Anode gas diffusion layer substrate
A carbon fiber and graphite particle-based gas diffusion layer with a specific aspect ratio and water-repellent treatment addresses the challenges of gas diffusivity and conductivity in fuel cells, enhancing power generation performance by efficient gas diffusion and water management.
Patent Information
- Application Number
- JP2021199484
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-12-08
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2041-12-08
AI Technical Summary
Existing gas diffusion layers for anode electrodes in fuel cells face challenges in achieving both high gas diffusivity and conductivity while maintaining optimal moisture levels and preventing flooding, which affects power generation performance.
A gas diffusion layer base material composed of carbon fibers and graphite particles with a specific aspect ratio and particle size distribution, combined with a water-repellent treatment, is used to enhance gas diffusion and conductivity, and prevent flooding.
The material enables fuel cells with high power generation performance by efficiently diffusing reactant gases and discharging water, reducing resistance and maintaining optimal moisture levels.
Smart Images

Figure 0007554175000002 
Figure 0007554175000005 
Figure 0007554175000006
Abstract
Description
[Technical field]
[0001] The present invention relates to an anode gas diffusion layer substrate, which is a material used for forming an anode gas diffusion layer of a polymer electrolyte fuel cell. [Background technology]
[0002] A polymer electrolyte fuel cell (hereinafter simply referred to as a "fuel cell"), which is widely used as a power source for automobiles and the like, is constructed by stacking a plurality of fuel cell units with separators between them, and in one unit cell, a membrane / electrode assembly is formed by arranging a cathode (+) side electrode and an anode (-) side electrode, each of which is composed of a catalyst layer made of a conductive material such as carbon carrying a catalyst such as platinum and an ion exchange resin, and a porous gas diffusion layer arranged on the outside of each catalyst layer, on both sides of a polymer electrolyte membrane that selectively transmits specific ions. Then, on the outside of the gas diffusion layer that constitutes this membrane / electrode assembly, a separator is arranged that supplies a fuel gas (anode gas) or an oxidizing gas (cathode gas) and has a gas flow path formed therein for discharging the generated gas and excess gas, and the membrane / electrode assembly is sandwiched between the separators.
[0003] In the fuel cell having the above-mentioned configuration, the gas diffusion layer constituting the electrode of the single cell battery is arranged to enhance the diffusibility of the reactant gas. Since the gas diffusion layer is responsible for diffusing the fuel gas or oxidizing gas supplied from the gas flow path of the separator to the catalyst layer adjacent to the gas diffusion layer (gas diffusibility), the gas diffusion layer is required to be gas permeable, and is also required to be conductive as a current collecting function for efficiently transferring electrons for the electrochemical reaction. In addition, the gas diffusion layer is required to always keep the polymer electrolyte membrane and the catalyst layer in an optimal wet state, while suppressing the flooding phenomenon (the phenomenon in which the pores of the gas diffusion layer are blocked by water) and to maintain stable power generation performance of the battery, and is also required to have water repellency (drainage property) to drain excess reaction water and condensation water generated by the electrochemical reaction of hydrogen and oxygen during power generation.
[0004] Conventionally, a substrate in the form of a sheet made of conductive fibers such as carbon fibers has been used to form a gas diffusion layer for a fuel cell. For example, Patent Document 1 discloses a carbon fiber sheet for a gas diffusion layer of a polymer electrolyte fuel cell, which comprises carbon fibers, carbon particles I having an average particle size (X) of 0.5 to 5 μm and carbon particles II having an average particle size (Y) of 7 to 20 μm, and amorphous carbon bonding the intersections of the carbon fibers, and has an average particle size ratio [(Y) / (X)] of the particle size (X) to the particle size (Y) of 1.5 to 20, and the amorphous carbon content (B), the carbon particle I content (C), and the carbon Disclosed is a carbon fiber sheet for use in gas diffusion layers of polymer electrolyte fuel cells, in which the mass ratio [(C+D) / (B+C+D)] of the sum of the carbon particle I content (C) and the carbon particle II content (D) to the sum of the carbon particle I content (C) and the elementary particle II content (D) is 0.65 to 0.95, and the mass ratio [(B+C+D) / A] of the sum of the amorphous carbon content (B), the carbon particle I content (C), and the carbon particle II content (D) to the carbon fiber content (A) is 1.50 to 5.00. Patent Document 2 describes a gas diffusion layer substrate that is porous and has a specific number of pores formed therein, and that has a basis weight of 30 g / cm. 2 The gas diffusion layer substrate is disclosed as follows: when dry nitrogen gas is passed through one surface of the gas diffusion layer substrate in the thickness direction of the gas diffusion layer substrate at a flow rate of 10 L / min, the pressure difference between the front and back of the gas diffusion layer substrate is within a range of 0.01 to 0.3 MPa. Patent Document 3 discloses a porous gas diffusion layer substrate that is made of a carbon fiber aggregate in which carbon fibers are entangled with one another, contains carbide binding the carbon fibers of the carbon fiber aggregate, and contains spherical graphite and / or artificial graphite having a median diameter in the range of 40 μm to 120 μm held between the carbon fibers of the carbon fiber aggregate. