Graphite negative electrode composite material, preparation method thereof and lithium ion battery

Through the coordinated modification methods of gas-phase etching, conductive agent dispersed coating and nitrogen-doped hard carbon coating, the problem of insufficient capacity and poor kinetics in high-energy density lithium-ion batteries is solved, and high Capacity, high compaction and fast charging performance improve the overall performance of lithium-ion batteries.

CN118929653APending Publication Date: 2024-11-12ZHEJIANG ZEEKR INTELLIGENT TECH CO LTD +2

Patent Information

Application Number
CN202410990628.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Graphite negative electrode materials have problems of insufficient capacity and poor kinetics in high-energy density lithium-ion batteries, and when improving graphite's high compaction and fast charging performance, the contradiction between capacity decay and kinetic decline is prone to the contradiction between capacity decay and kinetic decline.

Method used

Using a coordinated modification method of gas phase etching, conductive agent dispersed coating and nitrogen doped hard carbon coating, the porous graphite precursor is formed through primary heat treatment, and then dispersed in the conductive agent dispersant and undergoes secondary heat treatment, and finally in nitrogen The elemental polymer is coated to form a three-layer structure of graphite-conductive agent-hard carbon.

Benefits of technology

The high capacity, high compaction and fast charging performance of graphite negative electrode materials is achieved, the influence of conductive agents and hard carbon on performance is balanced, and the charging rate and high-temperature storage performance of lithium-ion batteries are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929653A_ABST
    Figure CN118929653A_ABST
Patent Text Reader

Abstract

The invention relates to a graphite negative electrode composite material, a preparation method thereof and a lithium ion battery, and the preparation method comprises the following steps: carrying out primary heat treatment on a graphite raw material to obtain a porous graphite precursor with a porous structure; dispersing the porous graphite precursor and a conductive agent in a dispersing agent to obtain porous graphite doped with the conductive agent; and carrying out coating modification on the porous graphite, and carrying out secondary heat treatment to obtain the graphite negative electrode composite material. The graphite negative electrode composite material synergistically modified through gas phase etching, conductive agent dispersion coating and nitrogen-doped hard carbon coating has the characteristics of high capacity, high compaction and high dynamics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a graphite negative electrode composite material and a preparation method thereof, and a lithium-ion battery. Background Art

[0002] Graphite has been used as the mainstream negative electrode material for lithium-ion batteries due to its low cost and stable performance. However, with the rapid development of the new energy industry, higher capacity and higher rate performance are regarded as important indicators. The theoretical capacity of graphite is only 372mAh / g, which seriously reduces the application of graphite materials in high energy density lithium-ion batteries. In addition, graphite materials also expose problems such as insufficient kinetics and severe lithium precipitation at high rates. Therefore, it is of great significance to modify graphite and develop a graphite negative electrode material with high capacity and high kinetics.

[0003] At present, there is a certain contradictory relationship between the high compaction, high capacity and fast charging performance of graphite. It is generally believed that increasing the graphitization degree of graphite can increase the capacity and compaction of graphite, but it will inevitably bring about the problem of decreased kinetics; surface coating of graphite can improve the kinetics of graphite, but it will also bring the risk of capacity decay and reduced compaction.

[0004] Therefore, there is an urgent need to provide a graphite negative electrode composite material and a preparation method thereof and a lithium ion battery to solve the above-mentioned technical problems. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present application provides a graphite negative electrode composite material, a preparation method thereof and a lithium-ion battery. The graphite negative electrode composite material synergistically modified by vapor phase etching, conductive agent dispersion coating, and nitrogen-doped hard carbon coating exhibits the characteristics of high capacity, high compaction, and high kinetics.

[0006] In order to achieve the purpose of this application, this application adopts the following technical solutions:

[0007] In a first aspect, a method for preparing a graphite negative electrode composite material is provided, comprising the following steps:

[0008] The graphite raw material is subjected to a primary heat treatment to obtain a porous graphite precursor having a porous structure;

[0009] Dispersing the porous graphite precursor and the conductive agent in a dispersant to obtain porous graphite doped with the conductive agent;

[0010] The porous graphite is coated and modified, and subjected to secondary heat treatment to obtain the graphite negative electrode composite material.

