Quantitative method for carbon in carbide
The method of combusting carbides with a composite metal member separates contaminant and carbide peaks, addressing inaccuracies in existing methods and enabling precise quantification of carbon in carbides, including fine carbides.
Patent Information
- Application Number
- JP2023519407
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-12-21
- Filing Date
- 2022-12-19
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2042-12-19
AI Technical Summary
Existing methods for quantifying carbon in carbides are inaccurate due to contaminant carbon interference and require complex cleaning steps, failing to precisely determine the amount of fine carbides.
A method involving combustion of carbides with a composite metal member composed of two or more metals with different main components, oxidizing carbon to carbon monoxide and/or dioxide, allowing peak separation and precise quantification.
Enables high-precision quantification of carbon in carbides with simplicity, including fine carbides, by effectively separating contaminant carbon peaks from carbide peaks.
Smart Images

Figure 0007552886000003 
Figure 0007552886000004 
Figure 0007552886000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for quantifying carbon in carbide. [Background technology]
[0002] The amount and form of carbides in steel have a significant effect on the properties of steel. Therefore, by analyzing the amount of carbides, it is possible to quantitatively evaluate the effect on the properties of steel, and it is possible to control the properties of steel. Conventionally, carbides have been quantified by quantifying the metal elements bonded to carbon. However, the above metal elements may exist as compounds such as nitrides, oxides, or sulfides other than carbides. In such cases, the analysis of nitrogen and sulfur is also required to quantify the carbides, which causes a problem that the analysis procedure becomes enormous. In addition, when quantifying metal elements and determining the amount of carbides from the above quantitative results, the carbides are assumed to have a stoichiometric composition. However, in actual steel, carbides often do not have a stoichiometric composition, so it is not possible to accurately determine the amount of carbides. Therefore, attempts have been made to directly quantify the carbon in carbides in steel.
[0003] The method for quantifying carbon in steel is the combustion-infrared absorption method (based on JIS G 1211-3 Part 3). Another method for extracting carbides from steel is the electrolytic extraction method. In the electrolytic extraction method, carbides are electrolytically extracted from steel, then sifted into a solvent using ultrasound or other methods to make a dispersion, and the carbides are collected by filtering the dispersion, and the carbon in the collected carbides is quantified using the combustion-infrared absorption method.
[0004] However, carbon contamination is attached to the charcoal collected by electrolytic extraction. There are three main types of carbon contamination. The first type is carbon from the organic solvent that remains in the charcoal after electrolytic extraction, because the electrolyte and solvent used for electrolytic extraction of charcoal are often organic solvents. The second type is carbon that is generated by the combustion of the filter, because when collecting the charcoal after electrolytic extraction, the filter is generally made of an organic material such as polycarbonate and then burned together with the charcoal. The third type is carbon that adheres from the atmosphere. These types of carbon contamination can cause errors when quantifying carbon in charcoal.
[0005] As a method for reducing these error factors, Patent Document 1 discloses a method for analyzing carbides in steel, in which, when quantitatively analyzing carbides in a steel sample from the electrolytic extraction residue of the steel sample, the electrolytic extraction residue is heated in a hydrogen atmosphere with a heating medium having a high energy density in order to remove carbon originating from organic matter present in the electrolytic solution, and then the amount of carbon in the electrolytic extraction residue is determined.
[0006] Patent Document 2 discloses a method for removing electrolytic solution, i.e., contaminating carbon, from the extraction residue of the steel to be analyzed when quantitatively analyzing carbon in carbides contained in the steel to be analyzed, which involves washing with methyl alcohol, then washing with hot water and an organic solvent, and then heating and drying in the air.Furthermore, a method is disclosed in which an inorganic filter that has been preheated to remove contaminating carbon is used when collecting the extraction residue of the steel to be analyzed using a filter. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 11-44687 [Patent Document 2] JP 2004-257920 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, in the method described in Patent Document 1, when removing carbon originating from organic matter present in the electrolyte, there is a possibility that unstable charcoal may also be removed along with contaminating carbon, and there is a problem with the accuracy of this method for quantifying carbon in charcoal.
[0009] The method described in Patent Document 2 requires many cleaning steps, which makes the work complicated, and the removal rate of contaminating carbon may vary depending on the worker, which causes problems with the accuracy of the method for quantifying carbon in charcoal. In addition, when charcoal is collected using an inorganic filter that has been preheated to remove contaminating carbon, and the carbon in the charcoal is quantified, there is also a problem that charcoal smaller than the pore size of the filter is not collected, making it impossible to quantify fine carbon in the charcoal.
