A method for preparing high purity metallic arsenic from arsenic-containing solid waste in a short process
By employing a synergistic crystallization process using polymeric organic materials to control arsenic acid double salt formation, the method effectively addresses the challenge of producing high-purity arsenic from arsenic-containing waste, achieving efficient and cost-effective separation from impurities.
Patent Information
- Application Number
- JP2023510380
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-03-25
- Filing Date
- 2022-10-19
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2042-10-19
AI Technical Summary
Existing methods for producing high-purity arsenic from arsenic-containing solid waste are complex, costly, and inefficient due to the difficulty in separating arsenic from impurities like antimony, selenium, and bismuth, leading to the need for additional purification steps.
A method involving the synergistic use of water-soluble and hydrophobic polymeric organic materials with specific functional groups to control the crystallization of arsenic acid double salt, followed by reduction roasting, to achieve high-purity arsenic by enhancing the separation of arsenic from impurities.
The method results in high-purity arsenic with a purity of 99% or more, simplifying the process, reducing costs, and meeting industrial production needs while achieving advanced separation of arsenic from impurities.
Smart Images

Figure 0007554517000001 
Figure 0007554517000002 
Figure 0007554517000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for recycling arsenic-containing solid waste from non-ferrous smelting, specifically to a method for preparing high-purity metallic arsenic from arsenic-containing solid waste, which is applicable to the technical fields of detoxification and recycling of arsenic-containing solid waste from non-ferrous smelting. [Background technology]
[0002] Traditionally, arsenic has been recognized as a serious environmental pollution and a threat to human life and health, and arsenic has always been feared. However, arsenic is an amphoteric element with very special physical and chemical properties, and is the core raw material of semiconductor materials, and is widely used in strategic emerging industries such as chips, electronic information, biomedicine, photovoltaics, military industry, and aerospace. The application of high-grade arsenic products made from high-purity arsenic in many fields such as new materials, electronic information, biomedicine, and high-end equipment manufacturing is rapidly replacing the application of low-grade arsenic products made from diarsenic trioxide in the fields of pesticides, corrosion prevention, glass, ceramics, etc., and the global demand continues to expand.
[0003] Most of the arsenic originates from the artificial mining, dressing and smelting of coexistent and associated arsenic metal ores, and is mainly present in the form of smelting by-products in arsenic-containing solid wastes such as flue dust, arsenic alkali slag, anode mud, arsenic sulfide slag, and arsenic coat, which have characteristics such as high arsenic content, complex composition, and difficulty in treatment, and pose a great threat to the surrounding environment. In fact, the arsenic content in these solid wastes is much higher than that of conventional arsenic minerals (rhododendrons), and there is a possibility of preparing arsenic products. Summary of the Invention [Problem to be solved by the invention]
[0005] In the conventional process, arsenic-containing solid waste is treated by dry roasting, and the by-product diarsenic trioxide is recovered, and then the diarsenic trioxide product is used to further prepare high-purity arsenic. However, the diarsenic trioxide product produced by dry roasting inevitably contains some impurity components similar to the properties of arsenic, such as selenium, antimony, and bismuth. To produce high-purity arsenic using this as raw material, it is necessary to repeatedly purify it, which makes the process complicated, the operation difficult, and the cost high. In a Chinese patent (CN101935767B), a method is used that combines multiple sublimation distillation and hydrogen reduction to remove impurities in diarsenic trioxide and prepare high-purity arsenic, but the operation is very complicated. At present, some research is being conducted on the development of technology to recover elemental arsenic from arsenic-containing solid waste, but the focus of the research is on improving the recovery rate of elemental arsenic, and does not attach importance to the quality of elemental arsenic. For example, a Chinese patent (CN1068936864A) provides a method for recovering arsenic from black copper mud, which first uses lime to precipitate the arsenic components in the black copper mud alkali leachate, and then reduces and roasts the arsenic components in the arsenic calcium slag to convert the arsenic-containing solid waste into elemental arsenic. However, the arsenic content in the prepared arsenic product is only above 95%, and the subsequent preparation of high-purity arsenic using the elemental arsenic still requires a complex purification and impurity removal process. As can be seen from the above, the key to producing high-purity arsenic is to develop a technology for highly separating arsenic from similar impurities such as antimony, selenium, and bismuth to prepare high-purity metallic arsenic raw material. A Chinese patent (CN108611494A) proposes a method for efficiently and comprehensively utilizing arsenic alkali slag as a resource. This method solves the problem of efficient separation of arsenic and alkali in alkaline leachate by crystallizing and precipitating double arsenic acid salt, and realizes the recovery of alkaline components as resources. Subsequent research has found that the high selectivity of the crystallization process of double arsenic acid salt not only ensures the separation of arsenic and alkali, but also realizes the initial separation of arsenic from impurity components (such as antimony, selenium, aluminum, etc.) in the leachate, providing the possibility for the purification and purification of arsenic.However, during the crystallization of arsenic acid double salt under normal conditions, a small amount of impurity ions can still be doped into the arsenic acid double salt crystals by the methods of adsorption or coating, etc., and the high degree of purification of arsenic and impurities cannot be realized. Therefore, by strengthening the adjustment and control of the crystallization process of the arsenic acid double salt, reducing the doping of impurities into the crystals, and preparing high-purity arsenic acid double salt, the arsenic acid double salt can be used to prepare high-purity metallic arsenic products. [Means for solving the problem]