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2009-289552 A [Patent Document 2] JP 2018-18665 A [Patent Document 3] JP 2020-87826 A Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide an anode gas diffusion layer substrate, which is a component used in forming an anode gas diffusion layer of a fuel cell, and which satisfies both gas diffusivity and electrical conductivity to provide a fuel cell with high power generation performance. [Means for solving the problem]
[0007] The present invention is illustrated below. [1] A gas diffusion layer substrate for an anode electrode of a fuel cell, comprising (A) carbon fibers and (B) graphite particles, the graphite particles (B) having a major axis of d L The minor axis is d S In this case, the major axis d L and minor axis d S Relative to Dr(=d L / d S 2. A gas diffusion layer substrate for an anode electrode, comprising graphite particles (B1) having an aspect ratio (hereinafter referred to as "aspect ratio Dr") of 5-100. [2] The anode gas diffusion layer substrate according to the above item [1], wherein the graphite particles (B1) have an average particle size d50 of 20 to 80 μm as measured by a laser diffraction method. [3] The gas diffusion layer substrate for an anode according to the above item [1] or [2], wherein a content ratio of the graphite particles (B) is 70 to 90 parts by mass per 100 parts by mass of the carbon fibers (A). [4] Weight per unit area is 40 to 100 g / m 2 The gas diffusion layer substrate for an anode electrode according to any one of the above items [1] to [3]. [5] The gas diffusion layer substrate for an anode according to any one of the above items [1] to [4], the surface of which is treated to be water repellent. Effect of the Invention
[0008] When the anode gas diffusion layer substrate of the present invention is used to form an anode gas diffusion layer constituting a membrane / electrode assembly for a fuel cell, a fuel cell having high power generation performance can be obtained. Therefore, a fuel cell obtained by using the anode gas diffusion layer substrate of the present invention is suitable for fuel cells for transportation such as vehicles, stationary fuel cells, etc. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view of an anode gas diffusion layer substrate of the present invention. [Diagram 2] FIG. 2 is a schematic explanatory diagram for obtaining the aspect ratio of the graphite particles (B1) contained in the anode gas diffusion layer substrate of the present invention. [Diagram 3] FIG. 1 is a schematic cross-sectional view of a membrane / electrode assembly obtained by using an anode gas diffusion layer substrate of the present invention. [Figure 4] 1 is a cross-sectional image of an anode gas diffusion layer substrate AS1 obtained in Example 1-1. [Diagram 5] 1 is a cross-sectional image of an anode gas diffusion layer substrate AS3 obtained in Comparative Example 1-1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The anode gas diffusion layer substrate of the present invention is, for example, a sheet-like (thin plate-like) material used for forming the anode gas diffusion layer 10 in a membrane / electrode assembly 100 including, in order, the anode gas diffusion layer 10, a microporous layer 15, a catalyst layer 40, an electrolyte layer 30, a catalyst layer 50, a microporous layer 25, and a cathode gas diffusion layer 20 as shown in FIG. 3.
[0011] The anode gas diffusion layer substrate of the present invention contains (A) carbon fibers (hereinafter also referred to as "component (A)") and (B) graphite particles (hereinafter also referred to as "component (B)"). The graphite particles (B) have a major axis length of d L Let the minor axis (minor axis length) be d S If the ratio of these lengths is dL / d S The anode gas diffusion layer substrate of the present invention contains graphite particles (B1) (hereinafter also referred to as "component (B1)" or "rod-shaped graphite particles") having an aspect ratio Dr of 5 to 100. The anode gas diffusion layer substrate of the present invention may contain other components (binder, carbide of organic component, additive, etc.) as necessary. In addition, the surface of the anode gas diffusion layer substrate of the present invention may be subjected to a water repellent treatment.
[0012] Fig. 1 is a schematic cross-sectional view of an anode gas diffusion layer substrate 1 of the present invention, which includes a plurality of carbon fibers 3 and a plurality of rod-shaped graphite particles 5. The blank areas in Fig. 1 are, for example, phases mainly composed of carbides of organic components that bind the carbon fibers together, the graphite particles together, or the carbon fibers and the graphite particles together. The porosity is low, usually 70% or less.
[0013] The component (A) according to the present invention is not particularly limited, and examples thereof include vapor-grown carbon fibers, carbon nanotubes (single-wall, double-wall, multi-wall, cup-laminated type, etc.), polyacrylonitrile (PAN)-based carbon fibers, pitch-based carbon fibers, rayon-based carbon fibers, etc. The component (A) contained in the anode gas diffusion layer substrate of the present invention may be one type or two or more types.
