Carbon dioxide reduction device and artificial photosynthesis device
The carbon dioxide reduction device uses a gas diffusion electrolytic flow cell with a metal complex catalyst and anion exchange membrane to achieve low-potential, high-efficiency carbon dioxide reduction to formate ions, addressing the inefficiencies of conventional methods.
Patent Information
- Application Number
- JP2022039248
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-03-14
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2042-03-14
AI Technical Summary
Conventional carbon dioxide reduction devices suffer from high operating potentials, leading to low energy conversion efficiency and high production of hydrogen by-products, with limitations in reaction current density and catalyst modularity.
A carbon dioxide reduction device employing a gas diffusion type electrolytic flow cell with an anode and cathode separated by an anion exchange membrane, utilizing a metal complex catalyst with diimine ligands and an alkaline solution, and a hydrophobic gas diffusion layer to facilitate low-potential carbon dioxide reduction to formate ions.
The device achieves a low cell potential of 2V or less, enabling high conversion efficiency and large reaction current density with reduced hydrogen by-products, while maintaining an optimal reaction environment at both electrodes.
Smart Images

Figure 0007552634000004 
Figure 0007552634000005 
Figure 0007552634000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbon dioxide reduction device and an artificial photosynthesis device. [Background technology]
[0002] In recent years, concerns have arisen over the depletion of fossil fuels such as oil and coal, and expectations are growing for sustainable renewable energy sources. From the perspective of such energy issues, as well as environmental issues, progress has been made in the development of artificial photosynthesis technology, which uses renewable energy such as sunlight to electrochemically reduce carbon dioxide and create a storable chemical energy source.
[0003] One method for reducing carbon dioxide is to electrochemically reduce carbon dioxide dissolved in an aqueous solution to formic acid (see, for example, Patent Document 1). However, conventional carbon dioxide reduction electrolysis devices such as the method in Patent Document 1 reduce carbon dioxide dissolved in a solution (see, for example, Figure 1 in Patent Document 1). In this example, metal nanowires such as copper (Cu) are used as a carbon dioxide reduction catalyst, and platinum (Pt) is used as a water (H2O) oxidation catalyst.
[0004] In recent years, the development of gas diffusion type carbon dioxide reduction electrodes has progressed, and for example, Non-Patent Document 1 reports a carbon dioxide reduction device in which an electrolyte solution for the anode chamber (potassium bicarbonate (KHCO3) aqueous solution), an ion conductive membrane, and an electrolyte solution for the cathode chamber (potassium hydroxide (KOH) aqueous solution) are arranged between a gas diffusion type negative electrode (cathode) for carbon dioxide reduction and a positive electrode (anode) for H2O oxidation (see Figure 2 in Non-Patent Document 1). In this example, tin oxide is used as the carbon dioxide reduction catalyst, and nickel (Ni) is used as the hydroxide catalyst.
[0005] As another example, Non-Patent Document 2 describes a carbon dioxide reduction device that is composed of an anion exchange membrane, an aqueous solution layer, and a cation exchange membrane between a gas diffusion type negative electrode and a positive electrode (see Figure 3 in Non-Patent Document 2). In this example, tin nanoparticles are used as the carbon dioxide reduction catalyst, and iridium oxide (IrO2) is used as the hydroxide catalyst.
[0006] In the case of the electrode immersion method as described in Patent Document 1, the concentration of carbon dioxide dissolved in the aqueous solution is low at room temperature and normal pressure, so the coexisting protons (H + ) is reduced, and hydrogen (H2) is produced as a by-product. In addition, because the mass diffusion of carbon dioxide in an aqueous solution is slow, the theoretical limit of the reaction current density for carbon dioxide reduction is <30 mAcm -2 and small.
[0007] In the case of the gas diffusion method as in Non-Patent Documents 1 and 2, carbon dioxide gas is mixed with water vapor gas and supplied directly to the negative electrode, so that the concentration ratio of carbon dioxide to water is large, and the by-production of hydrogen (H2) is suppressed. In addition, since the reaction proceeds in the gas phase with a fast diffusion rate, the limit of the reaction current density is greatly increased. Furthermore, since different electrolyte solutions can be used in the positive electrode chamber and the negative electrode chamber, it is possible to create an optimal reaction environment at both electrodes by supplying carbon dioxide to the negative electrode while making the positive electrode an alkaline environment in which water oxidation is easy. However, in the method of Non-Patent Document 1, the positive electrode and the negative electrode are arranged via two types of electrolyte solutions and a membrane membrane, and in the method of Non-Patent Document 2, the positive electrode and the negative electrode are arranged via an anion exchange membrane, an ion conductive resin layer, and a cation exchange membrane, and therefore, due to the resistance of these, a large iR potential drop occurs, and the operating potential becomes high.
