Polishing pad and method of manufacturing same
The polishing pad with a cushion and adhesive layer, featuring an uneven shape and through holes, addresses the challenge of uneven polishing by uniformly polishing flat and curved surfaces, enhancing surface finish quality.
Patent Information
- Application Number
- JP2020159098
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-23
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-09-23
AI Technical Summary
Existing polishing methods fail to uniformly polish both flat and curved surfaces without causing unevenness due to overpolishing, particularly at curved portions, as the polishing layer expands and creates repulsion forces.
A polishing pad with a cushion layer having an uneven shape and a polishing layer with through holes, bonded via an adhesive layer, allowing the polishing layer to deform and follow the surface contours, reducing unevenness by distributing pressure evenly.
The polishing pad effectively polishes both flat and curved surfaces simultaneously, minimizing overpolishing and unevenness by allowing the polishing layer to conform to the object's shape, ensuring uniformity and reducing surface roughness.
Smart Images

Figure 0007553299000004 
Figure 0007553299000003 
Figure 0007553299000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a polishing pad and a method for manufacturing the same. [Background technology]
[0002] In recent years, designs that curve the edges connecting the front and side of electronic devices such as smartphones have been used. The curved parts are formed by chamfering using a router or other processing method, but they leave cutting marks that need to be removed by polishing.
[0003] For example, Patent Document 1 discloses a method of polishing a curved portion by using a polishing pad consisting of an elastic pad having a polishing surface bonded to a deformable base layer, and pressing a workpiece against the polishing pad to bring the polishing surface into line with the curved portion. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5789634 Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the method described in Patent Document 1, when polishing the flat portion, the polishing surface does not fit the entire curved portion, so in addition to polishing the flat portion, it was necessary to polish the curved portion using a dedicated carrier. If the pressing force is increased to fit the entire curved portion, there is a concern that the polishing layer at the contact point with the curved portion will be greatly elongated along with the deformation of the base layer when the workpiece is pressed against the polishing pad, resulting in uneven elongation of the entire polishing layer. Therefore, a repulsive force (return force) is likely to be generated in the polishing layer at the contact point with the curved portion, and the pressing force on the curved portion in particular will be large, resulting in a problem of uneven polishing due to over-polishing of the curved portion.
[0006] One aspect of the present invention aims to provide a polishing pad and a method for manufacturing the same that can simultaneously polish flat and curved portions of an object to be polished and reduce uneven polishing caused by over-polishing of the curved portions. [Means for solving the problem]
[0007] In order to solve the above-mentioned problems, a polishing pad according to one embodiment of the present invention is a polishing pad formed by laminating a cushion layer, an adhesive layer, and a polishing layer in this order, wherein the cushion layer has a through hole and has an uneven shape consisting of a plurality of convex portions and a plurality of concave portions on the surface facing the polishing layer, the adhesive layer has a plurality of through holes that penetrate from the contact surface with the cushion layer to the contact surface with the polishing layer, the polishing layer has a through hole and is bonded to the cushion layer via the adhesive layer along the convex portions and the concave portions, thereby having an uneven shape consisting of a plurality of convex portions and a plurality of concave portions on its surface, and the uneven shape of the polishing layer is a curved shape, and is formed so that the convex portions and the concave portions are arranged in a regular pattern.
[0008] In order to solve the above-mentioned problems, one embodiment of the present invention provides a method for manufacturing a polishing pad, which includes a lamination process in which a cushion layer having an uneven shape consisting of a plurality of convex portions and a plurality of concave portions and a polishing layer having an uneven shape consisting of a plurality of convex portions and a plurality of concave portions and a polishing layer having an uneven shape consisting of a plurality of convex portions and a plurality of concave portions are laminated together via an adhesive layer so that the polishing layer conforms to the uneven shape, and a through hole forming process in which holes are drilled from the polishing surface side of the bonded laminate to form through holes that penetrate from the adhesive surface of the adhesive layer with the cushion layer to the polishing surface of the polishing layer, wherein the uneven shape is a curved shape and is formed so that the convex portions and the concave portions are arranged in a regular pattern. Effect of the Invention
[0009] According to one aspect of the present invention, it is possible to provide a polishing pad and a manufacturing method thereof that are capable of simultaneously polishing flat and curved portions of an object to be polished and that can reduce uneven polishing caused by over-polishing of the curved portions. [Brief description of the drawings]
[0010] [Figure 1] 1 is a cross-sectional view showing a configuration of a polishing pad according to one embodiment of the present invention. [Diagram 2] 1 is a cross-sectional view showing a state in which a polishing pad according to an embodiment of the present invention is used. [Diagram 3] 1 is a schematic diagram showing the arrangement pattern of the concave-convex shapes of a polishing layer when a polishing pad according to one embodiment of the present invention is viewed in plan from the polishing surface side. FIG. [Figure 4] 4A to 4C are schematic diagrams showing other arrangement patterns of the concave and convex shapes of the polishing layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] [Polishing pad] Fig. 1 is a partial cross-sectional view showing the configuration of a polishing pad 10 according to this embodiment. As shown in Fig. 1, the polishing pad 10 has a configuration in which a cushion layer 11, an adhesive layer 12, and a polishing layer 13 are laminated in this order.
[0012] The cushion layer 11 has an uneven shape consisting of a plurality of convex portions 111 and a plurality of concave portions 112 on the side facing the polishing layer 13. The polishing layer 13 is bonded to the cushion layer 11 via the adhesive layer 12 along the uneven shape of the cushion layer 11. As a result, an uneven shape consisting of a plurality of convex portions 131 and a plurality of concave portions 132 is formed on the surface of the polishing layer 13. Although details will be described later, when the polishing pad 10 is viewed in plan from the polishing surface side, the convex portions 131 and the concave portions 132 in the polishing pad 10 are formed so as to be alternately arranged vertically and horizontally (FIG. 3 described later). For convenience of explanation, the convex portions of the adjacent rows seen in the back are shown by dashed lines.