[0011] The present application uses a porous gas phase etching method to create a pore structure on the surface of graphite raw materials and modify the graphite morphology, thereby improving the capacity and compaction of graphite; by dispersing a conductive agent in a liquid phase and filling it into the pores of a porous graphite precursor, the specific surface area of ​​graphite is reduced and the overall conductivity is improved; then nitrogen-doped hard carbon is coated on its surface, which simultaneously plays a role in capping the conductive agent and enhancing the desolvation of lithium ions. The graphite negative electrode composite material synergistically modified by gas phase etching, conductive agent dispersion coating, and nitrogen-doped hard carbon coating exhibits the characteristics of high capacity, high compaction, and high kinetics.

[0012] Preferably, before the initial heat treatment, the method further includes: placing the graphite raw material in an oxidizing gas for oxidation, wherein the oxidizing gas is one or more of oxygen, carbon dioxide, air, and water vapor.

[0013] Preferably, the graphite raw material D50 ranges from 10μm to 18μm, for example, it can be 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm%, 17μm%, 18μm; further, the graphite raw material D50 ranges from 13μm to 16μm, for example, it can be 13μm, 14μm, 15μm, 16μm%.

[0014] Preferably, the temperature range of the initial heat treatment is between 800°C and 1200°C, for example, it can be 800°C, 1000°C, 1050°C, 1100°C, 1150°C, 1200°C; further, the time range of the initial heat treatment is between 2h and 12h, for example, it can be 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h.

[0015] Preferably, the temperature range of the initial heat treatment is between 1000°C and 1100°C, for example, it can be 1000°C, 1050°C, or 1100°C; further, the time range of the initial heat treatment is between 6h and 12h, for example, it can be 6h, 7h, 8h, 9h, 10h, 11h, or 12h.

[0016] Preferably, the specific surface area of ​​the porous graphite precursor is 3m 2 / g~4m 2 / g, and the pore size is 50nm~200nm.

[0017] Preferably, the weight ratio of the porous graphite precursor, the conductive agent and the dispersant is 85-95:2.5-7.5:2.5-7.5.

[0018] Preferably, the dispersant has a solid content of 1.5% to 3.5%, the solvent is water, and the solid content may be, for example, 1.5%, 2%, 2.5%, 3.0%, or 3.5%.

[0019] Preferably, the coating modification comprises: placing the porous graphite in a high molecular polymer containing nitrogen and stirring the mixture so that the high molecular polymer is uniformly coated on the surface of the porous graphite.

[0020] Preferably, the mass ratio of the porous graphite to the high molecular polymer is 6 to 3:1.

[0021] Preferably, the stirring time ranges from 4 h to 12 h, for example, it can be 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h, 12 h; further, the stirring time ranges from 6 h to 8 h, for example, it can be 6 h, 7 h, 8 h.

[0022] Preferably, the temperature range of the secondary heat treatment is between 600℃ and 1000℃, for example, it can be 600℃, 650℃, 700℃, 750℃, 800℃, 850℃, 900℃, 950℃, 1000℃; further, the temperature range of the secondary heat treatment is between 700℃ and 800℃, for example, it can be 700℃, 750℃, 800℃.

[0023] Preferably, the time range of the secondary heat treatment is 0.5h to 5h, for example, it can be 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h; further, the time range of the secondary heat treatment is between 2h and 3h, for example, it can be 2h, 2.5h, 3h.

[0024] In a second aspect, a graphite negative electrode composite material is provided, wherein the graphite negative electrode composite material is prepared by the above method.

[0025] The graphite negative electrode composite material in the present application has a three-layer structure of graphite-conductive agent-hard carbon, which makes up for the electron loss at the interface between the traditional hard carbon coating layer and the graphite, and improves the traditional efficiency of electrons at the interface by using the conductive agent intermediate layer as a bridge; the porous structure of the graphite provides a good base for the coating of the conductive agent, and the pore filling method increases the coating rate of the conductive agent, and the excellent capacity and compaction of the porous graphite balance the deterioration of these properties by the conductive agent and hard carbon, thereby obtaining fast-charging graphite with higher capacity and compaction.

[0026] Preferably, the specific surface area of ​​the graphite negative electrode composite material is 1.8 to 3 m 2 / g, for example, 1.8m 2 / g, 2.0m 2 / g, 2.5m 2 / g, 3.0m 2 / g.