[0008] In addition, in most of the conventional technologies, the carbon dioxide reduction catalyst was a metal such as tin (Sn) or its oxide. Meanwhile, metal complexes consisting of metal ions and organic ligands are known as carbon dioxide reduction catalysts. In the case of metal complexes consisting of metal ions and organic ligands, the design of the organic ligands can be freely modified, so the properties of the catalyst can be greatly changed. However, the properties of the metals or metal oxides used in most of the conventional technologies can only be modified by adjusting the metal-metal bond or metal-oxygen bond. For this reason, it is difficult to reduce the activation energy and reaction potential in the carbon dioxide reduction reaction as a catalyst.
[0009] For the above reasons, the operating potential of the carbon dioxide reduction device of the prior art is still high. In other words, the efficiency of energy conversion from electrical energy to chemical energy during operation is low. For example, in the electrolysis of carbon dioxide at a cell potential of 2 V, formate ions (HCOO - ), the energy conversion efficiency is 53%. If operation at a cell potential of 1.5V is achieved, the energy conversion efficiency will reach 74%. It is desirable to operate the cell at 1.24V or less, which corresponds to an energy conversion efficiency of 90% or more. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] JP 2017-057438 A [Non-patent literature]
[0011] [Non-Patent Document 1] ACS Sustainable Chem. Eng. 2021, 9, 11, 4213-4223 [Non-Patent Document 2] https: / / dioxidematerials.com / technology / formic-acid / Summary of the Invention [Problem to be solved by the invention]
[0012] An object of the present invention is to provide a carbon dioxide reduction device and an artificial photosynthesis device that are capable of obtaining formate ions at a low cell potential and with high conversion efficiency. [Means for solving the problem]
[0013] The present invention provides an electrochemical cell comprising an anode section including an anode that oxidizes water to produce oxygen and an anode solution flow path that supplies an anode solution to the anode, a cathode that reduces carbon dioxide to produce formic acid or formate ions and a cathode section including a gas flow path that supplies carbon dioxide gas to the cathode, and an anion exchange membrane sandwiched between the anode section and the cathode section, the cathode including, in order from the anion exchange membrane side, a catalyst layer including a metal complex as a cathode catalyst and a gas diffusion layer, and an alkaline solution is supplied as the anode solution. The metal complex has at least one metal selected from the group consisting of Ru, Mn, Fe, Co, Ni, Cu, Mo, and Re as a central metal, and has a diimine ligand as a ligand. It is a carbon dioxide reduction device.
[0015] In the carbon dioxide reduction device, the diimine ligand is preferably a diimine ligand having an electron-withdrawing substituent introduced therein.
[0016] In the carbon dioxide reduction device, it is preferable that the electron-withdrawing substituent is a carboxylic acid ester having a structural formula -COOR, R has a chemical structure consisting of an alkyl group and a pyrrole moiety, and the pyrrole moiety is polymerized through a polypyrrole chain.
[0017] In the carbon dioxide reduction device, the catalyst layer preferably contains a polymer compound that serves as an ion conductor and a binder, and conductive carbon.
[0018] In the carbon dioxide reduction device, the gas diffusion layer preferably includes a hydrophobic porous carbon substrate.
[0019] In the carbon dioxide reduction device, it is preferable that the anode comprises a substrate made of at least one material selected from the group consisting of Ni, Ti, Fe, and C, the substrate having at least one shape selected from the group consisting of a porous body, a mesh material, and a sintered fiber body, and the anode contains, as an anode catalyst, at least one selected from the group consisting of a metal containing at least one element selected from the group consisting of Ni, Fe, Co, Mn, Ru, and Ir, an oxide containing the metal, a hydroxide containing the metal, and an oxyhydroxide containing the metal.
[0020] In the carbon dioxide reduction device, the anode preferably contains, as the anode catalyst, at least one selected from the group consisting of iron oxyhydroxide and nickel oxyhydroxide.
[0021] In the carbon dioxide reduction device, it is preferable that the alkaline solution is an alkaline aqueous solution having a pH of 12 or more, the cell voltage between the anode and the cathode is 2 V or less, and the formic acid is produced in the cathode section.
[0022] The present invention is an artificial photosynthesis device comprising the carbon dioxide reduction device and a solar cell that generates electricity to be supplied to the anode and the cathode. Effect of the Invention
[0023] According to the present invention, it is possible to provide a carbon dioxide reduction device and an artificial photosynthesis device that are capable of obtaining formate ions at a low cell potential and with high conversion efficiency. [Brief description of the drawings]
[0024] [Figure 1] FIG. 1 is a schematic configuration diagram showing an example of a carbon dioxide reduction device according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic diagram showing the configuration of an electrode immersion type carbon dioxide reduction device used in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The following describes an embodiment of the present invention. The embodiment is merely an example of implementing the present invention, and the present invention is not limited to the embodiment.
[0026] FIG. 1 shows a schematic configuration of an example of a carbon dioxide reduction device according to this embodiment.
