Anti-vibration rubber composition and anti-vibration rubber member

The vibration-proof rubber composition with diene rubber, hydrazide, and disulfide compounds addresses the challenge of achieving high heat resistance and low dynamic magnification, enhancing durability and vibration isolation.

JP7553258B2Active Publication Date: 2024-09-18SUMITOMO RIKO CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020055853
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-26
Publication Date
2024-09-18
Estimated Expiration
2040-03-26

AI Technical Summary

Technical Problem

Existing anti-vibration rubber compositions face challenges in achieving both high heat resistance and low dynamic magnification while maintaining durability, as reducing sulfur content for improved heat resistance leads to deterioration in durability and dynamic magnification.

Method used

A vibration-proof rubber composition comprising diene rubber, a hydrazide compound, a disulfide compound, and a sulfur-based vulcanizing agent, with specific ratios and combinations to form monosulfide and disulfide crosslinks, enhancing heat resistance and reducing dynamic magnification.

Benefits of technology

The composition achieves both high heat resistance and low dynamic magnification, improving durability and vibration isolation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553258000011
    Figure 0007553258000011
  • Figure 0007553258000004
    Figure 0007553258000004
  • Figure 0007553258000005
    Figure 0007553258000005
Patent Text Reader

Abstract

To provide a vibration-proof rubber composition and a vibration-proof rubber member capable of highly achieving both heat resistance and a low dynamic-to-static modulus ratio.SOLUTION: The vibration-proof rubber composition contains a rubber component comprising the following (A) and further contains the following components (B)-(E): (A) a diene rubber mainly composed of natural rubber; (B) a filler; (C) a hydrazide compound; (D) a specific disulfide compound; and (E) a sulfur-based vulcanizing agent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an anti-vibration rubber composition and an anti-vibration rubber member used for vibration isolation in vehicles such as automobiles and trains. [Background technology]

[0002] In the technical field of anti-vibration rubber, there is a demand for high durability and low dynamic ratios (reducing the value of dynamic ratio [dynamic spring constant (Kd) / static spring constant (Ks)]) to enhance quietness. Under such circumstances, a method for lowering the dynamic magnification by adding a hydrazide compound to a rubber composition has been explored (see, for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2010-121082 A [Patent Document 2] JP 2001-172435 A Summary of the Invention [Problem to be solved by the invention]

[0004] Meanwhile, anti-vibration rubber is also required to have heat resistance, taking into consideration use in harsh hot areas, etc. Conventionally, diene rubber such as natural rubber has been used as the polymer for anti-vibration rubber, and a sulfur-based vulcanizing agent is generally used as the vulcanizing agent, but this type of anti-vibration rubber has a problem with heat resistance. In the above-mentioned anti-vibration rubber, reducing the sulfur content is usually effective for improving the heat resistance, but reducing the sulfur content leads to deterioration in durability and dynamic magnification. For this reason, there has been a demand for a high degree of compatibility between heat resistance and low dynamic magnification while maintaining durability. However, as in the above-mentioned patent documents, simply adding a hydrazide compound to a rubber composition has not yet been able to sufficiently solve these problems.

[0005] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide an anti-vibration rubber composition and an anti-vibration rubber member that can achieve both high heat resistance and low dynamic magnification at the same time. [Means for solving the problem]

[0006] The present inventors have conducted extensive research to solve the above problems. In the course of their research, they came up with the idea of ​​using a specific disulfide compound having nitrogen-containing heterocyclic groups at both ends in combination with a hydrazide compound in a sulfur-vulcanized anti-vibration rubber composition containing a diene rubber mainly composed of natural rubber as the rubber component. The specific disulfide compound is more likely to undergo a disulfide cleavage reaction when used in combination with the hydrazide compound. They then found that the disulfide compound whose cleavage reaction has been promoted in the above manner can efficiently form monosulfide or disulfide crosslinks in natural rubber, thereby minimizing deterioration in durability and dynamic magnification and improving heat resistance. Furthermore, they found that the hydrazide compound can also reduce the dynamic magnification, thereby achieving the desired object, and thus arrived at the present invention.

