Polymer composition, its method of manufacture, its use and compositions containing said polymer composition
A polymer composition with inorganic compounds and impact modifiers in a specific ratio, blended in an aqueous dispersion, addresses the issue of property loss in thermoplastic polymers, improving impact resistance and weld strength while maintaining efficient processing.
Patent Information
- Application Number
- JP2018563541
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2016-06-07
- Filing Date
- 2017-06-07
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2037-06-07
AI Technical Summary
The addition of multiple additives and fillers to thermoplastic polymers can adversely affect their properties, leading to a loss of specific characteristics and reduced impact resistance.
A polymer composition comprising 29% to 60% by weight of inorganic compounds and 40% to 71% by weight of impact modifiers, blended in an aqueous dispersion, which improves impact resistance and melting efficiency while maintaining acceptable processing times.
The composition enhances the impact resistance and corner weld strength of thermoplastic polymers without negatively impacting processing times, offering a cost-effective solution.
Smart Images

Figure 0007553225000001 
Figure 0007553225000002 
Figure 0007553225000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polymer composition comprising an impact modifier and an inorganic filler, and to a method for its preparation and use.
[0002] The present invention specifically relates to a polymer composition comprising an impact modifier and an inorganic filler, and its use for thermoplastic polymers.
[0003] The invention more particularly relates to a process for the preparation of a polymer composition containing an impact modifier and an inorganic filler, and its use to modify the impact properties of a thermoplastic polymer.
[0004] In thermoplastic polymer compositions in general, and halogenated polymer compositions in particular, many types of additives and fillers are used for a variety of reasons, among others. They can bulk up the composition, improve stiffness and strength, and reduce cycle times. They prevent blockages at the die and mitigate product degradation. Fillers can also be used to add color, opacity, and conductivity, or as low-cost materials that reduce the cost of the composition because they are less expensive than the other ingredients of the formulation.
[0005] However, the addition of additives and fillers to thermoplastic polymers, especially when several are added simultaneously or mixtures of additives, can adversely alter the properties of the thermoplastic polymer composition, i.e., certain characteristics or properties are lost or significantly reduced.
[0006] Polymer compositions containing polymers with specific characteristics (e.g., polymer composition, glass transition temperature, or structure, to name a few) are also used as additives for thermoplastic polymer compositions in general, and in halogenated polymer compositions, to improve the impact resistance of the composition or of objects made from these various polymers or plastic resins. These additives are therefore also called impact modifiers.
[0007] The polymeric composition of the additive is compatible with thermoplastic polymeric compositions in general, and halogenated polymeric compositions in particular.
[0008] The additive-containing thermoplastic polymer in general, and halogenated polymer composition in particular, is then processed and / or modified.
[0009] The processed and transformed composition is made into a polymeric article or used as a polymeric part in an article.
[0010] The object of the present invention is to propose a polymer composition which can be added as an additive to thermoplastic polymers.
[0011] It is also an object of the present invention to provide a polymer composition that can be used to improve the impact resistance of thermoplastic polymers.
[0012] It is also an object of the present invention to provide a polymer composition that can be used to improve the performance of extruded thermoplastic polymers.
[0013] A further object of the present invention is to reduce the cost of a polymer composition that acts as an impact modifier for a thermoplastic polymer composition by adding a low cost component without negatively impacting the performance of the thermoplastic polymer composition.
[0014] U.S. Patent Application Publication No. 2009 / 0111915 discloses acrylic copolymers for use in highly filled compositions, specifically filled polyvinyl chloride (PVC) materials as flooring compositions containing 70% to 95% by weight of filler, 1% to 15% by weight of PVC, and 0.5% to 4% by weight of acrylic copolymer, or siding or pipe compositions containing 15% to 35% by weight of filler, 50% to 95% by weight of PVC, and 0.25% to 6% by weight of acrylic copolymer.
[0015] WO 2010 / 099160 discloses a composite polymer modifier. This document discloses a composite polymer modifier consisting of 99% to 1% by weight of an inorganic filler, 1% to 99% by weight of a polymer processing aid, and 0% to 80% by weight of an impact modifier. The impact modifier is optional, but is used in some examples. This document does not disclose any particular advantage of a particular impact modifier.
[0016] WO 2007 / 093565 discloses a hybrid impact modifier containing an impact modifier and an inorganic filler, which attempts to address the segregation of different components across powder compositions and discloses and claims 3-20 wt.% inorganic filler.
[0017] None of the prior art documents discloses such a specific composition as the present invention.
[0018] Surprisingly, a) 29% to 60% by weight of an inorganic compound (F), b) 40% to 71% by weight of a polymeric impact modifier (IM1) It has been found that polymer composition P1, which comprises the two components a) and b) totalling 100% by weight, improves the impact resistance of thermoplastic polymers while still having acceptable melting times and better dissipating heat during cooling in high speed processing.
[0019] Also surprisingly, a) 29% to 60% by weight of an inorganic compound (F), b) 40% to 71% by weight of a polymeric impact modifier (IM1) % by weight, Blending two components a) and b), wherein component b) and at least 83.33% by weight of compound a) are in the form of a dispersion in the aqueous phase during the blending step. A method for producing the same, comprising: It has been found to improve the impact resistance of thermoplastic polymers while still having acceptable melting times and better dissipating heat during cooling for high speed processing.
[0020] Also surprisingly, a) 29% to 60% by weight of an inorganic compound (F), b) 40% to 71% by weight of a polymeric impact modifier (IM1) % by weight, i) blending two components a) and b), wherein component b) and at least 83.33% by weight of compound a) are in the form of a dispersion in an aqueous phase during the blending step; ii) drying the blend obtained in step i). A method for producing the same, comprising: It has been found to improve the impact resistance of thermoplastic polymers while still having acceptable melting times and better dissipating heat during cooling for high speed processing.
[0021] Also surprisingly, a) 29% to 60% by weight of an inorganic compound (F), b) 40% to 71% by weight of a polymeric impact modifier (IM1) It has been found that polymer composition P1, which comprises the two components a) and b) totalling 100% by weight, can be used to improve the impact resistance and corner weld strength of thermoplastic polymers.