[0006] technical solution In the prior art, in the process of preparing high-purity arsenic from arsenic-containing solid waste, it is difficult to separate arsenic from similar impurities. The present invention aims to provide a method for preparing high-purity metallic arsenic from arsenic-containing solid waste from non-ferrous smelting in a short process. The method adjusts and controls the mineralization and crystallization process of arsenic acid double salt by the synergistic effect of organic-inorganic interface matching generated in the reaction system by a water-soluble polymeric organic substance containing a carboxyl group and / or a hydroxyl group and a hydrophobic polymeric organic substance having a periodic geometric structure, and achieves high-precision separation of arsenic from various impurities such as antimony, selenium, and bismuth in the alkaline leachate of arsenic-containing solid waste, and obtains high-purity arsenic by reduction roasting. The method is rapid and efficient, has low cost, is simple in process and easy to operate, and meets the needs of industrial production.
[0007] In order to achieve the above technical objectives, the present invention provides a method for preparing high-purity metallic arsenic from arsenic-containing solid waste in a short process, the method including the following steps 1), 2) and 3).
[0008] 1) Arsenic-containing solid waste from non-ferrous smelting is subjected to oxidizing alkaline leaching to obtain arsenic-containing alkaline leachate.
[0009] 2) A mixed magnesium ammonium reagent composed of a water-soluble polymeric organic substance containing a carboxyl group and / or a hydroxyl group, a magnesium compound, and an ammonium compound, and a hydrophobic polymeric organic substance having a periodic geometric structure are added to the arsenic-containing alkaline leaching solution in this order, and the mixture is stirred and reacted to obtain an arsenic acid double salt crystal coated with an organic substance.
[0010] 3) After roasting the organically coated double arsenate crystals, they are mixed with carbon powder and reduced and roasted to condense and recover metallic arsenic from the exhaust gas.
[0011] The prior art has reported that the process of precipitating arsenic from arsenic-containing alkaline leaching solution using ammonium magnesium reagent is realized, but during the crystallization of arsenic acid double salt, a small amount of impurity ions may still be doped into the arsenic acid double salt crystals by the methods of adsorption or coating, etc., and the high degree of purification of arsenic and impurities cannot be realized, so that arsenic with higher purity cannot be obtained in the subsequent process. The key point of the technical solution of the present invention is to simultaneously use a water-soluble polymeric organic material containing carboxyl group and / or hydroxyl group and a hydrophobic polymeric organic material having strong complexing ability for metal ions to synergistically modify the arsenic precipitation effect of ammonium magnesium reagent, and the crystallization process of the arsenic acid double salt can be adjusted and controlled to reduce the doping of impurities into the crystals and obtain a high-purity arsenic acid double salt, so that a high-purity arsenic product can be obtained. In the process of precipitating arsenic with ammonium magnesium reagent, the alignment of the periodic geometric structure of the organic material with the crystal structure of arsenic acid double salt can induce accurate nucleation of arsenic acid double salt crystals on their surface, and the interface interaction between the functional groups contained in the organic material and the ions in the solution can control the nucleation rate, quantity, nucleation site and crystal orientation of arsenic acid double salt crystals, thereby ensuring high selectivity in the crystallization process of arsenic acid double salt and creating the possibility of advanced separation of arsenic acid double salt from impurities. To further illustrate, the alignment of the periodic geometric structure of chitosan molecule with the crystal structure of arsenic acid double salt can induce accurate nucleation of arsenic acid double salt crystals on their surface, and after the nucleation of arsenic acid double salt, the carboxyl functional groups (-COO) on both sides of the main chain of sodium polyacrylate molecule can be substituted with carboxyl functional groups (-COO) on both sides of the main chain of sodium polyacrylate molecule. - ) is the cation Mg in the arsenate double salt crystal nucleus. 2+The electrostatic interaction between the arsenic acid double salt and the metal arsenate is generated and adsorbed on the crystal surface, reducing the surface energy of the crystal, controlling the growth process of the arsenic acid double salt crystal, and realizing the highly accurate mineralization and crystallization of the arsenic acid double salt. Therefore, by introducing two kinds of organic substances, it is possible to produce an arsenic acid double salt containing almost no impurity components, which has properties similar to those of arsenic such as antimony, selenium, and tellurium, and the process of preparing high-purity arsenic using the metal arsenic in the post-process is greatly simplified. This method contributes to solving the "choking" problem of the shortage of high-quality raw materials in the high-purity arsenic production process, and promotes the sustainable development of the non-ferrous smelting industry and strategic emerging industries.