[0013] FIG. 2 is a cross-sectional view showing a state where polishing is performed using the polishing pad 10. The polishing pad 10 of this embodiment is preferably used in a method of pressing the polishing pad 10 from above the object to be polished to perform polishing. Therefore, in this specification, a method of pressing the polishing pad 10 from above the object to be polished is described as an example, but the use form of the polishing pad 10 is not limited to this. As shown in FIG. 2, the polishing table 20 has a polishing slurry supply unit 21 for supplying polishing slurry. The polishing pad 10 is attached to the polishing table 20 of the polishing device 1 via the polishing table side adhesive layer 30. The polishing table side adhesive layer 30 has a plurality of through holes 31 that penetrate from the contact surface with the polishing table 20 to the adhesive surface with the cushion layer 11. The through holes 31 of the polishing table side adhesive layer 30 communicate with the polishing slurry supply unit 21. In addition, the polishing pad 10 is pressed from above against the object to be polished W placed on the spacer 40 attached to the holding table 50. Here, the portion to be polished of the workpiece W includes a flat portion W1 and a curved portion W2. As shown in Fig. 2, in polishing the workpiece W, the polishing pad 10 is pressed from above against the workpiece W placed on the spacer 40, and the polishing pad 10 is deformed into a shape that follows the shape of the workpiece W. When the polishing pad 10 is released from pressing against the workpiece W, it returns to its original shape.
[0014] Since the polishing pad 10 is configured such that the polishing layer 13 is bonded along the cushion layer 11 having an uneven shape, the uneven shape of the polishing layer 13 can be deformed to follow the shape of the object W to be polished, even if the surface to be polished is a curved surface. In other words, the uneven shape of the convex parts 131 and the concave parts 132 disappears and the polishing layer 13 deforms to be substantially the same as the shape of the object W to be polished. As a result, the polishing layer 13 comes into contact with the object W to be polished not only at the convex parts 131 but also at the surfaces of the concave parts 132, and not only at the convex parts 131 but also at the surfaces of the concave parts 132 can contribute to the polishing of the object W to be polished. In this state, by rotating the polishing pad 10 while supplying the polishing slurry, the flat part W1 and the curved part W2 of the object W to be polished can be polished at the same time. Therefore, the polishing pad 10 is suitable for use in polishing the object W to be polished having a curved surface. In addition, since the polishing layer 13 is arranged along the uneven shape, the area between the convex portion 131 and the concave portion 132 of the polishing layer 13 is relatively more stretchable than the apexes of the convex portion 131 and the concave portion 132 of the polishing layer 13, and the bias in tension is alleviated. Therefore, it is possible to reduce uneven polishing caused by over-polishing of the curved portion W2 of the workpiece W.
[0015] As shown in FIG. 1, in the polishing pad 10, the uneven shape of the cushion layer 11 is a curved shape. As a result, the uneven shape of the polishing layer 13 is also a curved shape. That is, the convex portion 111 and the concave portion 112 of the cushion layer 11, and the convex portion 131 and the concave portion 132 of the polishing layer 13 are all curved shapes. As a result, when the polishing object W is pressed against the polishing pad 10, the polishing surface is easily deformed into a shape that follows the shape of the curved portion W2, and is easily contacted with the curved portion W2. Therefore, when the polishing pad 10 is pressed against the polishing object W, the polishing surface of the polishing pad 10 can be made to have a shape that follows the shape of the curved portion W2 of the polishing object W. Therefore, it is possible to reduce uneven polishing caused by over-polishing of the curved portion W2 of the polishing object W. In addition, since the uneven shape of the cushion layer 11 is a curved shape, when the polishing pad 10 is manufactured, it is easy to bond the polishing layer 13 without any gaps along the uneven shape of the cushion layer 11.
[0016] The shape of the convex portion 131 is an inverted shape of the concave portion 132. The cross-sectional shape of the convex portion 131 including the apex of the convex portion 131 is a curved shape that is linearly symmetrical with respect to an axis of symmetry including the apex. For example, the cross-sectional shape may be a circular or elliptical arc, a parabola, and a sine curve (sine curve). Therefore, in this embodiment, the shape of the polishing surface in a cross section including the apex of the convex portion 131 and the bottom point of the concave portion 132 is a wave-shaped shape formed by a curve. When the shape of the convex portion 131 is not an inverted shape of the concave portion 132, and the concave portion 132 is a curved shape and the convex portion 131 is a square pyramid or a prism having corners, or when the convex portion 131 is a curved shape and the concave portion 132 is a square pyramid or a prism having corners, polishing stress is likely to concentrate at the corners, and the corners may be torn off or the polished object W may be scratched. The amount of sinking may also be limited if the curved surface is not a continuous uneven shape, but if there is a flat surface between the convex portion 131 and the concave portion 132. If the shape of the convex portion 131 is an inverted shape of the concave portion 132, there is no inflection point, and therefore the polishing pad 10 can move smoothly relative to the workpiece W, which is preferable.
[0017] FIG. 3 is a schematic diagram showing an arrangement pattern of the concave-convex shape of the polishing layer 13 when the polishing pad 10 is viewed in plan from the polishing surface side. In the arrangement pattern (pattern A) shown in FIG. 3, all the convex parts 131 and the concave parts 132 are arranged in a regular single arrangement in the polishing layer 13. In pattern A, the convex parts 131 and the concave parts 132 are arranged alternately in the vertical and horizontal directions. That is, the convex parts 131 are arranged in a staggered pattern. Since the concave-convex shape of the polishing layer 13 is such a single arrangement pattern, when the polished object W is sunk into the polishing pad 10, it is possible to uniformly distribute the polishing pressure applied to the curved part W2 of the polished object W. Therefore, it is possible to reduce uneven polishing caused by over-polishing of the curved part W2 of the polished object W.
