GREEN RUST, ITS PRODUCTION METHOD, PIGMENT AND ANION EXCHANGER
A green last with controlled Fe III /Fe II ratio and interlayer ions is produced to enhance oxidation resistance and stability, addressing instability issues in conventional green last, suitable for cosmetics and drug delivery.
Patent Information
- Application Number
- JP2020191369
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-18
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-11-18
AI Technical Summary
Conventional green last lacks sufficient oxidation resistance, leading to instability and degradation over time, which is a concern for applications in cosmetics and drug delivery where stability and non-toxicity are crucial.
A green last composition with a specific atomic ratio of trivalent and divalent iron (Fe III and Fe II) in layered double hydroxides, along with the presence of carbonate and lactic acid ions between the layers, is produced through a controlled heat-treatment process, enhancing crystallinity and interlayer density to improve oxidation resistance.
The resulting green last exhibits high oxidation resistance, stability, and anion exchange capacity, making it suitable for cosmetics and drug delivery applications with minimal degradation and non-toxic properties.
Smart Images

Figure 0007553096000016 
Figure 0007553096000011 
Figure 0007553096000007
Abstract
Description
[Technical field]
[0001] The present invention relates to green rust, a method for producing the same, a pigment and an anion exchanger. [Background technology]
[0002] Green Rust, a blue-green substance consisting of layered hydroxides of ferrous and ferric iron, has the property of reducing and adsorbing heavy metals, and has therefore attracted attention as a substance that contributes to the purification and recycling of polluted water and sludge that contain heavy metals, as disclosed, for example, in Patent Document 1 and Non-Patent Document 1. Green Rust is also used as an intermediate treatment agent in the production of acicular goethite particle powder, as disclosed, for example, in Patent Document 2. When using Green Rust as an adsorbent, studies have been conducted on making it have a porous structure in order to increase the adsorption efficiency (Non-Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2007-117809 A [Patent Document 2] Japanese Patent Application Publication No. 5-70146 [Non-patent literature]
[0004] [Non-Patent Document 1] Dalt.Trans.,2016,Vol.45,Pages17508-17520 Summary of the Invention [Problem to be solved by the invention]
[0005] In order to stably treat heavy metals and contaminated water, it is necessary to improve the oxidation resistance of Green Rust, which is used as a treatment agent. Because contaminated water contains dissolved oxygen, increasing the oxidation resistance makes it a highly efficient and stable adsorbent. Increasing the oxidation resistance also makes it easier to improve stability over time when using Green Rust as an anion exchanger.
[0006] The metal contained in Green Rust is iron, and it is thought to have little adverse effects on the human body. Therefore, the inventors have also investigated new applications of Green Rust, such as in cosmetics that take advantage of its green color and harmlessness, and in drug delivery that takes advantage of its interlayer carrying ability and harmlessness, as well as its use as an adsorbent for polluted water, etc.
[0007] Even when aiming for such applications, Green Rust is required to have high oxidation resistance. When Green Last is used in cosmetics or drug delivery, its high oxidation resistance means that the cosmetics themselves change little over time, maintaining stable quality, and also suppressing the adverse effects of oxidation on the human body.