[0022] According to a first aspect, the present invention provides a) 29% to 60% by weight of an inorganic compound (F), b) 40% to 71% by weight of polymeric impact modifier (IM1) Including, It concerns a polymer composition P1, characterized in that the two components a) and b) add up to 100% by weight.
[0023] According to a second aspect, the present invention provides a) 29% to 60% by weight of an inorganic compound (F), the inorganic compound (F) consists of an inorganic filler (F1) and a fluidization aid (F2), the weight ratio of (F1) / (F2) being at least 5 / 1; b) 40% to 71% by weight of a polymeric impact modifier (IM1) Including, It concerns a polymer composition P1, characterized in that the two components a) and b) add up to 100% by weight.
[0024] In a third aspect, the present invention comprises a) 29% to 60% by weight of an inorganic compound (F), b) 40% to 71% by weight of a polymeric impact modifier (IM1) % by weight, Blending two components a) and b), wherein component b) and at least 83.33% by weight of compound a) are in the form of a dispersion in the aqueous phase during the blending step. The present invention relates to a method for producing the same,
[0025] In a fourth aspect, the present invention provides a method for producing ... composition comprising the steps of: a) 29% to 60% by weight of an inorganic compound (F), the inorganic compound (F) consists of an inorganic filler (F1) and a fluidization aid (F2), the weight ratio of (F1) / (F2) being at least 5 / 1; b) 40% to 71% by weight of polymeric impact modifier (IM1) Including, It concerns a method for the preparation of a polymer composition P1, in which the two components a) and b) add up to 100% by weight, said method comprising the steps of: Blending the two components a) and b), in which component b) and the inorganic filler (F1) are in the form of a dispersion in the aqueous phase during the blending step. The present invention is characterized by comprising:
[0026] In a fifth aspect, the present invention provides a method for producing a composition comprising the steps of: a) 29% to 60% by weight of an inorganic compound (F), b) 40% to 71% by weight of a polymeric impact modifier (IM1) wherein the two components a) and b) add up to 100% by weight, said process comprising the steps of: i) blending two components a) and b), wherein component b) and at least 83.33% by weight of compound a) are in the form of a dispersion in an aqueous phase during the blending step; ii) drying the blend obtained in step i). The present invention is characterized by comprising:
[0027] In a sixth aspect, the present invention provides a method for producing a composition comprising the steps of: a) 29% to 60% by weight of an inorganic compound (F), the inorganic compound (F) consists of an inorganic filler (F1) and a fluidization aid (F2), the weight ratio of (F1) / (F2) being at least 5 / 1; b) 40% to 71% by weight of a polymeric impact modifier (IM1) wherein the two components a) and b) add up to 100% by weight, said process comprising the steps of: i) blending components a) and b), wherein component b) and the inorganic filler (F1) are in the form of a dispersion in the aqueous phase during the blending step; ii) drying the blend obtained in step i). The present invention is characterized by comprising:
[0028] In a seventh aspect, the present invention provides a method for producing a composition comprising: a) 29% to 60% by weight of an inorganic compound (F), b) 40% to 71% by weight of a polymeric impact modifier (IM1) Including, A method for the preparation of a polymer composition P2 comprising a polymer composition P1 in which the two components a) and b) add up to 100% by weight, the polymer composition P2 being d) Thermoplastic polymer TP1 Also includes The method comprises: Blending composition P1 with thermoplastic polymer TP1 The present invention is characterized by comprising:
[0029] In an eighth aspect, the present invention provides a method for producing a composition comprising: a) 29% to 60% by weight of an inorganic compound (F), b) 40% to 71% by weight of a polymeric impact modifier (IM1) Including, The use of a polymer composition P1, in which the two components a) and b) total 100% by weight, for improving the corner weld strength of a thermoplastic polymer TP1 comprising the polymer composition P1.
[0030] As used herein, the term "polymer composition" means that the composition is made up of at least 40% by weight of polymer.
[0031] As used herein, the term "copolymer" refers to a polymer composed of at least two different monomers.
[0032] The term "(meth)acrylic" when used in combination with monomers refers to all types of acrylic and methacrylic monomers.
[0033] As used herein, the term "(meth)acrylic polymer" refers to a polymer that essentially comprises (meth)acrylic monomers that account for 50% or more by weight of the (meth)acrylic polymer.
[0034] The term "polymer powder" as used herein refers to a polymer having powder granules in the range of at least 1 micrometer (μm) obtained by agglomeration of a primary polymer containing particles in the nanometer range.
[0035] The term "primary particle size" as used herein refers to spherical polymer containing particles in the nanometer range. The primary particles preferably have a weight average particle size of 20 nm to 500 nm.
[0036] As used herein, the term "multi-stage polymer" refers to a polymer formed sequentially by a multi-stage polymerization process. Preferred is a multi-stage emulsion polymerization process in which a first polymer is a first stage polymer and a second polymer is a second stage polymer, i.e., the second polymer is formed by emulsion polymerization in the presence of the first emulsion polymer.
[0037] As used herein, the term "dispersion" refers to a colloidal system having a continuous liquid phase and a discontinuous solid phase distributed throughout the continuous phase.
[0038] As used herein, the term "emulsion" refers to a liquid / liquid mixture containing a liquid discontinuous phase encased in a liquid continuous phase.
[0039] The term "PVC" as used herein is understood to mean polyvinyl chloride in the form of a homopolymer or copolymer containing at least 50% by weight of vinyl chloride.
[0040] As used herein, the term "filler" is understood to be a solid extender that is added to a polymer to enhance properties and / or reduce cost.
[0041] The term "fluidization aid" as used herein is to be understood as an anti-caking agent, which allows good flowability of the powder and avoids caking.
[0042] The abbreviation "phr" means parts per hundred parts resin. For example, 15 phr of filler in a PVC formulation means that 15 kg of filler was added to 100 kg of PVC.
