Conductive polymer dispersion, conductive laminate and method for producing the same
Patent Information
- Application Number
- JP2020178902
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-26
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2040-10-26
AI Technical Summary
【0006】 本発明によれば、導電性に優れた導電層を形成できる導電性高分子分散液、及びこれを用いた導電性積層体及びその製造方法を提供できる。また、本発明の導電性高分子分散液の塗膜は、短時間で自然に乾燥させることができるので、加熱乾燥の前に予備乾燥することにより、加熱乾燥装置内に持ち込む分散媒の量を低減することができる。さらに、本発明の導電性高分子分散液によって形成した導電層は、高温高湿条件に対する耐久性にも優れる。
Smart Images

Figure 0007555234000002 
Figure 0007555234000003 
Figure 0007555234000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a conductive polymer dispersion, a conductive laminate, and a method for producing the same. [Background technology]
[0002] A π-conjugated conductive polymer, whose main chain is composed of a π-conjugated system, forms a conductive complex by doping with a polyanion having an anionic group, and becomes dispersible in water. A conductive laminate having a conductive layer (conductive film) can be produced by applying a conductive polymer dispersion containing the conductive complex to a glass substrate or a film substrate. In order to apply such conductive layers to various applications, it is necessary to improve their conductivity. For example, Patent Document 1 proposes a conductive polymer-containing liquid that contains a high concentration of polyol such as glycerin. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-007470 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, there are cases where a new conductive polymer dispersion different from the invention of Patent Document 1 is required. The present invention provides a conductive polymer dispersion capable of forming a conductive layer having excellent conductivity, a conductive laminate using the same, and a method for producing the same. [Means for solving the problem]
[0005] [1] A conductive polymer dispersion liquid containing a conductive complex including a π-conjugated conductive polymer and a polyanion, an unsaturated aliphatic alcohol compound having an unsaturated bond between carbon atoms and a hydroxyl group in the molecule, and a dispersion medium. [2] The conductive polymer dispersion according to [1], wherein the unsaturated aliphatic alcohol compound is a diol. [3] The conductive polymer dispersion liquid according to [1] or [2], wherein the unsaturated aliphatic alcohol compound has 4 or more and 8 or less carbon atoms. [4] The conductive polymer dispersion according to [1], wherein the unsaturated aliphatic alcohol compound includes at least one selected from the group consisting of cis-2-butene-1,4-diol, trans-2-butene-1,4-diol, 2-butyne-1,4-diol, and 2,4-hexadiyne-1,6-diol. [5] The conductive polymer dispersion according to any one of [1] to [4], wherein the content of the unsaturated aliphatic alcohol compound is 3 mass % or less. [6] The conductive polymer dispersion according to any one of [1] to [5], wherein the conductive polymer dispersion has a water content of 50 mass % or more. [7] The conductive polymer dispersion according to any one of [1] to [6], further comprising a binder component. [8] The conductive polymer dispersion according to any one of [1] to [7], further comprising a phenol-based antioxidant. [9] A conductive laminate comprising a substrate and a conductive layer formed on at least one surface of the substrate, the conductive layer being a cured layer of the conductive polymer dispersion according to any one of [1] to [8].
[10] A method for producing a conductive laminate, comprising applying the conductive polymer dispersion according to any one of [1] to [8] to at least one surface of a substrate. Effect of the Invention
[0006] According to the present invention, it is possible to provide a conductive polymer dispersion capable of forming a conductive layer having excellent conductivity, and a conductive laminate using the same and a method for producing the same. In addition, since the coating film of the conductive polymer dispersion of the present invention can be naturally dried in a short time, the amount of dispersion medium brought into the heat drying device can be reduced by pre-drying before heat drying. Furthermore, the conductive layer formed by the conductive polymer dispersion of the present invention has excellent durability against high temperature and high humidity conditions.
[0007] This invention is believed to contribute to SDGs Goal 12, "Responsible Consumption and Production."
[0008] In this specification and claims, the lower limit and upper limit of a numerical range indicated with "to" are included in the numerical range. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] ≪Conductive polymer dispersion liquid≫ A first aspect of the present invention is a conductive polymer dispersion liquid containing a conductive complex containing a π-conjugated conductive polymer and a polyanion, an unsaturated aliphatic alcohol compound having an unsaturated bond between carbon atoms and a hydroxyl group in the molecule, and a dispersion medium.
[0010] [Conductive composite] The conductive complex contained in the conductive polymer dispersion of this embodiment contains a π-conjugated conductive polymer and a polyanion. The polyanion in the conductive complex is doped into the π-conjugated conductive polymer to form a conductive complex having electrical conductivity. In the polyanion, only a part of the anionic groups is doped into the π-conjugated conductive polymer, and there are excess anionic groups that are not involved in the doping. Since the excess anionic groups are hydrophilic groups, the conductive composite has water dispersibility.
[0011] (π-conjugated conductive polymer) The π-conjugated conductive polymer may be an organic polymer whose main chain is composed of a π-conjugated system, and examples thereof include polypyrrole-based conductive polymers, polythiophene-based conductive polymers, polyacetylene-based conductive polymers, polyphenylene-based conductive polymers, polyphenylenevinylene-based conductive polymers, polyaniline-based conductive polymers, polyacene-based conductive polymers, polythiophenevinylene-based conductive polymers, and copolymers thereof. From the viewpoint of stability in air, polypyrrole-based conductive polymers, polythiophenes, and polyaniline-based conductive polymers are preferred, and from the viewpoint of transparency, polythiophene-based conductive polymers are more preferred.