[0018] Another embodiment of the arrangement pattern of the uneven shape is shown in FIG. 4. FIG. 4 is a schematic diagram showing another arrangement pattern (pattern B) of the uneven shape of the polishing layer 13 when the polishing pad 10 is viewed in plan from the polishing surface side. As shown in FIG. 4, pattern B is a composite arrangement in which a regular pattern B1 and a regular pattern B2 different from pattern B1 are alternately combined in the vertical direction in the polishing layer 13. Pattern B1 is formed so that the convex parts 131 and the concave parts 132 are alternately arranged in the vertical and horizontal directions. Pattern B2 is formed so that the convex parts 131' having a shape different from the shape of the convex parts 131 and the concave parts 132' having a shape different from the shape of the concave parts 132 are alternately arranged in the horizontal direction. In this way, the uneven shape in the polishing layer 13 is not limited to the case where the entire surface is formed in a single pattern, and another pattern may exist at a certain period. In other words, the uneven shape in the polishing layer 13 may be a single arrangement or a composite arrangement as long as the convex parts 131 and the concave parts 132 are arranged in a regular pattern.
[0019] The pitch P, which is the distance between the apexes of the adjacent convex portions 131 across one concave portion 132, may be set according to the thickness of the workpiece W and the curvature of the curved surface portion. The pitch P is preferably 5 mm or more, more preferably 10 mm or more, and more preferably 15 mm or more. The pitch P is preferably 50 mm or less, and more preferably 30 mm or less. The height H of the apex of the convex portion 131 when the bottom point of the concave portion 132 in the thickness direction is taken as the starting point may also be set according to the thickness of the workpiece W and the curvature of the curved surface portion. The height H is preferably 0.5 to 90% of the thickness of the polishing pad, more preferably 1 to 70%, and even more preferably 10 to 60%. Specifically, it is preferably 0.5 mm or more, more preferably 1 mm or more, and even more preferably 1.5 mm or more. The height H is preferably 30 mm or less, more preferably 20 mm or less, and even more preferably 15 mm or less. This makes it possible to reduce uneven polishing caused by over-polishing of the curved portion W2 of the workpiece W.
[0020] The polishing layer 13 is a layer that polishes the workpiece W, and has extensibility that allows it to be bonded along the uneven shape of the cushion layer 11. For example, a wet-formed polyurethane resin sheet, a nonwoven fabric, a woven fabric, a polyurethane resin molded body, etc. can be used as the polishing layer 13. Among these, a wet-formed polyurethane resin sheet is preferable because it has appropriate elasticity.
[0021] The polishing layer 13 has through holes that communicate from the contact surface of the polishing layer 13 with the adhesive layer 12 to the polishing surface. This allows the polishing slurry that has passed through the through holes 121 of the adhesive layer 12 to pass through the through holes of the polishing layer and reach the polishing surface. These through holes are formed by the communication of air bubbles that are generated when the polishing layer 13 is formed by a wet film formation method.
[0022] The polishing layer 13 also has a plurality of through holes 133 penetrating from the contact surface with the adhesive layer 12 to the polishing surface. When the polishing pad 10 is pressed, not only the polishing portion of the polishing layer 13 (the portion of the polishing layer 13 other than the through holes) is expanded, but also the inner wall portion surrounding the through holes 133 is deformed. Therefore, in the polishing layer 13 having the through holes 133, the expansion of the polishing portion is alleviated by the amount of the deformation of the inner wall portion of the through holes 133. Therefore, the polishing layer 13 having the through holes 133 is more easily deformed than a polishing layer without a through hole. This allows the polishing pad 10 to further improve its ability to follow the curved portion W2 of the polished object W.
[0023] The density of the through holes 133 in the polishing layer 13 is set to 0.5 / cm from the viewpoint of supplying a sufficient amount of polishing slurry and improving the ability to conform to the curved portion W2 of the workpiece W. 2 It is preferable that the number of particles is 1.0 or more per cm. 2 More preferably, it is 1.5 pieces / cm or more. 2 From the viewpoint of increasing the polishing power, the density of the through holes 133 in the polishing layer 13 is preferably 50 holes / cm. 2 Preferably, 30 pieces / cm or less. 2 More preferably, 10 particles / cm or less. 2 It is even more preferable that:
[0024] The diameter of the through holes 133 in the polishing layer 13 is preferably 0.05 mm or more, and more preferably 0.1 mm or more, from the viewpoint of sufficiently supplying the polishing slurry and improving the ability to follow the curved portion W2 of the workpiece W. Moreover, the diameter of the through holes 133 in the polishing layer 13 is preferably 2.0 mm or less, and more preferably 1.0 mm or less, from the viewpoint of improving the polishing power.
[0025] From the viewpoint of uniformly supplying the polishing slurry to the workpiece W, it is preferable that the through holes 133 of the polishing layer 13 are arranged in a regular pattern when viewed from the polishing surface side. The arrangement pattern of the through holes 133 of the polishing layer 13 may be, for example, a lattice pattern, a radial pattern, a concentric circle pattern, a spiral pattern, a staggered pattern, etc.
[0026] The thickness of the abrasive layer 13 may be, for example, 0.5 mm or more, alternatively 0.7 mm or more, and may be 5.0 mm or less, alternatively 3.0 mm or less.
[0027] The Shore A hardness of the abrasive layer 13 may be, for example, 8 or more, or 15 or more, and 40 or less, or 30 or less. The Shore A hardness is measured by preparing a sample piece (10 cm x 10 cm) and using an A-type hardness meter (Japanese Industrial Standards, JIS K 7311).
[0028] The apparent density of the polishing layer 13 is 0.1 g / cm 3 More than 0.4g / cm 3 It can be the following:
[0029] The adhesive layer 12 is a layer that bonds the polishing layer 13 and the cushion layer. The adhesive layer 12 is not particularly limited and may be a conventionally known adhesive, and may be a pressure-sensitive or heat-sensitive adhesive. For example, pressure-sensitive adhesives include silicone adhesives, modified silicone adhesives, acrylic adhesives, and rubber adhesives, while heat-sensitive adhesives include thermoplastic adhesives such as acrylic, nitrile, nitrile rubber, polyamide, polyurethane, and polyester.