[0043] As used herein, "two components a) and b) total 100% by weight" means that the ratio of the two components a) and b) is calculated only from the sum of these two components. If there is another component other than a) and b), this other component is not taken into account in calculating the weight ratio between these two.
[0044] In the present invention, a range from x to y means that the upper and lower limits of this range are included, and means at least from x to y.
[0045] In the present invention, x to y means that the upper and lower limits of the range are not included, and means more than x to less than y.
[0046] Polymer composition P1 of the present invention The polymer composition P1 of the invention comprises at least two components: a) from 29% to 60% by weight of an inorganic compound (F), b) from 40% to 71% by weight of a polymeric impact modifier.
[0047] Component b) may also be a mixture of several polymeric impact modifiers (IM1) to (IMx), in which case the total amount of each of the polymeric impact modifiers in the polymer composition is from 40% to 71% by weight. Each of the polymeric impact modifiers has its own different properties, such as composition or shape.
[0048] The inorganic compound (F) consists of an inorganic filler (F1) and a fluidization aid (F2), the weight ratio (F1) / (F2) being at least 5 / 1.
[0049] The polymer composition P1 preferably comprises a) from 29% to 60% by weight of an inorganic compound (F), and b) from 40% to 71% by weight of a polymeric impact modifier (IM1).
[0050] The polymer composition P1 of the invention more preferably comprises a) 31% to 59% by weight of the inorganic compound (F) and b) 41% to 69% by weight of the polymeric impact modifier (IM1).The composition P1 of the invention even more preferably comprises a) 33% to 58% by weight of the inorganic compound (F) and b) 42% to 67% by weight of the polymeric impact modifier (IM1), and the composition of the invention even more preferably comprises a) 35% to 55% by weight of the inorganic compound (F) and b) 45% to 65% by weight of the polymeric impact modifier (IM1).
[0051] The composition P1 of the invention advantageously comprises a) 40% to 55% by weight of an inorganic compound (F) and b) 45% to 60% by weight of a polymeric impact modifier (IM1), more advantageously a) 40% to 54% by weight of an inorganic compound (F) and b) 46% to 60% by weight of a polymeric impact modifier (IM1), and most advantageously a) 40% to 52% by weight of an inorganic compound (F) and b) 48% to 60% by weight of a polymeric impact modifier (IM1).
[0052] In one particular embodiment, the inventive polymer composition P1 comprises a) 42% to 47% by weight of the inorganic compound (F), and b) 53% to 58% by weight of the polymeric impact modifier (IM1).
[0053] The polymer composition P1 according to the invention is preferably in the form of a powder comprising two components. This powder is composed of granules of aggregated particles of the two components. These particles are primary particles.
[0054] The polymer powder of the present invention The polymer powder of the present invention has a volume median particle diameter D50 of 1 μm to 500 μm. The volume median particle diameter of the polymer powder is preferably 10 μm to 450 μm, more preferably 15 μm to 400 μm, advantageously 20 μm to 350 μm.
[0055] The particle size distribution by volume D10 is at least 7 μm, preferably 10 μm.
[0056] The particle size distribution by volume D90 is at most 800 μm, preferably at most 500 μm.
[0057] The powder according to the invention is homogeneous in terms of composition with respect to the two components.
[0058] In the present invention, homogeneity means that there is no significant difference throughout the composition. When one or several small samples (1 g or less) are taken from a relatively large amount (1 kg) of the composition, there is no significant difference in the composition in terms of the weight ratio of each of the two components in the small sample compared to other small samples and the entire composition P1. Small sample means 0.1% by weight or less of the polymer composition. No significant difference means that the difference is less than 30% relative to the entire composition. As an example, if the entire composition P1 contains 40% by weight of inorganic compound (F) and 60% by weight of polymeric impact modifier (IM1), a first small sample taken from the entire composition contains 35% by weight of inorganic compound (F) and 65% by weight of polymeric impact modifier (IM1), or a second small sample taken from the entire composition contains 42% by weight of inorganic compound (F) and 58% by weight of polymeric impact modifier (IM1), which represents a homogeneous composition, since the difference in the proportions of each component across the small samples is within 30% of the entire composition of the sample.
[0059] The variance of the components in the composition is preferably less than 25%, more preferably less than 20%.
[0060] In an ideal case, each powder particle or granule contains both of the two components a) and b) and is composed of aggregated particles of these two components. The difference in the weight ratio of the two components in a single powder particle or granule can be larger than the difference in the small sample described above.
[0061] The polymer composition P1 according to the invention is preferably in powder form, more preferably it is a dry powder, where dry means that the powder has a certain maximum moisture level.
[0062] The dry polymer composition P1 in powder form according to the invention has a wetness of less than 3% by weight, preferably a wetness of less than 1.5% by weight, more preferably a wetness of less than 1.2% by weight. The wetness of the polymer composition can be measured by means of a thermobalance.
[0063] The dry polymer composition P1 in powder form according to the invention may further comprise a fluidization aid (F2). The fluidization aid (F2) is preferably an inorganic compound. The fluidization aid (F2) is thus part of the inorganic compound (F) of the composition (P1). The inorganic compound (F) consists of the fluidization aid (F2) and the inorganic filler (F1): (F)=(F1)+(F2). The amount of the fluidization aid (F2) is much less than the inorganic filler (F1) in the polymer composition P1. The amount of (F1) is at least 5 times greater than the amount of (F2).
[0064] The density of the polymer composition P1 is at least 1.25 g / cm 3 , preferably at least 1.3 g / cm 3 , more preferably at least 1.33 g / cm 3 It is.
[0065] The density of the polymer composition P1 is up to 1.75 g / cm 3 , preferably up to 1.7 g / cm 3 , more preferably up to 1.67 g / cm 3 It is.
[0066] The density of the polymer composition P1 is advantageously 1.25 g / cm 3 ~1.75g / cm 3 , more advantageously 1.3 g / cm 3 ~1.7g / cm 3 It is.