[0012] Polythiophene-based conductive polymers include polythiophene, poly(3-methylthiophene), poly(3-ethylthiophene), poly(3-propylthiophene), poly(3-butylthiophene), poly(3-hexylthiophene), poly(3-heptylthiophene), poly(3-octylthiophene), poly(3-decylthiophene), poly(3-dodecylthiophene), poly(3-octadecylthiophene), poly(3-bromothiophene), poly(3-chlorothiophene), and poly(3-iodothiophene). thiophene), poly(3-cyanothiophene), poly(3-phenylthiophene), poly(3,4-dimethylthiophene), poly(3,4-dibutylthiophene), poly(3-hydroxythiophene), poly(3-methoxythiophene), poly(3-ethoxythiophene), poly(3-butoxythiophene), poly(3-hexyloxythiophene), poly(3-heptyloxythiophene), poly(3-octyloxythiophene), poly(3-decyloxythiophene), poly(3-dodecyloxythiophene), oxythiophene), poly(3-octadecyloxythiophene), poly(3,4-dihydroxythiophene), poly(3,4-dimethoxythiophene), poly(3,4-diethoxythiophene), poly(3,4-dipropoxythiophene), poly(3,4-dibutoxythiophene), poly(3,4-dihexyloxythiophene), poly(3,4-diheptyloxythiophene), poly(3,4-dioctyloxythiophene), poly(3,4-didecyloxythiophene), poly(3,4-di dodecyloxythiophene), poly(3,4-ethylenedioxythiophene), poly(3,4-propylenedioxythiophene), poly(3,4-butylenedioxythiophene), poly(3-methyl-4-methoxythiophene), poly(3-methyl-4-ethoxythiophene), poly(3-carboxythiophene), poly(3-methyl-4-carboxythiophene), poly(3-methyl-4-carboxyethylthiophene), and poly(3-methyl-4-carboxybutylthiophene). Examples of polypyrrole-based conductive polymers include polypyrrole, poly(N-methylpyrrole), poly(3-methylpyrrole), poly(3-ethylpyrrole), poly(3-n-propylpyrrole), poly(3-butylpyrrole), poly(3-octylpyrrole), poly(3-decylpyrrole), poly(3-dodecylpyrrole), poly(3,4-dimethylpyrrole), poly(3,4-dibutylpyrrole), poly(3-carboxypyrrole), poly(3-methyl-4-carboxypyrrole), poly(3-methyl-4-carboxyethylpyrrole), poly(3-methyl-4-carboxybutylpyrrole), poly(3-hydroxypyrrole), poly(3-methoxypyrrole), poly(3-ethoxypyrrole), poly(3-butoxypyrrole), poly(3-hexyloxypyrrole), and poly(3-methyl-4-hexyloxypyrrole). Examples of polyaniline-based conductive polymers include polyaniline, poly(2-methylaniline), poly(3-isobutylaniline), poly(2-anilinesulfonic acid), and poly(3-anilinesulfonic acid). Among these π-conjugated conductive polymers, poly(3,4-ethylenedioxythiophene) is particularly preferable because of its excellent conductivity, transparency, and heat resistance. The conductive composite may contain one type of π-conjugated conductive polymer, or two or more types of polymers.
[0013] (Polyanion) A polyanion is a polymer having two or more monomer units each having an anionic group in the molecule. The anionic group of the polyanion functions as a dopant for a π-conjugated conductive polymer, improving the conductivity of the π-conjugated conductive polymer. The anion group of the polyanion is preferably a sulfo group or a carboxy group. Specific examples of such polyanions include polymers having a sulfo group, such as polystyrene sulfonic acid, polyvinyl sulfonic acid, polyallyl sulfonic acid, polyacrylic acid esters having a sulfo group, polymethacrylic acid esters having a sulfo group (for example, poly(4-sulfobutyl methacrylate, polysulfoethyl methacrylate, polymethacryloyloxybenzenesulfonic acid), poly(2-acrylamido-2-methylpropanesulfonic acid), and polyisoprene sulfonic acid; and polymers having a carboxy group, such as polyvinyl carboxylic acid, polystyrene carboxylic acid, polyallyl carboxylic acid, polyacrylic acid, polymethacrylic acid, poly(2-acrylamido-2-methylpropanecarboxylic acid), and polyisoprene carboxylic acid. The polyanion may be a homopolymer in which a single monomer is polymerized, or a copolymer in which two or more monomers are polymerized. Among these polyanions, polymers having a sulfo group are preferred, and polystyrene sulfonic acid is more preferred, since they can provide higher electrical conductivity. The polyanions may be used alone or in combination of two or more kinds. The mass average molecular weight of the polyanion is preferably from 20,000 to 1,000,000, and more preferably from 100,000 to 500,000. The mass average molecular weight is the average molecular weight based on mass measured by gel filtration chromatography and calculated in terms of pullulan.
[0014] The content of the polyanion in the conductive complex is preferably in the range of 1 part by mass to 1000 parts by mass, more preferably 10 parts by mass to 700 parts by mass, and even more preferably 100 parts by mass to 500 parts by mass, relative to 100 parts by mass of the π-conjugated conductive polymer. If the content of the polyanion is equal to or greater than the lower limit, the doping effect on the π-conjugated conductive polymer tends to be stronger, and the conductivity becomes higher. On the other hand, if the content of the polyanion is equal to or less than the upper limit, the π-conjugated conductive polymer can be sufficiently contained, so that sufficient conductivity can be ensured.
[0015] The content of the conductive complex contained in the conductive polymer dispersion of this embodiment is preferably from 0.01% by mass to 5% by mass, more preferably from 0.1% by mass to 3% by mass, and even more preferably from 0.3% by mass to 1.5% by mass, relative to the total mass of the conductive polymer dispersion. When the content is at least as high as the lower limit of the above range, the conductivity of the conductive layer formed by applying the conductive polymer dispersion can be further improved. When it is equal to or less than the upper limit of the above range, the dispersibility of the conductive complex in the conductive polymer dispersion can be improved, and a uniform conductive layer can be formed.
[0016] [Unsaturated fatty alcohol compounds] The one or more unsaturated aliphatic alcohol compounds contained in the conductive polymer dispersion of this embodiment are alcohols having one or more double bonds or triple bonds between carbon atoms in the molecule and one or more hydroxyl groups (hydroxyl groups) in the molecule.
[0017] From the viewpoints of further improving the conductivity and durability of the conductive layer formed from the conductive polymer dispersion of this embodiment and further shortening the tack-free time when the conductive layer is formed, it is preferable that the unsaturated aliphatic alcohol compound is a diol having two hydroxyl groups. From the same viewpoint, the unsaturated aliphatic alcohol compound preferably has 4 or more and 12 or less carbon atoms, more preferably 4 or more and 10 or less, further preferably 4 or more and 8 or less, and particularly preferably 4 or more and 6 or less carbon atoms. From the same viewpoint, the number of unsaturated bonds contained in the unsaturated aliphatic alcohol compound is preferably 1 or more and 4 or less, more preferably 1 or more and 3 or less, and even more preferably 1 or 2.