[0030] The adhesive layer 12 has a plurality of through holes 121 penetrating from the contact surface with the cushion layer 11 to the contact surface with the polishing layer 13. This allows the polishing slurry supplied from the cushion layer 11 side to reach the polishing surface of the polishing layer 13, and the polishing slurry can be evenly supplied to the polishing surface.
[0031] The density of the through holes 121 in the adhesive layer 12 is set to 0.5 / cm from the viewpoint of supplying a sufficient amount of polishing slurry. 2 It is preferable that the number of particles is 1.0 or more per cm. 2 More preferably, it is 1.5 pieces / cm or more. 2 From the viewpoint of increasing the adhesive strength of the adhesive layer 12 to the cushion layer 11 and to the polishing layer 13, the density of the through holes 121 in the adhesive layer 12 is preferably 50 holes / cm. 2 Preferably, 30 pieces / cm or less. 2 More preferably, 10 particles / cm or less. 2 It is even more preferable that:
[0032] From the viewpoint of supplying the polishing slurry sufficiently, the diameter of the through hole 121 of the adhesive layer 12 is preferably 0.05 mm or more, more preferably 0.1 mm or more. The diameter of the through hole 121 of the adhesive layer 12 is preferably 2.0 mm or less, more preferably 1.0 mm or less. This makes it difficult for the polishing slurry to be sent to the through hole 121 of the adhesive layer 12 when the polishing pad 10 is not pressed, and the polishing slurry can be maintained in a state where it is held in the cushion layer 11. In addition, the adhesive strength of the adhesive layer 12 to the cushion layer 11 and the adhesive strength to the polishing layer 13 can be increased.
[0033] From the viewpoint of making the dispersibility of the polishing slurry into the polishing layer 13 via the adhesive layer 12 uniform throughout the polishing pad 10, it is preferable that the through holes 121 of the adhesive layer 12 are arranged in a regular pattern when viewed from the polishing surface side. The arrangement pattern of the through holes 121 of the adhesive layer 12 may be, for example, a lattice pattern, a radial pattern, a concentric circular pattern, a spiral pattern, a staggered pattern, or the like.
[0034] The thickness of adhesive layer 12 may be, for example, 0.1 mm or more, alternatively 0.2 mm or more, and may be 1.0 mm or less, alternatively 0.8 mm or less.
[0035] In addition, in the polishing pad 10 of this embodiment, after obtaining a laminate in which the cushion layer 11, the adhesive layer 12, and the polishing layer 13 are laminated, the through-hole 121 of the adhesive layer 12 and the through-hole 133 of the polishing layer 13 are integrally formed by drilling from the polishing surface of the polishing layer 13. Therefore, the through-hole 121 of the adhesive layer 12 and the through-hole 133 of the polishing layer 13 are aligned in a straight line. This allows the polishing slurry to be supplied more uniformly to the polishing surface. In addition, the adhesive strength of the adhesive layer 12 with the polishing layer 13 can be increased compared to when the through-hole 121 of the adhesive layer 12 and the through-hole 133 of the polishing layer are not aligned in a straight line.
[0036] The cushion layer 11 is a layer having cushioning properties. The cushion layer 11 in this embodiment includes through holes formed by air bubbles communicating with each other. The through holes communicate from the surface opposite to the contact surface with the adhesive layer 12 to the contact surface with the adhesive layer 12. This allows the cushion layer 11 to hold the polishing slurry. When the polishing pad 10 is pressed, the cushion layer 11 is deformed, and the polishing slurry held in the through holes is released from the surface on the adhesive layer 12 side. Since the adhesive layer 12 has through holes, the polishing slurry released from the cushion layer 11 passes through the adhesive layer 12 preferentially via the through holes 121 of the adhesive layer 12. Therefore, the adhesive layer 12 plays the role of a straightening plate, and the polishing slurry released from the cushion layer 11 is dispersed when passing through the adhesive layer 12, and is sent to the polishing layer 13. The cushion layer 11 may also have a plurality of through holes that penetrate from the contact surface with the adhesive layer 12 to the adhesive surface with the polishing platen side adhesive layer 30. The through holes increase the rate of open cells in the communicating holes, and increase the amount of polishing slurry that can be held. It is preferable that the through holes 121 in the adhesive layer 12, the through holes 133 in the polishing layer, and the through holes in the cushion layer are aligned in a straight line.
[0037] The cushion layer 11 may be made of, for example, polyethylene foam, polyurethane foam, ethylene-vinyl acetate copolymer foam, polystyrene foam, polypropylene foam, or the like.
[0038] The expansion ratio is preferably 6 to 60, and more preferably 10 to 40. When the expansion ratio of the foam is equal to or higher than the lower limit of the above range, excellent compressibility is obtained, and when the expansion ratio of the foam is equal to or lower than the upper limit of the above range, excellent durability is obtained.
[0039] If the open cell ratio is 95% or more, the polishing slurry can be sufficiently retained and excellent compressibility can be easily obtained, which is preferable.
[0040] Thickness T of the cushion layer 11 11is preferably 2 to 15 times the thickness of the workpiece W. For example, when the thickness of the workpiece W is 2.0 mm, the thickness T of the cushion layer 11 is 11 is preferably 4.0 mm or more, and more preferably 6.0 mm or more. This allows the cushion layer 11 to be easily deformed, and the workpiece W can be pushed sufficiently deeply into the polishing pad 10, making it easier to follow the shape of the curved portion W2 of the workpiece W. In addition, from the viewpoint of obtaining good polishing characteristics without insufficient polishing force, it is preferably 50 mm or less, and more preferably 20 mm or less. The thickness T of the cushion layer 11 11 This is the height from the surface of the cushion layer 11 opposite to the contact surface with the adhesive layer 12 to the apex of the protrusion 111 of the cushion layer.