[0007] That is, in order to achieve the above object, the present invention provides the following [1] to

[12] . [1] An anti-vibration rubber composition comprising the following rubber component (A) and the following components (B) to (E): (A) Diene rubber whose main component is natural rubber. (B) Filler. (C) Hydrazide compounds. (D) A disulfide compound represented by the following general formula (1): [ka] (E) Sulfur-based vulcanizing agents. [2] The vibration-proof rubber composition according to [1], wherein the content of the hydrazide compound (C) is within the range of 0.01 to 5.0 parts by weight per 100 parts by weight of the diene rubber (A). [3] The anti-vibration rubber composition according to [1] or [2], wherein the content of the disulfide compound (D) is within the range of 0.3 to 5.0 parts by weight per 100 parts by weight of the diene rubber (A). [4] The anti-vibration rubber composition according to any one of [1] to [3], wherein the weight ratio (C:D) of the hydrazide compound (C) to the disulfide compound (D) is 1:60 to 50:1. [5] The vibration-proof rubber composition according to any one of [1] to [4], wherein the hydrazide compound (C) is a dihydrazide compound represented by the following general formula (2): [ka] [6] The anti-vibration rubber composition according to any one of [1] to [4], wherein the hydrazide compound (C) is at least one selected from the group consisting of adipic dihydrazide and isophthalic dihydrazide. [7] The anti-vibration rubber composition according to any one of [1] to [6], wherein the disulfide compound (D) is at least one selected from 4,4'-dithiodimorpholine and dithiodicaprolactam. [8] The anti-vibration rubber composition according to any one of [1] to [7], wherein the content of the filler (B) is in the range of 5 to 100 parts by weight per 100 parts by weight of the diene rubber (A). [9] The anti-vibration rubber composition according to any one of [1] to [8], wherein the filler (B) is at least one selected from the group consisting of carbon black and silica.

[10] The vibration-proof rubber composition according to any one of [1] to [8], wherein the filler (B) is FEF grade carbon black.

[11] The anti-vibration rubber composition according to any one of [1] to [8], wherein the filler (B) comprises carbon black and silica, and the weight ratio thereof is carbon black:silica=8:2 to 2:8.

[12] An anti-vibration rubber member comprising a vulcanizate of the anti-vibration rubber composition according to any one of [1] to

[11] . Effect of the Invention

[0008] For the reasons described above, the anti-vibration rubber composition of the present invention can achieve both high heat resistance and low dynamic magnification. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Next, an embodiment of the present invention will be described in detail, although the present invention is not limited to this embodiment.

[0010] As described above, the anti-vibration rubber composition of the present invention contains the following rubber component (A) as well as the following components (B) to (E). (A) Diene rubber whose main component is natural rubber. (B) Filler. (C) Hydrazide compounds. (D) A disulfide compound represented by the following general formula (1): [ka] (E) Sulfur-based vulcanizing agents.

[0011] [Diene rubber (A)] As described above, in the anti-vibration rubber composition of the present invention, a diene rubber (A) containing natural rubber (NR) as a main component is used as the rubber component. Here, the term "main component" refers to a diene rubber (A) containing 50% by weight or more of natural rubber, and includes diene rubber (A) consisting only of natural rubber. By using natural rubber as a main component in this way, the strength and dynamic magnification are excellent. Examples of diene rubbers other than natural rubber include butadiene rubber (BR), styrene-butadiene rubber (SBR), chloroprene rubber (CR), isoprene rubber (IR), acrylonitrile-butadiene rubber (NBR), ethylene-propylene-diene rubber (EPDM), and butyl rubber (IIR). These may be used alone or in combination of two or more. Among these, butadiene rubber (BR) and isoprene rubber (IR) are more preferred because they can exhibit excellent vibration-proof rubber performance when used in combination with natural rubber.

