film

The film with an oil-containing layer and uneven surface effectively addresses the challenge of snow and ice accumulation by facilitating rapid snow and ice removal through reduced friction and enhanced sliding properties.

JP7553252B2Active Publication Date: 2024-09-18NITTO DENKO CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020044534
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-27
Filing Date
2020-03-13
Publication Date
2024-09-18
Estimated Expiration
2040-03-13

AI Technical Summary

Technical Problem

Existing films and sheets with snow sliding functions are inadequate in efficiently removing snow and ice as the amount of snow accumulation increases, necessitating improved snow sliding performance.

Method used

A film with an oil-containing layer that bleeds an oil component below a certain temperature and features an uneven surface structure, enhancing snow and ice sliding properties.

Benefits of technology

The film allows snow and ice to naturally fall in a shorter time by reducing friction and preventing accumulation, improving snow sliding performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553252000002
    Figure 0007553252000002
  • Figure 0007553252000001
    Figure 0007553252000001
  • Figure 0007553252000003
    Figure 0007553252000003
Patent Text Reader

Abstract

To provide a film that improves snow-gliding and enables excellent snow-accretion and / or ice-accretion prevention on structures.SOLUTION: Provided is a film, including an oil-containing layer containing an oil component in the resin as an outermost layer, and in which the oil component bleeds from the surface of the oil-containing layer at a predetermined temperature or lower, the surface of the oil-containing layer has an uneven shape, and the calculated average height (Sa) of the oil-containing layer in the area of 3.2 cm×3.2 cm on the surface is 4 μm or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a film, and more particularly to a film used as a surface covering material for preventing the adhesion of snow and ice to the surfaces of objects such as aircraft, trains, automobiles, wind power generators, houses, traffic lights, and signs. [Background technology]

[0002] The adhesion of ice to object surfaces (icing) and snowflakes due to snowfall (snow accretion) are the cause of damage and obstacles in various fields. For example, icing on aircraft wings, snow and ice on the underside of locomotives, snow on automobile headlights, icing on wind turbine blades, snow and ice on traffic lights, etc. can impede the operation, driving, and safety of these systems. Snow and ice on residential roofs and signs can also cause damage to these structures and injury to people due to falling snow.

[0003] In order to avoid such damage and obstacles, various measures have been considered for protecting structures from snow accumulation. For example, various films and sheets with snow-resistance and snow-sliding properties have been proposed.

[0004] For example, Patent Document 1 proposes an easy-sliding solid having a plurality of grooves extending in one direction on at least a part of the surface of the solid to form projections and recesses spaced at intervals of 2 μm or more and 4 mm or less, making the projections of the projections hydrophilic with a water contact angle of 30° or less and the recesses water-repellent with a water contact angle of 90° or more.

[0005] Patent Document 2 proposes a snow-adherence-resistant / snow-sliding film or sheet having an uneven shape formed by alternating peaks formed in a line along a predetermined direction and depressions formed in a line along the predetermined direction at a position lower than the peaks and adjacent to the peaks, and having a water-repellent surface, with at least a part of the surface extending between adjacent peaks across the depressions having a curved surface that is concavely curved in a direction perpendicular to the predetermined direction. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2003-226867 A [Patent Document 2] JP 2018-162553 A Summary of the Invention [Problem to be solved by the invention]

[0007] It is expected that films and sheets with snow-sliding properties as described above will be effective in removing snow and ice from the surface of structures. However, as the amount of snowfall per hour increases, the amount of snow that accumulates on structures also increases. As such, it is desirable to allow the snow to slide naturally in a shorter period of time, and further improvements in snow sliding properties have been required.

[0008] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a film that improves snow sliding properties and enables excellent prevention of snow and / or ice adhesion to structures. [Means for solving the problem]

[0009] As a result of extensive research, the inventors discovered that the above-mentioned problems could be solved by forming the film surface from an oil-containing layer from which oil components exude (bleed) at or below a certain temperature and by providing an uneven surface thereon, thus completing the present invention.

[0010] That is, the present invention includes an oil-containing layer containing an oil component in a resin as an outermost layer, the oil component bleeds from the surface of the oil-containing layer at a temperature equal to or lower than a predetermined temperature, the surface of the oil-containing layer has an uneven shape, and a calculated area of ​​3.2 cm x 3.2 cm on the surface of the oil-containing layer is technique A film is provided having an average height (Sa) of 4 μm or more.

[0011] In a preferred embodiment of the film, techniqueThe average height (Sa) is preferably 10 μm or more.

[0012] In a preferred embodiment of the above film, the maximum pitch distance of the concave and convex shapes is preferably 2000 μm or more.

[0013] In a preferred embodiment of the above film, the film is preferably a film for preventing snow or ice from accumulating over time on the surface of an object.