[0041] The 40% compression hardness of the cushion layer 11 using a circular pressure plate with a diameter of 50 mm is 10 gf / cm 2 or more than 20gf / cm 2 It can be more than 150gf / cm 2 Less than or equal to 100gf / cm 2 It can be the following:
[0042] The apparent density of the cushion layer 11 is 0.01 g / cm 3 More than 0.05g / cm 3 It can be the following:
[0043] The 40% compression hardness of the polishing pad 10 using a circular pressure plate with a diameter of 50 mm is 20 gf / cm 2 It is preferable that the resistance is 40 gf / cm or more. 2 More preferably, it is 60 gf / cm or more. 2 More preferably, it is 180 gf / cm or more. 2 It is preferable that the resistance is less than 150 gf / cm 2 More preferably, it is 120 gf / cm or less. 2It is more preferable that the 40% compression hardness of the polishing pad 10 using a circular pressure plate having a diameter of 50 mm is in such a small range, so that the workpiece W can be easily sunk into the polishing pad 10 to a depth greater than or equal to the thickness of the workpiece W.
[0044] Thickness T of polishing pad 10 10 is preferably 2 to 15 times the thickness of the workpiece W to be polished, from the viewpoint of being able to push the workpiece W sufficiently deep into the polishing pad 10 and being able to easily follow the shape of the curved portion W2 of the workpiece W. For example, when the thickness of the workpiece W is 2.0 mm, it is preferably 5.0 mm or more, and more preferably 8.0 mm or more. In addition, the thickness T of the polishing pad 10 10 The thickness T of the polishing pad 10 may be 55 mm or less, or 25 mm or less. 10 This refers to the height from the surface of the cushion layer 11 opposite to the contact surface with the adhesive layer 12 to the apex of the protrusion 131 of the polishing layer 13.
[0045] The polishing pad 10 may further include an adhesive layer such as a double-sided tape for adhering the polishing pad 10 to the polishing platen 20 on the surface of the cushion layer 11 opposite to the contact surface with the adhesive layer 12. A release paper may further be laminated on the surface of the adhesive layer opposite to the contact surface with the cushion layer 11. When using the polishing pad 10 including the release paper, the release paper may be peeled off, and then the polishing pad 10 from which the release paper has been peeled off may be attached to the polishing platen 20.
[0046] [Polishing pad manufacturing method] The method for manufacturing the polishing pad 10 includes a polishing layer forming step, a cushion layer forming step, a bonding step, and a through-hole forming step.
[0047] (Polishing layer production process) In the abrasive layer preparation step, the abrasive layer 13 is prepared. For example, when the abrasive layer 13 is a polyurethane resin sheet formed by a wet film formation method, it can be formed by a wet film formation method.
[0048] Here, the wet film forming method is a method in which a resin solution obtained by dissolving a resin to be formed in an organic solvent is applied to a sheet-shaped substrate, and then the resin solution is passed through a coagulating liquid in which the organic solvent dissolves but the resin does not dissolve, to replace the organic solvent, coagulate, and dry to form a foam layer. For example, the method can be produced by referring to Japanese Patent No. 5421635 and Japanese Patent No. 5844189.
[0049] After the film formation, the surface of the polyurethane sheet is buffed to form openings on the polished surface and to make the thickness uniform, thereby obtaining the polishing layer 13.
[0050] (Cushion layer manufacturing process) In the cushion layer preparation step, any method can be used as long as it can process the cushion material to have a curved surface shape and the convex portions and concave portions arranged in a regular pattern. Conventionally known methods can be used, and the cushion layer 11 can be obtained by, for example, profiling, two-dimensional cutting, CF cutting, thermoforming, etc. Among these, profiling is preferred because it is easy to process the cushion material to have a curved surface shape and the convex portions 111 and concave portions 112 arranged in a regular pattern.
[0051] For example, by performing profiling, a curved uneven shape can be imparted to one side of the cushion layer 11. The profiling can be performed, for example, by the method described in JP 2015-128483 A. By profiling, an uneven shape consisting of a plurality of recesses and a plurality of protrusions can be continuously formed, and unevenness of the same shape is formed on one side and the other side of the cut portion. Therefore, by a commonly known manufacturing method, it is possible to obtain a cushion layer 11 having an uneven shape in which the protruding shape of such a protrusion and the recessed shape of a recess are the same.
[0052] (Laminating process) In the lamination step, cushion layer 11 having an uneven shape consisting of a plurality of convex portions and a plurality of concave portions is laminated on polishing layer 13 via adhesive layer 12 so that polishing layer 13 fits the uneven shape of cushion layer 11. Then, the laminate thus obtained is bonded.
[0053] For example, when a heat-sensitive adhesive is used as the adhesive layer 12, the laminate is passed between a pair of heated heat rolls to thermally melt the adhesive layer 12. As a result, the polishing layer 13 is bonded to the cushion layer 11 by thermocompression bonding along the convex portions 111 and concave portions 112 of the cushion layer 11 via the adhesive layer 12. The heating temperature of the heat rolls may be appropriately set depending on the type of heat-sensitive adhesive used as the adhesive layer, and is preferably, for example, 80 to 120°C.
[0054] (Through hole formation process) In the through hole forming step, the through hole 121 in the adhesive layer 12 and the through hole 133 in the polishing layer 13 are formed by drilling holes from the polishing surface side of the bonded laminate. For example, a needle having a length equal to or longer than the total thickness of the adhesive layer 12 and the polishing layer 13 in the bonded laminate is inserted to form a through hole. The diameter of the needle may be appropriately selected according to the diameter of the through hole. This allows the adhesive layer 12 and the polishing layer 13 to form a through hole that penetrates from the adhesive surface of the adhesive layer 12 with the cushion layer 11 to the polishing surface of the polishing layer 13. In addition, by using a member having a plurality of such needles on its surface, the polishing pad 10 can be formed with a single pass or a relatively small number of passes.