[0067] Inorganic Compound (F) The inorganic compound (F) is either an inorganic or mineral filler (F1) or comprises both an inorganic or mineral filler (F1) and a fluidization aid (F2).
[0068] The inorganic compound (F) preferably comprises a mineral filler (F1) and a fluidization aid (F2). More preferably, the weight ratio (F1) / (F2) is at least 5 / 1.
[0069] Mineral filler (F1) As regards the mineral fillers (F1), mention may be made of glass fibres, hollow glass microbeads, inorganic compounds such as minerals and salts, including calcium carbonate (CaCO3), silica, silicates such as calcium silicate or calcium metasilicate, clays such as bentonite, mica, talc, alumina trihydrate, magnesium hydroxide, metal oxides, or combinations of two or more thereof.
[0070] The mineral filler (F1) may be chosen from calcium carbonate, titanium dioxide or calcined clay, silica (fumed or precipitated silica), clay, montmorillonite (nanoclay), zeolite, perlite or any other type of inorganic material that can be obtained as a slurry.
[0071] The mineral filler (F1) is more preferably calcium carbonate, calcined clay, silica (fumed or precipitated silica), clay, montmorillonite (nanoclay), zeolite or perlite.
[0072] The mineral filler (F1) of the inorganic compound (F) may be a mixture of several mineral fillers (F1a) to (F1x).
[0073] In an even more preferred embodiment, the mineral filler (F1) is calcium carbonate (CaCO3).
[0074] The calcium carbonate is advantageously selected from precipitated calcium carbonate (PCC), ground natural calcium carbonate (GCC) or nano-sized particles of precipitated calcium carbonate (NPCC).
[0075] The mineral filler (F1), or at least a part of the mineral filler (F1), may be in the form of a slurry for the preparation process of the polymer composition P1.
[0076] The filler (F1), or at least a portion of the mineral filler (F1) which is blended with the polymeric impact modifier (IM1), is preferably in the form of a slurry.
[0077] Mineral filler slurry The mineral filler slurry is preferably an aqueous dispersion of mineral filler having a solids content of 5-90% by weight, advantageously 50-80% by weight, which may contain any particular surfactant, dispersant, additive or filler surface treatment that may advantageously improve the slurry quality (stability, viscosity or compatibility with the host polymer matrix).
[0078] Fluidization aid (F2) The fluidization aid (F2) is an inorganic powder.
[0079] The fluidization aid (F2) may be a mixture of several fluidization aids (F2a) to (F2x).
[0080] The fluidization aid (F2) is advantageously selected from calcium carbonate (CaCO3).
[0081] Polymer Impact Modifier (IM1) The polymeric impact modifier (IM1) is preferably a polymer particle having a multistage structure.
[0082] The polymer particles having a multi-stage structure are more or less spherical. The polymer particles have a weight average particle size (diameter) of 20 nm to 500 nm. The weight average particle size of the polymer particles is preferably 50 nm to 400 nm, more preferably 75 nm to 350 nm, and advantageously 80 nm to 300 nm.
[0083] The polymer particles according to the invention can be obtained by a multi-stage process (for example two or three or more stages), each stage resulting in a layer, and the overall process resulting in particles with a multi-layer structure.
[0084] The polymeric impact modifier (IM1), in the form of polymer particles having a multilayer structure, comprises at least one layer (IM1L1) comprising a polymer (L1) having a glass transition temperature below 0°C and at least one other layer (IM1L2) comprising a polymer (L2) having a glass transition temperature above 45°C.
[0085] More preferably, the glass transition temperature Tg of the polymer (L1) is from -100 to 0°C, even more preferably from -80 to 0°C, advantageously from -80 to -20°C, and even more advantageously from -70 to 20°C.
[0086] The glass transition temperature Tg of the polymer (L2) is preferably 60 to 150° C. The glass transition temperature Tg of the polymer (L2) is more preferably 80 to 140° C., advantageously 90 to 135° C., and even more advantageously 90 to 130° C.
[0087] To obtain samples of each of the polymers (L1) and (L2) in order to more easily assess and measure the glass transition temperature Tg for each of the polymers in each stage, these can be prepared separately rather than in a multi-stage process.
[0088] The weight ratio of layer (IM1L1) / layer (IM1L2) in the multistage polymer is preferably at least 70 / 30, more preferably at least 80 / 20, even more preferably at least 85 / 15, advantageously at least 86 / 14, more advantageously 87 / 13, even more advantageously 88 / 12, and most advantageously 89 / 11.
[0089] The weight ratio of layer (IM1L1) / layer (IM1L2) in the multistage polymer is preferably in the range of 70 / 30 to 99 / 1 by weight, more preferably 80 / 20 to 98 / 2, even more preferably 85 / 15 to 97 / 3, advantageously 86 / 14 to 97 / 3, more advantageously 87 / 13 to 97 / 2, even more advantageously 88 / 11 to 96 / 4, and most advantageously 89 / 11 to 96 / 4.
[0090] Polymer L1 is preferably present in an amount of more than 85% by weight of the polymeric impact modifier (IM1), more preferably more than 86% by weight.
[0091] The multilayer structure of IM1 can have various structures. The layer (IM1L1) containing a polymer (L1) with a glass transition temperature below 0° C. can be the core of the polymeric impact modifier (IM1) or an intermediate layer, but is not the outermost layer. The layer (IM1L2) containing a polymer (L2) with a glass transition temperature above 45° C. can be the outermost layer.
[0092] The layer (IM1L2) containing the polymer (L2) is preferably a (meth)acrylic polymer containing at least 50% by weight of polymerized units derived from methyl methacrylate.
[0093] In a first preferred embodiment of (IM1), the polymer (L1) having a glass transition temperature below 0° C. is a (meth)acrylic polymer comprising at least 50% by weight of monomers from alkyl acrylates. The polymer (L2) or the majority of the polymer (L2) of the layer (IM1L2) is preferably grafted onto the underlying layer.
[0094] Polymer (L1) more preferably comprises one or more comonomers copolymerizable with alkyl acrylates, provided that polymer (A1) has a glass transition temperature below 0°C.