[0027] Preferably, the D50 of the graphite negative electrode composite material is in the range of 12 μm to 20 μm, for example, it can be 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, or 20 μm.

[0028] Preferably, the graphite negative electrode composite material is doped with nitrogen, and the nitrogen content ranges from 0.5 to 3%, for example, 0.5%, 1%, 1.5%, 2%, 2.5%, or 3.0%.

[0029] Nitrogen doping within a certain range can increase the pseudocapacitance of the battery and increase the capacity, but as the content increases, the graphite carbon structure gradually changes from a regular six-membered ring to an irregular structure, resulting in a decrease in the degree of graphitization and a decrease in conductivity.

[0030] In a third aspect, a lithium-ion battery is provided, the lithium-ion battery comprising a positive electrode sheet, a negative electrode sheet and a separator disposed between the positive electrode sheet and the negative electrode sheet, the negative electrode sheet comprising the graphite negative electrode composite material.

[0031] Compared with the prior art, this application has the following beneficial effects:

[0032] The present application provides a graphite negative electrode composite material, which further improves the capacity of the graphite by etching the microcrystalline area with low graphitization degree on the graphite surface by gas phase etching; and plays a shaping role on the graphite during the gas phase etching process, which can improve the compaction of the graphite; overcomes the problem of conductive agent agglomeration by liquid phase dispersion, and fills the conductive agent in the graphite pores by high-speed dispersion to reduce the specific surface area of ​​the graphite and improve the overall conductivity; nitrogen-doped hard carbon coating is performed on the outermost layer of the graphite, which, on the one hand, protects the conductive agent and prevents the electrolyte from directly contacting the conductive agent and causing a decrease in storage performance; on the other hand, the overall charging rate is improved by the fast lithium embedding speed of the hard carbon, and the doping of nitrogen elements makes its surface have lone pairs of electrons, which attract lithium ions; thus, the graphite negative electrode composite material synergistically modified by gas phase etching, conductive agent dispersion coating, and nitrogen-doped hard carbon coating exhibits the characteristics of high capacity, high compaction, and high kinetics. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 Schematic diagram of the process for preparing the graphite negative electrode composite material in this embodiment;

[0034] Figure 2 This is a SEM image of the graphite negative electrode composite material prepared in this example. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0036] It should be noted that the illustrations provided in this embodiment only illustrate the basic concept of the present application in a schematic manner, and therefore the drawings only show components related to the present application rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0037] The structures, proportions, sizes, etc. illustrated in the drawings of this specification are only used to match the contents disclosed in the specification so as to facilitate understanding and reading by persons familiar with this technology. They are not used to limit the conditions under which this application can be implemented, and therefore have no substantive technical significance. Any structural modification, change in proportion or adjustment of size, without affecting the effects and purposes that can be achieved by this application, should still fall within the scope of the technical contents disclosed in this application.

[0038] The directions or positional relationships indicated by the terms "upper", "lower", "left", "right", "middle", "longitudinal", "lateral", "horizontal", "inner", "outer", "radial", "circumferential" and the like in this specification are based on the directions or positional relationships shown in the drawings and are only for the convenience of simplifying the description. They do not indicate or imply that the devices or elements referred to must have a specific direction, be constructed and operate in a specific direction, and therefore cannot be understood as limiting the present application. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.

[0039] Example 1

[0040] Please refer to Figure 2 As shown, this embodiment provides a graphite negative electrode composite material, and the specific surface area of ​​the graphite negative electrode composite material is 2.5m 2 / g, the D50 range of the graphite negative electrode composite material is 16μm, and the graphite negative electrode composite material is also doped with 1.5% nitrogen element.

[0041] Please refer to Figure 1 As shown, the preparation method of the negative electrode composite material is as follows:

[0042] S1, placing a graphite raw material with an average particle size D50 of 15.3 in an oxidizing gas such as air for heating for 7 hours, and graphitizing it at a primary heat treatment temperature of 1050°C to obtain a porous graphite precursor. Preferably, the graphite raw material is one or more of artificial graphite with a secondary particle structure, natural graphite with a secondary particle structure, artificial graphite with a single particle structure, and natural graphite with a single particle structure. In this embodiment, artificial graphite with a secondary particle structure is preferably used.