[0014] The present invention also provides a method for producing a film, comprising the following steps (a) and (b), or step (c): (a) forming a coating film using a resin composition containing a polymer component and an oil component, and forming a concave-convex shape on the surface of the coating film; (b) a step of curing the coating film having the concave-convex shape formed thereon (c) forming a coating film using a resin composition containing a polymer component and an oil component, curing the coating film, and then placing a member having an uneven surface on one side of the cured coating film to form an uneven shape on the coating film surface; Effect of the Invention

[0015] The film of the present invention is composed of an oil-containing layer whose surface contains an oil component that bleeds below a specified temperature, and furthermore, this surface is provided with an uneven shape, which improves snow sliding properties and allows snow blocks and ice adhering to structures to fall naturally in a shorter period of time. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, the embodiments of the present invention will be described in more detail, but the present invention is not limited to the following embodiments. In the present invention, the term "film" includes both film and sheet as defined in JIS K 6900:1994. According to the definition in JIS K 6900:1994, a film is a thin, flat product whose thickness is extremely small compared to its length and width, and whose maximum thickness is arbitrarily limited, and is usually supplied in the form of a roll, while a sheet is a thin, flat product whose thickness is generally small compared to its length and width. The boundary between film and sheet is unclear, and in this specification, the term "film" also includes the concept of sheet.

[0017] The film of the present invention includes an oil-containing layer containing an oil component in a resin as the outermost layer, and the surface of the oil-containing layer has an uneven shape. The oil component bleeds from the surface of the oil-containing layer at a predetermined temperature or lower and covers the film surface. By providing the film of the present invention with such a configuration, snow blocks and ice attached to the surface of the film have a portion that does not directly contact the film, so that the frictional force is reduced and they are easily dropped by their own weight, and the bled oil component further improves the slipperiness of the film surface. Therefore, snow blocks and ice can be naturally dropped in a shorter time, and accumulation of snow and ice over time can be prevented. In the present invention, "having an uneven surface" means that when the surface of the film is photographed with a laser microscope and the average height is calculated in an area of ​​3.2 cm x 3.2 cm, the calculated average height (Sa) is 4 μm or more.

[0018] <Oil-containing layer> The oil-containing layer is a layer in which an oil component is contained in a resin. The oil-containing layer is configured to contain a polymer component and an oil component. The polymer component forms a matrix, and the oil component is contained in the matrix.

[0019] (Polymer component) The polymer component is not particularly limited, but examples thereof include silicone resin, polyurethane resin, polyurethane acrylic resin, vinyl chloride resin, polyester resin, elastomers, fluororesin, polyamide resin, polyolefin resin (polyethylene, polypropylene, etc.), acrylic resin, etc. Among these, silicone resin is preferred from the viewpoint of excellent bleeding effect of the oil component and durability against outdoor exposure.

[0020] Any suitable silicone resin may be used as long as it does not impair the effects of the present invention. The silicone resin may be one type or two or more types. Such a silicone resin may be a condensation type silicone resin or an addition type silicone resin. In addition, such a silicone resin may be a one-component silicone resin that is dried alone (for example, a one-component room temperature vulcanizable (RTV) resin), or a two-component silicone resin (for example, a two-component room temperature vulcanizable (RTV) resin).