[0012] [Filler (B)] As the filler (B), carbon black, silica, calcium carbonate, etc. are used alone or in combination. Carbon black and silica are preferred. Among them, carbon black is more preferred from the viewpoint of vibration characteristics. And, it is desirable that 50% by weight or more of the filler (B) is carbon black, and it is more desirable that 90% by weight or more of the filler (B) is carbon black.

[0013] As the carbon black, for example, various grades of carbon black such as SAF grade, ISAF grade, HAF grade, MAF grade, FEF grade, GPF grade, SRF grade, FT grade, MT grade, etc. are used. These may be used alone or in combination of two or more. Among them, FEF grade carbon black is preferably used from the viewpoint of vibration characteristics and fatigue resistance.

[0014] From the viewpoint of durability and low dynamic magnification, the carbon black preferably has an iodine adsorption of 10 to 110 mg / g and a DBP oil absorption (dibutyl phthalate oil absorption) of 20 to 180 ml / 100 g. The iodine adsorption amount of the carbon black is a value measured in accordance with JIS K 6217-1 (Method A), and the DBP oil absorption amount of the carbon black is a value measured in accordance with JIS K 6217-4.

[0015] As the silica, for example, wet silica, dry silica, colloidal silica, etc. are used. These may be used alone or in combination of two or more kinds.

[0016] From the viewpoint of achieving even higher durability and lower dynamic magnification, the BET specific surface area of ​​the silica is 50 to 320 m 2 / g, and 70 to 230m 2 It is more preferable that the molecular weight is / g. The BET specific surface area of ​​the silica was measured by, for example, degassing the sample at 200° C. for 15 minutes and then absorbing a mixed gas (N 2 The specific surface area can be measured using a BET specific surface area measuring device (Microdata Corporation, 4232-II) using a concentration of 100% NaCl, 70% NaCl, and 30% He.

[0017] When only carbon black and silica are used as the filler (B), the ratio by weight of carbon black:silica is preferably 8:2 to 2:8 from the viewpoint of fatigue resistance. From the same viewpoint, it is more preferable that the ratio of carbon black:silica is 4:6 to 2:8, and further preferably that the ratio of carbon black:silica is 3:7 to 2:8.

[0018] From the viewpoint of fatigue resistance, the total content of the filler (B) is preferably in the range of 5 to 100 parts by weight, more preferably in the range of 10 to 80 parts by weight, and even more preferably in the range of 15 to 75 parts by weight, per 100 parts by weight of the diene rubber (A).

[0019] [Hydrazide compounds (C)] As the hydrazide compound (C), a monohydrazide compound, a dihydrazide compound, etc. may be used alone or in combination of two or more kinds. Among these, the dihydrazide compounds represented by the following general formula (2) are preferably used because they can improve the dispersibility of the filler (B) and effectively suppress an increase in the dynamic magnification.

[0020] [ka]

[0021] In the above general formula (2), R is preferably an alkylene group having 4 to 12 carbon atoms or a phenylene group.

[0022] Specific examples of the monohydrazide compound include propionic acid hydrazide, thiocarbohydrazide, stearic acid hydrazide, salicylic acid hydrazide, 3-hydroxy-2-naphthoic acid hydrazide, p-toluenesulfonyl hydrazide, aminobenzhydrazide, and 4-pyridinecarboxylic acid hydrazide. These may be used alone or in combination of two or more. Among these, 3-hydroxy-2-naphthoic acid hydrazide is preferred from the viewpoint of reducing dynamic magnification.