[0027] 1 includes an anode section 10 including an anode 16 that oxidizes water to generate oxygen and an anode solution flow path 18 that supplies an anode solution to the anode 16, a cathode section 12 including a cathode 22 that reduces carbon dioxide to generate formic acid or formate ions and a gas flow path 24 that supplies carbon dioxide gas to the cathode 22, and an anion exchange membrane 14 sandwiched between the anode section 10 and the cathode section 12. The cathode 22 includes, in order from the anion exchange membrane 14 side, a catalyst layer 26 containing a metal complex as a cathode catalyst and a gas diffusion layer 28, and supplies an alkaline solution as the anode solution. The carbon dioxide reduction device 1 includes an anode current collector 20 and a cathode current collector 30.
[0028] The carbon dioxide reduction device 1 is a gas diffusion type electrolysis flow cell that directly supplies carbon dioxide gas to the catalyst layer 26 of the cathode 22. The carbon dioxide gas is a gas containing carbon dioxide, and preferably a gas containing carbon dioxide and water vapor.
[0029] The anode 16 is disposed between the anion exchange membrane 14 and the anode solution flow path 18 so as to be in contact with them. The anode solution flow path 18 is a flow path that supplies the anode solution to the anode 16, and is formed, for example, by a pit (groove or recess) provided in the anode current collector 20. The cathode 22 is disposed between the gas flow path 24 and the anion exchange membrane 14 so as to be in contact with them. The gas flow path 24 is a flow path that supplies carbon dioxide gas to the cathode 22, and is formed by a pit (groove or recess) provided in the cathode current collector 30. The anion exchange membrane 14 is sandwiched between the anode section 10 and the cathode section 12. The anode section 10 and the cathode section 12 are separated by the anion exchange membrane 14.
[0030] For example, a solution inlet and a solution outlet (neither shown) are connected to the anode current collector 20. The anode solution is introduced into the anode solution flow path 18 via the solution inlet, passes through the anode solution flow path 18 while in contact with the anode 16, and is discharged from the anode solution outlet.
[0031] For example, a gas inlet and a gas outlet (neither shown) are connected to the cathode current collector 30. Carbon dioxide gas is introduced into the gas flow passage 24 through the gas inlet, passes through the gas flow passage 24 while contacting the catalyst layer 26 via the gas diffusion layer 28, and is discharged from the gas outlet.
[0032] The carbon dioxide reduction device 1 includes a power supply 32 that electrically connects between the anode 16 and the cathode 22 and supplies power therebetween.
[0033] Next, an example of the operation of the carbon dioxide reduction device 1 shown in FIG. 1 will be described.
[0034] When a current is supplied between the anode 16 and the cathode 22 from the power source 32, an oxidation reaction of water (H2O) occurs at the anode 16 in contact with the anode solution. Specifically, the water (H2O) contained in the anode solution is oxidized to produce oxygen (O2).
[0035] On the cathode 22 side, carbon dioxide (CO2) contained in the carbon dioxide (CO2) gas supplied from the gas flow channel 24 to the catalyst layer 26 through the gas diffusion layer 28 is reduced to generate formic acid (HCOOH). The generated formic acid (HCOOH) is ionized to form formate ions (HCOO - The formate ion (HCOO) obtained at the cathode 22 is - ) permeates through the anion exchange membrane 14 and is obtained in the anode solution in the anode section 10. Overall, as shown in the reaction formula (1) below, formate ions (HCOO - ) is generated. CO2+OH - → HCO - +1 / 2O2ΔG=215.7kJ / mol ···(1)
[0036] The configurations of the anode section 10, the cathode section 12, and the anion exchange membrane 14 will be described below.
[0037] As described above, the anode 16 promotes the oxidation reaction of water (HO) in the anode solution to produce oxygen (O) and hydrogen ions (H + ) is an electrode (oxidation electrode).
[0038] The anode 16 preferably includes a base material made of at least one material selected from the group consisting of Ni, Ti, Fe, and C, in that it can reduce the overvoltage of the oxidation reaction. The metal material of Ni, Ti, or Fe also includes an alloy containing at least one of the metals Ni, Ti, and Fe. The base material preferably has a structure that allows the anode solution and ions to move between the anion exchange membrane 14 and the anode solution flow path 18, and preferably has at least one shape selected from the group consisting of, for example, a porous body, a mesh material, and a sintered fiber body.
[0039] The anode 16 includes an anode catalyst. The anode catalyst preferably includes at least one selected from the group consisting of a metal containing at least one element selected from the group consisting of Ni, Fe, Co, Mn, Ru, and Ir, an oxide containing the metal, a hydroxide containing the metal, and an oxyhydroxide containing the metal, in that it can reduce the overvoltage of the oxidation reaction. These may be used alone or in combination of two or more. The anode catalyst preferably includes at least one selected from the group consisting of iron oxyhydroxide and nickel oxyhydroxide in that it can cause the oxidation of water to proceed at a low potential. When using an anode catalyst, it is preferable to support the anode catalyst on the above-mentioned substrate.
[0040] It is preferable to use a material with low chemical reactivity and high conductivity for the anode current collector 20. Examples of such a material include metal materials such as Ti and SUS, and carbon.
