Circular polarizer

The optical laminate with an adhesive missing portion at the edge addresses the issue of hue uniformity deterioration in high-temperature environments by dispersing shrinkage stress, maintaining hue uniformity and preventing defects.

JP7555314B2Active Publication Date: 2024-09-24SUMITOMO CHEM CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2021127576
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-02
Filing Date
2021-08-03
Publication Date
2024-09-24
Estimated Expiration
2040-03-11

AI Technical Summary

Technical Problem

The uniformity of hue in reflected light from composite polarizing plates deteriorates in high-temperature environments due to changes in the hue at the edges, caused by shrinkage stress concentrating on the retardation film when the polarizing layer shrinks.

Method used

An optical laminate design with a polarizing layer, adhesive layer, and first retardation layer, featuring an adhesive missing portion at the edge, where the inner end of the adhesive layer aligns with the polarizing layer's edge, set at a distance of 3 μm or more inward, dispersing shrinkage stress and maintaining hue uniformity.

Benefits of technology

The design effectively suppresses the deterioration of hue uniformity in the optical laminate even in high-temperature conditions by dispersing shrinkage stress, preventing peeling and bubble formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555314000006
    Figure 0007555314000006
  • Figure 0007555314000007
    Figure 0007555314000007
  • Figure 0007555314000005
    Figure 0007555314000005
Patent Text Reader

Abstract

To provide a circular polarizer that can suppress degradation of the uniformity of the color phase of a reflected light in a plane under a high-temperature environment.SOLUTION: The circular polarizer includes a polarization layer, an adhesive layer, and a first phase difference layer. The first phase difference layer is a liquid crystal layer. The circular polarizer has a square shape with a glue missing part in an end part in a plane direction or a square shape with a notch part in at least a side. The square shape has a pair of longer sides and a pair of shorter sides. The glue missing part is formed so that the position of the innermost edge in the end part of the adhesive layer is 3 μm to 50 μm inner from the position of the outermost edge in the end part of the polarization layer, in a cross section which passes through the region where the polarization layer and the adhesive layer overlap with each other in the laminate direction.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical laminate. [Background technology]

[0002] Polarizing layers, retardation layers, and the like are widely used as optical components constituting organic EL displays using organic light-emitting diodes (OLEDs) and liquid crystal displays. For example, Patent Document 1 describes the use of a composite polarizing plate, in which a polarizer and a retardation film coated with a liquid crystal compound are laminated, in a liquid crystal display.

[0003] Patent Document 1 describes that by eliminating the unevenness present on the outer edge surface (cut surface) when a composite polarizing plate is cut by chip cutting or the like, problems such as peeling or floating of the retardation film can be suppressed even under humid and hot conditions. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2008-9237 A Summary of the Invention [Problem to be solved by the invention]

[0005] It has been found that when a composite polarizing plate composed of a polarizing layer and a retardation film is exposed to a high-temperature environment, the hue of the reflected light at the ends of the composite polarizing plate changes, and the uniformity of the hue of the reflected light within the plane deteriorates.

[0006] An object of the present invention is to provide an optical laminate capable of suppressing deterioration in the uniformity of the hue of in-plane reflected light even in a high-temperature environment. [Means for solving the problem]

[0007] The present invention provides the following optical laminate. [1] An optical laminate having a polarizing layer, a pressure-sensitive adhesive layer, and a first retardation layer in this order, The optical laminate has a glue chipping portion at an end portion in a surface direction thereof, The adhesive missing portion is formed such that, in a cross section passing through the portion where the polarizing layer and the pressure-sensitive adhesive layer overlap in the stacking direction, the position of the innermost end of the end of the pressure-sensitive adhesive layer is located 3 μm or more inward from the position of the outermost end of the end of the polarizing layer. [2] The optical laminate according to [1], wherein the polarizing layer is a polyvinyl alcohol-based resin film having a dichroic dye adsorbed and oriented thereon. [3] The optical laminate has a rectangular shape or a rectangular shape having a notch on at least one side, The optical laminate described in [1] or [2], wherein the glue missing portion is formed on at least one side of the rectangular shape. [4] The rectangular shape has a pair of long sides and a pair of short sides, the absorption axis direction of the polarizing layer forms an angle of 45°±10° with respect to the long side; The optical laminate described in [3], wherein the glue missing portion is formed on at least one of the pair of long sides and at least one of the pair of short sides. [5] The rectangular shape has a pair of long sides and a pair of short sides, the absorption axis direction of the polarizing layer forms an angle of 0°±10° with respect to the long side; The optical laminate described in [3], wherein the glue missing portion is formed on at least one of the pair of short sides. [6] The rectangular shape has a pair of long sides and a pair of short sides, the absorption axis direction of the polarizing layer forms an angle of 0°±10° with respect to the short side; The optical laminate described in [3], wherein the glue missing portion is formed on at least one of the pair of long sides. [7] The optical laminate according to any one of [1] to [6], which has a protective layer on one or both sides of the polarizing layer. [8] The optical laminate according to any one of [1] to [7], further comprising a second retardation layer on the side of the first retardation layer opposite to the pressure-sensitive adhesive layer. [9] The optical laminate according to [8], wherein the second retardation layer is provided on the first retardation layer via an adhesive layer.