[0055] [Polishing method] As a polishing method, first, the workpiece W is placed on the spacer 40. In this state, a polishing slurry is supplied from the polishing slurry supplying unit 21 provided on the polishing table 20. The polishing slurry supplied from the polishing slurry supplying unit 21 passes through the through holes 31 of the polishing table side adhesive layer 30 that communicates with the polishing slurry supplying unit 21 and reaches the cushion layer 11. The cushion layer 11 has a through hole and holds the supplied polishing slurry. By pressing the polishing pad 10 from above the workpiece W, the polishing slurry held in the through holes of the cushion layer 11 passes through the through holes 121 of the adhesive layer 12 and reaches the polishing layer 13. The polishing layer 13 has a through hole, and the polishing slurry passes through the through holes of the polishing layer 13 and reaches the workpiece W. The polishing slurry supplied between the polishing pad 10 and the workpiece W can be used to polish the workpiece W.
[0056] As described above, the method for polishing the workpiece W using the polishing pad 10 is a method for polishing the workpiece W by pressing the polishing pad 10 against the workpiece W. The polishing method includes a step of supplying a polishing slurry to the cushion layer 11. The method also includes a pressing step of sending the polishing slurry held in the communicating holes of the cushion layer 11 to the polishing layer 13 through the through holes 121 of the adhesive layer 12 by a pressing force, and supplying the polishing slurry to the workpiece W through the communicating holes of the polishing layer 13. The method of polishing the workpiece W using the polishing pad 10 allows the workpiece W to be deeply pressed against the polishing pad 10. The polishing slurry held in the cushion layer 11 is released by the volume of the pressed-in part, and even though the workpiece W is in close contact with the polishing layer 13, the polishing slurry is abundantly supplied between the workpiece W and the polishing layer 13 by the pressing force. In addition, since the polishing slurry is released only to the pressed-in part, the polishing slurry can be efficiently supplied. Therefore, it is possible to reduce the outflow of expensive polishing slurry without being used. In addition, since the supplied polishing slurry flows toward the holding platen 50, the polishing slurry does not return, and new polishing slurry is always supplied.
[0057] (summary) The polishing pad according to aspect 1 of the present invention is a polishing pad formed by laminating a cushion layer, an adhesive layer, and a polishing layer in this order, wherein the cushion layer has communicating holes and has an uneven shape consisting of multiple convex portions and multiple concave portions on the surface facing the polishing layer, the adhesive layer has multiple through holes that penetrate from the contact surface with the cushion layer to the contact surface with the polishing layer, the polishing layer has communicating holes and is attached to the cushion layer via the adhesive layer along the convex portions and the concave portions, thereby having an uneven shape consisting of multiple convex portions and multiple concave portions on its surface, and the uneven shape of the polishing layer is curved and is formed so that the convex portions and the concave portions are arranged in a regular pattern.
[0058] The polishing pad according to aspect 2 of the present invention may be configured as in aspect 1, wherein the polishing layer has a plurality of through holes extending from the contact surface with the adhesive layer to the polishing surface.
[0059] The polishing pad according to Aspect 3 of the present invention may be configured as in Aspect 2, wherein the through hole of the adhesive layer and the through hole of the polishing layer are aligned in a straight line.
[0060] The polishing pad according to aspect 4 of the present invention is the polishing pad according to aspect 2 or 3, wherein the density of the through holes in the polishing layer is 0.5 holes / cm 2 More than 50 pieces / cm 2 The following configuration may also be used.
[0061] The polishing pad according to a fifth aspect of the present invention may be configured as in any one of the second to fourth aspects, wherein the through holes in the polishing layer have a diameter of 0.05 mm or more and 2.0 mm or less.
[0062] The polishing pad according to a sixth aspect of the present invention may be configured as any one of the first to fifth aspects, wherein the convex portions of the polishing layer have an inverted shape of the concave portions of the polishing layer.
[0063] The polishing pad according to aspect 7 of the present invention may be configured as any one of aspects 1 to 6, such that, when viewed in a plane from the polishing surface side, the uneven shape of the polishing layer is formed so that the convex portions and the concave portions are arranged alternately in the vertical and horizontal directions.
[0064] The polishing pad according to aspect 8 of the present invention may be configured as in aspect 7, wherein the distance between apexes of adjacent convex portions in the polishing layer, sandwiching one concave portion, is 5 mm or more and 50 mm or less.
[0065] The polishing pad according to aspect 9 of the present invention may be configured as any one of aspects 1 to 8, wherein the height of the apex of the convex portion relative to the bottom point of the concave portion of the polishing layer is 0.5 mm or more and 30 mm or less.
[0066] The polishing pad according to aspect 10 of the present invention is any one of aspects 1 to 9, wherein the 40% compression hardness using a circular pressure plate having a diameter of 50 mm is 20 gf / cm 2 More than 180gf / cm 2 The following configuration may also be used.
[0067] A method for manufacturing a polishing pad according to aspect 11 of the present invention includes a bonding step of bonding a cushion layer having an uneven shape consisting of a plurality of convex portions and a plurality of concave portions, and a polishing layer having an uneven shape consisting of a plurality of convex portions and a plurality of concave portions, via an adhesive layer, to obtain a laminate obtained by bonding the polishing layer to the uneven shape, and a through hole forming step of drilling holes from the polishing surface side of the bonded laminate to form through holes that penetrate from the bonding surface of the adhesive layer with the cushion layer to the polishing surface of the polishing layer, wherein the uneven shape is a curved shape, and the convex portions and the concave portions are formed so as to be arranged in a regular pattern.
[0068] A method for producing a polishing pad according to a twelfth aspect of the present invention may be configured as in the eleventh aspect, further comprising a cushion layer producing step of imparting the uneven shape to the cushion layer by profiling.
[0069] A polishing method according to aspect 13 of the present invention is a polishing method for polishing an object to be polished by pressing an abrasive pad of any one of aspects 1 to 10 against the object to be polished, and may include a supplying step of supplying an abrasive slurry to the cushion layer, and a pressing step of sending the abrasive slurry held in the communicating holes of the cushion layer to the polishing layer through the through holes of the adhesive layer by a pressing force, and supplying the abrasive slurry to the object to be polished through the communicating holes of the polishing layer.