[0041] The anode solution is an alkaline solution, such as an aqueous potassium hydroxide solution, an aqueous sodium hydroxide solution, an aqueous potassium carbonate solution, or an aqueous potassium hydrogen carbonate solution. Since the higher the hydroxide ion concentration, the more favorable the oxidation of water, an aqueous potassium hydroxide solution or an aqueous sodium hydroxide solution having a concentration of 1 mol / L or more is preferred.
[0042] The alkaline anode solution is preferably an alkaline aqueous solution having a pH of 12 or more, from the viewpoint of preventing a decrease in cell voltage, for example.
[0043] As described above, the cathode 22 promotes the reduction reaction of carbon dioxide (CO2) to produce formic acid (HCOOH) or formate ions (HCOO - ) is an electrode that produces hydrogen (reduction electrode).
[0044] The gas diffusion layer 28 constituting the cathode 22 is not particularly limited as long as it ensures electrical conduction between the catalyst layer 26 and the power source 32 and efficiently supplies carbon dioxide gas to the catalyst layer 26, and examples of the material include a hydrophobic porous carbon substrate, carbon black, carbon nanotubes, etc. The gas diffusion layer 28 is preferably a hydrophobic porous carbon substrate, since it can reduce the amount of water that has moved from the cathode 22 side.
[0045] As described above, the catalyst layer 26 constituting the cathode 22 promotes the reduction reaction of carbon dioxide in the carbon dioxide gas to produce formic acid (HCOOH) or formate ions (HCOO - ) is produced. The catalyst layer 26 contains a metal complex as a cathode catalyst. The catalyst layer 26 preferably further contains a polymer compound that serves as an ion conductor and binder, and conductive carbon. The catalyst layer 26 preferably contains a porous structure such as carbon paper as a substrate in order to improve the diffusibility of carbon dioxide gas. The thickness of the catalyst layer 26 is, for example, in the range of 5 to 200 μm.
[0046] The metal complex serving as the cathode catalyst is, for example, a metal complex having a central metal and a diimine ligand. The central metal of the metal complex is not particularly limited as long as it is a metal that catalyzes the reduction reaction of carbon dioxide, but is preferably at least one metal selected from the group consisting of Ru, Mn, Fe, Co, Ni, Cu, Mo, and Re, and more preferably Mn or Ru, in that it is possible to reduce the overvoltage in the reduction reaction of carbon dioxide.
[0047] Examples of the diimine ligand of the metal complex include 2,2'-bipyridine derivatives, 1,10-phenanthroline derivatives, etc. The diimine ligand is preferably a diimine ligand having an electron-withdrawing substituent introduced therein, in that it can reduce the overvoltage caused by the reduction reaction of carbon dioxide.
[0048] Examples of electron-withdrawing substituents introduced into the diimine ligand include carboxylic acid groups, carbonyl groups, nitro groups, and carboxylic acid esters having the structural formula -COOR. Here, R is, for example, a linear or branched alkyl group having 1 to 10 carbon atoms. R has a chemical structure consisting of an alkyl group and a pyrrole moiety, and the pyrrole moiety is preferably polymerized by a polypyrrole chain, in order to ensure electrical conduction between the diimine ligand and a power source.
[0049] The metal complex is preferably a molecule in which the central metal is Ru and 2,2'-bipyridine and pyrrole are chemically bonded with a carboxylate of -COOR (R is an alkyl group having 1 to 10 carbon atoms), or a polymer in which the pyrrole moiety is polymerized with a polypyrrole chain to form a multimer.
[0050] An example of the metal complex is the metal complex represented by the following chemical formula: [Ru{4,4'-di(1H-pyrrolyl-3-propylcarbonate)-2,2'-bipyridine}Cl2(CO)(CH3CN)]. [ka]
[0051] Examples of the conductive carbon contained in the catalyst layer 26 include carbon black such as Ketjen Black and Vulcan XC-72, activated carbon, and carbon nanotubes. The conductive carbon is preferably used as a support for supporting the metal complex. By supporting the metal complex on the conductive carbon, for example, the reduction reactivity can be increased.
[0052] Examples of the polymer serving as the ion conductor and binder contained in the catalyst layer 26 include cation exchange resins such as Nafion (manufactured by DuPont) and Flemion (manufactured by Asahi Glass Co., Ltd.), and anion exchange resins such as Neocepta, Selemion, and Sustenion.
[0053] The catalyst layer 26 may include phenol or a salt thereof, which can enhance catalytic activity.
[0054] The cathode current collector 30 is preferably made of a material having low chemical reactivity and high conductivity, similar to the anode current collector 20. Examples of such materials include metal materials such as Ti and stainless steel (SUS), and carbon.
[0055] An alkaline solution is used for the anode solution, and the main ions are hydroxide ions (OH - ) is transferred using an anion exchange membrane 14. As the anion exchange membrane 14, for example, anion exchange membranes such as Neocepta (registered trademark), Selemion (registered trademark), and Sustenion (registered trademark) can be used.