[0012] In a preferred solution, the arsenic-containing solid waste from non-ferrous smelting includes at least one of arsenic alkali slag, copper smelting dust, and lead anode mud, which are common arsenic-containing solid waste from non-ferrous smelting in the prior art.
[0013] As a preferred solution, the conditions of the oxidation alkaline leaching are as follows: hydrogen peroxide or ozone is used as an oxidizing agent, sodium hydroxide and / or sodium carbonate is used as an alkaline leaching medium, the leaching temperature is 50-90°C, the stirring speed is 200-700 rpm, the leaching time is 1-3 h, the arsenic-containing solid waste from non-ferrous smelting is ground to a particle size of ≦1 mm, the concentration of the alkaline leaching medium is 0-4 mol / L, and the liquid-solid ratio is 4-10 mL / g. Under the preferred conditions, the arsenate is dissolved in the alkaline solution, but most of the metal components are not dissolved in the alkaline solution, so that the selective separation of the arsenic component and most of the metal components is realized. The specific leaching process is to crush the arsenic-containing solid waste from non-ferrous smelting, mix it with water, and then add the oxidizing agent and the alkali. In order to avoid introducing impurities, the oxidizing agent is preferably hydrogen peroxide or ozone, and the amount of the oxidizing agent used is 1.5 to 2.0 times the theoretical amount of the oxidizing agent required to oxidize trivalent arsenic in the arsenic-containing solid waste from non-ferrous smelting to pentavalent arsenic.
[0014] As a preferred solution, in the mixed ammonium magnesium reagent, the molar ratio of the magnesium compound to the ammonium compound is n(Mg / N)=0.2-1.0, and the ratio of the mass of the carboxyl- and / or hydroxyl-containing water-soluble organic polymer to the total mass of the magnesium compound and the ammonium compound is 1-10 mg / g. The mixed ammonium magnesium reagent is obtained by reacting a magnesium compound, an ammonium compound, and a carboxyl- and / or hydroxyl-containing water-soluble organic polymer in advance, that is, the carboxyl- and / or hydroxyl-containing water-soluble organic polymer is prepared into an aqueous solution with a concentration of 1-5 g / L, and then the magnesium compound and the ammonium compound are added at a desired mixing ratio.
[0015] As a preferred solution, the water-soluble organic polymer containing carboxyl and / or hydroxyl groups is sodium polyacrylate and / or polyethylene glycol. The preferred water-soluble organic polymer containing carboxyl and / or hydroxyl groups is capable of adsorbing to the crystal surface mainly by coordination action, reducing the surface energy of the crystal, controlling the growth process of the arsenic acid double salt crystal, and realizing high-precision mineralization and crystallization of the arsenic acid double salt.
[0016] In a preferred solution, the magnesium compound is at least one of magnesium oxide, magnesium chloride, and magnesium sulfate.
[0017] In a preferred solution, the ammonium compound is at least one of ammonium bicarbonate, ammonium chloride, and ammonium sulfate. The magnesium compound and the ammonium compound are common magnesium salts and ammonium salts, both of which can be converted into arsenate radicals and chemically stable magnesium ammonium arsenate precipitates.