[0010] The present invention has been made in consideration of the above circumstances, and has an object to provide a method for quantifying carbon in carbides, which is capable of quantifying the amount of carbon in carbides with high accuracy and in a simple manner. [Means for solving the problem]
[0011] The inventors of the present invention have conducted extensive research in order to solve the above problems. Generally, when carbon is quantified by the combustion-infrared absorption method, the peak derived from the contaminating carbon and the peak derived from the carbon in the carbide overlap, and the carbon in the carbide cannot be quantified. Therefore, first, a method for separating the peak derived from the contaminating carbon and the peak derived from the carbon in the carbide in the combustion-infrared absorption method was examined. As a result, the present inventors found that when a metal containing carbon is burned, the contaminating carbon is first oxidized to carbon monoxide and / or carbon dioxide, and a peak derived from the contaminating carbon is detected, and then the carbon in the metal is oxidized to carbon monoxide and / or carbon dioxide, and a peak derived from the carbon in the metal is detected. This is presumably because the heat amount due to heating is consumed in melting the metal before the oxidation of the carbon in the metal, making it difficult for the oxidation reaction of the carbon in the metal to occur. Based on this finding, the present inventors tried to burn the carbide together with a metal member made of metal. As a result, they found that it is possible to separate the peak derived from the contaminating carbon and the peak derived from the carbon in the carbide by burning the carbide together with the metal member. In addition, it was found that the spectrum after the appearance of the peak due to the contaminated carbon only has intensity due to the background, and this intensity is extremely small and has little fluctuation, so that even trace amounts of carbon can be quantified. However, it was found that the above effect can be obtained when the carbide is burned together with a composite material, but not when the carbide is burned together with a single metal material. Here, the composite material has two or more metal materials and has different main components.
[0012] According to the above-mentioned method for quantifying carbon in carbide, since it is not necessary to remove contaminating carbon from the carbide, the complicated cleaning work that was previously required is not necessary, and analytical values can be obtained without depending on the operator. It is also applicable to carbon in carbide obtained by a method of extracting carbide in a dispersion liquid and extracting it with a filter. Furthermore, it was found that even fine carbide that cannot be captured by a filter can be captured by dropping the dispersion liquid onto a metal member and drying it, and that carbon in carbide can be quantified with high accuracy by burning the metal member and the carbide. Thus, the present invention was completed.
[0013] The present invention which solves the above problems is as follows. [1] A method for quantifying carbon in a charcoal, comprising: a combustion step of heating the charcoal together with a composite member in the presence of oxygen to oxidize carbon in the charcoal to carbon monoxide and / or carbon dioxide; and a quantitative determination step of quantifying the carbon monoxide and / or carbon dioxide, The method for quantifying carbon in carbide, wherein the composite member comprises two or more metal members each having a different main component.
[0014] [2] The method for quantifying carbon in carbide according to [1] above, wherein the carbon content of each of the two or more metal components is 200 ppm or less.
[0015] [3] The method for quantifying carbon in carbides according to [1] or [2] above, wherein each of the two or more metal members is made of a sheet material having a thickness of 0.10 mm or less.
[0016] [4] A method for quantifying carbon in a charcoal described in [3], wherein in the combustion process, the charcoal is heated while wrapped in the sheet material.
[0017] [5] The method for quantifying carbon in a carbide according to any one of [1] to [4] above, wherein the analytical method in the quantifying step is an infrared absorption method.
[0018] [6] The method for quantifying carbon in carbides described in [5] above, wherein an amount of the metal component used in the combustion step is such that the degree of separation calculated from the peak due to contaminating carbon and the peak due to carbon in the carbides is 1.4 or more in the quantitative determination step.
[0019] [7] The method for quantifying carbon in a carbide according to any one of [1] to [6], wherein the temperature to which the carbide and the composite material are heated in the combustion step is 700°C or higher and 1200°C or lower.
[0020] [8] The melting point of the metal member is 200°C or higher and 3000°C or lower; The method for quantifying carbon in carbide according to any one of [1] to [7] above, wherein a difference in melting point between the metal members is 500° C. or more and 2400° C. or less.