[0014] The average fiber diameter of the component (A) is preferably 5 to 15 μm, more preferably 6 to 8 μm, from the viewpoint of gas diffusibility and drainage property of the anode gas diffusion layer to be formed. The upper limit of the fiber length of component (A) is usually 12 mm, and the lower limit is usually 2 mm. The average fiber length of component (A) is preferably 2 to 9 mm, more preferably 3 to 6 mm, from the viewpoints of gas diffusibility and drainage of the anode gas diffusion layer to be formed.
[0015] Component (B) according to the present invention includes component (B1), i.e., rod-shaped graphite particles (which may have an irregular shape) having an aspect ratio Dr of 5 to 100. Component (B) contained in the anode gas diffusion layer substrate of the present invention may consist of only component (B1), or may consist of a combination of component (B1) and other graphite particles (graphite particles having an aspect ratio Dr outside the above range, such as spherical graphite particles). In the latter case, the lower limit of the content of component (B1) relative to the total amount of component (B) contained in the anode gas diffusion layer substrate of the present invention is preferably 50 mass%, more preferably 70 mass%.
[0016] The aspect ratio Dr of the component (B1) is preferably 20 to 80, more preferably 30 to 70, since a membrane / electrode assembly constituting a fuel cell having high power generation performance can be obtained. The method for deriving the aspect ratio Dr is explained with reference to FIG. 2. That is, the major axis length d L and the minor axis (minor axis length) d, which is the maximum length of the component (B1) in the direction perpendicular to the major axis L. S Measure the length ratio d L / d S The aspect ratio Dr of the component (B1) contained in the anode gas diffusion layer substrate can be determined by applying a method of measuring the component (B1) extracted from the anode gas diffusion layer substrate, or a method of measuring it on a cross-sectional image of the anode gas diffusion layer substrate.
[0017] The average particle size d50 of component (B1) as measured by a laser diffraction method is preferably from 20 to 80 μm, more preferably from 30 to 50 μm, from the viewpoint of graphite fixation during papermaking.
[0018] Component (B) may be either a solid or hollow body, or may be an expanded graphite body. The shape of component (B1) may be any of a plate shape (e.g., a scale shape), an oval sphere shape, etc., as long as the aspect ratio Dr is satisfied.
[0019] The content of component (B) in the anode gas diffusion layer substrate of the present invention is preferably 70 to 90 parts by mass, and more preferably 75 to 88 parts by mass, relative to 100 parts by mass of component (A), because an anode gas diffusion layer of a membrane / electrode assembly constituting a fuel cell having high power generation performance can be obtained.
[0020] As described above, the anode gas diffusion layer substrate of the present invention may further contain other components (binder, carbonized organic components, additives, etc.). The binder may be derived from polyvinyl alcohol, polyvinyl acetate, polyolefins such as polyethylene and polypropylene, polyesters such as polyethylene terephthalate, polyacrylonitrile, cellulose, polyethylene oxide, polyacrylamide, phenolic resins, xylenol resins, styrene-butadiene rubber, starch, corn starch, and the like. The carbonized organic components may be derived from fiber materials such as resin fibers and cellulose fibers, adhesives that bond these fibers together, resins, additives, and the like.
[0021] The surface of the anode gas diffusion layer substrate of the present invention may be treated to be water repellent as described above. Examples of water repellent materials include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyvinyl fluoride (PVF), polyhexafluoropropylene (FEP), etc. In the water repellent treated anode gas diffusion layer substrate, the water repellent material is in the form of a film or is scattered.
[0022] The weight per unit area of the anode gas diffusion layer substrate of the present invention is preferably 40 to 100 g / m from the viewpoints of gas diffusibility and flexibility. 2 , more preferably 50 to 85 g / m 2 It is.
[0023] The anode gas diffusion layer substrate of the present invention is usually in the form of a sheet (thin plate), and its thickness is preferably 100 to 250 μm, more preferably 130 to 200 μm, from the viewpoints of the rigidity of the anode gas diffusion layer to be formed and the power generation performance of the resulting fuel cell.
[0024] The method for producing the anode gas diffusion layer substrate of the present invention is not particularly limited. A preferred production method includes an aggregate preparation step of preparing an aggregate containing carbon fiber (hereinafter also referred to as "raw material (a)"), graphite particles containing graphite particles (B1) (hereinafter also referred to as "raw material (b)"), and organic fiber to be carbonized in a subsequent carbonization step, a resin impregnation step of impregnating the aggregate with a carbon precursor resin to be carbonized in a subsequent carbonization step to prepare a resin impregnated body, and a carbonization step of heating and baking the resin impregnated body in a non-oxidizing atmosphere, as shown below.
[0025] The assembly preparation step is a step of preparing an assembly including a plurality of raw materials (a), a plurality of raw materials (b), and a plurality of organic fibers. Since there is no change in shape and properties of the raw materials (a) and (b) before and after the production of the anode gas diffusion layer substrate, the configurations described above as components (A) and (B) are applied to both of the raw materials (a) and (b).
[0026] The raw material (b) may consist of only the component (B1), or may consist of the component (B1) and other graphite particles. In the latter case, the upper limit of the content of the other graphite particles is preferably 50 mass%, more preferably 70 mass%. The amount of the raw material (b) used is preferably 70 to 90 mass parts, more preferably 75 to 88 mass parts, based on 100 mass parts of the raw material (a).