[0018] As a preferred solution, the hydrophobic organic polymer having a periodic geometric structure is added to the arsenic-containing alkaline leachate at a concentration of 1 to 5 g / L. The hydrophobic organic polymer having a periodic geometric structure is generally prepared in the form of a solution and then added, but is dispersed or dissolved in the aqueous solution by the action of heating and ultrasonic treatment. Specifically, for example, the hydrophobic organic polymer having a periodic geometric structure is mixed with hot water at 100°C at 10 to 20 mL / g, and the ultrasonic treatment time is 30 to 50 min.
[0019] As a preferred solution, the amount of the mixed ammonium magnesium reagent added to the arsenic-containing alkaline leachate is measured so that the molar ratio of magnesium to arsenic n (Mg / As) is 1.2 to 2.5.
[0020] In a preferred solution, the hydrophobic polymeric organic material having a periodic geometric structure is polyvinyl alcohol and / or chitosan. The preferred organic material having a periodic geometric structure is mainly for inducing the formation of crystal nuclei.
[0021] As a preferred solution, the stirring reaction conditions are: temperature 30-50°C, stirring speed 300-500 rpm, and time 1-3 h. Under the preferred stirring reaction conditions, the rapid precipitation process of ammonium magnesium arsenate precipitate can be controlled.
[0022] As a preferred solution, the roasting conditions are a temperature of 200-300° C. and a time of 2-3 hours. Under the preferred roasting conditions, the crystal water and free ammonia components in the ammonium magnesium arsenate precipitate can be volatilized, and the amount of processing required for reduction roasting can be reduced.
[0023] As a preferred solution, the conditions of the reduction roasting are as follows: under an inert atmosphere, the roasting temperature is 800-1200°C, the roasting time is 2-4h, and the amount of carbon powder used is 10%-15% of the mass of the roasted slag. The inert atmosphere is nitrogen gas, argon gas, etc. The preferred reduction roasting process can control the efficient reduction and volatilization process of arsenic.
[0024] The high purity metallic arsenic prepared by the solution of the present invention refers to a high purity metallic arsenic raw material having a purity of 99% or more. The high purity metallic arsenic having a purity of 99% or more can be further subjected to a conventional normal vacuum distillation process to obtain metallic arsenic with a purity of 5N to 7N. More specifically, metallic arsenic with a purity of 99% (i.e., metallic arsenic at a level of 2N) is placed in a vacuum tank, argon gas is introduced into the intake port to discharge the air, the vacuum tank is heated to 610 to 650°C to form arsenic vapor, hydrogen is then introduced into the intake port to form a mixed gas, a quartz reaction pipe is connected to the exhaust port, and the arsenic vapor is condensed on the inner wall of the quartz pipe to form high purity arsenic with a purity of 5N to 7N. Effect of the Invention
[0025] Beneficial effects In the process of using ammonium magnesium reagent to realize the precipitation of arsenic from arsenic-containing alkaline leachate, a small amount of impurity ions may still be doped into the arsenic double salt crystals by the methods of adsorption or coating, etc., and thus the high degree of purification of arsenic and impurities cannot be realized, and therefore higher purity arsenic cannot be obtained in the subsequent process. In order to solve the technical problem of the prior art, the key point of the technical solution of the present invention is to simultaneously use a water-soluble macromolecular organic material containing carboxyl groups and / or hydroxyl groups and a hydrophobic macromolecular organic material having a periodic geometric structure to synergistically modify the arsenic precipitation effect of ammonium magnesium reagent, and adjust and control the mineralization and crystallization process of arsenic double salt through the synergistic effect of organic-inorganic interface matching generated in the reaction system by the water-soluble organic material containing carboxyl groups and / or hydroxyl groups and the organic material having a periodic geometric structure, and achieve high degree of separation of arsenic from various impurities such as antimony, selenium, bismuth in the alkaline leachate of arsenic-containing solid waste through the high-precision mineralization and crystallization of arsenic double salt, and obtain high purity arsenic raw material through reduction roasting. The method is rapid and efficient, has low cost and simple process, is easy to operate, and meets the needs of industrial production. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] Best Mode for Carrying Out the Invention The following examples are intended to further illustrate the invention, but are not intended to limit the scope of protection of the claims of the invention.