[0021] Specific examples of silicone resins that are commercially available include one-component RTV rubbers manufactured by Shin-Etsu Chemical Co., Ltd. (e.g., KE-3423, KE-347, KE-3475, KE-3495, KE-4895, KE-4896, KE-1830, KE-1884, KE-3479, KE-348, KE-4897, KE-4898, KE-1820, KE-1825, KE-1831, KE-1833, KE-1885, KE-1056, KE-1151, KE-1842, KE-1886, KE-3424G, KE-3494, KE-1830 ... 3490, KE-40RTV, KE-4890, KE-3497, KE-3498, KE-3493, KE-3466, KE-3467, KE-1862, KE-1867, KE-3491, KE-3492, KE-3417, KE-3418, KE-3427, KE-3428, KE-41, KE-42, KE-44, KE-45, KE-441, KE-445, KE-45S, etc.), two-component RTV rubber manufactured by Shin-Etsu Chemical Co., Ltd. (e.g., KE-1800T-A / B, KE-66, KE-1031-A / B, KE-200, KE-118, KE-103 , KE-108, KE-119, KE-109E-A / B, KE-1051J-A / B, KE-1012-A / B, KE-106, KE-1282-A / B, KE-1283-A / B, KE-1800-A / B / C, KE-1801-A / B / C, KE-1802-A / B / C , KE-1281-A / B, KE-1204-A / B, KE-1204-AL / BL, KE-1280-A / B, KE-513-A / B, KE-521-A / B, KE-1285-A / B, KE-1861-A / B, KE-12, KE-14, KE-17, KE-113, KE- 24, KE-26, KE-1414, KE-1415, KE-1416, KE-1417, KE-1300T, KE-1310ST, KE-1314-2, KE-1316, KE-1600, KE-1603-A / B, KE-1606, KE-1222-A / B, KE-1241, etc.), silicone sealants manufactured by Shin-Etsu Chemical Co., Ltd. (e.g., KE-42AS, KE-420, KE-450, etc.), rubber compounds manufactured by Shin-Etsu Chemical Co., Ltd. (e.g., KE-655-U, KE-675-U, KE-931-U, KE-941-U, KE-951-U,KE-961-U, KE-971-U, KE-981-U, KE-961T-U, KE-971T-U, KE-871C-U, KE-9410-U, KE-9510-U, KE-9610-U, KE-9710-U, KE-742-U, KE-752-U, KE-762-U, KE-772-U, KE-782-U, KE-850-U, KE-870-U, KE-880-U, KE-890-U, KE-9590-U, KE-5590-U, KE-552-U, KE-582-U, KE-552B-U, KE-555-U, KE-575-U, KE-541-U, KE-551-U, KE-561-U, KE-571-U, KE-581-U, KE-520-U, KE-530B-2-U, KE-540B-2-U, KE-1551-U, KE-1571-U, KE-152-U, KE-174-U, KE-3601SB-U, KE-3711-U, KE-3801M-U, KE-5612G-U, KE-5620BL-U, KE-5620W-U, KE-5634-U, KE-7511-U, KE-7611-U, KE-765-U, KE-785-U, KE-7008-U, KE-7005-U, KE-503-U, KE-5042-U, KE-505-U, KE-6801-U, KE-136Y-U, etc.), LIMS (Liquid Silicone Rubber Injection Molding System) manufactured by Shin-Etsu Chemical Co., Ltd. (for example, KEG-2000-40A / B, KEG-2000-50A / B, KEG-2000-60A / B, KEG-2000-70A / B, KEG-2001-40A / B, KEG-2001-50A / B, KE-1950-10A / B, KE-1950-20A / B, KE-1950-30A / B, KE-1950-35A / B, KE-1950-40A / B, KE-1950-50A / B, KE-1950-60A / B, KE-1950-70A / B, KE-1935A / B, KE-1987A / B, KE-1988A / B, KE-2019-40A / B, KE-2019-50A / B, KE-2019-60A / B, KE-2017-30A / B, KE-2017-40A / B, KE-2017-50A / B, KE-2090-40A / B, KE-2090-50A / B, KE-2090-60A / B, KE-2090-70A / B, KE-2096-40A / B, KE-2096-50A / B,KE-2096-60A / B, etc.), LR7665 series manufactured by Wacker Asahi Kasei Silicone Corporation, LR3033 series manufactured by Wacker Asahi Kasei Silicone Corporation, TSE3032 series manufactured by Momentive Corporation, and Sylgard 184 manufactured by Dow Corning Toray Co., Ltd. Among these, from the viewpoint of phase separation with the oil component that bleeds to the surface at a specified temperature, two-component silicone resins are preferred, and specifically, KE-1950-10A / B, KE-1950-20A / B, KE-1950-30A / B, KE-1950-35A / B, KE-1950-40A / B, KE-1950-50A / B, KE-1950-60A / B, KE-1950-70A / B, KE-1935A / B, etc. are more preferred.

[0022] (Oil ingredients) The oil component is not particularly limited as long as it bleeds out onto the surface of the film and has either a snow accretion prevention function or an ice accretion prevention function (hereinafter also referred to as snow accretion prevention function). Examples of the oil component include silicone oil, fluorine oil, hydrocarbon oil, polyether oil, ester oil, phosphorus compound oil, mineral oil, etc. Among them, silicone oil is preferred from the viewpoint of snow accretion prevention effect and bleeding effect. The oil component may be used alone or in combination of two or more kinds.

[0023] The silicone oil may, for example, be one represented by the general formula (1).

[0024] [ka]

[0025] In general formula (1), each R1 independently represents an alkyl group having 1 to 10 carbon atoms, an aryl group, an aralkyl group, a fluoroalkyl group, a polyether group, a carbinol group, an amino group, an epoxy group, a silanol group, or a hydroxyl group, and n represents an integer of 0 to 150. Multiple n's may be the same or different.

[0026] R1 in the general formula (1) is preferably an alkyl group having 1 to 10 carbon atoms, a phenyl group, a polyether group, a carbinol group, an amino group, or an epoxy group.

[0027] Specifically, the silicone oil represented by general formula (1) can be exemplified by the dimethyl silicone oil in which all R1 are methyl groups, the phenylmethyl silicone oil in which a part of the methyl groups of these dimethyl silicone oils are substituted with phenyl groups, the polyether group-containing silicone oil in which polyether groups are substituted, the carbinol group-containing silicone oil in which carbinol groups are substituted, the amino group-containing silicone oil in which amino groups are substituted, or the epoxy group-containing silicone oil in which epoxy groups are substituted.Among them, the phenylmethyl silicone oil, the polyether group-containing silicone oil, and the carbinol group-containing silicone oil are preferred because they do not have reactivity or self-condensation with silicone resin when silicone resin is used as polymer component.

[0028] The silicone oil represented by the general formula (1) has a number average molecular weight of preferably 100 to 40,000, and more preferably 200 to 20,000.

[0029] The silicone oil preferably has a viscosity at 25° C. of 1 to 10,000 cSt, more preferably 5 to 5,000 cSt, even more preferably 8 to 1,000 cSt, and particularly preferably 10 to 500 cSt. When the viscosity at 25° C. is within the above range, the oil has excellent sliding properties on snow and ice, and therefore an excellent snow and icing prevention effect can be obtained.