[0027] The organic fibers may be any fibers that are carbonized in the subsequent carbonization step, and examples thereof include vegetable fibers (pulp such as wood, cellulose, cotton, bamboo, and hemp), animal fibers (wool, etc.), and resin fibers (polylactic acid, polyvinyl alcohol, polyethylene, polyolefin, polypropylene, polyurethane, polyester, polyamide, vinylon, acrylic, aramid, polyacetal, phenolic resin, etc.). When these organic fibers are pyrolyzed and burned by heating in the subsequent carbonization step, the burned area becomes pores (pores, air holes) for gas and moisture to pass through. Furthermore, the organic fibers also function as a binder that captures carbon fibers and binds them together to improve entanglement when preparing an aggregate by, for example, a papermaking method. In the present invention, it is preferable to use vegetable fibers and resin fibers in combination.
[0028] The average fiber diameter of the organic fibers is preferably 5 to 20 μm, and more preferably 6 to 8 μm, from the viewpoint of the mechanical strength of the aggregate to be formed. The upper limit of the fiber length of the organic fibers is usually 15 mm, and the lower limit is usually 1 mm. The average fiber length of the organic fibers is preferably 1 to 10 mm, and more preferably 1 to 5 mm. The amount of the organic fiber used is preferably 30 to 90 parts by mass, and more preferably 50 to 70 parts by mass, based on 100 parts by mass of the raw material (a).
[0029] In the above-mentioned assembly preparation step, it is preferable to apply a papermaking method. For example, there are a wet papermaking method in which paper is made using a raw material dispersion liquid (slurry) in which a plurality of raw materials (a), a plurality of raw materials (b), and a plurality of organic fibers are dispersed in a dispersion medium (water, organic solvent, etc.), and a dry papermaking method in which a mixture of these raw materials is allowed to fall and accumulate in the air, etc., but the wet papermaking method is preferable from the viewpoints of the uniformity, strength, productivity, thickness, and controllability of basis weight of the raw materials in the assembly.
[0030] For example, the slurry can be separated into solids and dispersion medium by scooping the slurry using a separating member such as a mesh member, or by vacuum suction or drying to form an aggregate. Specifically, the raw material dispersion is supplied to a wet papermaking machine having wires such as a fourdrinier, short wire, or cylinder wire, dehydrated in a dehydration part, and pressed to squeeze out the water to obtain an aggregate. The above slurry may contain binders such as polyvinyl alcohol, polyvinyl acetate, cellulose, polyethylene oxide, styrene-butadiene rubber, starch, and corn starch, coagulants, viscosity adjusters, surfactants, etc., in order to improve papermaking properties and the binding properties (strength) of the contained components. The method for preparing the slurry is not particularly limited, and for example, a rotary device such as a pulper can be used.
[0031] In the above papermaking method, entangling treatment such as mechanical entangling (needle punching, etc.), high pressure liquid jetting (water jet punching, etc.), high pressure gas jetting (steam jet punching, etc.) may be performed.
[0032] The aggregate obtained in the above-mentioned aggregate preparation step preferably has a basis weight of 40 to 100 g / m 2 and the thickness is preferably 100 to 500 μm.
[0033] The resin impregnation step is a step of impregnating the above-obtained assembly with a carbon precursor resin that will be carbonized in a subsequent carbonization step to produce a resin-impregnated body. The carbon precursor resin is not particularly limited, but is preferably a thermosetting resin such as a phenol resin, a furan resin, an epoxy resin, a melamine resin, an imide resin, a urethane resin, an aramid resin, a urea resin, or an unsaturated polyester resin, because it has excellent wettability with the raw material (a), the raw material (b), or the organic fiber, and is likely to form a conductive carbonized material in the subsequent carbonization step. Among these, a phenol resin is particularly preferred, because it has a high carbonization rate and becomes a highly conductive material after carbonization. The carbon precursor resin may be used as it is depending on its properties, but may also be used as a solution (resin solution) obtained by dissolving the carbon precursor resin in a solvent, or as a dispersion (resin dispersion) obtained by dispersing the carbon precursor resin in a dispersion medium. In the resin impregnation step, it is preferable to use a liquid containing a carbon precursor resin (hereinafter referred to as a "carbon precursor resin-containing liquid").
[0034] When the carbon precursor resin-containing liquid is used, a method of immersing an assembly in the carbon precursor resin-containing liquid, a method of applying the carbon precursor resin-containing liquid to an assembly (kiss coating method, spray method, curtain coating method, roller contact method, etc.), etc., can be applied. Of these, the method of immersing an assembly in the carbon precursor resin-containing liquid is preferred. When the carbon precursor resin-containing liquid is used, a resin-impregnated body that does not contain a solvent or dispersion medium can be obtained by using a non-contact drying method in which hot air is blown onto the liquid, the liquid is placed in a high-temperature atmosphere, an infrared heater is used, or microwaves are used, or a contact drying method in which the liquid is brought into contact with a heated roll, plate, or the like.