[0056] The power source 32 is not particularly limited, and examples thereof include a chemical battery (including a primary battery, a secondary battery, etc.), a constant voltage source, a solar cell, etc. By using a solar cell as the power source 32, an artificial photosynthesis device can be provided that includes the carbon dioxide reduction device 1 and a solar cell that generates power to be supplied to the anode 16 and the cathode 22 of the carbon dioxide reduction device 1. In the artificial photosynthesis device according to this embodiment, the anode 16 and the cathode 22 of the carbon dioxide reduction device 1 are connected via the solar cell, and the artificial photosynthesis device is driven by sunlight as an energy source.
[0057] It is preferred that the cell voltage between anode 16 and cathode 22 be 2V or less, more preferably 1.5V or less, and even more preferably 1.2V or less.
[0058] By using the carbon dioxide reduction device according to this embodiment, it is possible to generate a large reaction current density at a low cell potential and obtain formate ions with high conversion efficiency. The carbon dioxide reduction device according to this embodiment makes it possible to reduce carbon dioxide (CO2) to formic acid (HCOOH) with a low cell potential, a large reaction current density, and high selectivity, and to oxidize water (H2O) to generate oxygen (O2). In an alkaline solution, neutralization actually occurs, so that, overall, the reaction of storing electrical energy into chemical energy, as represented by the above reaction formula (1), can proceed.
[0059] By using the gas diffusion type carbon dioxide reduction device according to this embodiment, it becomes possible to supply carbon dioxide as a gas, thereby increasing the current density of the carbon dioxide reduction reaction and reducing the by-production of hydrogen (H2).
[0060] By using a gas diffusion type carbon dioxide reduction device equipped with a membrane / electrode assembly, the electrolyte solution is no longer interposed between the anode and cathode, and the iR potential drop can be suppressed by reducing the resistance between the two electrodes.
[0061] The oxidation of water (H2O) at the anode proceeds easily in an alkaline solution, but carbon dioxide is converted to HCO3 in an alkaline environment. - and CO3 2- Due to the equilibrium with cation, carbon dioxide cannot exist as carbon dioxide. By separating the two electrodes with an anion exchange membrane, it is possible to create an optimal reaction environment at both electrodes by providing carbon dioxide to the cathode while keeping the anode in an alkaline environment.
[0062] Furthermore, metal complexes such as Ru complexes having ligands in which electron-withdrawing substituents have been introduced as diimine ligands can act as catalysts for reducing carbon dioxide to produce formic acid at low potential. Therefore, by applying these complexes to a gas diffusion-type carbon dioxide reduction device equipped with a membrane / electrode assembly, it is possible to reduce carbon dioxide to produce formic acid (HCOOH) at extremely low potential.
[0063] In addition, by introducing an anode catalyst for hydroxylation onto the anode for hydroxylation, further reduction of the potential becomes possible.
Examples
[0064] Hereinafter, examples and comparative examples will be given to describe the present invention more specifically and in detail. However, the present invention is not limited to the following examples.
[0065] Using a Ru complex polymer having the chemical structure shown in the following (i) as a cathode catalyst, a carbon dioxide reduction device as shown in FIG. 1 was fabricated and evaluated.
[0066] [Fabrication of Electrodes] (Fabrication of Cathode) >[Fabrication of Ru Complex Catalyst-Supported Gas Diffusion-Type Cathode] Using carbon paper as a gas diffusion layer, a catalyst layer containing a mixture of a metal complex as a catalyst, an ion conductor, a polymer compound as a binder, and conductive carbon was laminated thereon. Specifically, 17.1 mg (0.0244 mmol) of [Ru{4,4’-di(1H-pyrrolyl-3-propylcarbonate)-2,2’-bipyridine}Cl2(CO)(CH3CN)] having the chemical structure of the following (i) was dissolved in 2.55 mL of acetonitrile, and 137 μL of a 0.5 vol% acetonitrile solution of pyrrole and 686 μL of a 0.2 M ethanol solution of FeCl3 were added thereto to prepare a solution of a metal complex polymer represented by the structural formula of the following (i). To this solution, 27.5 mg of carbon black (Vulcan XC-72R, manufactured by Cabot Corporation) as conductive carbon and 229.5 μL of an alcohol-water mixed solution (manufactured by Aldrich) of 5 mass% Nafion (registered trademark) 117 as an ion conductor and a polymer compound as a binder were added, and then ultrasonic dispersion was performed. This suspension was applied to a 1.13 cm substrate 2It was supported by repeating the operation of dropping 41 μL onto carbon paper with a microporous layer (manufactured by Avcarb, GDS3250) and drying at 60 °C 30 times. After standing in the dark for 12 hours or more, it was washed in water to remove FeCl3, which is the reaction catalyst.