[0030] Specific examples of silicone oils include silicone oils manufactured by Momentive Performance Materials Japan, LLC (e.g., TSF431, TSF433, TSF437, TSF451 series, etc.), silicone oils manufactured by Shin-Etsu Chemical Co., Ltd. (e.g., KF96L series, KF96 series, KF69 series, KF99 series, KF50 series, KF54 series, KF410 series, KF412 series, KF414 series, FL series, KF-6000, KF-6001, KF-6002, KF-6003, X-22-4039, PAM-E, KF-8010, KF- 8012, KF-8008, KF-4917, X-22-163, etc.), silicone oils manufactured by Dow Corning Toray Co., Ltd. (for example, BY16-846 series, SF8416 series, SH200 series, SH203 series, SH230 series, SF8419 series, FS1265 series, SH510 series, SH550 series, SH710 series, FZ-2110 series, FZ-2203 series, BY16-201, etc.), and silicone oils manufactured by Wacker Asahi Kasei Silicones Corp. (for example, AK series, AKF series, L series, W series, AP series, AR series, AS series). Among these, from the viewpoint of phase separation with the polymer component, it is preferable to use TSF437, KF50 series, KF54 series, KF-6000, KF-6001, KF-6002, etc., and it is more preferable to use the KF96 series, TSF451 series, etc. in combination to increase the affinity of these oil components with the polymer component.

[0031] Examples of fluorine oils include perfluoropolyether, perfluorodecalin, and perfluorooctane. Perfluoropolyether is preferred from the viewpoint of chemical stability. Examples of perfluoropolyether include those represented by the structural formula: A-(C3F6O) x (CF2O) y (C2F4O) z-B (wherein the terminal group A is any one of -F, -CF3, -C2F5, -C3F7, -CF(CF3)OCF3, -OF, -OCF3, -OC2F5, -OC3F7, -OCF(CF3)OCF3, the terminal group B is any one of -CF3, -C2F5, -C3F7, -CF(CF3)OCF3, x, y, and z are 0 or positive integers, x+y+z>1, and the viscosity at 25°C is 50 to 500,000 cSt). Specific examples of perfluoropolyethers include compounds represented by the formula: CF3O-(CF2CF(CF3)O) x (CF2O) y -CF3 (wherein x and y are as defined above), CF3O-(CF2O) y (C2F4O) z -CF3 (wherein y and z are as defined above), CF3O-(CF2CF(CF3)O) x -CF3 (wherein x is as defined above), and F-(CF2CF2CF2O) x -C2F5 (wherein x is as defined above), and the like.

[0032] (Other Ingredients) In addition, the oil-containing layer may contain other components according to the application, as long as the effects of the present invention are not impaired. Examples of other components include solvents, liquid paraffin, surfactants, antibacterial agents, ultraviolet absorbers, fillers, crosslinking agents, etc. These may be used alone or in combination of two or more.

[0033] Examples of the solvent include liquid hydrocarbons such as ethyl acetate, hexane, heptane, benzene, toluene, xylene, and 1-tetradecene.

[0034] Commercially available liquid paraffins include, for example, P-40, P-55, P-60, P-70, P-80, P-100, P-120, P-150, P-200, P-260, and P-350 manufactured by MORESCO Corporation, and hydrocarbon-based liquid paraffin manufactured by Wako Pure Chemical Industries, Ltd.

[0035] Examples of the surfactant include anionic surfactants, nonionic surfactants, amphoteric surfactants, and cationic surfactants. Examples of anionic surfactants include alkylbenzenesulfonates, alkyl or alkenyl ether sulfates, alkyl or alkenyl sulfates, α-olefinsulfonates, α-sulfofatty acids or ester salts, alkanesulfonates, saturated or unsaturated fatty acid salts, alkyl or alkenyl ether carboxylates, amino acid surfactants, N-acylamino acid surfactants, alkyl or alkenyl phosphates or salts thereof. Examples of nonionic surfactants include polyoxyalkylene alkyl or alkenyl ethers, polyoxyethylene alkylphenyl ethers, higher fatty acid alkanolamides or alkylene oxide adducts thereof, sucrose fatty acid esters, alkyl glycosides, fatty acid glycerin monoesters, alkylamine oxides, etc. Examples of amphoteric surfactants include carboxy or sulfobetaine amphoteric surfactants, etc. Examples of cationic surfactants include quaternary ammonium salts, etc.