[0095] The comonomer(s) in the polymer (L1) are preferably selected from (meth)acrylic and / or vinyl monomers.
[0096] The (meth)acrylic comonomers in the polymer (L1) comprise monomers selected from C1-C12 alkyl (meth)acrylates. Even more preferably, the (meth)acrylic comonomers in the polymer (L1) comprise monomers of C1-C4 alkyl methacrylates and / or monomers of C1-C8 alkyl acrylates.
[0097] Most preferably, the acrylic or methacrylic comonomers of polymer (L1) are selected from methyl acrylate, propyl acrylate, isopropyl acrylate, butyl acrylate, tert-butyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, and mixtures thereof, provided that polymer (L1) has a glass transition temperature below 0° C.
[0098] The polymer (A1) is preferably crosslinked, which means that a crosslinking agent has been added to the other monomer or monomers, the crosslinking agent having at least two groups capable of polymerization.
[0099] In one particular embodiment, the polymer (L1) is a homopolymer of butyl acrylate.
[0100] In another particular embodiment, the polymer (L1) is a copolymer of butyl acrylate and at least one crosslinking agent. The crosslinking agent is present in less than 5% by weight of the copolymer.
[0101] More preferably, the glass transition temperature Tg of the polymer (L1) is from -100 to 0°C, even more preferably from -100 to -5°C, advantageously from -90 to -15°C, and even more advantageously from -90 to 25°C.
[0102] In a second preferred embodiment, the polymer (L1) having a glass transition temperature of less than 0° C. comprises at least 50% by weight of polymerized units derived from isoprene or butadiene, and the stage of the layer (IML1) is the innermost layer of the polymer particle having a multilayer structure. In other words, the stage making up the layer (IM1L1) containing the polymer (L1) is the core of the polymer particle.
[0103] For example, the core polymer (L1) of the second embodiment may be an isoprene homopolymer or a butadiene homopolymer, an isoprene-butadiene copolymer, a copolymer of isoprene and up to 98% by weight of a vinyl monomer, and a copolymer of butadiene and up to 98% by weight of a vinyl monomer. The vinyl monomer is styrene, alkylstyrene, acrylonitrile, alkyl(meth)acrylate, or butadiene or isoprene. In one embodiment, the core is a butadiene homopolymer.
[0104] More preferably, the glass transition temperature Tg of the polymer (L1) of the second embodiment containing at least 50% by weight of polymerization units derived from isoprene or butadiene is -100 to 0°C, even more preferably -100 to -5°C, advantageously -90 to -15°C, and even more advantageously -90 to 25°C.
[0105] Thermoplastic Polymer TP1 The thermoplastic polymer TP1 is selected from halogen-containing polymers, such as polyvinyl chloride, polyamides, polymethyl methacrylate, polystyrene, polycarbonate, polyesters such as polyethylene terephthalate, polybutylene terephthalate, polycyclohexanedimethanol terephthalate, and polyolefins.
[0106] In a first preferred embodiment, the thermoplastic polymer TP1 is a halogen-containing polymer.
[0107] Halogen-Containing Polymers For halogen-containing polymers, examples include:
[0108] homopolymers and copolymers of vinyl chloride (PVC) and vinylidene chloride (PVDC), vinyl resins with vinyl chloride units in their structure, such as copolymers of vinyl chloride, vinyl esters of fatty acids, in particular vinyl acetate, copolymers of vinyl chloride with acrylic and methacrylic acid and acrylonitrile esters, copolymers of vinyl chloride with diene compounds and unsaturated dicarboxylic acids or their anhydrides, such as copolymers of vinyl chloride with diethyl maleate, diethyl fumarate or maleic anhydride, post-chlorinated polymers and copolymers of vinyl chloride, copolymers of vinyl chloride and vinylidene chloride with unsaturated aldehydes, ketones, such as acrolein, crotonaldehyde, vinyl methyl ketone, vinyl methyl ether, vinyl isobutyl ether, etc., polymers of vinylidene chloride and polymers of vinyl chloride and other polymerizable compounds;
[0109] Polymers of vinyl chloroacetate and dichlorodivinyl ether, chlorinated polymers of vinyl carboxylates (e.g. vinyl acetate, vinyl propionate, vinyl butyrate), chlorinated polymeric esters of acrylic acid and α-substituted acrylic acids (e.g. methacrylic acid), chlorinated polymeric esters of nitriles, amides, alkyl esters (e.g. acrylonitrile, (meth)acrylamide, methyl (meth)acrylate, butyl acrylate, ethyl acrylate, 2-ethylhexyl acrylate);
[0110] Polymers of vinyl aromatic derivatives (e.g. styrene, dichlorostyrene); chlorinated rubber;
[0111] Chlorinated polymers of olefins (e.g. ethylene, propene, 1-butene, (2.2.1) bicycloheptene-2, (2.2.1) bicycloheptadiene-2,5);
[0112] Polymers of chlorobutadiene and those which have been subsequently chlorinated, as well as copolymers of chlorobutadiene and vinyl chloride, chlorinated natural and synthetic rubber, and mixtures of these polymers with each other or with other polymerizable compounds.
[0113] Grafted halogen-containing copolymers, in which the halogen-containing polymer moieties are grafted in the form of particles to a homopolymer or copolymer of (meth)acrylic acid, which may be crosslinked or non-crosslinked.
[0114] The halogen-containing polymer is preferably a thermoplastic polymer and not an elastomeric polymer. The thermoplastic polymer has a glass transition temperature of at least 40°C, preferably 50°C.
[0115] The halogen in the halogen-containing polymer is preferably selected from fluorine or chlorine, and the halogen is advantageously chlorine.