[0021] [9] The method for quantifying carbon in carbide according to [8], wherein the metal component has one metal element selected from Sn, Ti, Ag, Fe, Mo, Cu and Ti as a main component.
[0022]
[10] The method for quantifying carbon in carbide according to [9], wherein the composite member is composed of a metal member whose main component is Sn and a metal member whose main component is Fe.
[0023]
[11] The method for quantifying carbon in carbide according to any one of [1] to
[10] above, wherein the carbide is a carbide in steel. Effect of the Invention
[0024] According to the present invention, it is possible to quantitatively determine the amount of carbon in carbides with high accuracy and in a simple manner. It is also possible to quantitatively determine the amount of carbon in fine carbides. [Brief description of the drawings]
[0025] [Figure 1] 1 shows examples of infrared absorption spectra obtained in the examples, where (a) is for Comparative Example 1 and Comparative Example 6, and (b) is for Invention Example 1 and Invention Example 6. [Diagram 2] 1 shows the relationship between the amount of carbon in the carbide and the peak intensity, where (a) relates to Comparative Examples 1 to 6 and (b) relates to Invention Examples 1 to 6. [Diagram 3] FIG. 1 is a graph showing the relationship between the heating temperature in the combustion process and the detection time and separation degree of the peak top derived from carbon in the charcoal. [Figure 4] FIG. 13 is a graph showing the relationship between the peak top detection time and resolution and the amount of Fe sheet material used. [Diagram 5] FIG. 1 shows the peak top detection times and resolutions in Examples 15 to 18. [Figure 6] 1 shows infrared absorption spectra obtained in Examples 19 and 20 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] Hereinafter, an embodiment of the present invention will be described. The method for quantifying carbon in a carbide according to the present invention includes a combustion step of heating the carbide together with a composite member in the presence of oxygen to oxidize the carbon in the carbide to carbon monoxide and / or carbon dioxide, and a quantitative determination step of quantifying the carbon monoxide and / or carbon dioxide. Here, the composite member includes two or more metal members and has mutually different main components.
[0027] (Preparation of carbide samples) The carbide to be analyzed is not particularly limited. The carbide to be analyzed can be, for example, a carbide in steel. Examples of carbides in steel include TiC, CrC, Cr3C2, Cr 23 Examples of carbides that can be analyzed include C6, NbC, Fe3C, and VC. Examples of carbides that can be analyzed other than those in steel include sodium carbonate and calcium carbonate.
[0028] When quantifying carbon in carbides in steel, the carbides are first extracted. The method for extracting the carbides is not particularly limited as long as the method can extract the carbides, and an example of the method is electrolytic extraction.
[0029] In the electrolytic extraction method, the carbide obtained by electrolytic extraction is dispersed in a solvent to obtain a dispersion liquid, and the carbide is extracted. The solvent is not limited, but it is preferable to use a solvent that is relatively easy to obtain and has a high purity, such as pure water, methanol, or ethanol.
[0030] The carbonized material dispersed in the dispersion liquid may be collected using a filter. In order to reduce the influence of contaminating carbon, it is preferable to use a filter that does not contain carbon. As such a filter, for example, an inorganic filter such as a glass filter, an alumina filter, or a silver membrane filter is preferable.
[0031] The carbide dispersed in the dispersion may be collected by dropping the dispersion onto a metal member (e.g., a metal member formed by processing a metal sheet material into a container shape) constituting a composite member to be heated together in the combustion process, and evaporating the solvent of the dispersion. A heating method can be used as a method for evaporating the solvent of the dispersion. If the heating temperature is too high, the carbide to be analyzed may evaporate, so the heating temperature is preferably 250°C or less, more preferably 200°C or less, more preferably 150°C or less, more preferably 100°C or less, more preferably 90°C or less, more preferably 70°C or less, and more preferably 50°C or less. When evaporating the solvent at room temperature, it is preferable to evaporate the solvent in a desiccator covered with a moisture absorbent that is not coated with Vaseline or the like in order to prevent contamination by carbon from the atmosphere.
[0032] (Combustion process) First, the carbide is heated together with the composite member in the presence of oxygen to oxidize the carbon in the carbide to carbon monoxide and / or carbon dioxide (combustion step). The composite member heated together with the carbide includes two or more metal members, and has different main components. This allows the peak derived from the contaminating carbon to be separated from the peak derived from the carbon in the carbide, and the carbon in the carbide to be quantified with high accuracy and in a simple manner. The metal member is a member made of metal. The metal member can be composed of a single metal. The metal member can also be composed of an alloy or an intermetallic compound. In this case, the main component refers to the metal element that constitutes the single metal in the case of a single metal, and in the case of an alloy or an intermetallic compound, refers to the metal element that is contained most abundantly among the metal elements that constitute the alloy or intermetallic compound. In this case, the concentration of the main component metal element in the metal member is more than 50 mass%.