[0018] The unsaturated aliphatic alcohol is preferably at least one selected from the group consisting of cis-2-butene-1,4-diol, trans-2-butene-1,4-diol, 2-butyne-1,4-diol, and 2,4-hexadiyne-1,6-diol. Further examples include 3,6-dimethyl-4-octyne-3,6-diol, 2,5-dimethyl-3-hexyne-2,5-diol, and the like.
[0019] In the conductive polymer dispersion of this embodiment, the total content of the unsaturated aliphatic alcohol compounds relative to 100 parts by mass of the conductive complex is preferably 50 parts by mass or more and 1000 parts by mass or less, more preferably 100 parts by mass or more and 5000 parts by mass or less, even more preferably 200 parts by mass or more and 2500 parts by mass or less, and particularly preferably 300 parts by mass or more and 1000 parts by mass or less. When the content is within the above preferred range, the effect of the present invention is further improved.
[0020] The content of the unsaturated aliphatic alcohol compound relative to the total mass of the conductive polymer dispersion of this embodiment is preferably 0.1 mass % or more and 3 mass % or less, more preferably 0.2 mass % or more and 2.5 mass % or less, and even more preferably 0.3 mass % or more and 2 mass % or less. When the content is equal to or greater than the lower limit of the above range, the conductivity and durability of the conductive layer can be sufficiently improved, and when the content is equal to or less than the upper limit of the above range, the tack-free time can be further shortened.
[0021] [Dispersion medium] Examples of the dispersion medium contained in the conductive polymer dispersion of this embodiment include water, an organic solvent, and a mixture of water and an organic solvent. The unsaturated aliphatic alcohol compound does not fall under the category of the dispersion medium contained in the conductive polymer dispersion liquid of this embodiment.
[0022] Examples of the organic solvent include alcohol-based solvents, ether-based solvents, ketone-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. Examples of alcohol-based solvents include monohydric alcohols such as methanol, ethanol, 1-propanol, 2-propanol, 2-methyl-2-propanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, allyl alcohol, propylene glycol monomethyl ether, and ethylene glycol monomethyl ether; and dihydric alcohols such as ethylene glycol, propylene glycol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, and 1,4-butanediol. Examples of the ether solvent include diethyl ether, dimethyl ether, and propylene glycol dialkyl ether. Examples of the ketone solvent include diethyl ketone, methyl propyl ketone, methyl butyl ketone, methyl isopropyl ketone, methyl isobutyl ketone, methyl amyl ketone, diisopropyl ketone, methyl ethyl ketone, acetone, and diacetone alcohol. Examples of the ester solvent include ethyl acetate, propyl acetate, and butyl acetate. Examples of aromatic hydrocarbon solvents include benzene, toluene, xylene, ethylbenzene, propylbenzene, and isopropylbenzene. An example of a solvent not classified into the above categories is dimethyl sulfoxide. The organic solvents may be used alone or in combination of two or more kinds.
[0023] From the viewpoint of enhancing the dispersibility of the conductive complex, the dispersion medium of the conductive polymer dispersion of this embodiment is preferably water, a water-soluble organic solvent, or a mixed solvent of water and a water-soluble organic solvent. Here, a water-soluble organic solvent is an organic solvent that dissolves in an amount of 1 g or more in 100 g of water at 20°C, and a water-insoluble organic solvent is an organic solvent that dissolves in an amount of less than 1 g in 100 g of water at 20°C. The water-soluble organic solvent is preferably one or more selected from alcohol-based solvents. From the viewpoint of further enhancing the dispersibility of the conductive composite, the alcohol-based solvent is preferably contained in combination with water.
[0024] Since the conductive complex has high dispersibility in water, the dispersion medium of the conductive polymer dispersion of this embodiment is preferably an aqueous dispersion medium containing water. The proportion of water relative to the total mass of the conductive polymer dispersion of this embodiment (water content in the conductive polymer dispersion) is, for example, preferably from 50 mass% to 99.9 mass%, more preferably from 55 mass% to 80 mass%, and even more preferably from 60 mass% to 75 mass%. The conductive polymer dispersion of this embodiment preferably contains 50 parts by mass or more and 250 parts by mass or less of water per part by mass of the conductive complex. As the dispersion medium other than water, the above-mentioned water-soluble organic solvents are preferable.
[0025] The content of the water-soluble organic solvent relative to the total mass of the conductive polymer dispersion of this embodiment is, for example, preferably from 10 mass % to 48 mass %, more preferably from 20 mass % to 45 mass %, and even more preferably from 30 mass % to 40 mass %.
[0026] [Binder components] The binder component is a compound other than the π-conjugated conductive polymer, the polyanion, and the unsaturated aliphatic alcohol compound, and is a component capable of binding the conductive complex to a substrate or the like. The binder component is preferably at least one selected from the group consisting of a thermoplastic resin, a curable monomer, a curable oligomer, and a silicon oxide compound (silica). The thermoplastic resin serves as a binder as it is, and the curable monomer, oligomer, and silicon oxide compound serve as a binder (binding material) when they are cured to form a cured product.
[0027] Specific examples of binders derived from binder components include acrylic resins, polyester resins, polyurethane resins, polyimide resins, polyether resins, melamine resins, silicones, alkoxysilane condensates, and silicate condensates. In this specification, the alkoxysilane condensate and the silicate condensate are sometimes collectively referred to as "silane compound." The conductive polymer dispersion liquid of this embodiment may contain one type of binder component, or two or more types of binder components.
[0028] When the binder component is a thermoplastic resin, the binder resin is preferably a water-dispersible resin that can be dispersed in the conductive polymer dispersion. The water-dispersible resin is an emulsion resin or a water-soluble resin. Specific examples of emulsion resins include acrylic resins, polyester resins, polyurethane resins, polyimide resins, melamine resins, etc., which are made into an emulsion with an emulsifier. Specific examples of the water-soluble resin include acrylic resin, polyester resin, polyurethane resin, polyimide resin, and melamine resin, which have an acid group such as a carboxy group or a sulfo group or a salt thereof. The water-soluble resin dissolves in distilled water at 25° C. at 1% by mass or more, preferably at 5% by mass or more, and more preferably at 10% by mass or more.
[0029] When the substrate to which the conductive polymer dispersion of this embodiment is applied is made of a polyester resin, the binder component preferably contains one or more types selected from the above-mentioned water-dispersible polyester resins.