[0008] However, conventional green rusts do not have sufficient stability against oxidation. Therefore, the present inventors have conducted research with the aim of providing a green rust that has improved oxidation resistance and is less susceptible to change over time. An object of the present invention is to provide a green rust which exhibits little change over time, is stable in quality, and has excellent oxidation resistance. [Means for solving the problem]
[0009] The configuration of the present invention for solving the problems is shown below. (Configuration 1) Trivalent iron (Fe) III and divalent iron Fe II A layered double hydroxide comprising: The Fe III and Fe II Atomic ratio of Fe III / (Fe III +Fe II) is between 0.80 and 0.99, Green rust, in which the full width at half maximum (FWHM) of a signal waveform at the fundamental spacing d(003) when the layered double hydroxide is subjected to X-ray diffraction measurement is 0.06° or more and 0.5° or less. (Configuration 2) The atomic ratio Fe III / (Fe III +Fe II 2. The green rust according to claim 1, wherein the ratio of the saturation temperature to the saturation temperature is 0.85 or more and 0.96 or less. (Configuration 3) The atomic ratio Fe III / (Fe III +Fe II 3. The green rust according to claim 1 or 2, wherein the ratio of the saturation coefficient to the total saturation coefficient is 0.90 or more and 0.95 or less. (Configuration 4) 4. The green rust according to any one of configurations 1 to 3, wherein the full width at half maximum (FWHM) is 0.1° or more and 0.3° or less. (Configuration 5) 5. The green rust according to any one of configurations 1 to 4, wherein at least one of carbonate ions and lactate ions is present between the layers of the layered double hydroxide. (Configuration 6) mixing a trivalent iron salt, a nucleating agent and a reducing solvent; subjecting the mixture to a heat treatment; and removing the solvent from the mixture and then washing the mixture. (Configuration 7) 7. The method for producing green rust according to claim 6, wherein the iron salt is one or more selected from the group consisting of FeCl3, Fe(NO3)3, Fe2(SO4)3 and Fe(OH)(CH3COO)2. (Configuration 8) The method for producing green rust according to aspect 6 or 7, wherein the iron salt is an anhydrous iron salt. (Configuration 9) 9. The method for producing green rust according to any one of configurations 6 to 8, wherein the nucleating agent is one or more selected from the group consisting of CH3COONa, CH3COOK, and CH3COONa·3H2O. (Configuration 10) 10. The method for producing green rust according to any one of claims 6 to 9, wherein the reducing solvent is an aqueous glycerol solution. (Configuration 11) 11. The method for producing green rust according to any one of configurations 6 to 10, wherein the temperature of the heat treatment is 50°C or higher and 350°C or lower. (Configuration 12) 11. The method for producing green rust according to any one of configurations 6 to 10, wherein the temperature of the heat treatment is 100°C or higher and 250°C or lower. (Configuration 13) 11. The method for producing green rust according to any one of configurations 6 to 10, wherein the temperature of the heat treatment is 150°C or higher and 250°C or lower. (Configuration 14) 14. The method for producing green rust according to any one of claims 6 to 13, wherein the heat treatment is carried out in an environment in which oxygen is present. (Configuration 15) 14. The method for producing green rust according to any one of claims 6 to 13, wherein the heat treatment is carried out in an inert gas environment or in a vacuum. (Configuration 16) A pigment comprising the green rust according to any one of configurations 1 to 5. (Configuration 17) 6. An anion exchanger comprising the green rust according to any one of configurations 1 to 5. Effect of the Invention
[0010] According to the present invention, there is provided a green rust which is highly resistant to oxidation, stable, changes little over time, and has a high anion exchange capacity. In addition, due to its light absorption properties, non-toxicity of the material, and oxidation resistance, it provides a green pigment suitable for cosmetics. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is an explanatory diagram showing a material structure of the present invention. [Diagram 2] FIG. 1 is a flow chart showing the manufacturing process of the material of the present invention. [Diagram 3] This is XRD measurement data. [Figure 4] This is Mössbauer spectrum measurement data. [Diagram 5] FTIR spectrum measurement data. [Figure 6] This is XPS spectrum measurement data. [Figure 7] 1 shows measurement data of TG-DTA characteristic curves. [Figure 8] 1 is a SEM photograph of the green rust of the present invention. [Figure 9] 1 is a TEM photograph of the green rust of the present invention. [Figure 10] 1 shows AFM measurement data of the green rust of the present invention. [Figure 11] TEM-EDX measurement data of the green rust of the present invention. [Figure 12] 1 is an XRD measurement data of the green rust of the present invention after treatment with aqueous solutions of various pH values; [Figure 13] FIG. 2 is a characteristic diagram showing the wavelength dependence of quantum yield (AQY) and light absorption of the green rust of the present invention. [Figure 14] FIG. 2 is a characteristic diagram showing the photocatalytic hydrogen desorption characteristics from ammonia borane of the Green Rust of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.
[0013] (First embodiment) The inventors discovered that conventional Green Rust has low crystallinity and many defects in its layered double hydroxide (LDH), which makes it easy for oxygen and substances containing oxygen to penetrate, resulting in oxidation and instability.