[0033] The present inventors have conducted a study focusing on the melting points of the metal members, and have found that if the melting points of the metal members are 200° C. or more and 3000° C. or less, and the difference in melting points between the metal members is 500° C. or more and 2400° C. or less, the peaks derived from the contaminating carbon and the peaks derived from the carbon in the carbide can be better separated, and the carbon in the carbide can be quantified with higher accuracy.
[0034] The metal member preferably comprises one metal element selected from Sn, Ti, Ag, Fe, Mo and Cu as a main component. The composite member is more preferably a composite member comprising a metal member whose main component is Ag and a metal member whose main component is Fe, a metal member whose main component is Sn and a metal member whose main component is Mo, a metal member whose main component is Sn and a metal member whose main component is Cu, a metal member whose main component is Sn and a metal member whose main component is Ti, or a metal member whose main component is Sn and a metal member whose main component is Fe. For example, when the member heated together with the carbide is a single metal member and the metal constituting the metal member is Sn, Sn melts immediately after heating in the combustion step, making it difficult to separate the peak derived from the contaminating carbon and the peak derived from the carbon in the carbide. Also, when the member heated together with the carbide is a single metal member and the metal constituting the metal member is Fe, Fe does not melt in the combustion step and the combustion of the carbide does not proceed. On the other hand, when the member to be heated together with the carbide is a composite member including a metal member composed of Sn and a metal member composed of Fe, the melting point of Fe is lowered by Sn, and Fe melts after the contaminating carbon is removed, and the carbide is burned, so that it is easy to separate the peak derived from the contaminating carbon and the peak derived from the carbon in the carbide. From the viewpoints of availability, workability, and purity, it is more preferable that the composite member includes a metal member whose main component is Sn and a metal member whose main component is Fe. The metal member is preferably composed of a pure metal composed of a single metal, since it is easy to predict and control the position where the peak derived from the carbide carbon appears, and the carbon content described later is reduced. In addition, the metal member may optionally contain unavoidable impurities and other elements, and may optionally contain other alloys, intermetallic compounds, etc., as long as the effects of the present invention are not hindered.
[0035] The carbon in the metal member is oxidized simultaneously with the oxidation reaction of the carbon in the carbide. Therefore, when the carbon amount of the carbon in the carbide is measured, the carbon amount of the carbon in the metal member is added to the true carbon amount. Therefore, the carbon content of the metal member is preferably 200 ppm or less, more preferably 100 ppm or less, even more preferably 10 ppm or less, even more preferably 6.6 ppm or less, and most preferably 2 ppm or less, taking into account the influence on the quantitative determination of the carbon in the carbide. If the carbon content of the metal member is 200 ppm or less, the carbon amount of the carbon in the carbide can be analyzed with high accuracy even if the carbon content varies due to the manufacturing lot, segregation, etc. It is preferable that each of the two or more metal members constituting the composite member satisfies the above requirements.
[0036] Each of the two or more metal members is preferably a sheet material having a thickness of 0.10 mm or less. If the thickness of the sheet material is 0.10 mm or less, it is easy to process into a container, the dispersion liquid in which the carbide is dispersed is easy to collect on the sheet material, and combustion is easy. The thickness of the sheet material is more preferably 0.05 mm or less. In addition, the thickness of the sheet material is preferably 0.001 mm or more, and more preferably 0.005 mm or more. If the thickness of the sheet material is 0.001 mm or more, there is no risk of the sheet material being torn, and it has a moderate rigidity, so that it is easy to process. When all of the two or more metal members constituting the composite member are made of sheet materials, it is preferable that each sheet material meets the above requirements. In addition, from the viewpoint of ease of prediction and control of the appearance position of the peak position derived from the carbide carbon and processability, it is preferable to use a pure metal composed of a single metal for each metal member.