[0035] Other methods that do not use the carbon precursor resin-containing liquid include a method in which at least a portion of the surface of the aggregate is covered with a resin film containing the carbon precursor resin, and the carbon precursor resin is dissolved by heating or a solvent and allowed to permeate the entire aggregate.
[0036] The resin-impregnated body obtained by the resin impregnation step may contain the carbon precursor resin used as is, or, in the case where the carbon precursor resin is a curable resin, may be a cured resin formed by, for example, an operation (heating, etc.) for removing the solvent or dispersion medium as described above. In order to obtain a resin-impregnated body in which the raw materials (a), (b) and organic fibers contained in the above-mentioned aggregate are bound by a cured resin, and which has a desired thickness and is free of raw materials (a), (b) or organic fibers and has excellent structural stability, a hot press (hydraulic press, hot press, belt press, roll press, etc.) can be performed with the carbon precursor resin in contact with the aggregate.
[0037] In the resin impregnation step, the amount of carbon precursor resin impregnated into the assembly is not particularly limited. In terms of the electrical conductivity and strength of the finally obtained anode gas diffusion layer substrate, the mass ratios of the assembly and the carbon precursor resin in the resin impregnated body are preferably 50 to 90 mass% and 10 to 50 mass%, more preferably 60 to 80 mass% and 20 to 40 mass%, respectively, when the total of the two is taken as 100 mass%.
[0038] The carbonization step is a step of heating and baking the resin-impregnated body in a non-oxidizing atmosphere, which may be an atmosphere containing an inert gas such as argon gas or helium gas, or nitrogen gas. The heating temperature of the resin-impregnated body is preferably 1800° C. to 2500° C., more preferably 1900° C. to 2200° C., in order not to cause a deterioration in the strength of the raw material (a) and to facilitate the carbonization of the resin fiber and the carbon precursor resin. The carbonization step may be performed using a multi-stage heating method in which a heat treatment is performed at a temperature lower than the preferred carbonization temperature. The heating time for the resin-impregnated body depends on the size of the resin-impregnated body, but is usually 1 minute or more.
[0039] The carbonization step carbonizes the resin fibers derived from the aggregate and the carbon precursor resin contained in the resin-impregnated body, and the carbon fibers are bound to each other, the graphite particles are bound to each other, or the carbon fibers and the graphite particles are bound to each other. As a result, an anode gas diffusion layer substrate having the structure shown in FIG. 1 can be obtained. The resulting anode gas diffusion layer substrate has a strong conductive path due to the phase mainly composed of carbide, and since the carbide is derived from a resin, it has elasticity and has high dimensional absorbency when bonded to an electrolyte layer or a catalyst layer during fuel cell production. When a fuel cell produced using this anode gas diffusion layer substrate is operated, the diffusion of water vapor is slowed (water vapor is difficult to escape) in the anode gas diffusion layer containing graphite particles made of component (B1), drying is suppressed, and water retention is maintained, so that it is believed to exhibit high power generation performance.
[0040] When producing an anode gas diffusion layer substrate having a water-repellent surface (hereinafter referred to as a "water-repellent gas diffusion layer substrate for anode"), a water-repellent step of attaching a water-repellent material to the anode gas diffusion layer substrate after the carbonization step can be further included. In this water-repellent step, for example, a method can be applied in which the anode gas diffusion layer substrate is contacted with a solution or dispersion of the water-repellent material, and then heat-treated as necessary. The water-repellent material is preferably composed mainly of a fluororesin such as polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-perfluoroalkylvinyl ether copolymer (PFA), or tetrafluoroethylene-ethylene copolymer (ETFE).
[0041] When manufacturing a fuel cell, the anode gas diffusion layer substrate of the present invention (including the above-mentioned water-repellent anode gas diffusion layer substrate) may be directly applied to a gas diffusion layer electrode, but it is preferable to use a laminate (anode gas diffusion layer laminate) having a microporous layer formed on one side. When a fuel cell obtained by using the anode gas diffusion layer laminate having this microporous layer is operated, flooding caused by large water droplets generated by condensation of water vapor can be suppressed.
[0042] The microporous layer is preferably a microporous layer containing a conductive material and a water-repellent resin, and having a thickness of up to about 100 μm. Examples of the conductive material include carbon black, carbon nanotubes, carbon nanofibers, chopped carbon fibers, graphene, and graphite. As the water-repellent resin, the above-mentioned fluororesin is preferably used.
[0043] The membrane / electrode assembly 100 shown in FIG. 3 can be manufactured using an anode gas diffusion layer substrate (including the above-mentioned water-repellent anode gas diffusion layer substrate) having a microporous layer on one side, a cathode gas diffusion layer substrate having a microporous layer on one side, and a laminate obtained by forming catalyst layers on both sides of an electrolyte membrane (polymer electrolyte membrane) that selectively allows specific ions to pass therethrough. A fuel cell (single cell) can be manufactured using this membrane / electrode assembly 100 and separators (anode side and cathode side).