[0036] Examples of antibacterial agents include azoxystrobin, benalaxyl, benomyl, bitertanol, bromuconazole, captafol, captan, carbendazim, quinomethionate, chlorothalonil, chlozolinate, cyprodinil, dichlofluanid, diclofen, diclomedine, dicloran, diethofencarb, dimethomorph, diniconazole, dithianon, epoxiconazole, famoxadone, fenarimol, fenbuconazole, fenfuram, fenpiclonil, fentin, fluazinam, fludioxonil, fluorimide, fluquinconazole, flusulfamide, flutolanil, folpet, hexachlorobe Examples of the antibacterial agents include benzodiazepine, hexaconazole, imibenconazole, ipoconazole, iprodione, kresoxim methyl, manzeb, maneb, mepanipyrim, mepronil, metconazole, metiram, nickel bis(dimethyldithiocarbamate), nuarimol, oxine copper, oxolinic acid, pencycuron, phthalide, procymidone, propineb, quintozene, sulfur, tebuconazole, tecloftalam, tecnazene, thifluzamide, thiophenate methyl, thiram, tolclofos methyl, tolylfluanid, triadimefon, triadimenol, triazoxide, triforine, triticonazole, vinclozolin, zineb, ziram, etc. Examples of the antibacterial agents of natural products include Chinese herbal medicine ingredients such as moso bamboo extract, hinokitiol, garlic extract, and licorice. In addition, inorganic antibacterial agents such as silver, copper, zinc, tin, lead, and gold can be used. If necessary, zeolite, hydroxyapatite, calcium carbonate, silica gel, calcium aluminum silicate, polysiloxane compounds, zirconium phosphate, zirconium sulfate, ion exchangers, zinc oxide, and the like can be used as carriers for these inorganic antibacterial agents. Examples of synthetic antibacterial agents include 2-pyridinethiol-1-oxide, p-chloro-m-cresol, polyhexamethylene hyguanide, hydrochloride, benzethonium chloride, alkyl polyaminoethyl glycine, benzisothiazoline, 5-chloro-2-methyl-4-isothiazolin-3-one, 1,2-benzisothiazolin-3-one, and 2,2'-dithio-bis-(pyridine-1-oxide).

[0037] Examples of commercially available ultraviolet absorbents include TINUVIN 571, TINUVIN 460, TINUVIN 213, TINUVIN 234, TINUVIN 329, and TINUVIN 326 manufactured by BASF.

[0038] Examples of the filler include silica particles and diatomaceous earth. From the viewpoint of dispersibility, the filler is preferably a particle whose surface has been hydrophobically treated. Examples of such a surface treatment method include a method of surface treatment with dimethylpolysiloxane, dimethyldichlorosilane, hexamethylenedisilazane, cyclic dimethylsiloxane, etc. The size of such particles whose surface has been hydrophobically treated is preferably an average particle size of 5 nm to 300 nm.

[0039] Examples of the crosslinking agent include isocyanate compounds, epoxy compounds, melamine compounds, metal chelate compounds, oxazoline compounds, aziridine compounds, and ethyleneimine.

[0040] The oil component is contained in the resin (matrix) formed by the polymer component, and the content ratio of the oil component to 100 parts by mass of the polymer component is, for example, 25 to 400 parts by mass, preferably 50 to 300 parts by mass, more preferably 75 to 250 parts by mass, and particularly preferably 100 to 200 parts by mass. By containing 25 parts by mass or more of the oil component to 100 parts by mass of the polymer component, the oil component can be sufficiently bled out, and the snow and ice adhesion prevention effect can be exhibited. In addition, by containing 400 parts by mass or less, the strength of the oil-containing layer is not reduced.

[0041] In the present invention, the content ratio of the polymer component to the entire oil-containing layer is preferably 10% by mass or more at the lower limit, more preferably 15% by mass or more, and even more preferably 25% by mass or more at the upper limit, and is preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less at the upper limit. When the content of the polymer component is within the above range, the oil component is sufficiently bled out, and the snow and ice adhesion prevention effect can be exhibited.

[0042] To incorporate the oil component into a resin made of a polymer component, for example, a method of heat-curing a resin composition obtained by mixing the polymer component, the oil component, and other components as necessary can be mentioned. By heating the resin composition, the polymer component forms a matrix, and the oil component is dispersed therein.

[0043] The thickness of the oil-containing layer may be appropriately determined depending on the application, but is preferably 0.05 to 3 mm (50 to 3000 μm). When the thickness of the oil-containing layer is 0.05 mm or more, the outdoor exposure durability is improved, and the amount of oil component contained can be increased, so that the bleeding effect is enhanced and the snow and ice adhesion prevention function can be improved. Furthermore, when the thickness of the oil-containing layer is 3 mm or less, the handleability is improved. The lower limit of the thickness of the oil-containing layer is more preferably 0.075 mm or more, more preferably 0.1 mm or more, and the upper limit is more preferably 2.5 mm or less, more preferably 2 mm or less.

[0044] The bleeding temperature of the oil-containing layer can be appropriately set according to the usage environment so that the oil component bleeds at a predetermined temperature or lower. For example, when the predetermined temperature is set to 0°C, the oil component that bleeds at 0°C or lower can be appropriately selected and used to bleed the oil component from the film when the outside air temperature becomes 0°C or lower.

[0045] <Base material> The film of the present invention preferably has a substrate to support the oil-containing layer and maintain the strength of the film.

[0046] The material constituting the substrate can be appropriately selected in consideration of the sticking property to the object, the strength of the entire product, etc., and examples thereof include polyurethane resin, polyurethane acrylic resin, rubber-based resin, vinyl chloride resin, polyester resin, silicone resin, elastomers, fluororesin, polyamide resin, polyolefin resin (polyethylene, polypropylene, etc.), ionomer, polyethylene terephthalate resin, etc. Among them, from the viewpoint of sticking property to the object, it is preferable to use polyester resin, ionomer, and polyethylene terephthalate resin. Such a substrate layer may be of only one type, or of two or more types.