[0043] S2, the porous graphite precursor and the conductive agent obtained in S1 are placed in a dispersant with a solid content of 2% and dispersed and mixed at a high speed in a mass ratio of 90:5:5, and then spray-dried to obtain porous graphite doped with a conductive agent, and the conductive agent below 2 μm not attached to the porous graphite is removed by sieving. Preferably, the conductive agent is one or more of acetylene black, graphene, and carbon nanotubes. In this embodiment, carbon nanotubes (Carbon Nanotubes, CNT) are preferably used. The dispersant is one or more of sodium carboxymethyl cellulose and lithium carboxymethyl cellulose. In this embodiment, sodium carboxymethyl cellulose (CMC-Na) is preferably used.

[0044] S3, the porous graphite obtained in S2 is placed in a polymer such as polyacrylamide containing 1.5% nitrogen element at a mass ratio of 4:1, and the mixture is mechanically stirred for 7 hours, so that the polyacrylamide is evenly coated on the surface of the porous graphite, and the coating is carried out at a secondary heat treatment temperature of 750°C after spray drying, and heated for 2.5 hours to obtain a high-density fast-charging graphite negative electrode composite material. Preferably, the high-molecular polymer containing nitrogen element is one or more of polydopamine, polyaniline, polyacrylamide, and polyurethane.

[0045] Example 2

[0046] This embodiment provides a graphite negative electrode composite material, the specific surface area of ​​the graphite negative electrode composite material is 1.8m 2 / g, the D50 range of the graphite negative electrode composite material is 12μm, and the graphite negative electrode composite material is also doped with 0.5% nitrogen element.

[0047] S1, placing a graphite raw material with an average particle size D50 of 15.3 in an oxidizing gas such as air and heating it for 2 hours, and graphitizing it at a primary heat treatment temperature of 1050° C. to obtain a porous graphite precursor.

[0048] S2. The porous graphite precursor and the conductive agent such as carbon nanotubes obtained in S1 are placed in a dispersant such as sodium carboxymethyl cellulose with a solid content of 1.5% and dispersed and mixed at a high speed in a mass ratio of 86:7:7, and then spray-dried to obtain porous graphite doped with carbon nanotubes, and the conductive agent with a particle size of less than 2 μm that is not attached to the porous graphite is removed by sieving.

[0049] S3. The porous graphite obtained in S2 is placed in a high molecular polymer such as polyacrylamide containing 0.5% nitrogen element at a mass ratio of 3:1, and the mixture is mechanically stirred for 4 hours to make the polyacrylamide evenly coated on the surface of the porous graphite. After spray drying, the coating is performed at a secondary heat treatment temperature of 750°C, and after heating for 0.5 hours, a high-density fast-charging graphite negative electrode composite material is obtained.

[0050] Example 3

[0051] This embodiment provides a graphite negative electrode composite material, the specific surface area of ​​the graphite negative electrode composite material is 3m 2 / g, the D50 range of the graphite negative electrode composite material is 20μm, and the graphite negative electrode composite material is also doped with 3% nitrogen element.

[0052] S1, placing a graphite raw material with an average particle size D50 of 15.3 in an oxidizing gas such as air and heating it for 12 hours, and graphitizing it at a primary heat treatment temperature of 1050° C. to obtain a porous graphite precursor.

[0053] S2. The porous graphite precursor and the conductive agent such as carbon nanotubes obtained in S1 are placed in a dispersant such as sodium carboxymethyl cellulose with a solid content of 3% and dispersed and mixed at a high speed in a mass ratio of 94:3:3, and then spray-dried to obtain porous graphite doped with carbon nanotubes, and the conductive agent with a particle size of less than 2 μm that is not attached to the porous graphite is removed by sieving.

[0054] S3. The porous graphite obtained in S2 is placed in a high molecular polymer such as polyacrylamide containing 3% nitrogen at a mass ratio of 6:1, and the mixture is mechanically stirred for 12 hours to uniformly coat the surface of the porous graphite with polyacrylamide. After spray drying, the mixture is coated at a secondary heat treatment temperature of 750°C, and heated for 5 hours to obtain a high-density fast-charging graphite negative electrode composite material.

[0055] Example 4

[0056] The only difference between Example 4 and Example 1 is that the average particle size D50 of the graphite raw material is 10.2, and the rest is the same as Example 1.