[0044] In a fuel cell configured as described above, when oxidizing gas is supplied from the outside to the oxidizing gas flow path of the cathode separator, a portion of the oxidizing gas flowing along this oxidizing gas flow path penetrates into the cathode gas diffusion layer. The remaining unreacted oxidizing gas that does not penetrate flows along the oxidizing gas flow path and is discharged to the outside of the fuel cell. Similarly, when fuel gas is supplied from the outside to the fuel gas flow path of the anode separator, a portion of the fuel gas flowing along this fuel gas flow path penetrates into the anode gas diffusion layer. The remaining unreacted fuel gas that does not penetrate flows along the fuel gas flow path and is discharged to the outside of the fuel cell. As a result of the reaction between the oxidizing gas and the fuel gas, electric power is generated between the cathode side separator and the anode side separator. EXAMPLES
[0045] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to these examples as long as the gist of the present invention is not exceeded.
[0046] 1. Raw materials for manufacturing anode gas diffusion layer substrates The manufacturing materials used in the examples and comparative examples are as follows.
[0047] 1-1.Carbon fiber Carbon fiber manufactured by Teijin Ltd. (fiber length: 3 mm, fiber diameter: 7 μm) was used.
[0048] 1-2. Pulp fiber Pulp fiber manufactured by Toyobo Co., Ltd. (fiber length: 2 mm, freeness: 550 ml) was used.
[0049] 1-3.Resin fiber Vinylon fiber (fiber length: 3 mm, fiber diameter: 11 μm) manufactured by Kuraray Co., Ltd. was used.
[0050] 1-4.Graphite particles (1) Graphite particles G1 The graphite powder used was "CMX-40" (product name) manufactured by Nippon Graphite Industries Co., Ltd. The minor axis (thickness) of the particles was 0.9 to 1.2 μm, the average particle diameter d50 measured by the laser diffraction method was 45.46 μm, and the aspect ratio was 45.9. (2) Graphite particles G2 The graphite powder used was "CGB-50" (product name) manufactured by Nippon Graphite Industries Co., Ltd. The particles were spherical, with a minor axis (thickness) of 30 to 50 μm, an average particle diameter d50 measured by laser diffraction method of 59.94 μm, and an aspect ratio of 1.6.
[0051] 2. Manufacturing of anode gas diffusion layer substrate The above-mentioned raw materials were used to produce an anode gas diffusion layer substrate.
[0052] Example 1-1 30 parts by mass of carbon fiber, 13 parts by mass of pulp fiber, 3 parts by mass of resin fiber, and 25 parts by mass of graphite particles G1 were mixed and continuously papered using a cylinder papermaking machine to obtain a roll-shaped raw material sheet in which the carbon fiber, pulp fiber, and resin fiber were entangled and the graphite particles G1 were sandwiched between the gaps between the fibers. The rolled sheet was then impregnated with a binder solution and dried to obtain a graphite particle-attached sheet in which the carbon fibers, pulp fibers, resin fibers, and graphite particles G1 were bound by the binder. The amount of the binder attached was 25 parts by mass per 100 parts by mass of the graphite particle-attached sheet. Thereafter, this graphite particle-attached sheet was pressed with a double belt press (pressure: 1 MPa, temperature: 250° C.) to obtain a compressed sheet having a thickness of 200 μm. Next, this compressed sheet was heat-treated (time: 1 minute) in a graphitization furnace with an internal temperature of 2000°C and a nitrogen gas atmosphere to carbonize the binder, pulp fibers, and resin fibers, thereby obtaining a graphite particle-supported carbon fiber sheet in which graphite particles G1 are encapsulated and the resin carbide bonds the carbon fibers together. 2 The thickness was about 170 μm. Hereinafter, this graphite particle-supporting carbon fiber sheet is referred to as "anode gas diffusion layer substrate AS1." A cross section of the obtained anode gas diffusion layer substrate AS1 was photographed with an electron microscope, obtaining the image shown in Fig. 4. As can be seen from Fig. 4, flake-like graphite with a large aspect ratio is filled between the carbon fibers.
[0053] Example 1-2 The same operation as in Example 1-1 was carried out except that the amounts of carbon fiber, pulp fiber, resin fiber and graphite particles G1 used were changed to 36 parts by mass, 15 parts by mass, 3 parts by mass and 31 parts by mass, respectively, to obtain a fiber sheet having a basis weight of 85 g / m. 2 Thus, an "anode gas diffusion layer substrate AS2" having a thickness of approximately 190 μm was obtained.
[0054] Comparative Example 1-1 The same procedure as in Example 1-1 was repeated except that graphite particles G2 were used instead of graphite particles G1. The basis weight was 92 g / m 2 Thus, an "anode gas diffusion layer substrate AS3" having a thickness of approximately 200 μm was obtained. A cross section of the resulting anode gas diffusion layer substrate AS3 was photographed with an electron microscope, and the image shown in FIG. 5 was obtained.
