (second additive element) that is difficult to form into a wire shape is supplied to the molten metal as a lump (ingot) 44 to add the second additive element to the base material is provided in combination with a first addition step in which an additive element (first additive element) is supplied to the molten metal as a wire to add the first additive element to the base material. This makes it possible to stably manufacture rough wire made of a cast alloy in which the concentrations of each of two or more types of additive elements are stabilized by continuous casting.
[0025] From the viewpoint of stabilizing the concentration of the additive element added to the base metal, it is preferable that the second adding step of adding the second additive element as lumps 44 satisfies the following conditions. This makes it difficult for the concentration of the additive element present in the base metal to vary when the second additive element is supplied to the molten metal as lumps 44.
[0026] First, each of the multiple lumps 44 added in the above-mentioned second adding step preferably has a mass of 100 g or more and 300 g or less. By making the mass of the lumps 44 300 g or less, the dissolution rate of the lumps 44 in the molten metal can be accelerated, and the variation in the concentration of the added element caused by the variation in the dissolution rate can be reduced. Furthermore, from the viewpoint of suppressing scattering of the lumps 44 due to the influence of the surrounding environment when the lumps 44 are supplied into the molten metal, the mass of the lumps 44 is preferably 100 g or more.
[0027] In the second addition step, it is preferable to supply a plurality of lumps 44 intermittently to the molten metal. In this case, in order to stabilize the concentration of the second additive element present in the base material constituting the molten metal, it is preferable to shorten the interval at which the lumps 44 are supplied to the molten metal (the interval from when the lumps 44 are supplied to the molten metal until the next lumps 44 are supplied to the molten metal). In the second addition step, it is preferable to supply the lumps 44 intermittently to the molten metal at intervals of 1 second or more and 30 seconds or less. By shortening the interval at which the lumps 44 are supplied, it is possible to reduce unevenness in the concentration of the additive element dissolved in the base material constituting the molten metal, and therefore it is possible to reduce variation in the concentration distribution of the additive element added to the cast alloy constituting the obtained rough wire. It is possible to change the interval at which the lumps 44 are supplied to the molten metal according to changes in the flow rate of the molten metal and the flow rate of the molten metal.
[0028] FIG. 2 is a perspective view showing an example of the shape of the lump supplied from the lump supply unit shown in FIG. 1 to the molten metal. FIG. 3 is a cross-sectional view showing a cut surface of the lump shown in FIG. 2. In this example, the lump 44 composed of the second additive element has an ingot shape. The ingot shape can be defined as follows. The lump 44 has a quadrangular upper surface 44t, a quadrangular lower surface 44b having the same area as the upper surface 44t or a larger area than the upper surface 44t, and a side surface 44s connected to the upper surface 44t and the lower surface 44b on the opposite side to the upper surface 44t. In addition, the shape of a cross section 44cv along a plane passing through the center of the upper surface 44t and the center of the lower surface 44b is a trapezoid as shown in FIG. 3. The shape of the cross section 44cv of the lump 44 is not limited to a trapezoid, and may be a shape consisting of a rectangle.
[0029] There are various modified shapes of the ingot 44. For example, the ingot 44 may be a shape obtained by deforming a linear shape into an ingot shape. However, in the above-mentioned second addition step, a plurality of ingots 44 are intermittently supplied. For this reason, from the viewpoint of stabilizing the mass of each of the plurality of ingots 44, it is preferable that the plurality of ingots 44 are shaped into the same shape. This can reduce the variation in the mass of the ingots 44, and therefore, by controlling the timing of supply, it is possible to reduce the variation in the concentration distribution of the additive element added to the cast alloy constituting the obtained rough wire. In addition, in the case of the ingot shape exemplified in FIG. 2 and FIG. 3, the shaping operation is easier and there is less raw material loss than in the case of shaping into a linear shape. For this reason, it is preferable to use the ingot-shaped ingot 44 in terms of improving the manufacturing efficiency of the ingots 44.
[0030] <Modification> Next, a modified example of Fig. 1 will be described. Fig. 4 is an explanatory diagram showing a modified example of Fig. 1. The modified wire rod manufacturing apparatus 101 shown in Fig. 4 differs from the wire rod manufacturing apparatus 100 shown in Fig. 1 in that the lump supplying section 42 is arranged upstream of the wire rod supplying section 41. In the case of the manufacturing method of the wire rod using the wire rod manufacturing apparatus 101, the second adding step is performed before the first adding step. That is, in the molten metal supplied from the holding furnace 20, a lump 44 made of the second additive element is intermittently supplied first, and then the wire rod 43 made of the first additive element is continuously supplied. In this way, the order of the first adding step and the second adding step described with reference to FIG. 1 is not particularly limited. Except for the above-mentioned differences, the manufacturing method of the wire rod using the wire rod manufacturing apparatus 101 shown in FIG. 4 is the same as the manufacturing method of the wire rod described with reference to FIG. 1, so that a duplicated description will be omitted. Note that, in the case where the lump 44 made of the second additive element is intermittently supplied first, and then the wire rod 43 made of the first additive element is continuously supplied into the molten metal supplied from the holding furnace 20, the supply position of the wire rod 43 made of the first additive element is relatively close to the mold 50, so that the first additive element can be easily melted during metal melting even if the first additive element is composed of a metal highly active against oxygen.
[0031] The present invention is not limited to the above-described embodiment and examples, and various modifications can be made without departing from the spirit and scope of the present invention. [Industrial Applicability]
[0032] The present invention is widely applicable to the production of alloy wires that constitute conductors used in electric wires, cables, and the like. [Explanation of symbols]
[0033] 10 Melting furnace 11 Transport trough 20 Holding furnace 30 Tundish 31 Spout (nozzle) 40 Additive element supply section 41 Wire supply section 42 Lump supply section 43 Wire rod 44 Lump 44t top surface 44b Bottom side 44s side 44cv cross section 50 Mold 51 Casting Wheel 53 Casting Belt 54 Mold 54 Pool Club 60 Rolling Section 70 Winding section 80 Arahiki line 81 Casting material (ingot) 100,101 Rough wire manufacturing equipment r1 Rotation direction
Claims
1. A method for producing a wire rod obtained by continuous casting and rolling, comprising the steps of: (a) obtaining a molten metal comprising a base material; (b) continuously supplying a first additive element to the molten metal as a wire; (c) before or after the step (b), intermittently supplying a second additive element different from the first additive element as a lump to the molten metal; (d) continuously casting the molten metal containing the first additive element and the second additive element in a mold to form a casting material; having The second additional element is composed of a metal having a smaller Brinell hardness value than the first additional element. A method for manufacturing a wire rod.
2. The method for producing a rough wire rod according to claim 1, The method for producing a wire rod, wherein the second additional element is indium.
Citation Information
Patent Citations
Continuous casting and rolling method of al or al alloy
JP1984035863A
Heat-resistant and highly conductive composite linear body
JP1993267090A
Extra fine copper wire and its production
JP1999152532A
Production of high-strength high-electrical conductivity copper wire
JP1999277184A
Method for producing oxygen-free copper wire rod with belt and wheel type continuous casting and rolling method for producing copper alloy wire rod
JP2002120050A