[0037] The carbide is preferably heated in a state wrapped in the sheet material. The presence of the metal member around the carbide uniformly suppresses the oxidation of the carbide, improving the analytical accuracy. In this case, it is preferable to first wrap the carbide in a metal member having a relatively low melting point, and then wrap it in a metal member having a relatively high melting point. Specifically, when a composite member composed of a metal member whose main component is Sn and a metal member whose main component is Fe is used as the composite member, it is preferable to first wrap the carbide in a metal member whose main component is Sn, and then wrap the metal member whose main component is Sn in a metal member whose main component is Fe. This makes it possible to satisfactorily separate the peaks derived from the contaminating carbon and the peaks derived from the carbon in the carbide. In addition, as long as the above effect is obtained, other members may be provided in addition to the metal members constituting the composite member, and such cases are also included in the scope of the present invention.
[0038] There is no limitation on the heating temperature in the combustion step, but it is preferably 700°C or higher and 1200°C or lower. If the heating temperature exceeds 1200°C, melting of the composite material and combustion of the contaminating carbon may occur almost simultaneously, making it difficult to separate the peak derived from the contaminating carbon from the peak derived from the carbon in the carbide to be analyzed. The heating temperature is preferably 1100°C or lower, more preferably 1000°C or lower. On the other hand, if the heating temperature is less than 700°C, melting of the composite material may not occur stably, that is, combustion of the carbide may not occur stably. The heating temperature is preferably 700°C or higher, more preferably 800°C or higher, and even more preferably 900°C or higher.
[0039] (Quantitative process) The analytical method for quantifying carbon monoxide and / or carbon dioxide is not particularly limited as long as it is an analytical method capable of quantifying the amount of carbon monoxide and / or carbon dioxide generated in the combustion process, but it is preferable to quantify the amount by infrared absorption method.
[0040] When an infrared absorption method is used as an analytical method, it is preferable to use an amount of metal member in the quantitative determination step such that the degree of separation calculated from the peak due to contaminating carbon and the peak due to carbon in the carbide is 1.4 or more, more preferably 1.7 or more. If the degree of separation is less than 1.4, the metal member melts quickly, the peak due to carbon in the carbide approaches the peak due to contaminating carbon, and the separation accuracy of both peaks decreases. Here, the degree of separation is a value calculated from the following formula. Separation degree R=1.18×(tR2-tR1) / (W1+W2) Here, tR1 and tR2 are the times at which the peak tops of the contaminating carbon and carbon in the carbide were detected, respectively, and W1 and W2 are the full widths at half maximum of the peaks of the contaminating carbon and carbon in the carbide, respectively. EXAMPLES
[0041] Examples of the present invention will be described below, but the present invention is not limited to these examples.
[0042] (Comparative Examples 1 to 6) First, a single metal member was prepared as a member to be burned together with the carbide in the combustion process. Here, a Sn capsule (manufactured by LUDISWISS, thickness: 0.01 mm, size: diameter 5 mm × height 9 mm, mass: 27 mg, purity: 99.999 mass%) made of a Sn sheet material with a C content of 1.6 ppm was prepared. In addition, sodium carbonate with a purity of 99.0 mass% or more made by Tokyo Chemical Industry was prepared as the carbide. Then, sodium carbonate was added to pure water and stirred to prepare a dispersion in which sodium carbonate as the carbide was dispersed. The prepared dispersion was divided into Sn capsules so that the carbon amount was 0 μg (Comparative Example 1), 0.1 μg (Comparative Example 2), 0.3 μg (Comparative Example 3), 0.5 μg (Comparative Example 4), 1.0 μg (Comparative Example 5), and 1.5 μg (Comparative Example 6), and the pure water was evaporated by heating at 90 ° C. for 2 hours, and the carbide was extracted in the Sn capsule. In Comparative Example 1, about 0.1 ml of pure water was put into a Sn capsule and evaporated. Next, the Sn capsule was folded to encase the carbide (wrapped in a Sn sheet material) and placed in a ceramic crucible. The Sn capsule was then heated to 800°C in the presence of O2, and the peak positions and intensities of the generated carbon monoxide and / or carbon dioxide were measured by infrared absorption.