[10] The optical laminate according to any one of [1] to [9], which is a circular polarizing plate. Effect of the Invention

[0008] According to the present invention, it is possible to provide an optical laminate in which deterioration of the uniformity of the hue of the in-plane reflected light is suppressed even in a high-temperature environment. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a cross-sectional view illustrating an example of an optical laminate of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view illustrating a schematic diagram of another example of the optical laminate of the present invention. [Diagram 3] 1(a) and 1(b) are schematic diagrams illustrating a method for producing a pressure-sensitive adhesive layer in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, preferred embodiments of the optical laminate of the present invention will be described with reference to the drawings. Note that the scope of the present invention is not limited to the embodiments described here, and various modifications can be made without departing from the spirit of the present invention.

[0011] Fig. 1 is a cross-sectional view showing a schematic example of an optical laminate of this embodiment. In the drawing, W represents the plane direction. As shown in Fig. 1, the optical laminate 11 of this embodiment has a polarizing plate 40, a pressure-sensitive adhesive layer 31, and a first retardation layer 21 in this order. The polarizing plate 40 of the optical laminate 11 shown in Fig. 1 has a first protective layer 42 (protective layer), a polarizing layer 41, and a second protective layer 43 (protective layer) in this order, and in the optical laminate 11, the pressure-sensitive adhesive layer 31 is provided on the first protective layer 42 side.

[0012] The polarizing layer 41 may be a polyvinyl alcohol resin film (hereinafter, sometimes referred to as a "PVA resin film") in which a dichroic dye such as iodine is adsorbed and aligned, and the PVA resin film is usually a stretched polyvinyl alcohol resin film. The polarizing layer 41 may be a layer in which a dichroic dye is aligned in a cured liquid crystal compound. The first protective layer 42 and the second protective layer 43 are layers for protecting the polarizing layer 41. The first retardation layer 21 may be a retardation film or a liquid crystal layer containing a liquid crystal compound. The liquid crystal layer may be a cured layer formed by polymerizing a polymerizable liquid crystal compound, for example. When the first retardation layer 21 is a liquid crystal layer, the optical laminate 11 may have an alignment layer for aligning the liquid crystal compound constituting the first retardation layer 21 on the side opposite to the pressure-sensitive adhesive layer 31 of the first retardation layer 21.

[0013] The optical laminate 11 has a glue chipping portion 5 at an end in the planar direction W. As shown in FIG. 1, the glue chipping portion 5 is formed such that, in a cross section passing through a portion where the polarizing layer 41 and the adhesive layer 31 overlap in a lamination direction perpendicular to the planar direction W, the position of the innermost end at the end of the adhesive layer 31 is located inward from the position of the outermost end at the end of the polarizing layer 41 by a distance L1. In this specification, the position of the innermost end at the end of the adhesive layer 31 refers to the position of the end of the adhesive layer 31 that is the innermost in the planar direction W, and the position of the outermost end at the end of the polarizing layer 41 refers to the position of the end of the polarizing layer 41 that is the outermost in the planar direction W.

[0014] The distance L1 of the glue missing portion 5 is 3 μm or more, preferably 5 μm or more, and may be 6 μm or more, 7 μm or more, or 8 μm or more. The distance L1 is usually 120 μm or less, may be 100 μm or less, may be 75 μm or less, may be 50 μm or less, or may be 25 μm or less.