[0057] Example 5

[0058] The only difference between Example 5 and Example 1 is that the average particle size D50 of the graphite raw material is 17.8, and the rest is the same as Example 1.

[0059] Example 6

[0060] The only difference between Example 6 and Example 1 is that the oxidizing gas is oxygen, and the rest is the same as Example 1.

[0061] Example 7

[0062] The only difference between Example 7 and Example 1 is that the oxidizing gas is carbon dioxide, and the rest is the same as Example 1.

[0063] Example 8

[0064] The only difference between Example 8 and Example 1 is that the oxidizing gas is water vapor, and the rest is the same as Example 1.

[0065] Example 9

[0066] The only difference between Example 9 and Example 1 is that the initial heat treatment temperature in S1 is 750°C, and the rest is the same as Example 1.

[0067] Example 10

[0068] The only difference between Example 10 and Example 1 is that the initial heat treatment temperature in S1 is 1150°C, and the rest is the same as Example 1.

[0069] Embodiment 11

[0070] The only difference between Example 11 and Example 1 is that the conductive agent is SP (SUPER PL i, SP), and the rest is the same as Example 1.

[0071] Example 12

[0072] The only difference between Example 12 and Example 1 is that the conductive agent is graphene, and the rest is the same as Example 1.

[0073] Example 13

[0074] The only difference between Example 13 and Example 1 is that the dispersant is lithium carboxymethyl cellulose (CMC-Li), and the rest is the same as Example 1.

[0075] Embodiment 14

[0076] The only difference between Example 14 and Example 1 is that the dispersant is polyacrylic acid (PAA), and the rest is the same as Example 1.

[0077] Embodiment 15

[0078] The only difference between Example 15 and Example 1 is that the high molecular polymer is polydopamine, and the rest is the same as Example 1.

[0079] Example 16

[0080] The only difference between Example 16 and Example 1 is that the secondary heat treatment temperature in S3 is 950°C, and the rest is the same as Example 1.

[0081] Embodiment 17

[0082] The only difference between Example 17 and Example 1 is that the secondary heat treatment temperature in S3 is 650°C, and the rest is the same as Example 1.

[0083] Comparative Example 1

[0084] The difference between Comparative Example 1 and Example 1 is that the operation of step S1 is not performed, and the rest is the same as Example 1.

[0085] Comparative Example 2

[0086] The difference between Comparative Example 2 and Example 1 is that the operation of step S2 is not performed, and the rest is the same as Example 1.

[0087] Comparative Example 3

[0088] The difference between Comparative Example 3 and Example 1 is that the operation of step S3 is not performed, and the rest is the same as Example 1.

[0089] Comparative Example 4

[0090] The only difference between Comparative Example 4 and Example 1 is that the average particle size D50 of the graphite raw material is 8.7, and the rest is the same as Example 1.

[0091] Comparative Example 5

[0092] The only difference between Comparative Example 5 and Example 1 is that the average particle size D50 of the graphite raw material is 19.5, and the rest is the same as Example 1.

[0093] Comparative Example 6

[0094] The only difference between Comparative Example 6 and Example 1 is that the initial heat treatment temperature in S1 is 650° C., and the rest is the same as Example 1.

[0095] Comparative Example 7

[0096] The only difference between Comparative Example 7 and Example 1 is that the initial heat treatment temperature in S1 is 1300° C., and the rest is the same as Example 1.

[0097] Comparative Example 8

[0098] The only difference between Comparative Example 8 and Example 1 is that the secondary heat treatment temperature in S3 is 1100° C., and the rest is the same as Example 1.

[0099] Comparative Example 9

[0100] The only difference between Comparative Example 9 and Example 1 is that the secondary heat treatment temperature in S3 is 550° C., and the rest is the same as Example 1.

[0101] Comparative Example 10

[0102] The only difference between Comparative Example 10 and Example 1 is that the mass ratio of graphite, conductive agent and dispersant is 86:7:7.

[0103] Comparative Example 11

[0104] The only difference between Comparative Example 11 and Example 1 is that the mass ratio of graphite, conductive agent and dispersant is 94:3:7.

[0105] Comparative Example 12

[0106] The only difference between Comparative Example 12 and Example 1 is that the mass ratio of graphite to high molecular polymer is 3:1.

[0107] Comparative Example 13

[0108] The only difference between Comparative Example 13 and Example 1 is that the mass ratio of graphite to high molecular polymer is 6:1.