[0047] The thickness of the substrate may be appropriately determined depending on the application, but is preferably 10 to 300 μm, more preferably 30 to 250 μm, and further preferably 50 to 200 μm. By adjusting the layer thickness of the substrate as described above, the film has an appropriate strength and is easy to handle.

[0048] <Film Preparation> The film of the present invention can be produced, for example, by a method of forming a coating film using a resin composition containing a polymer component and an oil component, imparting irregularities to the surface of the coating film, and then curing the coating film; or by a method of directly or indirectly placing another component having irregularities on the cured coating film formed using the resin composition, so that the cured coating film follows the irregularities of the other component.

[0049] Specifically, the method for producing the film of the present invention includes the following steps (a) and (b), or the following step (c): (a) forming a coating film using a resin composition containing a polymer component and an oil component, and forming a concave-convex shape on the surface of the coating film; (b) a step of curing the coating film having the concave-convex shape formed thereon (c) forming a coating film using a resin composition containing a polymer component and an oil component, curing the coating film, and then placing a member having an uneven surface on one side of the cured coating film to form an uneven shape on the coating film surface; The film of the present invention can be suitably produced by the above-mentioned production method.

[0050] (Step (a)) In step (a), a resin composition containing a polymer component and an oil component in an arbitrary ratio is first prepared. The resin composition may contain other components as described above. The resin mixture is preferably stirred until the raw material components become uniform, and a stirrer may be used.

[0051] If air is contained in the resin mixture, there is a risk that air bubbles will be contained in the oil-containing layer after molding, which may reduce the film strength or deteriorate the product appearance, so it is preferable to degas the mixture. Examples of degassing methods include a method of degassing the mixture using a planetary stirring device for several seconds to 5 minutes, and a method of reducing the pressure under vacuum for several seconds to 30 minutes.

[0052] The resin composition obtained as described above is applied onto a coating table or a substrate to form a coating film (oil-containing layer). The coating method is not particularly limited as long as the coating film is applied so that the film thickness after drying is 0.05 to 3 mm, and examples of the coating method include a casting method using an applicator and a brush coating method.

[0053] Then, the surface of the coating film is formed with a concave-convex shape. Examples of methods for forming a concave-convex shape on the coating film include a method in which a roller having a concave-convex shape on the peripheral surface is brought into close contact with the coating film to transfer the concave-convex shape to the coating film, a method in which a punching sheet having a concave-convex shape on its surface is pressed against the coating film to transfer the concave-convex shape to the coating film, and a method in which sandpaper having a concave-convex shape on its surface is pressed against the coating film to transfer the concave-convex shape to the coating film. When the resin composition is applied using a brush, the desired concave-convex shape can be formed on the coating film surface during application depending on the material of the brush.

[0054] The height of the unevenness can be adjusted appropriately by adjusting the pressing force of a processing member such as a roller or a punching sheet that imparts the uneven shape.

[0055] (Step (b)) In step (b), the coating film having the concave-convex shape formed in step (a) is cured. The curing method can be a conventionally known method, such as a method of drying by heating, a method of curing by irradiation with ultraviolet light, a method of adding a crosslinking agent, etc. When drying by heating, it is preferable to heat at 100 to 160° C. for 1 to 300 minutes.

[0056] (Process (c)) In step (c), a coating film is formed using a resin composition containing a polymer component and an oil component in an arbitrary ratio. The coating film can be formed in the same manner as in step (a).

[0057] The coating is then cured to obtain a cured coating, which can be cured by a conventional method, such as drying by heating, curing by UV irradiation, or adding a crosslinking agent. When drying by heating, it is preferable to heat at 100 to 160° C. for 1 to 300 minutes.

[0058] After curing, a member having an uneven surface is placed on one side of the cured coating film, specifically, on the substrate surface behind the coating film when the cured coating film has a substrate, or on one of the two main surfaces when the cured coating film is the only film. Examples of the member include an adhesive layer having an uneven surface (e.g., a substrate-less adhesive sheet), a substrate having an uneven surface, etc. This allows the cured coating film to follow the unevenness of the member having an uneven surface, forming an uneven shape on the coating film surface.

[0059] In this manner, the film of the present invention is obtained.

[0060] The thickness of the film of the present invention can be appropriately selected within the range of 0.06 to 3.5 mm, taking into consideration the desired strength of the film and the size of the object (structure) to which the film is to be applied.

[0061] In the present invention, the calculated average height (Sa) of a 3.2 cm x 3.2 cm area on the surface of the oil-containing layer of the film is 4 μm or more. technique When the average height (Sa) is 4 μm or more, the desired effect of the present invention can be obtained. technique The average height (Sa) has a lower limit of preferably 4.3 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more, and an upper limit of preferably 100 μm or less, more preferably 75 μm or less, and even more preferably 50 μm or less. In addition, technique The average height (Sa) can be determined by photographing the surface of the film with a laser microscope (for example, "OPTELICS HYBRID" manufactured by Lasertec) and calculating the average height in an area of ​​3.2 cm x 3.2 cm.