[0014] As a result of detailed research by the inventors, it was found that Green Rust has high oxidation resistance and stability when the full width half maximum (FWHM) of the signal waveform in the basal spacing (003) when X-ray diffraction measurement is performed on Green Rust layered double hydroxide is 0.06° to 0.5°, more preferably 0.1° to 0.5°. Here, the FWHM of 0.06° in the basal spacing (003) corresponds to a theoretical value simulated based on the Green Rust structure obtained by structural calculation.
[0015] Furthermore, the inventors have found that in order to improve the oxidation resistance and stability of green rust, it is important to make the LDH layers dense.
[0016] In LDH, if the charge density of the layer is increased, it becomes easier to attract substances with the opposite charge between the layers. Therefore, by giving the layer a positive charge and increasing the charge density, the space between the layers is densely filled with anions, making it possible to improve oxidation resistance and stability. Furthermore, if more anions can be introduced between the layers, the number of anions that can be replaced also increases, resulting in a more powerful anion exchanger.
[0017] The Green Rust of the present invention contains trivalent iron, Fe III and divalent iron Fe II A layered double hydroxide (LDH) containing Fe III and Fe II Atomic ratio of Fe III / (Fe III +Fe II ) (iron trivalent ratio) is 0.80 or more and 0.99 or less, preferably 0.85 or more and 0.96 or less, and more preferably 0.90 or more and 0.95 or less. For reference, the structure of this green rust is shown in Figure 1. In the figure, 11 indicates iron (Fe), 12 indicates oxygen (O), 13 indicates carbon (C), and 14 indicates hydrogen (H) atoms.
[0018] Here, if the trivalent iron ratio falls below 0.80, stability is impaired, if it is 0.85 or more, stability and interlayer density increase, and if it is 0.90 or more, stability and interlayer density increase even further. On the other hand, if it exceeds 0.99, the structure of LDH cannot be maintained. If it is 0.96 or less, it becomes possible to use relatively bulky anions in the interlayer space, widening the range of application as an anion exchanger. If it is 0.95 or less, it becomes possible to use even bulkier anions in the interlayer space, widening the range of application as an anion exchanger.
[0019] This structure, with its high crystallinity and a defined ratio of the number of trivalent and divalent iron atoms, prevents oxygen from penetrating through defects such as dangling bonds and crystal defects, and also provides a dense interlayer structure that makes unstable oxidation less likely to occur, making it possible to provide green rust that is stable, changes little over time, and has high anion exchange properties. In addition, the divalent iron ratio Fe III / (Fe III +Fe II ) can be measured by Mössbauer spectroscopy.
[0020] It is also preferable that at least one of carbonate ions and lactate ions is present between the layers of the layered double hydroxide.
[0021] Carbonate ions can be easily introduced between the layers of the layered double hydroxide by synthesizing the material in an oxygen-containing environment such as the air.
[0022] Lactate ions can be easily introduced between the layers of the layered double hydroxide by synthesizing the material using a reducing solvent such as glycerol, ethylene glycol, etc. Lactate ions have a suitable size and electronegativity, so they can easily replace anions present outside the green rust, making them suitable for providing an anion exchanger with versatile ion exchange properties and high exchange performance.
[0023] It is also preferable that chloride ions are present between the layers of the layered double hydroxide. Since chloride ions have a moderate electronegativity, they are easily substituted for anions present outside the green rust, and are suitable for providing an anion exchanger with high substitution performance. The introduction of chloride ions between the layers of the layered double hydroxide can be carried out by material synthesis using a reducing inorganic solvent containing chlorine under a vacuum or inert gas environment.
[0024] As shown in FIG. 2, which is a flow chart showing the manufacturing process, this Green Rust can be manufactured by mixing a trivalent iron salt, a nucleating agent, and a reducing solvent (step S1), subjecting the mixture to a heat treatment (step S2), removing the solvent from the mixture (step S3), and washing the mixture (step S4).
[0025] Here, the iron salt may be one or more selected from the group consisting of FeCl3, Fe(NO3)3, Fe2(SO4)3 and Fe(OH)(CH3COO)2. By using such iron salt, it is possible to provide green rust that is stable, changes little over time and has high anion exchange capacity. Furthermore, when the iron salt is anhydrous, there is an effect of increasing the efficiency of production of the layered double hydroxide.