[0067]
Chemical formula
[0068] <Fabrication of Sn-Supported Gas Diffusion Anode> By RF magnetron sputtering, an amount of Sn equivalent to 10 nm was sputtered onto carbon paper with a microporous layer (manufactured by Avcarb, GDS3250), and it was cut out to 1.13 cm 2 in size.
[0069] <Fabrication of Ru Complex Catalyst-Supported Immersion Anode> A catalyst layer containing a mixture of a metal complex as a catalyst, an ionic conductor, a polymer compound as a binder, and conductive carbon was laminated on an electrode with microporous layer-attached carbon paper (manufactured by Avcarb, GDS3250) pasted on a stainless steel plate. Specifically, 18.76 mg of [Ru{4,4’-di(1H-pyrrolyl-3-propylcarbonate)-2,2’-bipyridine}Cl2(CO)(CH3CN)] as a metal complex was dissolved in 3.3 mL of acetonitrile, and 75 μL of an acetonitrile solution of 0.5 vol% pyrrole and 375 μL of a 0.2 M FeCl3 ethanol solution were added thereto to prepare a solution of the metal complex polymer represented by the structural formula (1) above. 15 mg of carbon black (manufactured by Cabot, Vulcan XC-72R) as conductive carbon was added to this solution, and the solvent was distilled off under reduced pressure to complex carbon and the catalyst. To this composite powder, 1.1 mL of 2-propanol and 106 μL of an alcohol-water mixed solution (manufactured by Aldrich) of 5 mass% Nafion (registered trademark) 117 as an ionic conductor and a polymer compound as a binder were added, and then ultrasonic dispersion was performed. This suspension was dropped in an amount of 117 μL onto 1.5 cm × 2.5 cm microporous layer-attached carbon paper as a substrate and dried at 60 °C, and this operation was repeated twice to support it. After standing in the dark for 12 hours or more, it was washed with water to remove FeCl3 as a reaction catalyst.
[0070] (Fabrication of Anode) <Fabrication of Nickel Foam Electrode> Nickel foam (manufactured by MTI, EQ-BCNF-16m) was cut into 1.13 cm 2 and used as it was.
[0071] <Fabrication of Nickel Foam Supporting Fe-Ni Added β-FeOOH> A Ni-doped β-FeOOH colloidal solution was prepared by mixing 0.1 M iron chloride aqueous solution, 0.05 M nickel nitrate aqueous solution, and ethylenediamine hydrochloride aqueous solution and adjusting the pH to 2.3. 10 mL of this Ni-doped β-FeOOH colloidal solution was mixed with 10 mL of an aqueous solution of 0.063 M nickel chloride and 0.055 mM iron chloride, and a 1.13 cm2 substrate was prepared. 2 After immersing nickel foam (EQ-BCNF-16m, manufactured by MTI) in the solution, it was heated and dried at 150°C for 8 hours to produce a nickel foam carrying Fe-Ni-doped β-FeOOH.
[0072] [Electrolysis of carbon dioxide] <Carbon dioxide electrolysis using a gas diffusion method with a membrane / electrode assembly> An electrolytic cell having the configuration shown in FIG. 1 was used. The anode electrode prepared as described above was used as the anode, and the cathode electrode prepared as described above was used as the cathode. An anion-conductive resin (Sustainion (registered trademark) X37-50 Grade) was placed between the two electrodes as an anion exchange membrane so as to be in contact with the catalyst. This membrane / electrode assembly was sandwiched between a cathode current collector and an anode current collector with flow paths so as to be in contact with the gas flow path and the alkaline solution flow path, and then fastened with bolt screws. Here, a stainless steel cathode current collector and a titanium anode current collector were used. Carbon dioxide gas was supplied to the flow path of the cathode section at a flow rate of 30 mL / min, and a 1 M potassium hydroxide aqueous solution was supplied to the flow path of the anode section as an alkaline solution at a flow rate of 100 mL / min. This electrolytic cell was connected to a potentiostat in a two-pole manner, and a constant potential was applied to electrolyze carbon dioxide. After electrolysis, the concentration of formate ions in the electrolyte on the anode side was quantified by ion chromatography (ICS-1100, manufactured by Dionex).
[0073] <Electrolysis of carbon dioxide using the electrode immersion method> An electrode-immersion type carbon dioxide reduction device 50 as described in Patent Document 1 having the configuration shown in FIG. 2 was used. Electrochemical measurements were performed using a potentiostat in a three-electrode system in which the above-mentioned Ru complex catalyst-supported immersion type negative electrode was installed as the working electrode 54, a platinum wire was installed as the counter electrode 52, and an Ag / AgCl electrode was installed as the reference electrode 56 in an electrolyte tank 62. A 0.4 mol / L aqueous phosphate buffer solution was used as the electrolyte solution 58. Measurements were performed by passing carbon dioxide through the container and then sealing it. After applying a potential of -0.96 V vs Ag / AgCl for a predetermined time using a power source 60, the gas phase in the cell was measured by gas chromatography (Inficon, Fusion) and the liquid phase was measured by ion chromatography, and the products were quantified.