[0043] (Examples 1 to 6) The amount of carbon in the carbide was quantified in the same manner as in Comparative Examples 1 to 6. However, a composite member was used as a member that burns with the carbide. As the composite member, a composite member (melting point difference between the metal members constituting the composite member: 1306°C) was used, which is composed of two metal members, that is, a Sn capsule (manufactured by LUDISWISS, thickness: 0.01 mm, size: diameter 5 mm x height 9 mm, mass: 27 mg, melting point: 232°C, purity: 99.999% by mass) made of a Sn sheet material with a C content of 1.6 ppm and a Fe sheet material (manufactured by Toho Zinc, Myron (registered trademark) UHP, thickness 0.005 mm, 10 mm x 10 mm, mass: 4 mg, melting point: 1538°C, purity: 99.999% by mass) with a C content of 2 ppm. In addition, the dispersion liquid in which sodium carbonate was dispersed as carbide was taken into Sn capsules so that the carbon amount was 0 μg (invention example 1), 0.1 μg (invention example 2), 0.3 μg (invention example 3), 0.5 μg (invention example 4), 1.0 μg (invention example 5), and 1.5 μg (invention example 6), and the pure water was evaporated by heating at 90 ° C for 2 hours, and the carbide was extracted in the Sn capsule. Then, the Sn capsule was folded to enclose the carbide, and the Sn capsule was further encased in an Fe sheet material, and then the capsule was placed in a ceramic crucible. All other conditions were the same as those in Comparative Examples 1 to 6.
[0044] FIG. 1 shows an example of the obtained infrared absorption spectrum, where (a) is for Comparative Example 1 and Comparative Example 6, and (b) is for Inventive Example 1 and Inventive Example 6. For the spectrum of Comparative Example 1 in FIG. 1(a), the detection time of the peak top was around 30 seconds. This is a peak derived from contaminating carbon. On the other hand, for the spectrum of Comparative Example 6 in FIG. 1(a), a peak was detected twice, with the detection time of the first peak top being around 10 seconds and the detection time of the second peak top being around 25 seconds. It is considered that the first peak is a peak derived from carbon in the carbide, and the second peak is a peak derived from contaminating carbon. The peak intensity derived from carbon in the carbide is equal to or less than the peak intensity derived from contaminating carbon, and is considered to be strongly influenced by contaminating carbon.
[0045] On the other hand, in the spectrum of Example 6 in FIG. 1(b), two peaks were detected, the first peak top detection time was around 30 seconds, and the second peak top detection time was around 90 seconds. It is considered that the first peak is a peak derived from contaminating carbon, and the second peak is a peak derived from carbon in carbide. From this result, it can be seen that when a composite member composed of a Sn capsule and an Fe sheet material is used as a metal member that burns with carbide, the peak derived from contaminating carbon and the peak derived from carbon in carbide can be clearly separated. In this case, the separation degree of Examples 2 to 6 was 4.3 (Example 2), 4.5 (Example 3), 3.6 (Example 4), 2.7 (Example 5), and 3.2 (Example 6). However, as is clear from the spectrum of Example 1, even when the Sn capsule and the Fe sheet material containing pure water not containing carbide were heated, a peak was detected at a detection time of around 90 seconds. This is considered to be derived from the carbon contained in the Fe sheet material. The effect of carbon contained in the Fe sheet material can be reduced by creating a calibration curve and making corrections.
[0046] FIG. 2 shows the relationship between the amount of carbon in the carbide and the peak intensity, where (a) is for Comparative Examples 1 to 6 and (b) is for Examples 1 to 6. From FIG. 2(a), it can be seen that for Comparative Examples 1 to 6, in which the member that burns with the carbide is a single metal member composed only of a Sn capsule, the slope of the straight line fitting is small and the correlation coefficient R is low at 0.4252, so that the linearity is also unfavorable. On the other hand, from FIG. 2(b), it can be seen that for Examples 1 to 6, in which the member that burns with the carbide is a composite member composed of two metal members composed of a Sn capsule and an Fe sheet material, and composed of metal members whose main components are different from each other, the slope of the straight line fitting is large and the correlation coefficient R is high at 0.9868, so that the linearity is also favorable.
[0047] In addition, when the dispersion liquid in which carbide was dispersed was dropped directly onto the Fe sheet material, dried, and the carbide was wrapped in the Fe sheet material and then heated, the peak top was detected only at around 10 seconds. This is thought to be because the Fe sheet material did not melt during the combustion process, and the carbide did not burn.