[0070] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention. EXAMPLES
[0071] The following polishing tests were carried out on the examples according to the present invention and comparative examples prepared for comparison, but the present invention is not limited to the following examples.
[0072] Example 1 As the polishing layer, 100 parts by mass of a solution containing 30 parts by mass of a polyester polyurethane resin with a 100% modulus of 7.8 MPa and 70 parts by mass of N,N-dimethylformamide (DMF) were added to 60 parts by mass of DMF and 5 parts by mass of water and mixed. The mixed solution was filtered to remove insoluble components, and a resin-containing solution was obtained.
[0073] The resin-containing solution was applied to a polyester sheet using a knife coater to a thickness of 0.8 mm. The polyester sheet to which the resin-containing solution was applied was immersed in a coagulation bath (coagulation liquid: water) to coagulate the resin-containing solution. The polyester sheet was then peeled off, washed and dried to obtain a polyurethane resin sheet with an elongation of 350%.
[0074] The surface of the resulting polyurethane resin sheet was buffed to a thickness of 0.73 mm to obtain an abrasive layer.
[0075] For the cushion layer, a polyurethane foam (Everlight SF, manufactured by Bridgestone Chemical Products Co., Ltd.) was subjected to a profile processing. Specifically, the polyurethane foam was passed through a rotating roller having an uneven shape, and a blade was inserted into the center of the sponge compressed by being sandwiched between the rollers to cut into an uneven shape. As a result, a cushion layer was obtained having an uneven shape formed such that the height from the bottom point of the recess to the top of the protrusion in the thickness direction was 6 mm, the pitch (the distance between adjacent protrusions sandwiching one recess) was 20 mm, and the protrusions and recesses were arranged alternately in the vertical and horizontal directions when viewed in plan from the polished surface side. The thickness of the cushion layer at the protrusions was 10 mm.
[0076] An adhesive layer, Hibon (a urethane-based heat-sensitive adhesive manufactured by Hitachi Chemical Co., Ltd.), was sandwiched between the polishing layer and the cushioning layer to obtain a laminate in which the cushioning layer, adhesive layer, and polishing layer were laminated in this order. The laminate was passed between a pair of heat rolls heated to a temperature of 90°C, and the entire surface of the cushioning layer on the concave-convex shape side was bonded to the entire surface of the polishing layer that had not been buffed, via the adhesive layer.
[0077] By drilling holes from the polished surface of the obtained laminate, the diameter was 0.4 mm and the density was 4 / cm 2 Then, a double-sided tape having a release paper with a slurry hole punched at a position corresponding to the polishing slurry supply part of the polishing platen was attached to the surface of the cushion layer opposite to the contact surface with the adhesive layer so that the adhesive surface opposite to the release paper side of the double-sided tape was in contact with the cushion layer, to prepare a polishing pad.
[0078] Comparative Example 1 A polishing pad was produced in the same manner as in Example 1, except that a flat sheet of polyurethane foam (Everlight SF, manufactured by Bridgestone Chemical Products Co., Ltd.) with a thickness of 10 mm was used as the cushion layer without profiling. Since the cushion layer was not profiled, the surface of the polishing layer was also flat.
[0079] [Compression hardness measurement] The polishing pad to be measured was cut into a rectangle of 100 mm x 100 mm to prepare a sheet-like test piece. The test piece was fixed with double-sided tape in the center of the table of a micro strength evaluation tester (Shimadzu Corporation, Micro Autograph, MST-I). The point where a load of 5 g was applied with a circular pressure plate (flat plate) with a diameter of 50 mm was set as the origin, and a load was applied in the thickness direction at a speed of 1 mm / min until the thickness of the cushion layer became 40% of the thickness in the natural state without pressure, and the stress at that time was taken as the compression hardness. At this time, the area of the test piece that was in contact with the pressure plate and included at least one protrusion was measured.
[0080] [Polishing test] For the polishing test, a single-sided polisher having a polishing slurry supply section on a polishing table as shown in Figure 1 was used as the polishing device, and an acrylic resin plate (rectangular shape of 65 mm x 65 mm, thickness of 2 mm, with a curved section formed on the end by curved surface processing) was used as the object to be polished.
[0081] A spacer having the same shape as the acrylic resin plate and a thickness of 5 mm was attached to the holding platen of the polishing device, and 10 acrylic resin plates were held on the spacer. The polishing pads according to the examples and comparative examples were fixed to the polishing platen with double-sided tape.
[0082] The polishing test was performed with a load of 470g / cm 2 The polishing speed was set at 22 rpm for the holding platen and 26 rpm for the polishing platen, and the polishing time was 10 min.
[0083] As the slurry used for polishing, a colloidal silica slurry ("COMPOL80" manufactured by Fujimi Incorporated) diluted two-fold was used, and the polishing slurry was supplied at a flow rate of 30 ml / min.
[0084] The results of the polishing were evaluated as follows.
[0085] <Polishing performance evaluation> Before polishing, marks were made with an oil-based pen on a total of five locations on the flat surface that would become the polishing surface and on the four curved side surfaces (A to D) of the workpiece. The polishing performance was evaluated by assigning a "good" to cases where all marks had disappeared after polishing and an "ungood" to cases where any marks remained.
[0086] <Surface roughness evaluation> After polishing, the surface roughness of the flat surface and the four curved side surfaces of the object to be polished was measured, and a surface roughness of less than 40 nm was rated as ◯, and a surface roughness of 40 nm or more was rated as ×. The curved side surfaces of the object to be polished were measured directly above the curved side surfaces, with the object held at an inclination of 30°.
[0087] Here, the surface roughness was measured using a non-contact roughness measuring instrument (manufactured by ZYGO Corporation under the product name "NewView5022"), with a measurement magnification of 2 and a measurement field of view set to a range of 307.609 μm horizontal × 307.609 μm vertical, to measure the surface roughness Sa.
[0088] The results of Example 1 and Comparative Example 1 are shown in Table 1.