[0027] Example 1
[0028] 5kg of arsenic alkaline slag (main components are As4.29%, Sb1.62%, Al2.41%, Fe0.89%, alkali (mainly sodium carbonate)54.71%) is mixed with 20L of water. Since the arsenic alkaline slag itself contains alkali, there is no need to replenish sodium hydroxide or sodium carbonate in the leaching process. Only an appropriate amount of hydrogen peroxide is replenished. The leaching temperature is controlled to 50℃, the stirring intensity is 500rpm, and the leaching time is 1.5h. After the leaching is completed, solid-liquid separation is performed to obtain an alkaline arsenic-containing leachate whose main components are as shown in Table 1. The arsenic leaching rate is 92.15%.
[0029] Magnesium oxide and ammonium bicarbonate are mixed in a molar ratio of n (Mg / N) = 0.5, and then sodium polyacrylate and the mixed reagent are mixed in a mass ratio of 5 mg / g to prepare a mixed magnesium ammonium reagent. Chitosan is mixed with hot water at 100 ° C at 15 mL / g, and ultrasonicated for 50 min to thoroughly disperse it. Then, the mixed magnesium ammonium reagent and chitosan solution are added to the alkaline leachate in order at n (Mg / As) = 1.5: 1 and a concentration of 5 g / L, and the mixture is thoroughly stirred at 50 ° C and 500 rpm for 3 h. After the reaction is completed, it is filtered to obtain organic-coated double arsenic acid salt crystals.
[0030] The arsenic acid double salt crystals are roasted at a high temperature of 300℃ for 3 hours, and then the roasted slag and carbon powder are mixed uniformly (the mass of the carbon powder is 15% of the mass of the roasted slag), and then placed in a tube furnace and heated to 900℃ under a nitrogen gas atmosphere for 3 hours, and the metal arsenic product is recovered from the condensation tube. The detection results show that the purity of the metal arsenic reaches 99.84%, and the contents of impurities such as antimony, selenium, and aluminum are all less than 0.01%. TIFF0007554517000001.tif33169
[0031] Furthermore, the obtained 99.84% metallic arsenic product is placed in a vacuum tank, argon gas is introduced into the intake port to expel the air, and the vacuum tank is heated to 610°C to form arsenic vapor. Then, hydrogen is introduced into the intake port to form a mixed gas, and a quartz reaction pipe is connected to the exhaust port, and the arsenic vapor is condensed on the inner wall of the quartz pipe to form high-purity arsenic with a higher purity of 6N.
[0032] Comparative Example 1
[0033] 5 kg of arsenic alkaline slag is mixed with 15 L of water, and the leaching temperature is controlled to be 40°C, the stirring intensity is 500 rpm, and the leaching time is 1.5 h. After the leaching is completed, solid-liquid separation is performed to obtain an alkaline arsenic-containing leachate with an arsenic leaching rate of 85.32%.
[0034] Comparative Example 2
[0035] The alkaline leaching solution is prepared according to the experimental parameters of Example 1. No chitosan is added during the preparation of arsenic acid double salt crystals, and other conditions are the same as those of Example 1. The reaction parameters of the reduction roasting process of arsenic acid double salt are the same as those of Example 1, and the purity of the final metal arsenic product is 97.89%, the content of impurity selenium is 0.05%, and the content of impurity antimony is 0.1%.
[0036] Comparative Example 3
[0037] The alkaline leaching solution is prepared according to the experimental parameters of Example 1. During the preparation of arsenic acid double salt crystals, sodium polyacrylate is not added to the solution for preparing magnesium ammonium admixture, and other conditions are the same as those of Example 1. The reaction parameters of the arsenic acid double salt reduction roasting process are the same as those of Example 1, and the purity of the final metal arsenic product is 96.98%, the content of impurity selenium is 0.09%, and the content of impurity antimony is 0.15%.
[0038] Comparative Example 4
[0039] The reaction parameters of the leaching of arsenic alkali slag and the crystallization of arsenic acid double salt are controlled as in Example 1. In the reduction roasting process, the mass of carbon powder is 8% of the mass of roasted slag, and other conditions are the same as in Example 1. The purity of the final metal arsenic product is 81.55%, the oxygen content reaches 15.31%, and the contents of antimony, selenium, aluminum and other impurities are all less than 0.01%.
[0040] Comparative Example 5
[0041] The alkaline leachate is prepared according to the experimental parameters of Example 1. Sufficient lime is added to the leachate with n(Ca / As)=3.0, and the leachate is causticized under the conditions of temperature 80°C, time 1h, and stirring speed 300rpm. After the causticization is completed, solid-liquid separation is carried out. A large amount of calcium carbonate is co-precipitated with calcium arsenic slag, so the arsenic content in the arsenic slag is only 8.49%, and the precipitation rate of arsenic is only 67.44%.