[0116] The chlorine-containing polymer is selected from a polymer or mixture of polymers selected from the following: homopolymers of vinyl chloride, such as polyvinyl chloride, polyvinylidene chloride, chlorinated polyvinyl chloride, post-chlorinated polyvinyl chloride, and copolymers formed by polymerization of vinyl chloride monomer with up to 40% by weight of a comonomer, such as vinyl acetate, vinyl butyrate, vinylidene chloride, propylene, methyl methacrylate, etc., and also chlorine-containing polymers including other polymers, such as chlorinated polyethylene, terpolymers of acrylonitrile, butadiene, styrene, terpolymers of methyl methacrylate, butadiene, styrene; polyacrylate resins, polymethyl methacrylate resins, and terpolymers of alkyl acrylate, methyl methacrylate, butadiene. The chlorine-containing polymer is preferably polyvinyl chloride or post-chlorinated polyvinyl chloride.
[0117] The chlorine-containing polymer is preferably chosen from homopolymers and copolymers of vinyl chloride (VC) containing at least 50% by weight of VC units, preferably at least 70% by weight of VC units, more preferably at least 80% by weight of VC units and advantageously at least 85% by weight of VC units, or mixtures thereof.
[0118] Process for producing the polymer composition P1 according to the invention a) 29% to 60% by weight of an inorganic compound (F), b) 40% to 71% by weight of a polymeric impact modifier (IM1) The process for the preparation of the polymer composition P1, which comprises the steps of: Blending two components a) and b), wherein component b) and at least 83.33% by weight of compound a) are in the form of a dispersion in the aqueous phase during the blending step. The present invention is characterized by comprising:
[0119] A first preferred method for producing the polymer composition P1 according to the invention: a) 29% to 60% by weight of an inorganic compound (F), b) 40% to 71% by weight of a polymeric impact modifier (IM1) The process for the preparation of the polymer composition P1, which comprises the steps of: i) blending two components a) and b), wherein component b) and at least 83.33% by weight of compound a) are in the form of a dispersion in an aqueous phase during the blending step; ii) drying the blend obtained in step i). The present invention is characterized by comprising:
[0120] A second preferred method for producing the polymer composition P1 according to the invention: a) 29% to 60% by weight of an inorganic compound (F), the inorganic compound (F) consists of an inorganic filler (F1) and a fluidization aid (F2), the weight ratio of (F1) / (F2) being at least 5 / 1; b) 40% to 71% by weight of a polymeric impact modifier (IM1) The process for the preparation of the polymer composition P1, which comprises the steps of: blending the two components a) and b), wherein the two components b) and (F1) are in the form of a dispersion in an aqueous phase during the blending step; The present invention is characterized by comprising:
[0121] More preferably, a) 29% to 60% by weight of an inorganic compound (F), the inorganic compound (F) consists of an inorganic filler (F1) and a fluidization aid (F2), the weight ratio of (F1) / (F2) being at least 5 / 1; b) 40% to 71% by weight of a polymeric impact modifier (IM1) The process for the preparation of the polymer composition P1, which comprises the steps of: i) blending the two components a) and b), wherein the two components b) and (F1) are in the form of a dispersion in an aqueous phase during the blending step; ii) drying the blend obtained in step i). The present invention is characterized by comprising:
[0122] Further steps that the method may include The method may further comprise the step of recovering the blend obtained in the previous step to form a polymer powder or recovering the blend obtained in the previous step as a polymer powder.
[0123] The amounts of the two components a) and b), or (F1), in the aqueous dispersion are selected based on the solids content of each of the dispersions, to obtain the composition of each polymer composition P1 based on the solids portion.
[0124] The recovery step of the method for making the polymer composition according to the invention is preferably carried out by coagulation or by spray drying, the latter obviously combining recovery and drying in one process step.
[0125] For spray drying, the dispersions of components a) and b) can be blended or mixed and then the liquid mixture added to the spray drying equipment.Alternatively, the dispersions can be blended or mixed inside the spray drying equipment during the recovery step.
[0126] Spray drying is the preferred method for recovering and / or drying for the process for producing the polymer composition P1.
[0127] After drying, the polymer composition P1 has a wetness of less than 3% by weight, preferably a wetness of less than 1.5% by weight, more preferably a wetness of less than 1.2% by weight.
[0128] The present invention also provides a) 29% to 60% by weight of an inorganic compound (F), b) 40% to 71% by weight of a polymeric impact modifier (IM1) and a method for producing a polymer composition P2 comprising the steps of: d) Thermoplastic polymer TP1 Also includes The method comprises: Blending the composition P1 with a thermoplastic polymer TP1. The present invention is characterized by comprising:
[0129] Preferably in the process for preparing the polymer composition P2, the polymer composition P1 is prepared according to the process described above.
[0130] The inorganic compound (F), the polymeric impact modifier (IM1), the polymer composition P1 and the thermoplastic polymer TP1 are the same as defined above.
[0131] The blending of composition P1 with the thermoplastic polymer TP1 is preferably carried out by means of polymer composition blending, known to those skilled in the art as a dry blend or as compounding of the components, which are then melt processed.
[0132] The proportion of polymer composition P1 in polymer composition P2 is between 1 and 20 phr, preferably between 2 and 15 phr, more preferably between 3 and 12 phr and advantageously between 3 and 10 phr.
[0133] The present invention relates to a) 29% to 60% by weight of an inorganic compound (F), b) 40% to 71% by weight of a polymeric impact modifier (IM1) wherein the two components a) and b) amount to 100% by weight in total, for improving the impact resistance of a thermoplastic polymer TP1 and for dissipating heat during cooling in high speed processing.
[0134] After this use the thermoplastic polymer TP1 comprises a polymer composition P1, resulting in a polymer composition P2.
[0135] Preferably in the process for preparing the polymer composition P2, the polymer composition P1 is prepared according to the process described above.
[0136] The inorganic compound (F), the polymeric impact modifier (IM1), the polymer composition P1 and the thermoplastic polymer TP1 are the same as defined above.
[0137] The present invention relates to a) 29% to 60% by weight of an inorganic compound (F), b) 40% to 71% by weight of a polymeric impact modifier (IM1) wherein the two components a) and b) total 100% by weight, for improving the corner weld strength of a polymer composition P2 comprising the polymer composition P1 and a thermoplastic polymer TP1.