[0026] The nucleating agent may be one or more selected from the group consisting of CH3COONa (sodium acetate), CH3COOK (potassium acetate), and CH3COONa·3H2O (sodium acetate trihydrate). By using such a nucleating agent, it is possible to provide a green rust that is stable, changes little over time, and has high anion exchange capacity.
[0027] As the reducing solvent, a glycerol aqueous solution is preferably used. Alternatively, an ethylene glycol aqueous solution can be used as the reducing solvent. By using such a reducing solvent, lactate ions are introduced between the layers of the layered double hydroxide, making it possible to provide a green rust that is stable, changes little over time, and has high anion exchange properties.
[0028] The heat treatment temperature is preferably 50° C. or higher and 350° C. or lower. A temperature of 50° C. or higher increases the reaction efficiency, enabling efficient production of green rust, while a temperature of 350° C. or lower prevents structural changes to the layered double hydroxide and inhibits deterioration of the organic solvent, enabling the stable production of high-quality green rust. The heat treatment temperature is more preferably 100° C. or higher and 250° C. or lower, and even more preferably 150° C. or higher and 250° C. or lower. By setting the temperature at 100° C. or higher, more preferably 150° C. or higher, the reaction efficiency is further improved, making it possible to produce green rust more efficiently. By setting the temperature at 250° C. or lower, it is possible to further suppress the deterioration and alteration of the organic solvent.
[0029] Here, when the heat treatment is carried out in an environment in which oxygen is present, carbonate ions are introduced between the layers of the layered double hydroxide, which is expected to have the effect of increasing the density between the layers of the layered double hydroxide and improving stability. Furthermore, when the heat treatment is carried out in an inert gas environment or in a vacuum, there is an effect that it becomes easy to introduce anions other than carbon ions, such as chloride ions.
[0030] The above-mentioned Green Rust has absorption bands in the ultraviolet-visible region below 500 nm and in the near-infrared region from 550 nm, has high oxidation resistance, and is made of non-toxic materials, making it an ideal green pigment for cosmetics. Green pigments are rare and highly valuable. In addition, since the above-mentioned Green Rust is densely packed with a large amount of ion exchanger, which is the target of replacement of ions to be incorporated between the layers of the layered double hydroxide, it has high anion exchange properties and is stable and changes little over time, making it ideal as an anion exchanger. EXAMPLES
[0031] The present invention will be described in more detail below with reference to examples. However, these examples are provided merely to aid in the understanding of the present invention and are not intended to limit the present invention thereto.
[0032] Example 1 <Material synthesis> Anhydrous FeCl3 (2.7 mg, 0.0167 mol, Merck, purity 98% or higher) was prepared as a trivalent iron salt, and sodium acetate trihydrate (7.2 mg, 0.05 mol, Merck, purity 99.0% or higher) was prepared as a nucleating agent. These were dissolved in glycerol (100 mL, 1.37 mol, Sigma Aldrich, purity 99.5% or higher), which is a reducing solvent, and stirred in a glass beaker at 80°C for 30 minutes. The solution was then transferred into a Teflon-lined autoclave (200 mL), sealed, and heated at 200° C. under static conditions for 24 h. Finally, the green wet powder was collected from the reaction mixture, washed three times with a mixture of ultrapure water (Milli-Q water) and ethanol (1:1 by volume, 200 mL), and air-dried at 60 °C to obtain the green rust. The synthesis conditions described above are summarized in Table 1. Table 1 also shows the results of experiments in which the main conditions were changed to those described in the table, and the other conditions were the same as the green rust synthesis conditions described above, as reference examples. Here, except for No. 1, which synthesized green rust, magnetite, hematite, or charcoal were obtained.