[0042] Example 2
[0043] 5kg of lead anode mud (specific composition: Pb12.88%, As27.53%, Sb24.92%, Ag5.08%, arsenic mainly exists in elemental and oxidized states) is taken for oxidation alkaline leaching, and an appropriate amount of hydrogen peroxide water is added as oxidant during the leaching process, the liquid-solid ratio is 10:1, the amount of sodium carbonate and sodium hydroxide used is both 1mol / L, the temperature is 60℃, the leaching time is 2h, and the stirring speed is 500rpm. After the leaching reaction is completed, solid-liquid separation is performed to obtain an alkaline arsenic-containing leaching solution whose main components are as shown in Table 2, and the arsenic leaching rate is 90.47%.
[0044] Mix magnesium chloride and ammonium chloride in a molar ratio of n (Mg / N) = 0.4, then mix polyethylene glycol with the mixed reagent in a mass ratio of 8 mg / g to prepare mixed magnesium ammonium reagent. Mix polyvinyl alcohol and 100 ° C hot water at 18 mL / g, and ultrasonicate for 50 min to thoroughly disperse. Add mixed magnesium ammonium reagent and polyvinyl alcohol solution in order at n (Mg / As) = 2.0: 1 and concentration of 5 g / L to the alkaline leachate, and stir thoroughly at 50 ° C and 500 rpm for 3 h. After the reaction is completed, filter to obtain organic-coated arsenic acid double salt crystals.
[0045] The arsenic acid double salt crystals are roasted at a high temperature of 250℃ for 3 hours, and then the roasted slag and carbon powder are mixed uniformly (the mass of the carbon powder is 12% of the mass of the roasted slag), and then placed in a tube furnace and heated to 1100℃ under a nitrogen gas atmosphere for 3 hours, and the metal arsenic product is recovered from the condensation tube. The detection results show that the purity of the metal arsenic reaches 99.89%, and the contents of impurities such as lead, antimony, and silver are all less than 0.01%. TIFF0007554517000002.tif34169
[0046] Furthermore, the 99.89% metallic arsenic obtained above is placed in a vacuum tank, argon gas is introduced into the intake port to expel the air, and the vacuum tank is heated to 620°C to form arsenic vapor. Then, hydrogen is introduced into the intake port to form a mixed gas, and a quartz reaction pipe is connected to the exhaust port. The arsenic vapor is condensed on the inner wall of the quartz pipe to form metallic arsenic of higher purity with a purity level of 5N.
[0047] Comparative Example 6
[0048] Take 5 kg of lead anode mud and carry out oxidative alkaline leaching. In the leaching process, add an appropriate amount of hydrogen peroxide water as oxidant, control the liquid-solid ratio to be 10:1, the amounts of sodium carbonate and sodium hydroxide used are both 0.5 mol / L, the temperature is 60°C, the leaching time is 2 h, and the stirring speed is 500 rpm. After the leaching reaction is completed, carry out solid-liquid separation to obtain an alkaline arsenic-containing leaching solution with an arsenic leaching rate of 74.52%.
[0049] Comparative Example 7
[0050] The alkaline leaching solution is prepared according to the experimental parameters of Example 2. In the process of preparing the mixed magnesium ammonium reagent, the mixing ratio of the soluble organic matter to the total mass of magnesium chloride and ammonium chloride is 0.5mg / g, and other conditions are the same as those of Example 2. The reaction parameters of the arsenic acid double salt reduction roasting process are the same as those of Example 2, and the purity of the final metal arsenic product is 98.38%, and the content of antimony impurities is 0.02%.
[0051] Comparative Example 8
[0052] The alkaline leaching solution is prepared according to the experimental parameters of Example 2. The hot water temperature during the preparation of the hydrophobic organic matter is 50°C, and other conditions are the same as those of Example 2. The reaction parameters of the arsenic acid double salt reduction roasting process are the same as those of Example 2, and the purity of the final metal arsenic product is 97.18%, and the content of impurity antimony is 0.15%.
[0053] Comparative Example 9
[0054] The alkaline leaching solution is prepared according to the experimental parameters of Example 2. In the process of preparing mixed magnesium ammonium reagent, magnesium chloride and ammonium chloride are mixed with n(Mg / N)=2.0, and other conditions are the same as those of Example 2. The reaction parameters of the arsenic acid double salt reduction roasting process are the same as those of Example 2, and the purity of the final metal arsenic product is 96.33%, and the contents of impurities such as lead, antimony, and silver are all higher than 0.02%.