[0023] Specific examples of the dihydrazide compound include adipic acid dihydrazide, isophthalic acid dihydrazide, phthalic acid dihydrazide, terephthalic acid dihydrazide, succinic acid dihydrazide, azelaic acid dihydrazide, sebacic acid dihydrazide, oxalic acid dihydrazide, and dodecanoic acid dihydrazide. These may be used alone or in combination of two or more. Among these, adipic acid dihydrazide and isophthalic acid dihydrazide are preferred from the viewpoint of reducing dynamic magnification.

[0024] From the viewpoint of lowering the dynamic magnification, the content of the hydrazide compound (C) is preferably 0.01 to 5.0 parts by weight, more preferably 0.1 to 5.0 parts by weight, and even more preferably 0.3 to 3.0 parts by weight, per 100 parts by weight of the diene rubber (A).

[0025] [Disulfide Compound (D)] As the disulfide compound (D), a disulfide compound represented by the following general formula (1) is used.

[0026] [ka]

[0027] In the above general formula (1), ring A and ring B may be the same or different. As described above, ring A and ring B are nitrogen-containing heterocyclic groups having 4 to 24 carbon atoms, preferably nitrogen-containing heterocyclic groups having 4 to 20 carbon atoms, and more preferably nitrogen-containing heterocyclic groups having 4 to 16 carbon atoms.

[0028] Examples of the disulfide compound (D) include 4,4'-dithiodimorpholine (DTDM) shown in the following chemical formula (1-1) and dithiodicaprolactam (DTDC) shown in the following chemical formula (1-2). These may be used alone or in combination of two or more. Among them, 4,4'-dithiodimorpholine and dithiodicaprolactam are preferred from the viewpoint of heat resistance and the like.

[0029] [ka]

[0030] [ka]

[0031] From the viewpoint of solving the problems of the present invention, it is preferable that the hydrazide compound (C) and the disulfide compound (D) are contained in a weight ratio of hydrazide compound (C):disulfide compound (D)=1:60 to 50:1. From the same viewpoint, it is more preferable that the hydrazide compound (C):disulfide compound (D) is contained in a weight ratio of 1:4 to 50:3, and even more preferable that the hydrazide compound (C):disulfide compound (D) is contained in a weight ratio of 1:4 to 10:1.

[0032] From the viewpoint of solving the problems of the present invention, the content of the disulfide compound (D) is preferably 0.3 to 5.0 parts by weight, more preferably 0.5 to 5.0 parts by weight, and even more preferably 0.5 to 3.0 parts by weight, relative to 100 parts by weight of the diene rubber (A).

[0033] [Sulfur-based vulcanizing agent (E)] Examples of the sulfur-based vulcanizing agent (E) include sulfur-containing compounds such as sulfur (powdered sulfur, precipitated sulfur, insoluble sulfur) (however, disulfide compounds including the component (D) and compounds that do not function as vulcanizing agents (vulcanization accelerators, vulcanization aids, etc.) are excluded). These may be used alone or in combination of two or more kinds.

[0034] The content of the sulfur-based vulcanizing agent (E) is preferably in the range of 0.05 to 5 parts by weight, more preferably in the range of 0.3 to 3.5 parts by weight, and further preferably in the range of 0.5 to 3 parts by weight, based on 100 parts by weight of the diene rubber (A). That is, if the content of the sulfur-based vulcanizing agent (E) is too low, the vulcanization reactivity tends to deteriorate, whereas if the content of the sulfur-based vulcanizing agent (E) is too high, the rubber physical properties (breaking strength, breaking elongation) tend to deteriorate.

[0035] In addition, in the anti-vibration rubber composition of the present invention, in addition to the essential components (A) to (E), it is also possible to appropriately contain a silane coupling agent, a vulcanization accelerator, a vulcanization aid, an antioxidant, a process oil, etc., as necessary.

[0036] Examples of the silane coupling agent include mercapto-based silane coupling agents, sulfide-based silane coupling agents, amine-based silane coupling agents, epoxy-based silane coupling agents, vinyl-based silane coupling agents, etc. These are used alone or in combination of two or more. Among them, when the silane coupling agent is a mercapto-based silane coupling agent or a sulfide-based silane coupling agent, the vulcanization density increases, and it is particularly effective in low dynamic magnification and durability, so it is preferable.