[0074] [Measurement electrode] As examples and comparative examples, electrodes carrying the following catalysts were placed in the above electrolytic cell and measurements were carried out.
[0075] <Example 1: Carbon dioxide electrolysis using Ru complex polymer-Ni foam in a membrane / electrode assembly gas diffusion system> The Ru complex catalyst-supported gas diffusion type negative electrode was used as the cathode, and the nickel foam electrode was used as the anode, and electrolytic reduction of carbon dioxide was carried out in a gas diffusion system equipped with the membrane / electrode assembly.
[0076] <Example 2: Carbon dioxide electrolysis using Ru complex polymer-Fe-Ni-added β-FeOOH supported Ni foam in a membrane / electrode assembly gas diffusion system> The above-mentioned Ru complex catalyst-supported gas diffusion type negative electrode was used as the cathode, and the above-mentioned Fe-Ni-added β-FeOOH-supported nickel foam was used as the anode, and electrolytic reduction of carbon dioxide was performed using a gas diffusion type equipped with the above-mentioned membrane / electrode assembly.
[0077] <Comparative Example 1: Carbon dioxide electrolysis using Sn-Fe-Ni-added β-FeOOH-supported Ni foam in a membrane / electrode assembly gas diffusion system> The above Sn-supported gas diffusion type negative electrode was used as the cathode, and the above Fe-Ni-added β-FeOOH-supported nickel foam was used as the anode, and electrolytic reduction of carbon dioxide was carried out in a gas diffusion system equipped with the above membrane / electrode assembly.
[0078] <Comparative Example 2: Electrolysis of carbon dioxide using Ru complex polymer-Pt in the electrode immersion method> The above-mentioned Ru complex catalyst-supported immersion-type negative electrode was used as the cathode, Pt was used as the anode, and Ag / AgCl was used as the reference electrode, and electrolytic reduction of carbon dioxide was carried out by the above-mentioned electrode immersion method.
[0079] [result] (Action and effect of catalyst) In order to compare the catalytic effects of metal complexes having ligands in which electron-withdrawing substituents have been introduced into the diimine ligand, Table 1 shows the current values per unit volume of the electrode when various cell potentials were applied in Examples 1 and 2 and Comparative Example 1, and the ratios of various products to the current values (Faraday efficiency (FE)).
[0080] [Table 1]
[0081] In Examples 1-1, 1-2, and 1-3, observations were performed at potentials of 1.2 V, 1.3 V, and 1.4 V, and the observed values were 1.2, 4.8, and 10.9 mA cm, respectively. -2 The current was observed. Furthermore, the Faraday efficiency FE HCOOH = 81, 89, 89% of the formate ion (HCOO - ) was obtained.
[0082] At an applied potential of 1.3 V, in Example 1-2, it was 4.8 mA cm -2 The current of 1000 u / s flows, and the ratio of the product to the charge (Faraday efficiency) is about 89%. -) was obtained. At the same time, carbon monoxide (CO) equivalent to 5% of the faradaic efficiency and hydrogen (H2) equivalent to 3% were obtained as by-products. Furthermore, in Example 2, the current density was 12.5 mAcm -2 The faradaic efficiency of formate ions was 89%. In other words, by using the Fe-Ni-added β-FeOOH-supported Ni foam as the anode catalyst, the amount of formate ions produced increased by 2.3 times. On the other hand, in Comparative Example 1, the current density was 0.04 mAcm -2 No formate ion generation was confirmed, and the carbon dioxide reduction reaction hardly proceeded at all. These results show that by using a metal complex, such as a Ru complex, in which an electron-withdrawing substituent has been introduced into the diimine ligand as a catalyst, selective reduction of carbon dioxide to formate ions proceeds under the condition of a low cell potential of 1.3 V, which did not proceed with conventional catalysts.
[0083] The reason why metal complexes having diimine ligands showed excellent carbon dioxide reduction performance at low potentials is the high electron-accepting ability of the diimine ligands. In metal complexes having diimine ligands, the diimine ligands can accept electrons at a lower potential than the central metal ion, so when a potential is applied to the electrode, the diimine ligands accept electrons. It is speculated that the diimine ligands become a reducing species that accepts these electrons, making it possible to react with carbon dioxide. It is speculated that the introduction of an electron-withdrawing substituent into the diimine ligand makes it possible to accept electrons at a lower potential, making carbon dioxide reduction at a low potential possible. It is speculated that the reduction in the potential of the carbon dioxide reduction reaction by the diimine ligands will occur in the same way with other central metals other than Ru.