[0109] The process parameter settings of the above-mentioned Example 1, Examples 4-17 and Comparative Examples 1-9 are shown in Table 1:

[0110] Table 1

[0111]

[0112] The graphite negative electrode composite materials provided in Example 1, Examples 4-17 and Comparative Examples 1-9 were tested, and the test results are shown in Table 2:

[0113] Table 2

[0114]

[0115] The graphite negative electrode composite materials provided in Example 1 and Comparative Examples 10-13 were tested, and the test results are shown in Table 3:

[0116] Table 3

[0117]

[0118] Combining the analysis of Example 1 and Comparative Examples 1, 2 and 3, in Comparative Example 1, only the graphite raw material was coated with a conductive agent and nitrogen-doped hard carbon, in Comparative Example 2, only the graphite raw material was etched to form pores and nitrogen-doped hard carbon was coated, and in Comparative Example 3, only the graphite raw material was etched to form pores and coated with a conductive agent; from the performance comparison between Example 1 and the comparative example, it can be seen that Example 1, which is coated with an etching agent and a nitrogen-doped hard carbon, has improved capacity, compaction, double charge capacity retention rate and high-temperature storage performance, among which the improvement in capacity and compaction is related to the etching of microcrystals with low graphitization degree on the graphite surface by etching and forming pores and the morphology modification of graphite; Comparative Example 1 Since no etching is performed to form pores, the conductive agent and nitrogen-doped hard carbon are directly coated on the graphite surface. Compared with Example 1, in which the conductive agent is filled in the graphite pores during the dispersion process and the surface is coated with hard carbon to act as a cap, the graphite negative electrode composite material in Example 1 has a three-layer structure of graphite-conductive agent-nitrogen-doped hard carbon. The conductive agent makes up for the poor electron transmission ability between hard carbon and graphite, thereby significantly improving its charging capacity. In addition, the specific surface area of ​​porous graphite is reduced by coating with the conductive agent and hard carbon, and dispersing the conductive agent and embedding it in the pores also reduces the direct contact between the conductive agent and the electrolyte, thereby improving the high-temperature storage performance.

[0119] It can be seen from Comparative Examples 2 and 3 that only coating with conductive agent or nitrogen-doped hard carbon cannot achieve a relatively ideal fast charging rate and high temperature storage performance. This is because if the porous graphite is only coated with conductive agent, on the one hand, the coated conductive agent will directly contact with the electrolyte, resulting in electron loss and thus poor high temperature storage performance; on the other hand, the graphite surface lacks an amorphous carbon layer that meets the requirements for rapid lithium insertion, resulting in a decrease in its rate performance; if only porous graphite is coated with nitrogen-doped hard carbon, the electron transfer at the interface between hard carbon and graphite is hindered, so the rate performance in Comparative Example 3 is poor.

[0120] In combination with Example 1, Example 4, Example 5, and Comparative Examples 4-5, the effect of the particle size of the graphite raw material on the graphite negative electrode composite material was investigated; when the graphite particle size is too large (Comparative Example 5), the gas etching of the graphite may be concentrated on a certain side, resulting in insufficient etching, and due to the limitation of the particle size, the rate performance in Comparative Example 5 is poor; when the graphite particle size is too small (Comparative Example 4), it may cause storage performance to deteriorate.

[0121] In combination with Example 1, Examples 6-7, and Comparative Examples 6-7, the effect of the initial heat treatment temperature in S1 on the performance of the graphite negative electrode composite material was investigated. When the temperature is too low (such as Comparative Example 6), the reaction activity between air and graphite is low, resulting in insufficient surface pore formation and morphology finishing; when the temperature is too high (such as Comparative Example 7), excessive reaction between air and the graphite surface occurs, resulting in the collapse of the surface pore structure and a reduction in particle size, which leads to a serious deterioration in its high-temperature storage performance.

[0122] In combination with Example 1, Examples 16-17, and Comparative Examples 8-9, the effect of the secondary heat treatment temperature in S3 on the performance of the graphite negative electrode composite material was investigated. The carbonization temperature during the carbonization process of the hard carbon coating layer has a decisive influence on its performance. When the carbonization temperature is high (such as Comparative Example 8), the coated hard carbon will be over-graphitized, resulting in a decrease in its fast charging performance; when the carbonization temperature is too low (Comparative Example 9), the degree of graphitization of the hard carbon is low and there are a large number of defects and pores on the surface, which causes its storage performance to deteriorate seriously.