[0030] When the conductive polymer dispersion of this embodiment contains the thermoplastic resin, the content of the solids (non-volatile components) is preferably from 10 to 5,000 parts by mass, more preferably from 50 to 2,000 parts by mass, and even more preferably from 100 to 1,000 parts by mass, relative to 100 parts by mass of the conductive composite. When the content of the thermoplastic resin is at least the lower limit of the above range, the strength of the conductive layer and the adhesion to the substrate can be further improved. When the content of the thermoplastic resin is equal to or less than the upper limit of the above range, a decrease in electrical conductivity due to a relative decrease in the content of the conductive composite can be suppressed.
[0031] In this specification, alkoxysilane refers to a compound having one silicon atom in the molecule, with one or more alkoxy groups bonded to the silicon atom. The alkoxysilane included in this embodiment preferably has a methoxy group or an ethoxy group because it is easily hydrolyzed. The alkoxysilane may have, as a functional group other than the alkoxy group, for example, an epoxy group, an allyl group, a vinyl group, a glycidyl group, or the like. Specific preferred alkoxysilanes include, for example, tetramethoxysilane, tetraethoxysilane, methyltriethoxysilane, tetraisopropoxysilane, tetrabutoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, vinyltrimethoxysilane, and vinyltriethoxysilane.
[0032] The content of alkoxysilane in the conductive polymer dispersion of this embodiment is preferably 10 parts by mass or more and 10,000 parts by mass or less, more preferably 50 parts by mass or more and 5,000 parts by mass or less, and even more preferably 100 parts by mass or more and 2,000 parts by mass or less, relative to 100 parts by mass of the conductive composite. When the content of alkoxysilane is equal to or more than the lower limit, the hardness of the conductive layer formed from the conductive polymer dispersion can be sufficiently increased, and when the content is equal to or less than the upper limit, a decrease in the conductivity of the conductive layer formed from the conductive polymer dispersion can be prevented.
[0033] In the present specification, a silicate is a compound having two or more silicon atoms in one molecule, at least one pair of silicon atoms being ether-bonded via one oxygen atom. The number of silicon atoms in one molecule of the silicate is preferably 4 or more, more preferably 6 or more, and even more preferably 8 or more, since the hardness of the conductive layer formed from the conductive polymer dispersion of this embodiment is higher. In addition, from the viewpoint of increasing the solubility of the silicate in the conductive polymer dispersion of this embodiment, the number of silicon atoms in one molecule of the silicate is preferably 40 or less, more preferably 30 or less. Silicate SiO 2 The content of the SiO unit is preferably 15% by mass or more and 70% by mass or less, and more preferably 25% by mass or more and 50% by mass or less, based on the total mass of the silicate. 2 When the content of the unit is equal to or more than the lower limit, the hardness of the conductive layer formed from the conductive polymer dispersion of this embodiment becomes higher, and when the content is equal to or less than the upper limit, a decrease in the conductivity of the conductive layer can be prevented. Here, the SiO 2 The content of the unit is the SiO contained in the silicate relative to 100% by mass of the molecular weight of the silicate. 2 This refers to the mass ratio of units (-O-Si-O- units) and can be measured by elemental analysis.
[0034] The silicate is preferably a compound represented by the following chemical formula (X). (X)…R 3 O-[(R 4 O-)(R 5 O-)Si-O-] s -R 6
[0035] In formula (X), R 3 , R 4 , R 5 , and R 6 each independently represents a linear or branched alkyl group having 1 to 4 carbon atoms, and s is an integer of 2 to 100. The alkyl group having 1 to 4 carbon atoms may be linear or branched, and specific examples thereof include a methyl group, an ethyl group, a propyl group, and a butyl group. s is preferably 2-50, more preferably 3-25, and further preferably 4-10.
[0036] The silicate is more preferably at least one of a compound represented by the following chemical formula (x1) and a compound represented by the following chemical formula (x2). (x1)… Si m O m-1 (OCH 3 ) 2m+2 (x2)…Si n O n-1 (OCH 2 CH 3 ) 2n+2 In the above formulae (x1) and (x2), m is 2 or more and 100 or less, and n is 2 or more and 100 or less. In the above formulae (x1) and (x2), Si and O are bonded, and Si's and O's are not adjacent to each other.
[0037] The preferred content of silicate in the conductive polymer dispersion is SiO 2 The content of the unit is appropriately selected. SiO of silicate 2 When the content of the unit is within the preferred range described above, the content of the silicate is preferably 1 part by mass or more and 100,000 parts by mass or less, more preferably 10 parts by mass or more and 10,000 parts by mass or less, and even more preferably 100 parts by mass or more and 2,000 parts by mass or less, per 100 parts by mass of the conductive composite. When the silicate content is equal to or more than the lower limit, the hardness of the conductive layer formed from the conductive polymer dispersion can be sufficiently increased, and when the silicate content is equal to or less than the upper limit, a decrease in the conductivity of the conductive layer formed from the conductive polymer dispersion can be prevented.
[0038] When the substrate to which the conductive polymer dispersion of this embodiment is applied is made of glass, the binder component preferably contains one or more selected from the above-mentioned alkoxysilanes or silicates.
[0039] As the silica, colloidal silica is preferred from the viewpoint of dispersibility, and colloidal silica dispersible in an organic solvent (hereinafter also referred to as "organosilica sol") is more preferred. Examples of commercially available organosilica sol products include methanol silica sol, MA-ST-M, IPA-ST, IPA-ST-L, IPA-ST-ZL, IPA-ST-UP, EG-ST, EG-ST-ZL, DMAC-ST, DMAC-ST-ZL, NPC-ST-30, PGM-ST, MEK-ST, MEK-ST-L, MEK-ST-ZL, MEK-ST-UP, MIBK-ST, MIBK-SD, PMA-ST, EAC-ST, NBAC-ST, XBA-ST, TOL-ST, MEK-AC-2101, MEK-AC-4101 (trade names, manufactured by Nissan Chemical Industries, Ltd.); OSCAL-1432, OSCAL-1132, OSCAL-1632, OSCAL-1421 (trade names, manufactured by Nikki Catalysts and Chemicals Co., Ltd.), and Snowtex ST-OS (trade name, manufactured by Nissan Chemical Industries, Ltd.).