[0037] Examples of the mercapto-based silane coupling agent include 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, etc. These may be used alone or in combination of two or more kinds.

[0038] Examples of the sulfide-based silane coupling agent include bis-(3-(triethoxysilyl)-propyl)-disulfide, bis(3-triethoxysilylpropyl)trisulfide, bis-(3-(triethoxysilyl)-propyl)-tetrasulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(3-triethoxysilylpropyl)disulfide, and 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamoyltetrasulfide. rusulfide, 3-triethoxysilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, 2-trimethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, 3-trimethoxysilylpropyl benzothiazolyl tetrasulfide, 3-triethoxysilylpropyl benzothiazole tetrasulfide, 3-triethoxysilylpropyl methacrylate monosulfide, 3-trimethoxysilylpropyl methacrylate monosulfide, etc. These may be used alone or in combination of two or more.

[0039] Examples of the amine-based silane coupling agent include 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-(N-phenyl)aminopropyltrimethoxysilane, etc. These may be used alone or in combination of two or more.

[0040] Examples of the epoxy-based silane coupling agent include 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, etc. These may be used alone or in combination of two or more.

[0041] Examples of the vinyl-based silane coupling agent include vinyltriethoxysilane, vinyltrimethoxysilane, vinyltris(β-methoxyethoxy)silane, vinyldimethylchlorosilane, vinyltrichlorosilane, vinyltriisopropoxysilane, vinyltris(2-methoxyethoxy)silane, etc. These may be used alone or in combination of two or more.

[0042] The content of these silane coupling agents is preferably 0.5 to 20 parts by weight, more preferably 1.0 to 10 parts by weight, based on 100 parts by weight of the diene rubber (A) because they are excellent in low dynamic magnification, durability, and the like.

[0043] Examples of the vulcanization accelerator include thiazole-based, sulfenamide-based, thiuram-based, aldehyde ammonia-based, aldehyde amine-based, guanidine-based, and thiourea-based vulcanization accelerators. These are used alone or in combination of two or more. Among these, sulfenamide-based vulcanization accelerators are preferred because of their excellent crosslinking reactivity.

[0044] The content of the vulcanization accelerator is preferably in the range of 0.1 to 10 parts by weight, and particularly preferably in the range of 0.3 to 5 parts by weight, based on 100 parts by weight of the diene rubber (A).

[0045] Examples of the thiazole-based vulcanization accelerator include dibenzothiazyl disulfide (MBTS), 2-mercaptobenzothiazole (MBT), 2-mercaptobenzothiazole sodium salt (NaMBT), 2-mercaptobenzothiazole zinc salt (ZnMBT), etc. These may be used alone or in combination of two or more.

[0046] Examples of the sulfenamide vulcanization accelerator include N-oxydiethylene-2-benzothiazolylsulfenamide (NOBS), N-cyclohexyl-2-benzothiazolylsulfenamide (CBS), Nt-butyl-2-benzothiazoylsulfenamide (BBS), N,N'-dicyclohexyl-2-benzothiazoylsulfenamide, etc. These may be used alone or in combination of two or more.

[0047] Examples of the thiuram vulcanization accelerator include tetramethylthiuram disulfide (TMTD), tetraethylthiuram disulfide (TETD), tetrabutylthiuram disulfide (TBTD), tetrakis(2-ethylhexyl)thiuram disulfide (TOT), tetrabenzylthiuram disulfide (TBzTD), etc. These may be used alone or in combination of two or more.

[0048] Examples of the vulcanization aid include stearic acid, magnesium oxide, etc. These may be used alone or in combination of two or more kinds.