[0055] Example 3
[0056] 5kg of copper smelting dust (specific composition: Pb24.95%, Cu14.21%, As5.78%, Bi2.50%, Zn2.335%, arsenic is mainly present in mixed sulfate) is taken and subjected to oxidative alkaline leaching. In the leaching process, an appropriate amount of hydrogen peroxide solution is added as oxidizing agent, the liquid-solid ratio is 5:1, the amount of sodium carbonate used is 1.5mol / L, the amount of sodium hydroxide used is 0.5mol / L, the temperature is 50℃, the leaching time is 1h, and the stirring speed is 600rpm. After the leaching reaction is completed, solid-liquid separation is performed to obtain an alkaline arsenic-containing leachate whose main components are as shown in Table 2, and the arsenic leaching rate is 82.38%.
[0057] Mix magnesium sulfate and ammonium sulfate at a molar ratio of n (Mg / N) = 0.5, then mix sodium polyacrylate with the mixed reagent at a mass ratio of 6 mg / g to prepare mixed magnesium ammonium reagent. Mix chitosan with 100 ° C hot water at 20 mL / g, and ultrasonicate for 50 min to thoroughly disperse. Add mixed magnesium ammonium reagent and chitosan solution to the alkaline leachate at n (Mg / As) = 2.5: 1, concentration 5 g / L in sequence, and thoroughly stir at 50 ° C and 600 rpm for 2 h. After the reaction is completed, filter to obtain organic-coated arsenic acid double salt crystals.
[0058] The arsenic acid double salt crystals are roasted at a high temperature of 300℃ for 3 hours, and then the roasted slag and carbon powder are mixed uniformly (the mass of the carbon powder is 10% of the mass of the roasted slag), and then placed in a tube furnace and heated to 1000℃ under a nitrogen gas atmosphere for 2.5 hours, and the metal arsenic product is recovered from the condensation tube. The detection results show that the purity of the metal arsenic reaches 99.38%, and the contents of copper, lead, zinc and other impurities are all less than 0.01%. TIFF0007554517000003.tif33164
[0059] Metallic arsenic is placed in a vacuum tank, argon gas is introduced into the intake port to expel the air, and the vacuum tank is heated to 650°C to form arsenic vapor. Then, hydrogen is introduced into the intake port to form a mixed gas, and a quartz reaction pipe is connected to the exhaust port. The arsenic vapor condenses on the inner wall of the quartz pipe to form high-purity arsenic with a purity of 7N.
[0060] Comparative Example 10
[0061] Take 5kg of copper smelting ash to carry out oxidation alkaline leaching. Add an appropriate amount of hydrogen peroxide water as oxidant during the leaching process. Control the liquid-solid ratio to be 2:1, the amount of sodium carbonate used to be 1.5mol / L, the amount of sodium hydroxide used to be 0.5mol / L, the temperature to be 50℃, the leaching time to be 1h, and the stirring speed to be 600rpm. After the leaching reaction is completed, carry out solid-liquid separation to obtain an alkaline arsenic-containing leaching solution with an arsenic leaching rate of 61.37%.
[0062] Comparative Example 11
[0063] The alkaline leaching solution and mixed magnesium ammonium reagent are prepared according to the experimental parameters of Example 3. When preparing double arsenic acid salt, mixed magnesium ammonium reagent is added with n(Mg / As)=1:1, and other conditions are the same as those of Example 3. The final arsenic removal rate in the alkaline leaching solution is 71.69%, the arsenic grade in double arsenic acid salt is 28.38%, and the purity of metallic arsenic reaches 98.94%.
[0064] Comparative Example 12
[0065] The alkaline leaching solution and arsenic acid double salt were prepared according to the experimental parameters of Example 3. During the reduction roasting, the roasting temperature was 600°C, and the other conditions were the same as those of Example 3, and finally no metal arsenic product was recovered.
[0066] Comparative Example 13
[0067] The alkaline leaching solution and arsenic acid double salt were prepared according to the experimental parameters of Example 3. During the reduction roasting, the mass of the carbon powder was 5% of the mass of the roasted slag when the roasted slag was mixed with the carbon powder, and the other conditions were the same as those of Example 3. Finally, no metal arsenic products were recovered.