[0033] [Table 1]
[0034] <Materials evaluation> First, the structure of the synthesized green rust was evaluated by the various methods shown below. (1) XRD evaluation The results of measuring the green rust (GR) sample synthesized in this example by XRD (X-ray diffraction) are shown in Figure 3 together with the measurement results of the carbonate type green rust sample (Reference GR) and magnetite. Here, the XRD measurement was performed using a Smart-lab Rigaku X-ray diffractometer with a Cu target under the conditions of 40 kV and 40 mA. As a result, the carbonate-type green rust sample ([Fe II 4Fe III 2(OH) 12 ]·[CO3]·4[H2O]) changed to a more stable phase containing magnetite when freshly stored in air at room temperature for several hours. However, the GR in this example was stable and showed no significant changes even when freshly stored in air at room temperature for 90 days, despite its similar XRD pattern to that of carbonate-type GR. What is characteristic here is that the GR of this example has a fundamental spacing (d(003) value) of 0.794 nm, which is slightly larger than the reported value (0.750-0.787 nm) for carbonate-type green rust. This value can be calculated using the Bragg's formula from the 2θ value of the XRD measurement data in Figure 3.
[0035] The FWHM of the XRD measurement signal in the basic interval d(003) of the GR of this example was 0.32°. On the other hand, that of the carbonate-type green rust was about 1.0°, and the GR of this example had a half-width much narrower than that of the conventional green rust.
[0036] (2) Mössbauer spectroscopic evaluation The results of evaluating the GR of this example by Mössbauer spectroscopy are shown in Figure 4. 57 The Mössbauer spectrum of Fe was measured. Here, Mössbauer spectroscopy is a method for determining the divalent iron ratio Fe III / (Fe III +Fe II ) has high sensitivity for the measurement of As a result, the divalent iron ratio Fe III / (Fe III +Fe II ) was 0.94, more than three times higher than the previously reported value of 0.25-0.33 for green rust.
[0037] (3) FTIR evaluation The GR of this example was subjected to Fourier transform infrared (FTIR) measurement to identify the interlayer anion species. The Shimadzu FTIR-4200 was used as the device.
[0038] The results shown in Figure 5 indicate that the GR in this example had absorption at locations corresponding to the carboxylate group, the hydroxyl group, CH linked to the hydroxyl group, and the methyl group, suggesting the presence of lactate ions (CH3-CHOH-COO-).
[0039] In addition, an absorption band due to an ether group was also detected, suggesting that a part of the lactate ions was oligomerized. In addition, the absorption band due to carbonate ions is 1373 cm -1 has been detected. From the above, it was confirmed that the GR of this example has carbonate ions and lactate ions present between the layers.
[0040] (4) XPS evaluation XPS (X-ray photoelectron spectroscopy) measurements were performed on the GR of this example. Here, the JPS-9010 (manufactured by JEOL) was used as the apparatus, and all binding energies were calibrated with Cl (285.0 eV). As a result, the carbon element, which is thought to be derived from lactate ions and carbonate ions, was detected, while the Cl, which is a typical interlayer ion in conventional green rust, was detected. - No Cl element derived from the chlorine was detected (Figure 6).
[0041] (5)TG-DTA evaluation The GR of this example was evaluated in air by TG-DTA (Thermogravimetric-differential thermal analysis). Here, the Hitachi TG / DTA6200 was used as the device, and measurements were performed in air from room temperature to 1000°C at a heating rate of 10°C / min. As a result, mass loss due to the oxidative decomposition of lactate ions (330-360°C and 480-680°C) and a signal due to the release of CO2 from carbonate ions (360-480°C) were detected (Figure 7).
[0042] (6) CHN elemental analysis Based on the inset in Figure 6, a CHN elemental analysis of the GR of this example was performed, and the molar ratio of lactate ions to carbonate ions was estimated to be approximately 3. The results are based on the following evaluation: CHN elemental analysis was performed using a PerkinElmer 2400II CHN analyzer at the Natural Sciences Research and Development Center (N-BARD), Hiroshima University (C = 14.90 wt%, H = 3.23 wt%, N = trace). Here, the H value is derived from lactate anion, adsorbed water, and structural water. The H content of the adsorbed water was calculated as 0.1 wt% based on the estimated adsorbed water from the TG-DTA curve at about 330°C (mass loss at about 330°C). Due to the ash content (49.5%) after TG-DTA, the H content of the structural water was calculated as 1.2 wt%. The H content of the lactate anion was estimated to be 1.9 wt% (3.23-0.1-1.2). The C value of the CHN analysis (14.90 wt%) was divided into 13.6 wt% of lactate ions and 1.3 wt% of carbonate ions (14.90-13.6), and the molar ratio of lactate anions to carbonate anions was calculated to be approximately 3, taking into account the error of the CHN analysis (±0.5 wt%).