[0055] 3. Fuel Cell Production and Evaluation The surface of the above-mentioned anode gas diffusion layer substrate AS1, AS2 or AS3 was subjected to a water-repellent treatment to obtain a water-repellent gas diffusion layer substrate for the anode electrode, and then a microporous layer-forming paste was applied to one side of the obtained water-repellent gas diffusion layer substrate for the anode electrode to prepare a gas diffusion layer laminate for the anode electrode having a microporous layer (15). On the other hand, the surface of the cathode gas diffusion layer substrate CS1 was subjected to a water-repellent treatment, and then a microporous layer-forming paste was applied to one side of the substrate to prepare a gas diffusion layer laminate for the cathode electrode having a microporous layer (25). Thereafter, these gas diffusion layer laminates and an electrolyte layer (30) made of a Nafion (registered trademark) series electrolyte membrane "NRE-212" (product name) were coated with a microporous layer-forming paste made of 50 mass% Pt / C with a Pt loading of 0.5 mg / cm on both sides. 2 A membrane / electrode assembly (100) shown in Fig. 3 was produced using a fuel cell electrode membrane having catalyst layers (40, 50) formed of the above-mentioned material. This membrane / electrode assembly (100) sequentially comprises an anode gas diffusion layer (10) derived from a water-repellent anode gas diffusion layer substrate that has been subjected to a water-repellent treatment, a microporous layer (15), a catalyst layer (40), an electrolyte layer (30), a catalyst layer (50), a microporous layer (25), and a cathode gas diffusion layer (20). Next, a JARI standard cell was produced using this membrane / electrode assembly (100) together with a separator, a current collector, etc., and this was incorporated into a single cell for fuel cell evaluation, and the power generation performance was evaluated.
[0056] Example 2-1 (1) Manufacturing of gas diffusion layer laminate for anode A 40 μm-thick polyethylene film was placed on both sides of the anode gas diffusion layer substrate AS1, and the surface pressure was 1.5 MPa to remove free fuzz from the carbon fibers. Next, this film laminate was impregnated with a PTFE dispersion manufactured by Daikin Industries, Ltd., and subjected to a heat treatment (temperature: 200° C., pass time: 5 minutes) to obtain a water-repellent anode gas diffusion layer substrate in which 0.5 parts by mass of PTFE was spread on 100 parts by mass of the anode gas diffusion layer substrate AS1. Thereafter, a paste for forming a microporous layer containing carbon black, fluororesin and water was applied to one side of the water-repellent gas diffusion layer substrate for the anode electrode, and heat treatment was performed (temperature: 320°C, pass time: 5 minutes) to obtain a gas diffusion layer laminate AB1 for the anode electrode in which 3 parts by mass of the microporous layer was spread per 100 parts by mass of the water-repellent gas diffusion layer substrate for the anode electrode.
[0057] (2) Manufacturing of gas diffusion layer laminate for cathode 28 parts by mass of carbon fiber, 10 parts by mass of pulp fiber, 2 parts by mass of resin fiber, and 10 parts by mass of graphite particles G2 were mixed and continuously papered using a cylinder papermaking machine to obtain a roll-shaped raw material sheet in which the carbon fiber, pulp fiber, and resin fiber were entangled and graphite particles were sandwiched in the gaps between the fibers. The rolled sheet was then impregnated with a binder solution and dried to obtain a graphite particle-attached sheet in which the carbon fibers, pulp fibers, resin fibers, and graphite particles G2 were bound by the binder. The amount of the binder attached was 25 parts by mass per 100 parts by mass of the graphite particle-attached sheet. Thereafter, this graphite particle-attached sheet was pressed with a double belt press (pressure: 1 MPa, temperature: 250° C.) to obtain a compressed sheet having a thickness of 200 μm. Next, this compressed sheet was heat-treated (time: 1 minute) in a graphitization furnace with an internal temperature of 2000°C and a nitrogen gas atmosphere to carbonize the binder, pulp fibers, and resin fibers, thereby obtaining a graphite particle-supported carbon fiber sheet in which graphite particles G1 are encapsulated and the resin carbide bonds the carbon fibers together. 2 The thickness was about 150 μm. Hereinafter, this graphite particle-supporting carbon fiber sheet was referred to as "cathode gas diffusion layer substrate CS1." Thereafter, in the same manner as for the anode gas diffusion layer substrate AS1, the cathode gas diffusion layer substrate CS1 was subjected to a water repellent treatment, and then a microporous layer was formed on one side thereof to obtain a cathode gas diffusion layer laminate CB1.