[0123] Combined with the analysis of Example 1 and Comparative Examples 10-11, the hard carbon formed after the carbonization of the conductive agent and the dispersant provides less capacity. Therefore, as the graphite content decreases, the capacity, compaction and high-temperature storage performance of the graphite negative electrode composite material will decrease rapidly. However, the increase in the conductive agent content is beneficial to the improvement of the fast charging performance of the material.

[0124] Combined with the analysis of Example 1 and Comparative Examples 12-13, the proportion of the polymer is mainly used to adjust the N element doping content and the surface hard carbon coating amount; the higher the hard carbon content, the faster charging performance will be improved, but the high temperature storage performance and compaction will be lost.

[0125] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0126] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.

Claims

1. A method for preparing a graphite negative electrode composite material, characterized in that: The following steps are involved: The graphite raw material is subjected to a primary heat treatment to obtain a porous graphite precursor having a porous structure; Dispersing the porous graphite precursor and the conductive agent in a dispersant to obtain porous graphite doped with the conductive agent; The porous graphite is coated and modified, and subjected to secondary heat treatment to obtain the graphite negative electrode composite material.

2. The method according to claim 1, characterized in that Before the initial heat treatment, the method further includes: placing the graphite raw material in an oxidizing gas for oxidation, wherein the oxidizing gas is one or more of oxygen, carbon dioxide, air, and water vapor.

3. The method according to claim 1 or 2, characterized in that: The D50 of the graphite raw material ranges from 10 μm to 18 μm; and / or, The temperature range of the initial heat treatment is between 800°C and 1200°C; and / or, The time range of the initial heat treatment is between 2h and 12h; and / or, The specific surface area of ​​the porous graphite precursor is 3m 2 / g~4m 2 / g, and the pore size is 50nm~200nm.

4. The method according to claim 1, characterized in that The weight ratio of the porous graphite precursor, the conductive agent and the dispersant is 85 to 95: 2.5~7.5:2.5~7.5。 5. The method according to claim 1 or 4, characterized in that: The solid content of the dispersant is 1.5% to 3.5%, and the solvent is water.

6. The method according to claim 1, characterized in that The coating modification comprises: placing the porous graphite into a high molecular polymer containing nitrogen and stirring the mixture, so that the high molecular polymer is evenly coated on the surface of the porous graphite.

7. The method according to claim 6, characterized in that The mass ratio of the porous graphite to the high molecular polymer is 6 to 3:

1.

8. The method according to claim 6 or 7, characterized in that: The stirring time ranges from 4h to 12h; and / or, The temperature range of the secondary heat treatment is between 600°C and 1000°C; and / or, The time range of the secondary heat treatment is between 0.5h and 5h.

9. A graphite negative electrode composite material, characterized in that: The graphite negative electrode composite material is prepared by the method according to any one of claims 1 to 8; and / or, The specific surface area of ​​the graphite negative electrode composite material is 1.8 to 3 m 2 / g; and / or, The D50 range of the graphite negative electrode composite material is between 12 μm and 20 μm; and / or, The graphite negative electrode composite material is doped with nitrogen, and the nitrogen content ranges from 0.5 to 3%.

10. A lithium ion battery, characterized in that: The lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet, and a separator disposed between the positive electrode sheet and the negative electrode sheet, and the negative electrode sheet comprises the graphite negative electrode composite material as claimed in claim 9.

Citation Information

Patent Citations

  • Nitrogen-doped carbon-coated hybrid graphite composite material, preparation method thereof and application in lithium ion battery

    CN109449428A

  • Preparation method of graphite negative electrode of lithium battery

    CN114784231A

  • Graphite composite material, preparation method and application thereof and lithium ion battery

    CN117638060A

  • Graphite negative electrode material for high-performance lithium ion battery and preparation method therefor

    WO2021189836A1

Cited By

  • Polymer modified graphite material as well as preparation method and application thereof

    CN119170788A

  • Secondary battery and preparation method thereof, energy storage battery pack and electric equipment

    CN120199762A

  • Secondary battery and preparation method thereof, energy storage battery pack and electrical equipment

    CN120199762B