[0089] [Table 1]
[0090] As a result of the experiment, no ink marks were found on the surface of the workpiece after polishing in Example 1 and Comparative Example 1. Furthermore, the surface roughness of both the flat surface and the curved side surface was reduced in Example 1, and a good evaluation was obtained. In contrast, in Comparative Example 1, although the flat surface was polished, the surface roughness of the curved side surface could not be reduced.
[0091] Example 1, which used a cushion layer that had been subjected to profile processing, had a smaller compression hardness and was able to reduce surface roughness compared to Comparative Example 1, which used a cushion layer that had not been subjected to profile processing.
[0092] Since the polishing pad of Comparative Example 1 uses a soft cushion layer, it was possible to sink the flat surface and all four curved side surfaces of the polished object into the polishing pad. Therefore, in the polishing performance evaluation, all the marks disappeared after polishing, and it was found that the flat surface and all four curved side surfaces of the polished object were in contact with the polishing surface. However, the polishing pad of Comparative Example 1, which does not have an uneven shape, does not have room to extend into the polishing layer. Therefore, when the polished object is sunk into the polishing pad, the pressing force on the curved portion of the polished object becomes large, so that the polished object is polished excessively, which causes polishing scratches, and it is considered that the surface roughness could not be reduced.
[0093] On the other hand, in Example 1 having a cushion layer with a profile processing, the polishing layer follows the uneven shape, so there is room for the polishing layer to expand. Therefore, when the polished object is sunk into the polishing pad, the bias of the pressing force on the curved part of the polished object can be reduced. It is considered that this further reduces the surface roughness of the polished object. [Industrial Applicability]
[0094] The present invention can be used for polishing an object having a curved surface. [Explanation of symbols]
[0095] 1 Polishing equipment 10 Polishing Pad 11 Cushioning layer 12 Adhesive layer 13 Polishing layer 111 Convex 112 Recess 121 Through hole 131, 131' convex part 132, 132' recess 133 Through hole
Claims
1. A polishing pad comprising a cushion layer, an adhesive layer, and a polishing layer laminated in this order, the cushion layer has a through hole extending from a surface opposite to a surface in contact with the adhesive layer to the surface in contact with the adhesive layer, and has an uneven shape on the surface on the polishing layer side, the uneven shape being composed of a plurality of convex portions and a plurality of concave portions; the adhesive layer has a plurality of through holes extending from a contact surface with the cushion layer to a contact surface with the polishing layer, the polishing layer has a through hole that communicates from the contact surface with the adhesive layer to the polishing surface, and is bonded to the cushion layer via the adhesive layer along the convex portions and the concave portions, so that the polishing layer has an uneven surface formed of a plurality of convex portions and a plurality of concave portions; A polishing pad, wherein the uneven shape of the polishing layer is a curved shape, and the convex portions and the concave portions are formed so as to be arranged in a regular pattern.
2. The polishing pad according to claim 1 , wherein the polishing layer has a plurality of through holes extending from the contact surface with the adhesive layer to the polishing surface.
3. The polishing pad according to claim 2 , wherein the through hole of the adhesive layer and the through hole of the polishing layer are aligned in a straight line.
4. The density of the through holes in the polishing layer is 0.5 holes / cm 2 Above, 50 pieces / cm 2 4. The polishing pad according to claim 2 or 3, wherein:
5. 5. The polishing pad according to claim 2, wherein the through holes of the polishing layer have a diameter of 0.05 mm or more and 2.0 mm or less.
6. 6. The polishing pad according to claim 1, wherein the convex portions of the polishing layer have an inverted shape of the concave portions of the polishing layer.
7. The polishing pad according to any one of claims 1 to 6, wherein when viewed in a plane from the polishing surface side, the uneven shape of the polishing layer is formed so that the convex portions and the concave portions are arranged alternately in the vertical and horizontal directions.
8. 8. The polishing pad according to claim 7, wherein the distance between apexes of adjacent convex portions across one concave portion in the polishing layer is 5 mm or more and 50 mm or less.
9. 9. The polishing pad according to claim 1, wherein the height of the apex of the convex portion relative to the bottom point of the concave portion of the polishing layer is 0.5 mm or more and 30 mm or less.
10. The 40% compression hardness using a circular pressure plate with a diameter of 50 mm is 20 gf / cm 2 Above, 180gf / cm 2 The polishing pad according to any one of claims 1 to 9, wherein:
11. A method for manufacturing a polishing pad having a cushion layer, an adhesive layer, and a polishing layer laminated in this order, comprising: a lamination process in which the cushion layer has through holes that communicate from the surface opposite to the contact surface with the adhesive layer to the contact surface with the adhesive layer and has an uneven shape consisting of a plurality of convex portions and a plurality of concave portions, and the polishing layer has through holes that communicate from the contact surface with the adhesive layer to the polishing surface, and the laminate is bonded via the adhesive layer such that the polishing layer conforms to the uneven shape; a through-hole forming step of drilling holes from the polishing surface side of the polishing layer of the bonded laminate to form through-holes that extend from the bonding surface of the adhesive layer to the cushion layer to the polishing surface of the polishing layer, A method for manufacturing a polishing pad, wherein the uneven shape is a curved shape, and the convex portions and the concave portions are formed so as to be arranged in a regular pattern.
12. The method for producing a polishing pad according to claim 11, further comprising a cushion layer preparation step of imparting the uneven shape to the cushion layer by profiling.
13. A polishing method for polishing an object by pressing the polishing pad according to any one of claims 1 to 10 against the object, comprising: a supplying step of supplying a polishing slurry to the cushion layer; a pressing step of sending the polishing slurry held in the communicating holes of the cushion layer through the through holes of the adhesive layer by a pressing force to the polishing layer, and supplying the polishing slurry to the workpiece through the communicating holes of the polishing layer.
Citation Information
Patent Citations
Yarn treating nozzle
JP1982089634A
Cleaning member of end of contactor
JP2000332069A
Laminated polishing pad
JP2006346805A
Polishing pad
JP2010082707A
Polishing pad, and method for manufacturing the same
JP2012130992A