[0049] The content of the vulcanization aid is preferably in the range of 0.1 to 10 parts by weight, and particularly preferably in the range of 0.3 to 7 parts by weight, based on 100 parts by weight of the diene rubber (A).

[0050] Examples of the antiaging agent include carbamate-based antiaging agents, phenylenediamine-based antiaging agents, phenol-based antiaging agents, diphenylamine-based antiaging agents, quinoline-based antiaging agents, imidazole-based antiaging agents, waxes, etc. These may be used alone or in combination of two or more kinds.

[0051] The content of the antioxidant is preferably in the range of 0.5 to 15 parts by weight, more preferably 1 to 10 parts by weight, and particularly preferably 1 to 8 parts by weight, based on 100 parts by weight of the diene rubber (A).

[0052] Examples of the process oil include naphthenic oil, paraffinic oil, aromatic oil, etc. These may be used alone or in combination of two or more kinds.

[0053] The content of the process oil is preferably in the range of 1 to 35 parts by weight, more preferably 3 to 30 parts by weight, and particularly preferably 3 to 20 parts by weight, based on 100 parts by weight of the diene rubber (A).

[0054] [Method for preparing anti-vibration rubber composition] Here, the vibration-proof rubber composition of the present invention can be prepared by kneading the essential components (A) to (E) and, if necessary, the other materials listed above, using a kneading machine such as a kneader, a Banbury mixer, an open roll, a twin-screw mixer, etc. In particular, it is preferable to knead all the materials except the vulcanizing agent and the vulcanization accelerator at the same time, and then add the vulcanizing agent and the vulcanization accelerator.

[0055] The anti-vibration rubber composition of the present invention thus obtained can be molded in a mold at high temperature (150 to 170°C) for 5 to 30 minutes by injection molding or the like to produce the desired anti-vibration rubber member (vulcanizate).

[0056] Anti-vibration rubber members made of a vulcanizate of the anti-vibration rubber composition of the present invention are preferably used as components for engine mounts, stabilizer bushes, suspension bushes, motor mounts, subframe mounts, etc., used in automobile vehicles, etc. In particular, since they have a low dynamic magnification and excellent heat resistance and durability, they can be advantageously used for components for motor mounts, suspension bushes, subframe mounts, etc. (anti-vibration rubber members for electric vehicles) for electric vehicles (including electric vehicles (EVs), fuel cell vehicles (FCVs), plug-in hybrid vehicles (PHVs), hybrid vehicles (HVs), etc.) that use electric motors as their power source. In addition to the above applications, the material can also be used in vibration dampers for computer hard disks, vibration dampers for general home appliances such as washing machines, and vibration control devices and seismic isolation devices such as architectural vibration control walls and vibration control dampers in the construction and housing fields. EXAMPLES

[0057] Next, examples will be described together with comparative examples, but the present invention is not limited to these examples.

[0058] First, prior to the Examples and Comparative Examples, the materials shown below were prepared.

[0059] [NR] Natural rubber

[0060] [IR] Nipol IR2200, manufactured by Zeon Corporation

[0061] [BR] Nipol 1220, manufactured by Zeon Corporation

[0062] [Zinc oxide] Zinc oxide type 2, manufactured by Sakai Chemical Industry Co., Ltd.

[0063] [Stearic acid] Beads Stearic Acid Sakura, NOF Corporation

[0064] [Anti-aging agent] Antigen 6C, manufactured by Sumitomo Chemical Co., Ltd.

[0065] [Carbon black (i)] FEF grade carbon black (Seat SO, manufactured by Tokai Carbon Co., Ltd., iodine adsorption: 44 mg / g, DBP oil absorption: 115 ml / 100 g)

[0066] [Carbon black (II)] FT-class carbon black (Seat TA, manufactured by Tokai Carbon Co., Ltd., iodine adsorption: 18 mg / g, DBP oil absorption: 42 ml / 100 g)

[0067] [Silica(i)] Nipsil VN3, manufactured by Tosoh Silica Corporation, BET specific surface area 200m 2 / g

[0068] [Silica(II)] Nipsil ER, manufactured by Tosoh Silica Corporation, BET specific surface area 100m 2 / g

[0069] [Process oil] Sansen 410, manufactured by Nippon San Oil Co., Ltd.