[0043] (7) Shape evaluation The shape of the GR in this example was measured using a SEM (Scanning electron microscope), a TEM (Transmittance electron microscope), and an AFM (Atomic force microscope). Here, the SEM and TEM devices used were JEOL JEM-2100F, and the AFM device used was an SPA-400 system (manufactured by Seiko Instruments). The measurement results of the SEM, TEM, and AFM are shown in Figures 8, 9, and 10, respectively. As a result, the GR in this example was in the form of nanoneedles / nanoplates with a length of up to 1 μm and a thickness of up to 20 nm.
[0044] (8)EDX elemental analysis The GR of this example was subjected to TEM energy dispersive X-ray (EDX) measurement to examine the distribution of C, Fe, and O elements. The apparatus used was a JEOL JEM-2100F. As a result, as shown in FIG. 11, the elements C, Fe and O were uniformly distributed, and the element C was completely and densely distributed on and inside the particles. Considering the dense interlayer space and non-porous nature of the GR in this example, it is considered difficult for reactants / substrates to penetrate into the interlayer space, and therefore the nanoneedle or nanoplate morphology with a high surface to body ratio is considered to be suitable for applications such as catalysis.
[0045] (9) Structural calculation evaluation The structure was simulated using density functional theory (DFT) calculations. The simulated optimal structure of GR has an orthorhombic unit cell with a = 0.327655 nm, b = 1.70256 nm, and c = 2.39178 nm and the chemical formula [Fe II 0.33 Fe III 5.67 (OH) 12 The interlayer distance of the GR was 0.796 nm, which was in good agreement with the experimental value of 0.794 nm obtained by XRD measurement. The interlayer space was filled with carbonate ions and lactate ions, forming a dense structure.
[0046] The details of the simulation are given below. Spin-polarized self-consistent density functional tight-binding (DFTB) calculations are performed using the +This was done using the code and the trans3d element interaction library to generate atomic geometries. Electronic settings include 0.5 nm -1 A fine Monkhorst-Pack k-point grid with spacing of 0.01 kcal / mol and 0.5 kcal / mol / nm was used, and geometry optimizations were performed with energy and force convergence criteria of 0.01 kcal / mol and 0.5 kcal / mol / nm, respectively. Next, 9 C3H5O3 - and four CO3 2- Three ions (anions) were inserted into the interlayer space to optimize the structure. As a result of this optimization, the divalent iron ratio Fe III / (Fe III +Fe II ) showed a value of 0.944, consistent with Mössbauer spectroscopy measurements. To find the lowest energy position of the intercalated species, 20 ionic configurations were considered, the most stable of which is shown in Figure 2. The interlayer distance between the Fe(OH)2 sheets in this state is 0.796 nm, in good agreement with the experimental measurement of 0.794 nm based on XRD. Finally, to investigate the stability, we performed molecular dynamics analysis of the optimized structure for 5 ps with 1 fs step at 300 °C, and found that neither significant motion of the anions nor significant changes in the lattice parameters were observed, indicating that the material is stable.
[0047] <Characteristics evaluation> The oxidation stability of the GR of this example was examined by the following method. The GR of this example was immersed in an aqueous solution containing dissolved O2 with a pH ranging from 2 to 12, and the change in the GR when air-dried overnight at 60°C was evaluated by XRD. As a result, as shown in Figure 12, no significant change was observed in the XRD pattern, confirming the stability of the GR of this example.
[0048] Next, the optical absorption characteristics of the GR of this example were investigated. A JASCO (V-570) spectrophotometer equipped with an integrating sphere (ISV-722) was used for the measurement. The results are shown in FIG. 13. As a result, the GR of this embodiment has a minimum value of absorbance at a wavelength of about 500 nm. Also, from the bandwidth in the vicinity of the minimum, it is found that the GR has light absorption characteristics suitable for a green pigment. The figure also shows the calculated quantum yield (AQY) of GR in the presence of glycerol. The results show that the AQY characteristics do not coincide with the light absorption characteristics.