[0058] (3) Fuel cell manufacturing and evaluation Anode gas diffusion layer substrate AS1 was abutted against one side of the fuel cell electrode membrane so that the microporous layer of the anode gas diffusion layer substrate AS1 faced, and cathode gas diffusion layer substrate CS1 was abutted against the other side of the fuel cell electrode membrane so that the microporous layer of the cathode gas diffusion layer substrate CS1 faced, and these were stacked and pressed (pressure: 1 MPa, temperature: 100° C.) using a double belt press device to obtain a membrane / electrode assembly (MEA) 100 with a thickness of 360 μm (see FIG. 3). Next, a JARI standard cell was produced using this membrane / electrode assembly 100, a serpentine separator with one flow channel having a flow channel width of 1.0 mm, a rib width of 1.0 mm, and a groove depth of 1.0 mm, and a current collector plate. This was then incorporated into a single cell for fuel cell evaluation, and a current density of 1.0 A / cm was obtained. 2 The power generation performance was evaluated (cell voltage measurement) under the conditions of a cell temperature of 80° C., an anode side dew point temperature of 77° C., and a cathode side dew point temperature of 60° C. The results are shown in Table 1.
[0059] Example 2-2 An anode gas diffusion layer laminate AB2 was produced in the same manner as in Example 2-1, except that an anode gas diffusion layer substrate AS2 was used instead of an anode gas diffusion layer substrate AS1. A JARI standard cell and a single cell for fuel cell evaluation were then produced in the same manner as in Example 2-1, using this anode gas diffusion layer laminate AB2 together with the cathode gas diffusion layer substrate CS1 in Example 2-1, and the power generation performance was evaluated (see Table 1).
[0060] Comparative Example 2-1 An anode gas diffusion layer laminate AB3 was produced in the same manner as in Example 2-1, except that an anode gas diffusion layer substrate AS3 was used instead of an anode gas diffusion layer substrate AS1. A JARI standard cell and a single cell for fuel cell evaluation were then produced in the same manner as in Example 2-1, using this anode gas diffusion layer laminate AB3 together with the cathode gas diffusion layer substrate CS1 in Example 2-1, and the power generation performance was evaluated (see Table 1).
[0061] [Table 1]
[0062] Examples 2-1 and 2-2 are examples in which an anode gas diffusion layer substrate containing graphite particles according to the present invention was used, and a higher cell voltage was obtained and the resistance values in the thickness direction and the plane direction were reduced compared to Comparative Example 2-1 in which an anode gas diffusion layer substrate containing graphite particles with an aspect ratio of less than 2 was used. From these results, it is understood that the anode gas diffusion layer substrate of the present invention is suitable for producing a fuel cell which has both gas diffusibility and electrical conductivity, and which efficiently discharges water generated during power generation to the outside of the system, thereby suppressing a decrease in power generation performance.
[0063] Incidentally, the present invention is not limited to the above-mentioned specific examples, and various modifications can be made within the scope of the present invention according to the purpose and application. [Industrial Applicability]
[0064] The anode gas diffusion layer substrate of the present invention is suitable as a material for forming an anode gas diffusion layer constituting a membrane / electrode assembly included in a fuel cell. Therefore, a fuel cell including such an anode gas diffusion layer has high power generation performance and can be used as a fuel cell for transportation such as a vehicle, a stationary fuel cell, etc. The anode gas diffusion layer substrate of the present invention can also be used as an electromagnetic shielding material, a conductive sheet, a carbonaceous cushioning material, a furnace wall insulating material for a high-temperature vacuum furnace, and the like. [Explanation of symbols]
[0065] 1: Gas diffusion layer substrate for anode 3: Carbon fiber 5: (rod-shaped) graphite particles 7: (Spherical) graphite particles 10: Gas diffusion layer for anode 15: Microporous layer 20: Gas diffusion layer for cathode 25: Microporous layer 30: Electrolyte layer 40: Catalyst layer 50: Catalyst layer 100: Membrane / electrode assembly
Claims
1. (A) carbon fibers; (B) graphite particles; A gas diffusion layer substrate for an anode electrode of a fuel cell, comprising: The graphite particles (B) have a major axis of d L The minor axis is d S In this case, the major diameter d L and the minor diameter d S The ratio Dr (= d L / d S ) contains 20 to 100 rod-shaped graphite particles (B1).
2. 2. The anode gas diffusion layer substrate according to claim 1, wherein the graphite particles (B1) have an average particle size d50 of 20 to 80 μm as measured by a laser diffraction method.
3. 3. The anode gas diffusion layer substrate according to claim 1, wherein a content ratio of the graphite particles (B) is 70 to 90 parts by mass relative to 100 parts by mass of a content of the carbon fibers (A).
4. Weight per unit area: 40 to 100 g / m 2 The anode gas diffusion layer substrate according to claim 1 , wherein
5. 5. The gas diffusion layer substrate for an anode according to claim 1, wherein the surface of the substrate is treated to be water repellent.
Citation Information
Patent Citations
Electrode catalyst layer and manufacture thereof and fuel cell using electrode catalyst layer
JP2000353528A
nonwoven web
JP2002536565A
Gas diffusion electrode for fuel cell and manufacturing method thereof
JP2004055393A
gas diffusion substrate
JP2008503043A
Carbon fiber sheet and its manufacturing method
JP2009289552A