[0062] In the present invention, the maximum pitch distance of the uneven shape is preferably 2000 μm or more. If the maximum pitch distance is 2000 μm or more, a sufficient uneven shape is formed on the film surface, and the film has excellent snow sliding properties. The maximum pitch distance of the uneven shape is more preferably 2500 μm or more, and the upper limit is preferably 60000 μm or less, more preferably 55000 μm or less.

[0063] The film of the present invention is used as a surface covering material by being provided on the surface of an object (structure). The object can be used without any particular limitation as long as it is an object exposed to natural environments such as snowfall, wind and rain, etc. Specific examples of the object include aircraft, trains, automobiles, wind power generators, houses, traffic lights, signs, etc. EXAMPLES

[0064] The present invention will be further described below with reference to examples and comparative examples, but the present invention is not limited to the following examples. In the examples and comparative examples, "parts" refers to parts by mass.

[0065] (Production Example 1: Preparation of resin composition) A resin composition was prepared by uniformly mixing 50 parts of a silicone resin (both manufactured by Shin-Etsu Chemical Co., Ltd., two-component RTV rubber) prepared by mixing KE-1950-50A and KE-1950-50B in a mass ratio of 1:1, 30 parts of KF-96-50cs (silicone oil manufactured by Shin-Etsu Chemical Co., Ltd.), and 20 parts of TSF-437 (silicone oil manufactured by Momentive Performance Materials Japan, LLC).

[0066] (Production Example 2: Preparation of resin composition) A resin composition was prepared by uniformly mixing 50 parts of a silicone resin (both manufactured by Shin-Etsu Chemical Co., Ltd., two-component RTV rubber) prepared by mixing KE-1950-50A and KE-1950-50B in a mass ratio of 1:1, and 50 parts of ethyl acetate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.).

[0067] Example 1 The resin composition prepared in Production Example 1 was uniformly applied onto a polyethylene terephthalate (PET) film (film thickness 125 μm) using an applicator so that the thickness of the oil-containing layer after drying would be 150 μm. Using a roller having an uneven surface, unevenness was formed on the coating film. Thereafter, the film was dried at 150° C. for 10 minutes to form an oil-containing layer, and the film of Example 1 was prepared. The surface of the film was photographed using a laser microscope (Lasertec's "OPTELICS HYBRID"), measurements were taken over an area of ​​3.2 cm x 3.2 cm, and the average height was calculated. technique The average height (Sa) was 4.4±1.0 μm.

[0068] Example 2 The film of Example 2 was produced in the same manner as in Example 1, except that a punching sheet was used to form irregularities on the coating film. technique The average height (Sa) was 15.9±6.1 μm.

[0069] Example 3 The film of Example 3 was produced in the same manner as in Example 1, except that a different roller was used. technique The average height (Sa) was 20.9±3.3 μm.

[0070] Example 4 The film of Example 4 was produced in the same manner as in Example 1, except that a roller different from that in Example 1 was used. technique The average height (Sa) was 21.4±5.3 μm.

[0071] Example 5 The film of Example 5 was produced in the same manner as in Example 2, except that a different punching sheet was used. technique The average height (Sa) was 24.9±5.0 μm.

[0072] Example 6 The film of Example 6 was produced in the same manner as in Example 1, except that a roller different from that in Example 1 was used. technique The average height (Sa) was 26.1±5.2 μm.

[0073] Example 7 The film of Example 7 was produced in the same manner as in Example 1, except that a roller different from that in Example 1 was used. technique The average height (Sa) was 30.3±6.1 μm.

[0074] Example 8 The film of Example 8 was produced in the same manner as in Example 1, except that a different roller was used. technique The average height (Sa) was 46.2±10.2 μm.

[0075] Example 9 The resin composition prepared in Production Example 1 was uniformly applied to a polyethylene terephthalate (PET) film (film thickness 125 μm) using an applicator so that the oil-containing layer after drying would be 150 μm thick, and the film was dried at 150° C. for 10 minutes to form an oil-containing layer. Thereafter, a pressure-sensitive adhesive having an uneven shape with a minimum pitch distance of 1500 μm and a maximum pitch distance of 5000 μm was placed on the substrate surface of the film to prepare the film of Example 9. Calculation of the film surface technique The average height (Sa) was 8.7±2.8 μm.

[0076] Comparative Example 1 The resin composition prepared in Production Example 1 was uniformly applied to a polyethylene terephthalate (PET) film (film thickness 125 μm) using an applicator so that the oil-containing layer after drying would be 150 μm thick, and the film was dried at 150° C. for 10 minutes to form an oil-containing layer, thereby preparing the film of Comparative Example 1. technique The average height (Sa) was 3.4±1.2 μm.

[0077] Comparative Example 2 A film of Comparative Example 2 was produced in the same manner as in Comparative Example 1, except that the resin composition produced in Production Example 2 was used. technique The average height (Sa) was 4.1±0.5 μm.