[0138] Preferably in the process for preparing the polymer composition P2, the polymer composition P1 is prepared according to the process described above.
[0139] The inorganic filler (F), the polymeric impact modifier (IM1), the polymer composition P1 and the thermoplastic polymer TP1 are the same as defined above.
[0140] The transformation of the polymer composition P2 comprising the polymer composition P1 and the thermoplastic polymer P2 is preferably carried out by extrusion.
[0141] The polymer composition P1 is used in the polymer composition P2 in a proportion ranging from 1 to 20 phr, preferably from 2 to 15 phr, more preferably from 3 to 12 phr and advantageously from 3 to 10 phr.
[0142] The polymer composition P2 can be processed and transformed into articles.
[0143] The present invention also relates to an article comprising the above-mentioned polymer composition P2, which may be a profile, a pipe, a siding, a foam, a film, a sheet, a flooring film or a sheet.
[0144] In a first preferred embodiment, the article according to the invention is a profile. In a first advantageous embodiment, the article according to the invention is a siding or window profile.
[0145] Evaluation method Glass transition temperature The glass transition temperature (Tg) of a polymer or polymer blend is measured by an instrument capable of thermomechanical analysis. The RDAII "RHEOMETRICS DYNAMIC ANALYSER" manufactured by Rheometrics Company was used. Thermomechanical analysis accurately measures the viscoelastic changes of a sample as a function of temperature, applied strain or deformation. The frequency used is 1 Hz. This instrument continuously records the deformation of the sample during a controlled program of temperature change while keeping the strain constant. The results are obtained by plotting the elastic modulus (G'), the elastic modulus loss, and tan δ as a function of temperature. Tg is the value of the temperature read off on the curve of tan δ where the value derived from tan δ is equal to zero.
[0146] To evaluate the volume average powder particle size, particle size distribution, and percentage of fine particles, a Malvern Mastersizer 300 instrument with a 300 mm lens is used (measuring the range 0.5-880 μm). D(v, 0.5) is the particle size below which 50% of the sample has a size smaller than and above which 50% of the sample has a size larger than, in other words, it is the same as the volume diameter at 50% cumulative volume. This size is also known as the volume median diameter (abbreviated as D50), which correlates with the mass or weight median diameter by the particle density, assuming a size-independent density for the particles.
[0147] Melting Efficiency
[0148] The melting efficiency of the polymer composition is evaluated by measuring the melting time using a torque rheometer according to ASTM D2538-02 (revised in 2010). A shorter melting time indicates a better melting efficiency, which translates into a more efficient process.
[0149] Shock-resistance
[0150] The British Standard BSI 2783 method was used to evaluate the single V-notch impact resistance. A notch of 0.1 mm radius was used. The impact resistance test was evaluated at controlled room temperature. The pendulum energy was 1 J. Ten specimens were used to evaluate the average impact energy with standard deviation.
[0151] The double V-notch impact resistance was evaluated using the DIN 53753 method. A notch with a radius of 0.1 mm was used. The impact resistance test was evaluated at controlled room temperature. The pendulum energy was 1 J. Ten specimens were used to evaluate the average impact energy with standard deviation. Information on the type of fracture (ductile or brittle) is also given.
[0152] Corner Weld Strength (CWS)
[0153] Corner weld strength resistance was evaluated using an in-house methodology. After extrusion, the samples were welded under pressure at 240°C. The specimens were then subjected to the weld resistance test at controlled room temperature of 25°C. The average strength at which five specimens broke was evaluated.
[0154] Microscopy
[0155] Microscopic examination of the powders is performed using a scanning electron microscope (SEM). For backscattered electron detection, the inorganic fillers (e.g. calcium carbonate) can be easily detected in each powder granule. EXAMPLES
[0156] The following materials are used or manufactured:
[0157] A polymeric impact modifier (IM1) is prepared according to the techniques described in US Pat. No. 4,278,576 using standard emulsion polymerization techniques.
[0158] A core / shell acrylic polymer impact modifier (IM1) is prepared using 89.2 parts butyl acrylate, 0.4 parts butylene glycol diacrylate, and 0.4 parts diallyl maleate as the elastomeric core, followed by polymerization of 10 parts methyl methacrylate. The solids content is 40% of the aqueous dispersion of (IM1a).
[0159] The inorganic mineral filler (F1) is calcium carbonate (CaCO3). The slurry or dispersion of CaCO3 is prepared according to the technology described in Japanese Patent No. 59057913. That is, 270 parts of water, 0.72 parts of sodium polyacrylate, and 729.3 parts of CaCO3 with a diameter of 0.2-0.6 μm and a moisture content of 0.6% are mixed, and a slurry is obtained by stirring five times at a shear rate of 102 / s for 20 minutes. The solid content obtained is 73% by weight.
[0160] As thermoplastic polymer TP1, polyvinyl chloride PVC S110P from Kemone is used.
[0161] As fluidization aid (F2) calcium carbonate (PCC, 0.07 microns) is used.
[0162] The sample compositions described in Table 1 are prepared in powder form, either as polymer composition P1 or as compositions for comparative examples.
[0163] Comparative Example 1: The dispersion of (IM1) and the slurry of mineral filler (F1) are mixed in the following ratio: 9.11 kg (9110 parts) of dispersion and 0.705 kg (705 parts) of slurry and spray dried under conditions conventionally used for latex dispersion alone. The resulting powder has a particle size of about 150 μm. 3% by weight of calcium carbonate (PCC, 0.07 microns) is added to the recovered powder as a flow aid (F2). The resulting powder has a ratio of acrylic impact modifier (IM1) / inorganic compound (F) CaCO3 of 85 / 15.
[0164] Comparative Example 2: The dispersion of (IM1) and the slurry of mineral filler (F1) are mixed in the following ratio: 2.679 kg (2679 parts) of dispersion and 3.968 kg (3968 parts) of slurry, and spray-dried under conditions conventionally used for latex dispersions alone. The resulting powder has a particle size of about 150 μm. 5% by weight of calcium carbonate (PCC, 0.07 microns) is added to the recovered powder as a flow aid (F2). The resulting powder has a ratio of impact modifier (IM1) / inorganic compound (F) CaCO3 of 25 / 75.