[0040] [Antioxidants] The conductive polymer dispersion of this embodiment may contain an antioxidant (stabilizer). Among the antioxidants, phenol-based antioxidants are preferred. Among the phenol-based antioxidants, at least one of gallic acid and esters of gallic acid is preferred. Gallic acid and esters of gallic acid have high antioxidant properties and also have the effect of improving electrical conductivity. Examples of esters of gallic acid include methyl gallate, ethyl gallate, and propyl gallate. As other phenol-based antioxidants, bisphenol compounds having a sulfide group or a sulfone group can also be suitably used. Examples of bisphenol compounds having a sulfide group or a sulfone group include bis(4-hydroxyphenyl)sulfide, bis(4-hydroxyphenyl)disulfide, bis(4-hydroxyphenyl)sulfone, and bis(2,4-dihydroxyphenyl)sulfide.
[0041] The content of the antioxidant is preferably 5 parts by mass or more and 200 parts by mass or less, more preferably 10 parts by mass or more and 100 parts by mass or less, and even more preferably 20 parts by mass or more and 80 parts by mass or less, relative to 100 parts by mass of the conductive composite. If the content is equal to or more than the lower limit of the above range, oxidation of the conductive composite can be further prevented. When it is equal to or less than the upper limit of the above range, a decrease in the conductivity of the conductive composite can be prevented.
[0042] [Other additives] The conductive polymer dispersion may contain other additives. The additives are not particularly limited as long as the effects of the present invention can be obtained. For example, surfactants, inorganic conductive agents, antifoaming agents, coupling agents, antioxidants, ultraviolet absorbing agents, etc. can be used. However, the additives are other than the above-mentioned π-conjugated conductive polymer, polyanion, unsaturated aliphatic alcohol compound, dispersion medium, binder component, and phenol-based antioxidant. The surfactant may be a nonionic, anionic or cationic surfactant, with the nonionic surfactant being preferred from the standpoint of storage stability. A polymer surfactant such as polyvinylpyrrolidone may also be added. Examples of the inorganic conductive agent include metal ions, conductive carbon, etc. Metal ions can be generated by dissolving a metal salt in water. The antifoaming agent includes silicone resin, polydimethylsiloxane, silicone oil, and the like. The coupling agent may be a silane coupling agent having an epoxy group, a vinyl group or an amino group. Examples of the antioxidant include phenol-based antioxidants, amine-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, and sugars. Examples of the ultraviolet absorber include benzotriazole-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, salicylate-based ultraviolet absorbers, cyanoacrylate-based ultraviolet absorbers, oxanilide-based ultraviolet absorbers, hindered amine-based ultraviolet absorbers, and benzoate-based ultraviolet absorbers.
[0043] When the conductive polymer dispersion contains the additive, the content ratio thereof is appropriately determined depending on the type of additive, but can be, for example, in the range of 0.001 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the conductive composite.
[0044] <Method of manufacturing conductive polymer dispersion> As a method for producing the conductive polymer dispersion of this embodiment, for example, a method in which a dispersion medium, a binder component, an unsaturated aliphatic alcohol compound, etc. are added to an aqueous dispersion of a conductive complex can be mentioned. The aqueous dispersion of the conductive complex may be obtained by chemically oxidizing and polymerizing a monomer that forms a π-conjugated conductive polymer in an aqueous solution of a polyanion, or a commercially available product may be used.
[0045] The chemical oxidative polymerization can be carried out using a known catalyst and oxidizing agent. Examples of the catalyst include transition metal compounds such as ferric chloride, ferric sulfate, ferric nitrate, and cupric chloride. Examples of the oxidizing agent include persulfates such as ammonium persulfate, sodium persulfate, and potassium persulfate. The oxidizing agent can return the reduced catalyst to its original oxidized state.
[0046] <Conductive laminate> A second aspect of the present invention is a conductive laminate comprising a substrate and a conductive layer formed on at least one surface of the substrate, the conductive layer being a cured layer of the conductive polymer dispersion of the first aspect.
[0047] [Conductive layer] The average thickness of the conductive layer provided on at least one surface of the substrate is, for example, preferably 10 nm to 100 μm, more preferably 20 nm to 50 μm, and even more preferably 30 nm to 30 μm. When the average thickness of the conductive layer is equal to or greater than the lower limit, a sufficiently high conductivity can be exhibited, and when the average thickness is equal to or less than the upper limit, the adhesion of the conductive layer to the substrate is further improved.
[0048] As an indicator of good conductivity of the conductive layer of this embodiment, for example, it is preferable for the conductive layer to have a surface resistance value of 10 Ω / sq. or more and 10,000 Ω / sq. or less, more preferably a surface resistance value of 10 Ω / sq. or more and 5,000 Ω / sq. or less, even more preferably a surface resistance value of 10 Ω / sq. or more and 2,500 Ω / sq. or less, and particularly preferably a surface resistance value of 10 Ω / sq. or more and 1,000 Ω / sq. or less.
[0049] [Base material] The substrate constituting the conductive laminate of this embodiment may be a substrate made of an insulating material or a substrate made of a conductive material. The shape of the substrate is not particularly limited, and examples thereof include a shape mainly having a flat surface such as a film or a substrate. Examples of insulating materials include glass, synthetic resin, and ceramics. The conductive material may be a metal, a conductive metal oxide, carbon, or the like.
[0050] (Film substrate) When a film substrate is used as the substrate, the conductive laminate becomes a conductive film. The film substrate may be, for example, a plastic film made of a synthetic resin, such as ethylene-methyl methacrylate copolymer resin, ethylene-vinyl acetate copolymer resin, polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyvinyl alcohol, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyacrylate, polycarbonate, polyvinylidene fluoride, polyarylate, styrene-based elastomer, polyester-based elastomer, polyethersulfone, polyetherimide, polyetheretherketone, polyphenylene sulfide, polyimide, cellulose triacetate, cellulose acetate propionate, etc. From the viewpoint of improving the adhesion between the film substrate and the conductive layer, the synthetic resin for the film substrate is preferably the same type of resin as the binder resin, and among these, a polyester resin such as polyethylene terephthalate is preferred.
[0051] The synthetic resin for the film substrate may be either amorphous or crystalline. The film substrate may be either unstretched or stretched. The film substrate may be subjected to a surface treatment such as a corona discharge treatment, a plasma treatment, or a flame treatment in order to further improve the adhesiveness of the conductive layer formed from the conductive polymer dispersion.