[0048] In addition, a sample without added carbide was used as a blank, and the blank sample was measured three times. The standard deviation was calculated from the value obtained from the blank sample, and the lower limit of quantification of the carbon amount was obtained by multiplying the calculated standard deviation by 10. As a result, the lower limit of quantification of the carbon amount was 6.5 μg when only a Sn capsule (single metal member) was used as a member, and 0.11 μg when a composite member consisting of two metal members, consisting of a Sn capsule and an Fe sheet material, and consisting of metal members whose main components are different from each other, was used. From this result, it was confirmed that the analytical accuracy was improved by using a composite member consisting of two metal members, consisting of a Sn capsule and an Fe sheet material, as a member that burns together with carbide.
[0049] (Examples 7 to 10) The carbon content in the charcoal was quantified in the same manner as in Examples 1 to 6. However, a dispersion liquid in which sodium carbonate was dispersed was taken so that the carbon content was 20 μg. The heating temperatures in the combustion process were 700°C (Example 7), 800°C (Example 8), 900°C (Example 9), and 1000°C (Example 10). All other conditions were the same as in Examples 1 to 6.
[0050] FIG. 3 shows the relationship between the heating temperature in the combustion process and the detection time and separation degree of the peak top originating from carbon in the charcoal. As is clear from FIG. 3, it can be seen that the detection time of the peak top becomes shorter as the heating temperature increases. From this result, it can be seen that by increasing the heating temperature, it is possible to shorten the detection time of the peak top, that is, to shorten the measurement time. On the other hand, although the separation degree decreases by increasing the heating temperature, it shows a value of 1.4 or more, and it can be seen that the separation accuracy between the peak originating from carbon in the charcoal and the peak originating from the contaminating carbon is sufficiently ensured. From the above, it can be seen that by increasing the heating temperature, it is possible to improve the efficiency of the analysis while ensuring the analytical accuracy.
[0051] (Invention Examples 11 to 14, Comparative Example 7) The carbon in the carbide was quantified in the same manner as in Example 7. However, the amount of the Fe sheet material used was 0 mg (Comparative Example 7), 8 mg (Example 11), 16 mg (Example 12), 32 mg (Example 13), and 64 mg (Example 14). All other conditions were the same as in Example 7.
[0052] FIG. 4 shows the relationship between the detection time and the degree of separation of the peak top originating from carbon in the carbide and the amount of Fe sheet material used. It can be seen that the detection time of the peak top becomes shorter as the amount of Fe sheet material used increases. From this result, it can be seen that by increasing the amount of Fe sheet material used, it is possible to shorten the detection time of the peak top, that is, to shorten the measurement time. On the other hand, the degree of separation shows a tendency to decrease as the amount of Fe sheet material used increases, but it shows a value of 1.4 or more, and it can be seen that the separation accuracy of the peak originating from carbon in the carbide and the peak originating from the contaminating carbon is sufficiently ensured. From the above, it can be seen that by increasing the amount of Fe sheet material used, it is possible to improve the efficiency of the analysis while ensuring the analytical accuracy.
[0053] (Examples 15 to 18) The carbon in the carbide was quantified in the same manner as in Example 9. However, instead of the Sn capsule in Example 9, an Ag capsule (manufactured by LUDISWISS, thickness: 0.01 mm, size: diameter 5 mm × height 9 mm, mass: 42 mg, melting point: 962°C, purity: 99.99 mass%) made of an Ag sheet material with a C content of 56 ppm was used as Example 15 (melting point difference between metal members constituting the composite member: 576°C). In addition, instead of the Fe sheet material of Example 9, a Mo sheet material (thickness 0.01 mm, 10 mm x 10 mm, mass: 10 mg, melting point: 2623°C, purity: 99.99 mass%) with a C content of 16 ppm was used to obtain Example 16 (melting point difference between the metal components constituting the composite material: 2391°C), a Cu sheet material (thickness 0.01 mm, 10 mm x 10 mm, mass: 9 mg, melting point: 1085°C, purity: 99.99 mass%) with a C content of 68 ppm was used to obtain Example 17 (melting point difference between the metal components constituting the composite material: 853°C), and a Ti sheet material (thickness 0.01 mm, 10 mm x 10 mm, mass: 5 mg, melting point: 1668°C, purity: 99.9 mass%) with a C content of 159 ppm was used to obtain Example 18 (melting point difference between the metal components constituting the composite material: 1436°C). All other conditions are the same as those in Example 9.
[0054] 5 shows the peak top detection time and resolution in Examples 15 to 18. The resolution in Examples 15 to 18 is 1.5 or more, and it is clear that the separation accuracy between the peaks derived from carbon in the charcoal and the peaks derived from the contaminating carbon is sufficiently ensured. In addition, the peak top detection time is 32 to 48 seconds, and it is clear that sufficient analytical efficiency is obtained.