Claims
1. 1) performing oxidative alkaline leaching on arsenic-containing solid waste from non-ferrous smelting to obtain an arsenic-containing alkaline leachate; 2) adding a mixed ammonium magnesium reagent consisting of a water-soluble organic polymer containing a carboxyl group and / or a hydroxyl group, a magnesium compound, and an ammonium compound, and polyvinyl alcohol and / or chitosan as a hydrophobic organic polymer having a periodic geometric structure to the arsenic-containing alkaline leaching solution in this order, and stirring and reacting the mixture to obtain an arsenic acid double salt crystal coated with an organic substance; 3) a step of roasting the arsenic acid double salt crystals coated with an organic substance, followed by reduction roasting with carbon powder, and condensing and recovering the metallic arsenic from the exhaust gas.
2. The method for preparing high-purity metallic arsenic from arsenic-containing solid waste in a short process according to claim 1, characterized in that the arsenic-containing solid waste from non-ferrous smelting includes at least one of arsenic alkali slag, copper smelting dust, and lead anode mud.
3. The method for preparing high-purity metallic arsenic from arsenic-containing solid waste in a short process according to claim 1, characterized in that the conditions of the oxidation alkaline leaching are as follows: hydrogen peroxide and / or ozone are used as oxidizing agents, sodium hydroxide and / or sodium carbonate are used as alkaline leaching media, the leaching temperature is 50-90°C, the stirring speed is 200-700 rpm, the leaching time is 1-3 h, the arsenic-containing solid waste from non-ferrous smelting is ground to a particle size of ≦1 mm, the concentration of the alkaline leaching media is 0-4 mol / L, and the liquid-solid ratio is 4-10 mL / g.
4. The method for preparing high-purity metallic arsenic from arsenic-containing solid waste in a short process according to claim 1, characterized in that in the mixed ammonium magnesium reagent, the molar ratio of the magnesium compound to the ammonium compound is n (Mg / N) = 0.2 to 1.0, and the ratio of the carboxyl group- and / or hydroxyl group-containing water-soluble polymeric organic matter to the total mass of the magnesium compound and the ammonium compound is 1 to 10 mg / g.
5. The method for preparing high-purity metallic arsenic from arsenic-containing solid waste in a short process according to claim 1 or 4, characterized in that the carboxyl group- and / or hydroxyl group-containing water-soluble polymeric organic substance is sodium polyacrylate and / or polyethylene glycol.
6. The magnesium compound is at least one of magnesium oxide, magnesium chloride, and magnesium sulfate; 2. The method for preparing high purity metallic arsenic from arsenic-containing solid waste in a short process according to claim 1, wherein the ammonium compound is at least one of ammonium bicarbonate, ammonium chloride, and ammonium sulfate.
7. 2. The method for preparing high-purity metallic arsenic from arsenic-containing solid waste in a short process according to claim 1, characterized in that the concentration of polyvinyl alcohol and / or chitosan as the hydrophobic macromolecular organic substance having a periodic geometric structure added to the arsenic-containing alkaline leaching solution is 1 to 5 g / L, and the amount of the mixed ammonium magnesium reagent added to the arsenic-containing alkaline leaching solution is metered at a molar ratio of magnesium to arsenic n (Mg / As) of 1.2 to 2.
5.
8. The method for preparing high purity metallic arsenic from arsenic-containing solid waste in a short process according to claim 1, characterized in that the stirring reaction conditions are a temperature of 30 to 50°C, a stirring speed of 300 to 500 r / pm, and a reaction time of 1 to 3 h.
9. The roasting conditions are a temperature of 200 to 300°C and a time of 2 to 3 hours. The method for preparing high-purity metallic arsenic from arsenic-containing solid waste in a short process according to claim 1, characterized in that the conditions of the reduction roasting are in an inert atmosphere, the roasting temperature is 800-1200°C, the roasting time is 2-4h, and the amount of carbon powder used is 10%-15% of the mass of the roasted slag.
Citation Information
Patent Citations
Absorbent material for selectively absorbing As<+5> ions and preparation method thereof
CN102172514A
Method for preparing arsenic by direct reduction and roasting of arsenic-containing material
CN106636678A
Method for selective arsenic removal from lead anode slime and wastewater treatment zero discharge
CN107794372A
Method for achieving efficient and comprehensive resource utilization of arsenic-alkali residues
CN108611494A
Method for removing arsenic from acidic arsenic-containing solution by using iron salt
CN110104753A