[0052] The average thickness of the film substrate is preferably 5 μm to 500 μm, more preferably 20 μm to 200 μm. If the average thickness of the film substrate is equal to or more than the lower limit, the film is less likely to break, and if the average thickness is equal to or less than the upper limit, the film can have sufficient flexibility. The average thickness of the film substrate is calculated by measuring the thickness at 10 randomly selected points and averaging the measured values.
[0053] (Glass substrate) Examples of the glass substrate include an alkali-free glass substrate, a soda-lime glass substrate, a borosilicate glass substrate, and a quartz glass substrate. If the substrate contains an alkali component, the conductivity of the conductive layer tends to decrease, so among the above glass substrates, an alkali-free glass is preferred. Here, the alkali-free glass refers to a glass composition in which the content of the alkali component is 0.1 mass% or less with respect to the total mass of the glass composition.
[0054] The average thickness of the glass substrate is preferably 100 μm or more and 3000 μm or less, and more preferably 100 μm or more and 1000 μm or less. If the average thickness of the glass substrate is equal to or more than the lower limit, the substrate is less likely to be broken, and if the average thickness is equal to or less than the upper limit, the substrate can contribute to making the conductive laminate thinner. The average thickness of the glass substrate is calculated by measuring the thickness at 10 randomly selected points and averaging the measured values.
[0055] <Method for manufacturing conductive laminate> A third aspect of the present invention is a method for producing a conductive laminate, the method comprising applying the conductive polymer dispersion of the first aspect to at least one surface of a substrate. The conductive laminate of the second aspect can be produced by the production method of this aspect.
[0056] Examples of a method for applying (coating) the conductive polymer dispersion of the first embodiment on an arbitrary surface of a substrate include a method using a coater such as a gravure coater, a roll coater, a curtain flow coater, a spin coater, a bar coater, a reverse coater, a kiss coater, a fountain coater, a rod coater, an air doctor coater, a knife coater, a blade coater, a cast coater, or a screen coater; a method using a sprayer such as an air spray, an airless spray, or a rotor dampening; and an immersion method such as dipping.
[0057] The amount of conductive polymer dispersion applied to the film substrate is not particularly limited, but taking into consideration uniform and even application, conductivity, and film strength, a solid content of 0.01 g / m 2 More than 10.0g / m2 The following ranges are preferred:
[0058] The coating film made of the conductive polymer dispersion applied onto the substrate is dried to remove the dispersion medium, thereby obtaining a conductive laminate in which a conductive layer (conductive film) is formed by hardening the coating film. Methods for drying the coating film include heat drying, vacuum drying, etc. Examples of heat drying that can be used include hot air heating and infrared heating. When applying heat drying, the heating temperature is appropriately set depending on the dispersion medium used, but is usually within the range of 50° C. to 150° C. Here, the heating temperature is the set temperature of the drying device. A suitable drying time within the above heating temperature range is preferably 1 minute to 30 minutes, more preferably 5 minutes to 15 minutes.
[0059] Since the conductive polymer dispersion applied in this embodiment has a short touch-dry time, a pre-drying step of drying without heating may be provided before the heat-drying step. By performing the pre-drying step, a part of the dispersion medium can be removed in advance from the coating film to be subjected to the heat-drying step, and the amount of the dispersion medium that volatilizes during the heat-drying step is reduced, which makes it easier to prevent the volatilized dispersion medium from remaining around the heat-drying machine or the like. As a method of pre-drying, the substrate may be left to dry naturally at room temperature (20 to 25° C.), may be placed in a vacuum environment at room temperature, or may be sprayed with air or an inert gas at room temperature. The pre-drying time when drying naturally at room temperature is preferably a time that is equal to or longer than the touch-drying time described below, and can be, for example, about 1 to 20 minutes. When room temperature air or an inert gas is sprayed, the tack-dry time can be further shortened, for example to about 30 seconds to 5 minutes. Furthermore, the shorter the pre-drying time, the less risk there is of dust adhering to the coating film during drying. The conductivity of the coating film (conductive layer) that is only pre-dried is inferior to that of the coating film that is heat-dried, and there may be a problem that the conductivity decreases after production. For this reason, it is preferable to carry out the above-mentioned heat drying after the pre-drying step. The heating temperature at this time is preferably 60°C or higher and 150°C or lower, more preferably 80°C or higher and 140°C or lower, and even more preferably 100°C or higher and 130°C or lower.
[0060] When the applied conductive polymer dispersion contains a silicon oxide-containing compound such as the above-mentioned alkoxysilane, silicate, or silica as a binder component, the coating film can be heated to cause the binder components to react with each other, thereby forming a cured conductive layer. EXAMPLES
[0061] (Production Example 1) 206 g of sodium styrenesulfonate was dissolved in 1000 ml of ion-exchanged water, and while stirring at 80° C., 1.14 g of an oxidizing agent solution of ammonium persulfate previously dissolved in 10 ml of water was added dropwise over 20 minutes, and the solution was stirred for 12 hours. 1000ml of sulfuric acid diluted to 10% by mass was added to the obtained sodium polystyrene sulfonate-containing solution to obtain a polystyrene sulfonic acid-containing solution. Then, about 1000ml of the polystyrene sulfonic acid-containing solution was removed by ultrafiltration, 2000ml of ion-exchanged water was added to the remaining liquid, and about 2000ml of the solution was removed by ultrafiltration. The above ultrafiltration operation was repeated three times. Furthermore, about 2000ml of ion-exchanged water was added to the obtained filtrate, and about 2000ml of the solution was removed by ultrafiltration. This ultrafiltration operation was repeated three times. Water in the resulting solution was removed under reduced pressure to obtain colorless solid polystyrene sulfonic acid.
[0062] (Production Example 2) 14.2 g of 3,4-ethylenedioxythiophene and a solution in which 36.7 g of polystyrene sulfonic acid was dissolved in 2000 ml of ion-exchanged water were mixed at 20°C. The resulting mixed solution was kept at 20° C., and while stirring, 29.64 g of ammonium persulfate and 8.0 g of an oxidation catalyst solution of ferric sulfate dissolved in 200 ml of ion-exchanged water were slowly added, followed by stirring for 3 hours to carry out the reaction. 2000 ml of ion-exchanged water was added to the reaction solution, and about 2000 ml of the solution was removed by ultrafiltration. This procedure was repeated three times. Then, 200 ml of sulfuric acid diluted to 10% by mass and 2000 ml of ion-exchanged water were added to the obtained solution, about 2000 ml of the solution was removed by ultrafiltration, 2000 ml of ion-exchanged water was added to this, and about 2000 ml of the solution was removed by ultrafiltration. This operation was repeated three times. Furthermore, 2000 ml of ion-exchanged water was added to the obtained solution, and about 2000 ml of the solution was removed by ultrafiltration. This operation was repeated five times to obtain a 1.2 mass% aqueous dispersion of polystyrenesulfonic acid-doped poly(3,4-ethylenedioxythiophene) (PEDOT-PSS aqueous dispersion).