[0055] (Examples 19-20) The carbon in the carbide was quantified in the same manner as in invention examples 1 to 6. However, in invention example 19, instead of a dispersion liquid in which sodium carbonate was dispersed as a carbide, a dispersion liquid in which TiC (manufactured by Kojundo Chemical Laboratory, purity 99% by mass or more) was dispersed to simulate the carbide contained in the steel was used, and the carbon amount was set to 2.0 μg. In addition, in invention example 20, a dispersion liquid in which Cr3C2 (manufactured by STREM CHEMICALS, purity 97.5% by mass or more) was dispersed was used, and the carbon amount was set to 2.0 μg. All other conditions were the same as in invention examples 1 to 6.
[0056] 6 shows the infrared absorption spectra obtained in Examples 19 and 20. As in Example 6, a peak derived from contaminating carbon appears at about 24 seconds, and a peak derived from carbon in carbides appears at about 55 seconds, showing that the effects of the present invention can be obtained even when carbides generally contained in steel are analyzed. [Industrial Applicability]
[0057] INDUSTRIAL APPLICABILITY The present invention makes it possible to quantitatively determine the amount of carbon in carbides with high accuracy and in a simple manner, and is therefore useful in the steel industry.
Claims
1. A method for quantifying carbon in a charcoal, the method comprising: a combustion step of heating the charcoal together with a composite member in the presence of oxygen to oxidize carbon in the charcoal to carbon monoxide and / or carbon dioxide; and a quantitative determination step of quantifying the carbon monoxide and / or carbon dioxide, The composite member includes a first metal member and a second metal member having a melting point higher than that of the first metal member, the first metal member and the second metal member being each made of a sheet material and having a different main component from each other, A method for quantifying carbon in a carbide, wherein the combustion step is performed by wrapping the carbide in the first metal member and then wrapping the first metal member in the second metal member.
2. 2. The method for quantifying carbon in carbide according to claim 1, wherein the carbon content of each of the first metal member and the second metal member is 200 ppm or less.
3. 3. The method for quantifying carbon in carbide according to claim 1, wherein the sheet material has a thickness of 0.10 mm or less.
4. 3. The method for quantifying carbon in carbide according to claim 1 or 2, wherein the analytical method in the quantitative determination step is an infrared absorption method.
5. The method for quantifying carbon in carbides according to claim 4, wherein the first metal component and the second metal component are used in the combustion step in amounts such that the degree of separation calculated from the peak due to contaminating carbon and the peak due to carbon in the carbides is 1.4 or more in the quantitative determination step.
6. 3. The method for quantifying carbon in a carbide according to claim 1, wherein the temperature at which the carbide and the composite material are heated in the combustion step is 700°C or higher and 1200°C or lower.
7. The melting points of the first metal member and the second metal member are 200° C. or higher and 3000° C. or lower, 3. The method for quantifying carbon in carbide according to claim 1, wherein a difference in melting point between the first metal member and the second metal member is 500° C. or more and 2400° C. or less.
8. The method for quantifying carbon in carbide according to claim 7, wherein the first metal member and the second metal member each have one metal element selected from Sn, Ti, Ag, Fe, Mo, and Cu as a main component.
9. 9. The method for quantifying carbon in carbide according to claim 8, wherein the composite member is composed of the first metal member whose main component is Sn and the second metal member whose main component is Fe.
10. 3. The method for quantifying carbon in carbides according to claim 1 or 2, wherein the carbides are carbides in steel.
11. The method for quantifying carbon in carbide according to claim 3, wherein the analytical method in the quantitative determination step is an infrared absorption method.
12. The method for quantifying carbon in carbides according to claim 11, wherein an amount of the metal component used in the combustion step is such that a degree of separation calculated from a peak derived from contaminating carbon and a peak derived from carbon in the carbides is 1.4 or more in the quantitative determination step.
Citation Information
Patent Citations
Method and instrument for analyzing carbon of solid sample
JP1988009861A
Method and apparatus for analyzing trace element in metallic material
JP1990136743A
Centrifugal casting method for tube body containing strong oxidizing element as effective element
JP1994087057A
Analytical method for carbon and / Or sulfur in solid sample
JP1998260175A
Analytical method for carbide in steel
JP1999044687A