[0078] Comparative Example 3 The resin composition prepared in Production Example 2 was uniformly applied onto a polyethylene terephthalate (PET) film (film thickness 125 μm) using an applicator so that the oil-containing layer after drying would be 150 μm thick. A roller with an uneven surface was used to form unevenness in the coating film. Thereafter, the film was dried at 150° C. for 10 minutes to form an oil-containing layer, thereby producing a film of Comparative Example 3. Calculation of the film surface technique The average height (Sa) was 20.4±7.0 μm.

[0079] Comparative Example 4 The film of Comparative Example 4 was produced in the same manner as in Comparative Example 3, except that a roller different from that in Comparative Example 3 was used. technique The average height (Sa) was 29.9±4.6 μm.

[0080] Comparative Example 5 The film of Comparative Example 5 was produced in the same manner as in Comparative Example 3, except that a roller different from that in Comparative Example 3 was used. technique The average height (Sa) was 32.2±2.1 μm.

[0081] The films of the examples and comparative examples prepared above were subjected to the following snow skiing experiment. The film prepared in each example was 10 cm long x 10 cm wide (area 100 cm 2 ) and cut it into pieces 10cm long x 10cm wide (area 100cm 2 The film was attached to an acrylic plate of 100 mm thick (350 mm thick) with the oil-containing layer facing outward, and then placed in a test room with an environmental temperature set at 1°C. Approximately 20 g of wet snow was attached to the horizontally placed film surface. The acrylic plate with the snow attached was placed at an angle of 60° to the floor. The time it took for the snow block to fall (snow sliding time) was then measured. The results are shown in Table 1.

[0082] [Table 1]

[0083] Comparative Example 1 is a film having an oil-containing layer on the film surface and no uneven shape, and Comparative Examples 2 to 5 are examples in which the film surface is composed of a non-oil-containing layer (Comparative Examples 3 to 5 have uneven shapes). Comparative Example 1 had a shorter snow sliding time than Comparative Examples 2 to 5, but Examples 1 to 9 had a significantly shorter snow sliding time than Comparative Example 1, allowing snow blocks to fall naturally in a shorter time, and it was found that they had an excellent snow and icing prevention effect. [Industrial Applicability]

[0084] The film of the present invention is useful for preventing the adhesion of snow and ice to the surfaces of aircraft, trains, automobiles, wind power generators, houses, traffic signals, signs, and the like.

Claims

1. The present invention comprises an oil-containing layer as an outermost layer, the oil component being contained in a resin, the resin containing a silicone resin, the oil component containing a silicone oil, the oil component bleeding out from a surface of the oil-containing layer at a temperature equal to or lower than a predetermined temperature, and the surface of the oil-containing layer having an uneven shape, A film, wherein the arithmetic mean height (Sa) of the oil-containing layer in an area of ​​3.2 cm x 3.2 cm on the surface is 4 μm or more.

2. The film described in claim 1, wherein the silicone oil is a silicone oil represented by general formula (1). [Formula 1] (In general formula (1), each R 1 independently represents an alkyl group having 1 to 10 carbon atoms, an aryl group, an aralkyl group, a fluoroalkyl group, a polyether group, a carbinol group, an amino group, an epoxy group, a silanol group, or a hydroxyl group, and n represents an integer of 0 to 150. Multiple n's may be the same or different.)

3. The film of claim 1 , wherein the arithmetic mean height (Sa) is 10 μm or more.

4. The film according to claim 1 or 2, wherein the maximum pitch distance of the concave-convex shapes is 2000 μm or more.

5. The film according to any one of claims 1 to 3, which prevents snow and ice from accumulating on a surface of an object over time.

6. A coating composition for a coating film comprising an oil-containing layer as an outermost layer, the oil component being contained in a resin, the oil component bleeding out from a surface of the oil-containing layer at a temperature equal to or lower than a predetermined temperature, the surface of the oil-containing layer having an uneven shape, A method for producing a film, wherein the arithmetic mean height (Sa) of the surface of the oil-containing layer in an area of ​​3.2 cm x 3.2 cm is 4 μm or more, A method for producing a film, comprising the following steps (a) and (b), or step (c): (a) A step of forming a coating film using a resin composition containing a polymer component containing a silicone resin and an oil component containing a silicone oil, and forming a concave-convex shape on the surface of the coating film. (b) A step of curing the coating film having the concave-convex shape formed thereon (c) forming a coating film using a resin composition containing a polymer component and an oil component, curing the coating film, and then placing a member having an uneven surface on one side of the cured coating film to form an uneven shape on the coating film surface;

7. A method for producing a film as described in claim 6, wherein the arithmetic mean height (Sa) is 10 μm or more.

8. A method for manufacturing a film as described in claim 6 or 7, wherein the maximum pitch distance of the uneven shape is 2000 μm or more.

9. A method for manufacturing a film described in any one of claims 6 to 8, which prevents snow or ice from accumulating on the surface of an object over time.

Citation Information

Patent Citations

  • Material having ice covering proof function, and preparation method and application thereof

    CN102241886A

  • Ice coated snow-adhesion preventive sheet

    JP1995148879A

  • Coating material for water-repellent coating film and coating film obtained therefrom

    JP2000026844A

  • Solid easily slipping on snow and method for producing the same

    JP2003226867A

  • Ice / Snow accretion preventing rubber mat

    JP2003328308A