[0063] Example 1 To 25 g of the PEDOT-PSS aqueous dispersion obtained in Production Example 2, 0.5 g of cis-2-butene-1,4-diol as an unsaturated aliphatic alcohol compound, 35 g of pure water and 35 g of ethanol as dispersion media, and 3 g of a water-dispersible polyester resin (PES Resin A645GH, manufactured by Takamatsu Oil Co., Ltd., solids concentration 30 mass%) as a binder component were added, and after thorough mixing at room temperature, 0.1 g of gallic acid and 0.01 g of an acetylene-based surfactant (Surfynol 420, manufactured by Nissin Chemical Industry Co., Ltd.) were added as stabilizers, and the mixture was further stirred and mixed for 1 hour to obtain a conductive polymer dispersion with a water content of 63%.
[0064] Example 2 A conductive polymer dispersion liquid with a water content of 63% was obtained in the same manner as in Example 1, except that the unsaturated aliphatic alcohol compound was changed to 0.5 g of 2-butyne-1,4-diol.
[0065] Example 3 To 25 g of the PEDOT-PSS aqueous dispersion obtained in Production Example 2, 1.5 g of 2-butyne-1,4-diol as an unsaturated aliphatic alcohol compound, 47 g of pure water and 24 g of methanol as dispersion media, and 3 g of a water-dispersible polyester resin (RZ-105, manufactured by GOO Chemical Industry Co., Ltd., solid content concentration 25% by mass) as a binder component were added, and after thorough mixing at room temperature, 0.1 g of gallic acid and 0.01 g of an acetylene-based surfactant (Surfynol 420, manufactured by Nissin Chemical Industry Co., Ltd.) were added as stabilizers, and the mixture was further stirred and mixed for 1 hour to obtain a conductive polymer dispersion with a water content of 73%.
[0066] Example 4 To 15 g of the PEDOT-PSS aqueous dispersion obtained in Production Example 2, 0.5 g of 2-butyne-1,4-diol as an unsaturated aliphatic alcohol compound, 47 g of pure water and 34 g of methanol as dispersion media, and 3 g of a water-dispersible polyester resin (RZ-105, manufactured by GOO Chemical Industry Co., Ltd., solid content concentration 25% by mass) as a binder component were added, and after thorough mixing at room temperature, 0.1 g of gallic acid was added as a stabilizer, and the mixture was further stirred and mixed for 1 hour to obtain a conductive polymer dispersion with a water content of 64%.
[0067] Example 5 A conductive polymer dispersion liquid with a water content of 62% was obtained in the same manner as in Example 1, except that 2 g of 2,4-hexadiyn-1,6-diol was used as the unsaturated aliphatic alcohol compound.
[0068] Example 6 To 25 g of the PEDOT-PSS aqueous dispersion obtained in Production Example 2, 1 g of 2-butyne-1,4-diol as an unsaturated aliphatic alcohol compound, 70 g of pure water as a dispersion medium, and 3 g of a water-dispersible polyester resin (PES Resin A640, manufactured by Takamatsu Oil Co., Ltd., solids concentration 25% by mass) as a binder component were added, and after thorough mixing at room temperature, 0.1 g of methyl gallate and 0.1 g of 4-hydroxypyridine were added as stabilizers, and 0.02 g of an acetylene-based surfactant (Olfine 4200, manufactured by Nissin Chemical Industry Co., Ltd.) was added, and the mixture was further stirred and mixed for 1 hour to obtain a conductive polymer dispersion with a water content of 98%.
[0069] Example 7 To 40 g of the PEDOT-PSS aqueous dispersion obtained in Production Example 2, 1 g of trans-2-butene-1,4-diol as an unsaturated aliphatic alcohol compound, 26 g of pure water and 30 g of methanol as dispersion media, and 3 g of a water-dispersible polyester resin (PES Resin A640, solids concentration 25% by mass, manufactured by Takamatsu Oil Co., Ltd.) as a binder component were added, and after thorough mixing at room temperature, 0.1 g of gallic acid as a stabilizer and 0.01 g of an acetylene-based surfactant (Olfine 4200, manufactured by Nissin Chemical Industry Co., Ltd.) were added, and the mixture was further stirred and mixed for 1 hour to obtain a conductive polymer dispersion with a water content of 68%.
[0070] Example 8 To 25 g of the PEDOT-PSS aqueous dispersion obtained in Production Example 2, 1 g of 2-butyne-1,4-diol as an unsaturated aliphatic alcohol compound, 40 g of pure water and 30 g of ethanol as dispersion media, and 3 g of tetraethoxysilane as a binder component were added, and mixed at room temperature for 48 hours. After that, 0.05 g of bis(4-hydroxyphenyl)sulfide and 0.05 g of bis(4-hydroxyphenyl)sulfone as stabilizers and 0.01 g of a silicone surfactant (Silface SJM002, manufactured by Nissin Chemical Industry Co., Ltd.) were added, and the mixture was stirred and mixed for another hour to obtain a conductive polymer dispersion with a water content of 65%.
[0071] Example 9 To 40 g of the PEDOT-PSS aqueous dispersion obtained in Production Example 2, 0.5 g of cis-2-butene-1,4-diol as an unsaturated aliphatic alcohol compound, 25 g of pure water and 30 g of ethanol as a dispersion medium, and tetraethoxysilane (KBE-04, manufactured by Shin-Etsu Chemical Co., Ltd., SiO 2 3 g of the resulting mixture (converted solids concentration: 28.8% by mass) and 1 g of water-dispersed silica sol (Snowtex ST-OS, manufactured by Nissan Chemical Industries, Ltd., solids concentration: 20% by mass) were added and mixed at room temperature for 48 hours, after which 0.05 g of bis(4-hydroxyphenyl)sulfide and 0.05 g of bis(4-hydroxyphenyl)sulfone as stabilizers and 0.01 g of a silicone-based surfactant (Silface SJM002, manufactured by Nissin Chemical Industry Co., Ltd.) were added and stirred for a further hour to obtain a conductive polymer dispersion with a water content of 68%.