[0070] [Hydrazide compounds (i)] Isophthalic dihydrazide (IDH), manufactured by Otsuka Chemical Co., Ltd.

[0071] [Hydrazide compound (ii)] Adipic dihydrazide (ADH), manufactured by Otsuka Chemical Co., Ltd.

[0072] [Hydrazide compound (iii)] 3-Hydroxy-2-naphthoic acid hydrazide (HNH), manufactured by Otsuka Chemical Co., Ltd.

[0073] [Silane coupling agents] NXT Z45, manufactured by MOMENTIVE

[0074] [Disulfide compound (i)] Dithiodicaprolactam (DTDC) (RHENOGRAN CLD-80, LANXESS)

[0075] [Disulfide compound (ii)] 4,4'-Dithiodimorpholine (DTDM) (Balnoc R, manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)

[0076] [Vulcanization accelerator (i)] Suncellar CZ-G, manufactured by Sanshin Chemical Industry Co., Ltd.

[0077] [Vulcanization accelerator (ii)] Suncellar TT-G, manufactured by Sanshin Chemical Industry Co., Ltd.

[0078] [sulfur] Sulfur, produced by Karuizawa Smelter

[0079] [Examples 1 to 15, Comparative Examples 1 and 2] The above materials were mixed and kneaded in the ratios shown in Tables 1 and 2 below to prepare anti-vibration rubber compositions. The above kneading was carried out by first mixing the materials other than the vulcanizing agent (sulfur) and vulcanization accelerator at 140°C for 5 minutes using a Banbury mixer, then mixing the vulcanizing agent and vulcanization accelerator and kneading the mixture at 60°C for 5 minutes using an open roll.

[0080] The vibration-proof rubber compositions of the Examples and Comparative Examples thus obtained were used to evaluate the various properties according to the following criteria, and the results are shown in Tables 1 and 2 below.

[0081] ≪Dynamic magnification≫ Each vibration-proof rubber composition was press-molded (vulcanized) under the condition of 160°C x 20 minutes to prepare a test piece. The static spring constant (Ks) of the test piece was measured in accordance with JIS K 6394. The storage spring constant (Kd100) of the test piece at a frequency of 100 Hz was also determined in accordance with JIS K 6385. The value obtained by dividing the storage spring constant (Kd100) by the static spring constant (Ks) was defined as the dynamic magnification (Kd100 / Ks). In the following Tables 1 and 2, the measured values ​​of the dynamic magnification in each Example and Comparative Example are shown as index values, with the measured value of the dynamic magnification (Kd100 / Ks) in Comparative Example 1 being taken as 100. Values ​​less than 95% of the dynamic magnification in Comparative Example 1 were evaluated as "◯", and values ​​95% or more were evaluated as "X".

[0082] ≪Heat resistance≫ Each vibration-proof rubber composition was press-molded (vulcanized) under the condition of 160°C x 20 minutes to prepare a test piece. Then, in accordance with JIS K 6251, the initial elongation at break (Eb) was measured in an atmosphere of 23°C. Next, the above-prepared test piece was left in a high-temperature atmosphere of 100°C for 70 hours (heat aging test), and then the elongation at break (Eb) was measured in the same manner as above. Then, the reduction rate (ΔEb) of the elongation at break after the heat aging test relative to the initial elongation at break was calculated. In the heat resistance evaluation, a value of the rate of decrease (ΔEb) of less than 25% was evaluated as "○", a value of 25% or more and less than 27% was evaluated as "△", and a value of 27% or more was evaluated as "×".