[0049] Figure 14 shows the production of H2 from NH3BH3 in a solution containing glycerol. Here, glycerol acts as an electron donor. The GR in this example showed almost the same properties repeatedly without losing its initial activity, suggesting that it can be reused.
[0050] Example 2 In Example 2, the iron salt, reducing agent, nucleating agent and preparation environment were changed to the conditions shown in Table 2, and the product was produced according to the procedure shown in Example 1. As a result, it was confirmed that green rust was produced whether the nucleating agent was sodium acetate (CH3COONa) or sodium acetate trihydrate (CH3COONa·3H2O). It was also confirmed that green rust could be produced whether the preparation environment was air or argon. In Table 2, Ac stands for acetic acid. On the other hand, when no nucleating agent was used, the product was not green rust but charcoal, and when FeCl3·6H2O was used as the iron salt, the product was magnetite and no green rust was produced.
[0051] [Table 2] [Industrial Applicability]
[0052] As described above, the green rust of the present invention has anion exchange properties and is stable. There are many substances that can exchange cations, but there are few substances that can exchange anions. One example of a market for anion exchangers is drug delivery. Since Green Rust of the present invention is made of non-toxic materials, it is expected to be used in this field. For this reason, we believe that Green Rust of the present invention will contribute to industry as an anion exchanger. Furthermore, the Green Rust of the present invention has properties suitable for use in cosmetics as a green pigment due to its light absorption characteristics, non-toxicity of the material, and oxidation resistance, and is therefore believed to contribute to the cosmetics industry. [Explanation of symbols]
[0053] 1: Green Rust (layered double hydroxide) 11: Iron (Fe) 12: Oxygen (O) 13: Carbon (C) 14: Hydrogen (H)
Claims
1. The framework is divalent iron (Fe). II and trivalent iron Fe III A layered double hydroxide consisting of Contains lactate ions, When the layered double hydroxide is subjected to X-ray diffraction measurement, the full width at half maximum (FWHM) of a signal waveform at a fundamental spacing d(003) is 0.06° or more and 0.5° or less, Green rust, wherein the atomic ratio of Fe III to Fe II , Fe III / (Fe III +Fe II ), is 0.80 or more and 0.99 or less.
2. The green rust according to claim 1, wherein the full width at half maximum (FWHM) is 0.1° or more and 0.3° or less.
3. The green rust of claim 1 or 2, wherein the lactate ions include oligomerized lactate ions.
4. Anhydrous FeCl 3 and a solution preparation step of preparing a solution in which the nucleating agent is dissolved in glycerol without adding water; a heat treatment step of heat treating the solution to obtain a reaction mixture; collecting a green wet powder from the reaction mixture; A washing step of washing the wet powder; A drying step of drying the washed wet powder, The method for producing green rust, wherein the nucleating agent is one or more selected from the group consisting of CH3COONa, CH3COOK and CH3COONa.3H2O.
5. The method for producing green rust according to claim 4, wherein the temperature of the heat treatment is 50°C or higher and 350°C or lower.
6. The method for producing green rust according to claim 4, wherein the temperature of the heat treatment is 100°C or higher and 250°C or lower.
7. The method for producing green rust according to claim 4, wherein the temperature of the heat treatment is 150°C or higher and 250°C or lower.
8. The method for producing green rust according to any one of claims 4 to 7, wherein the heat treatment is carried out in an environment in which oxygen is present.
9. The method for producing green rust according to any one of claims 4 to 7, wherein the heat treatment is carried out in an inert gas environment or in a vacuum.
10. A pigment comprising the green rust according to any one of claims 1 to 3.
11. An anion exchanger comprising the green rust according to any one of claims 1 to 3.
Citation Information
Patent Citations
Environmentally-friendly metal printing ink and its preparation method
CN102732086A
Method for producing needle-like goethite particle powder
JP1993070146A
Cleaning method of soil and cleaning device
JP2007117809A
Use of oxy hydroxy salt related to family of lamellar double hydroxide for design and manufacture of electrode to store electrical energy
JP2017126561A
Method for treating selenium-containing soil and rock
JP2019037929A