[0165] Example 1: The two acrylic dispersions and the inorganic slurry are mixed in the following ratio: 5.305 kg (5305 parts) of the impact modifier dispersion (IM1a), 0.617 kg (617 parts) of the (meth)acrylic copolymer processing aid (A1a), and 2.469 kg (2469 parts) of the inorganic mineral filler slurry (F1) and spray-dried under conditions conventionally used for the dispersions alone. The resulting powder has a particle size of about 150 μm. 3% by weight of calcium carbonate (PCC, 0.07 microns) is added to the recovered powder as a flow aid (F2). The resulting powder has a polymer / inorganic compound CaCO3 ratio of 55 / 45.
[0166] Example 2: The dispersion of (IM1) and the slurry of mineral filler (F1) are mixed in the following ratio: 7.902 kg (7902 parts) of dispersion and 1.587 kg (1587 parts) of slurry, and spray-dried under conditions conventionally used for latex dispersions alone. The resulting powder has a particle size of about 150 μm. 3% by weight of calcium carbonate (PCC, 0.07 microns) is added to the recovered powder as a flow aid (F2). The resulting powder has a ratio of impact modifier (IM1) / inorganic compound (F) CaCO3 of 70 / 30.
[0167] TIFF0007553225000001.tif57170
[0168] The powder samples prepared as comparative examples and examples in Table 1 are prepared with PVC as thermoplastic polymer TP1 at 5.5 phr in a PVC composition. The composition is dry blended in a Papenmeyer apparatus at increasing temperature. The PVC composition is prepared according to the amounts listed in Table 2.
[0169] TIFF0007553225000002.tif91170
[0170] The different compositions in Table 2 were extruded on a Haake Polylab extruder. The melt time of each composition was also measured.
[0171] The melting time results are summarized in Table 3.
[0172] TIFF0007553225000003.tif48170
[0173] Examples 1 and 2 show melt times that are still acceptable for Comparative Example 1, and much better than Comparative Example 2.
[0174] TIFF0007553225000004.tif85170
[0175] Examples 1 and 2 exhibit comparable levels of impact resistance and also show significant improvements in corner weld strength.
[0176] Comparative Example 1 has a significantly low corner weld strength.
[0177] Comparative Example 2 has poorer impact resistance than Examples 1 and 2.
Claims
1. a) 29% by weight or more and 60% by weight or less of an inorganic mineral-based compound (F), which consists of an inorganic filler (F1) and a fluidization aid (F2), the weight ratio of (F1) / (F2) being at least 5 / 1; b) 40% by weight or more and 71% by weight or less of a polymeric impact modifier (IM1), which is a polymer particle having a multilayer structure comprising at least one layer (IM1L1) comprising a polymer (L1) having a glass transition temperature below 0° C. and at least another layer (IM1L2) comprising a polymer (L2) having a glass transition temperature above 45° C. Including, Polymer composition P1, characterized in that the two components a) and b) add up to 100% by weight, the weight ratio of layers (IM1L1) / layers (IM1L2) in the multistage polymer is greater than 88 / 12 and less than 97 / 3, and in powder form having a volume median particle size D50 greater than 1 μm and less than 500 μm.
2. a) more than 31% by weight and less than 59% by weight of an inorganic compound (F); b) More than 41% and less than 69% by weight of polymeric impact modifier (IM1) The composition of claim 1 , comprising:
3. a) more than 42% by weight and less than 47% by weight of an inorganic compound (F); b) greater than 53% and less than 58% by weight of polymeric impact modifier (IM1) The composition of claim 1 , comprising:
4. 4. The composition according to claim 1, wherein a small sample of 0.1% by weight taken from a larger amount of the polymer composition P1 has a difference of less than 30% in the weight ratio of each of the two components a) and b) relative to the entire composition P1.
5. 5. The composition of any one of claims 1 to 4, wherein the weight ratio of layer (IM1L1) / layer (IM1L2) in the multistage polymer is in the range of greater than 89 / 11 and less than 96 / 4.
6. 5. The composition of claim 1, wherein the weight ratio of layer (IM1L1) / layer (IM1L2) in the multistage polymer is at least 89 / 11.
7. 7. The composition according to claim 1, wherein the polymer (L1) having a glass transition temperature below 0° C. is a (meth)acrylic polymer comprising at least 50% by weight of monomers from alkyl acrylates.
8. 8. The composition according to claim 1, wherein at least a part of the inorganic mineral filler (F) is a mineral filler selected from calcium carbonate, calcined clay, silica (fumed or precipitated silica), clay, montmorillonite (nanoclay), zeolite or perlite, titanium dioxide.
9. A method for producing a polymer composition P2 comprising a polymer composition P1 according to any one of claims 1 to 8, comprising the steps of: The polymer composition P2 is d) Thermoplastic polymer TP1 Also includes Blending the composition P1 with a thermoplastic polymer TP1 A manufacturing method comprising the steps of:
10. Use of a composition according to any one of claims 1 to 8 for improving the corner weld strength of a thermoplastic polymer TP1.
11. Use of a composition according to any one of claims 1 to 8 for processing a polymer composition P2 comprising a polymer composition P1 and a thermoplastic polymer TP1.
12. 9. An article comprising a polymer composition P2 comprising a polymer composition P1 according to any one of claims 1 to 8, characterized in that it is a profile, a pipe, a siding, a foam, a film, a sheet, a film or a sheet for flooring, The article, wherein said polymer composition P2 also comprises a thermoplastic polymer TP1.
Citation Information
Patent Citations
Co-extruded item and window molding
JP2001270052A
Powdery impact modifier composition
JP2002146197A
Hybrid impact modifiers and methods of making them
JP2009526886A
Use of High Rubber Impact Modifiers in Thermoplastic Compounds
JP2017511422A
Composite polymer modifiers
US20110305862A1