[0083] [Table 1]

[0084] [Table 2]

[0085] From the results in Tables 1 and 2 above, it was found that the anti-vibration rubber compositions of the examples achieved both low dynamic magnification and heat resistance. In contrast, the anti-vibration rubber composition of Comparative Example 1 contains the specific disulfide compound used in the present invention but does not contain a hydrazide compound, resulting in a higher dynamic magnification ratio than those of the Examples. The anti-vibration rubber composition of Comparative Example 2 contains the same hydrazide compound as in Example 1 but does not contain the specific disulfide compound used in the present invention, resulting in a lower heat resistance than that of Example 1, and also a lower dynamic magnification ratio that was not sufficient compared to all the Examples. [Industrial Applicability]

[0086] The anti-vibration rubber composition of the present invention is preferably used as a material for components (anti-vibration rubber members) such as engine mounts, stabilizer bushings, suspension bushings, motor mounts, subframe mounts, etc. used in automobile vehicles, but it can also be used as a material for components (anti-vibration rubber members) such as vibration dampers for computer hard disks, vibration dampers for general home appliances such as washing machines, and vibration control (vibration control) devices and seismic isolation devices such as architectural vibration control walls and vibration control (vibration control) dampers in the construction and housing fields.

Claims

1. A vibration-proof rubber composition comprising the following rubber component (A) and the following components (B) to (E), wherein the content of component (C) is within the range of 0.01 to 5.0 parts by weight per 100 parts by weight of component (A), the content of component (D) is within the range of 0.3 to 1 part by weight per 100 parts by weight of component (A), and the weight ratio of component (C) to component (D) (C:D) is 1:60 to 50:

1. (A) Diene rubber whose main component is natural rubber. (B) Filler. (C) Hydrazide compounds. (D) A disulfide compound represented by the following general formula (1): 【Chemistry 1】 (E) Sulfur-based vulcanizing agents.

2. 2. The vibration-proof rubber composition according to claim 1, wherein the content of said hydrazide compound (C) is in the range of 0.1 to 5.0 parts by weight per 100 parts by weight of said diene rubber (A).

3. 3. The anti-vibration rubber composition according to claim 1, wherein the content of said disulfide compound (D) is in the range of 0.5 to 1 part by weight per 100 parts by weight of said diene rubber (A).

4. The vibration-proof rubber composition according to any one of claims 1 to 3, wherein the hydrazide compound (C) is a dihydrazide compound represented by the following general formula (2): 【Chemistry 2】

5. 4. The anti-vibration rubber composition according to claim 1, wherein the hydrazide compound (C) is at least one selected from the group consisting of adipic acid dihydrazide and isophthalic acid dihydrazide.

6. 6. The anti-vibration rubber composition according to claim 1, wherein the disulfide compound (D) is at least one selected from the group consisting of 4,4'-dithiodimorpholine and dithiodicaprolactam.

7. 7. The vibration-proof rubber composition according to claim 1, wherein the content of the filler (B) is in the range of 5 to 100 parts by weight per 100 parts by weight of the diene rubber (A).

8. 8. The anti-vibration rubber composition according to claim 1, wherein the filler (B) is at least one selected from the group consisting of carbon black and silica.

9. The vibration-proof rubber composition according to any one of claims 1 to 7, wherein the filler (B) is FEF grade carbon black.

10. 8. The vibration-proof rubber composition according to claim 1, wherein the filler (B) comprises carbon black and silica, and the weight ratio of carbon black:silica is from 8:2 to 2:

8.

11. 11. An anti-vibration rubber member comprising a vulcanizate of the anti-vibration rubber composition according to claim 1.

Citation Information

Patent Citations

  • Rubber ocmposition having low heat-generation

    JP1993051486A

  • Method for producing rubber composition and pneumatic tire

    JP2001172435A

  • Rubber vibration insulator

    JP2006143860A

  • Rubber composition

    JP2010121082A

  • JPP6644962B