[0072] Comparative Example 1 A conductive polymer dispersion liquid with a water content of 63% was obtained in the same manner as in Example 1, except that no unsaturated aliphatic alcohol compound was used.
[0073] Comparative Example 2 A conductive polymer dispersion liquid with a water content of 63% was obtained in the same manner as in Example 1, except that 0.5 g of ethylene glycol was used instead of the unsaturated aliphatic alcohol compound.
[0074] Comparative Example 3 A conductive polymer dispersion liquid with a water content of 62% was obtained in the same manner as in Example 1, except that 1 g of 1,4-butanediol was used instead of the unsaturated aliphatic alcohol compound. The compositions of the above examples are shown in Table 1. In the table, "parts by weight" is synonymous with "parts by mass."
[0075] [Table 1]
[0076] <Evaluation> The results for the following evaluation items are shown in Tables 2 and 3. [Measurement of dry-to-touch time] The conductive polymer dispersion of each example was applied to a polyethylene terephthalate film (Lumirror T60, manufactured by Toray Industries, Inc.) using a bar coater (wet film thickness 16 μm) to form a coating film. This coating film was stored under conditions of 24°C and 40% RH, and a nonwoven fabric was pressed against it at regular intervals with a load of 20 gf. The time when no trace remained was recorded as the tactile dry time. The shorter the tactile dry time, the faster the coating film dries, improving yield and productivity.
[0077] [Surface resistance measurement] The conductive polymer dispersions of Examples 1 to 7 and Comparative Examples 1 to 3 were applied to a polyethylene terephthalate film (Lumirror T60, manufactured by Toray Industries, Inc.) using a bar coater (wet film thickness 16 μm), and then heated and dried at a drying temperature of 100° C. for 5 minutes to obtain a conductive film. The conductive polymer dispersions of Examples 8 and 9 were applied to alkali-free glass (Corning Eagle XG 75 mm × 75 mm × 0.7 mm) using a spin coater (Mikasa MS-B100, rotation speed 1000 rpm, time 10 seconds), and then heated and dried at a drying temperature of 120°C for 30 minutes to obtain conductive glass. The surface resistance values of the conductive film and the conductive glass obtained above were measured using a resistivity meter (Loresta manufactured by Nitto Seiko Analytech Co., Ltd.) at an applied voltage of 10V.
[0078] [Durability evaluation] The conductive polymer dispersions of Examples 1 and 2 and Comparative Examples 2 and 3 were applied to a polyethylene terephthalate film (Lumirror T60, manufactured by Toray Industries, Inc.) using a bar coater (wet film thickness 16 μm), and then heated and dried at a drying temperature of 100° C. for 5 minutes to prepare a conductive film. After measuring the initial surface resistance immediately after preparation using the above method, the conductive film was placed under high temperature and high humidity conditions (temperature 85°C and humidity 85%) and the conductive layer surface was left exposed for 500 hours, after which the surface resistance (surface resistance after exposure to high temperature and humidity) was measured. The rate of change in surface resistance (surface resistance after exposure / initial surface resistance) was used as an index of durability. The closer the rate of change in surface resistance is to 1, the higher the durability.
[0079] [Table 2]
[0080] [Table 3]
[0081] Since the conductive polymer dispersions of Examples 1 to 9 contain an unsaturated aliphatic alcohol compound, it is clear that the conductivity of the coating film is excellent and the tack-dry time is short. As confirmed in Examples 1 and 2, since the conductive polymer dispersion according to the present invention contains an unsaturated aliphatic alcohol compound, the durability of the coating film (conductive layer) is also excellent. Since the conductive polymer dispersion of Comparative Example 1 does not contain a diol compound, the conductivity of the coating film is significantly inferior to that of the Examples. The conductive polymer dispersion of Comparative Example 2 contains ethylene glycol having no unsaturated bonds, but the conductivity and durability of the coating film are significantly inferior to those of the Examples. The conductive polymer dispersion of Comparative Example 3 contains butanediol having no unsaturated bonds, and the conductivity of the coating film is equivalent to that of the Examples, but the tack-free time and durability are inferior. It should be noted that Example 5 is a reference example.
Claims
1. A conductive polymer dispersion liquid containing a conductive complex including a π-conjugated conductive polymer and a polyanion, an unsaturated aliphatic alcohol compound which is a diol compound having 4 to 6 carbon atoms and one double bond or triple bond between carbon atoms in the molecule, and a dispersion medium.
2. 2. The conductive polymer dispersion according to claim 1, wherein the unsaturated aliphatic alcohol compound comprises at least one selected from the group consisting of cis-2-butene-1,4-diol, trans-2-butene-1,4-diol, and 2-butyne-1,4-diol.
3. The conductive polymer dispersion according to claim 1 , wherein the content of the unsaturated aliphatic alcohol compound is 3% by mass or less.
4. The conductive polymer dispersion according to any one of claims 1 to 3, wherein the conductive polymer dispersion has a water content of 50 mass % or more.
5. The conductive polymer dispersion according to any one of claims 1 to 4, further comprising a binder component.
6. The conductive polymer dispersion according to any one of claims 1 to 5, further comprising a phenol-based antioxidant.
7. A conductive laminate comprising a substrate and a conductive layer formed on at least one surface of the substrate, the conductive layer being a cured layer of the conductive polymer dispersion according to any one of claims 1 to 6.
8. A method for producing a conductive laminate, comprising applying the conductive polymer dispersion according to any one of claims 1 to 6 to at least one surface of a substrate.
Citation Information
Patent Citations
Photoelectric conversion element, solar cell module, and method of manufacturing photoelectric conversion element
JP2014027174A
Conductive polymer and conductive composition containing the same, and film having coating film containing the polymer or the composition
JP2014040549A
Conductive laminate
JP2016221874A
Conductive polymer aqueous dispersion liquid, alcohol containing conductive polymer aqueous dispersion liquid, and method for producing conductive film
JP2017057335A
Conductive polymer-containing solution, method for producing the same, and method for producing conductive film
JP2020007470A