[0084] (Reactor action and effect) The reactor function was estimated by comparing Example 1, in which carbon dioxide electrolysis was performed using a membrane / electrode assembly gas diffusion method, with Comparative Example 2, in which it was performed using an electrode immersion method. Both Example 1 and Comparative Example 2 used the same cathode, but differed in that Ni foam and Pt were used as the anodes, respectively. Also, Example 1 was a two-electrode type, while Comparative Example 2 was a three-electrode type using a reference electrode. These results are shown in Table 1. Example 1-2 had a current of 4.8 mAcm when 1.3 V was applied between the electrodes. -2 A current of 2.6 mA cm was generated, of which 89% was converted to formate ions. In Comparative Example 2, when −0.34 V was applied against the standard hydrogen reversible potential (RHE), a current of 2.6 mA cm was generated. -2 of current was generated, 43% of which was converted to formate ions. Comparative Example 2 ignores the potential of the positive electrode, but theoretically a potential of 1.23 V or more, which is the oxidation potential of water, must be applied. Therefore, the potential difference between the anode and the cathode is 1.57 V or more. Therefore, Example 1 can generate a large carbon dioxide electrolysis current at a lower potential than Comparative Example 2, and can obtain formate ions with high conversion efficiency, and it has been made clear that the membrane / electrode assembly gas diffusion method exhibits higher performance than the electrode immersion method.
[0085] In this way, the carbon dioxide reduction device of the embodiment was able to obtain formate ions at a low cell potential and with high conversion efficiency. [Explanation of symbols]
[0086] 1 carbon dioxide reduction device, 10 anode part, 12 cathode part, 14 anion exchange membrane, 16 anode, 18 anode solution flow path, 20 anode current collector, 22 cathode, 24 gas flow path, 26 catalyst layer, 28 gas diffusion layer, 30 cathode current collector, 32, 60 power source, 50 electrode immersion type carbon dioxide reduction device, 52 counter electrode, 54 working electrode, 56 reference electrode, 58 electrolyte, 62 electrolyte tank.
Claims
1. an anode section including an anode for oxidizing water to generate oxygen and an anode solution flow path for supplying an anode solution to the anode; a cathode part including a cathode for producing formic acid or formate ions by reducing carbon dioxide, and a gas flow path for supplying carbon dioxide gas to the cathode; an anion exchange membrane sandwiched between the anode portion and the cathode portion; Equipped with the cathode includes, in order from the anion exchange membrane side, a catalyst layer including a metal complex as a cathode catalyst, and a gas diffusion layer; An alkaline solution is supplied as the anode solution; The metal complex has at least one metal selected from the group consisting of Ru, Mn, Fe, Co, Ni, Cu, Mo, and Re as a central metal, and has a diimine ligand as a ligand.
2. The carbon dioxide reduction device according to claim 1, The carbon dioxide reduction device is characterized in that the diimine ligand is a diimine ligand having an electron-withdrawing substituent introduced therein.
3. The carbon dioxide reduction device according to claim 2, The electron-withdrawing substituent is a carboxylic acid ester having a structural formula of -COOR, R has a chemical structure consisting of an alkyl group and a pyrrole moiety, and the pyrrole moiety is polymerized by a polypyrrole chain.
4. The carbon dioxide reduction device according to any one of claims 1 to 3, The carbon dioxide reduction device is characterized in that the catalyst layer contains a polymer compound that serves as an ion conductor and a binder, and conductive carbon.
5. The carbon dioxide reduction device according to any one of claims 1 to 4, The carbon dioxide reduction device, wherein the gas diffusion layer includes a hydrophobic porous carbon substrate.
6. The carbon dioxide reduction device according to any one of claims 1 to 5, The anode comprises a substrate made of at least one material selected from the group consisting of Ni, Ti, Fe, and C; The substrate has at least one shape selected from the group consisting of a porous body, a mesh material, and a sintered fiber body; The anode contains, as an anode catalyst, at least one selected from the group consisting of a metal containing at least one element selected from the group consisting of Ni, Fe, Co, Mn, Ru, and Ir, an oxide containing the metal, a hydroxide containing the metal, and an oxyhydroxide containing the metal.
7. The carbon dioxide reduction device according to claim 6, 11. A carbon dioxide reduction device, wherein the anode contains, as the anode catalyst, at least one selected from the group consisting of iron oxyhydroxide and nickel oxyhydroxide.
8. The carbon dioxide reduction device according to any one of claims 1 to 7, The alkaline solution is an alkaline aqueous solution having a pH of 12 or more, A carbon dioxide reduction device, characterized in that a cell voltage between the anode and the cathode is 2 V or less, and the formic acid is generated in the cathode section.
9. A carbon dioxide reduction device according to any one of claims 1 to 8, and a solar cell that generates electricity to be supplied to the anode and the cathode.
Citation Information
Patent Citations
Copper-based monatomic alloy catalyst, preparation method and application thereof and membrane electrode electrolyte battery for preparing formic acid through carbon dioxide electroreduction
CN113020614A
Reduction electrode and method of manufacturing the same, and electrolytic apparatus
JP2017057438A
Reactor and production method of carbohydrate
JP2019127641A
Electrolysis system and artificial photosynthesis system
JP2019127646A
Oxidation electrode, and electrochemical reaction device using the same
JP2019167558A