[0015] The polarizing plate 40 included in the optical laminate 11 has a polarizing layer 41. The polarizing layer 41 may shrink in a high-temperature environment. Therefore, when the optical laminate 11 is exposed to a high-temperature environment, it is considered that the shrinkage stress of the polarizing layer 41 is concentrated at the end of the first retardation layer 21 laminated on the polarizing plate 40 via the adhesive layer 31 due to the shrinkage of the polarizing layer 41 (polarizing plate 40). When the above-mentioned shrinkage stress is concentrated at the end of the first retardation layer 21, the difference between the hue of the reflected light at the end of the optical laminate 11 and the hue of the reflected light of the other parts other than the end becomes large due to the influence of the photoelasticity of the first retardation layer 21, and it is presumed that the uniformity of the hue of the reflected light in the plane of the optical laminate 11 is deteriorated. In this embodiment, as described above, the distance L1 at the glue chipping portion 5 of the optical laminate 11 is set to 3 μm or more. This makes it easier to disperse the shrinkage stress of the polarizing layer 41 when the optical laminate 11 is exposed to a high-temperature environment, so that the shrinkage stress applied to the end of the first retardation layer 21 can be reduced. As a result, it is possible to reduce the difference in hue between the reflected light at the end of the optical laminate 11 and the hue of the reflected light at other parts other than the end, which is caused by the photoelasticity of the first retardation layer 21, and it is therefore possible to suppress deterioration in the uniformity of the hue of the reflected light within the surface of the optical laminate 11.

[0016] Furthermore, if the distance L1 of the glue missing portion 5 in the optical laminate 11 is too large, the adhesion area between the polarizing plate 40 and the first retardation layer 21 becomes small, making it easier for the ends to peel off or for defects such as air bubbles to occur during a high-temperature durability test.

[0017] The effect of shrinkage of the polarizing layer 41 in a high-temperature environment is more noticeable when the polarizing layer 41 is a polarizing layer in which the dichroic dye is adsorbed and aligned on a PVA-based resin film, particularly when the polarizing layer is formed by dyeing a PVA-based resin film and then stretching the film, than when the polarizing layer 41 is a layer in which the dichroic dye is oriented in a cured liquid crystal compound. Therefore, when the polarizing layer 41 is a PVA-based resin film in which the dichroic dye is adsorbed and aligned, by setting the distance L1 at the glue chipping portion 5 to 3 μm or more, deterioration of the uniformity of the hue of the reflected light within the plane of the optical laminate 11 can be more suitably suppressed.

[0018] The distance L1 of the glue chipping portion 5 can be calculated based on the position of the innermost end of the end of the pressure-sensitive adhesive layer 31 and the position of the outermost end of the end of the polarizing layer 41, which are determined based on the profile of the cross section of the optical laminate 11 measured using a laser microscope. When the outer shape of the optical laminate 11 has straight sides and the glue chipping portion 5 is formed on the sides, the cross section of the optical laminate 11 is taken as a cross section cut along a direction perpendicular to the sides at the position where the glue chipping portion 5 is formed on the sides. When the outer shape of the optical laminate 11 has curved parts and the glue chipping portion 5 is formed on the curved parts, the cross section of the optical laminate 11 is taken as a cross section cut along a direction passing through the position P of the tangent line in the surface direction of the optical laminate 11 at the position P where the glue chipping portion 5 is formed and perpendicular to the tangent line.

[0019] The shape of the glue chipping portion 5 in the optical laminate 11 is not particularly limited, and the end of the adhesive layer 31 may have a tapered shape as shown in FIG. 1, may be parallel to the lamination direction perpendicular to the surface direction W, and may be formed in a sawtooth shape, uneven shape, curved shape, etc. As shown in FIG. 1, the adhesive layer 31 in the glue chipping portion 5 may have a tapered shape in which the end position of the surface on the polarizing plate 40 side is located inside the surface direction of the end position of the surface on the first retardation layer 21 side of the adhesive layer 31, or conversely, the end position of the surface on the polarizing plate 40 side is located outside the surface direction of the end position of the surface on the first retardation layer 21 side of the adhesive layer 31, and may have a tapered shape. In the latter tapered shape, it is considered that the shrinkage stress of the polarizing layer 41 in a high temperature environment is easily dispersed, and therefore it is easy to suppress the deterioration of the uniformity of the hue of the reflected light in the surface of the optical laminate 11.

[0020] The external shape of the optical laminate 11 can be a square shape in the surface direction (plan view) or a square shape having a notch on at least one side. In this specification, a square shape refers to a rectangular shape or a square shape, and includes a square shape in which at least one of the four corners of the square shape is rounded. The boundary between two sides that are continuous through a rounded corner portion is a position that bisects the contour length of the rounded corner portion. The contour length of the rounded corner portion is the length between the ends of the straight line parts of the two sides that are continuous through the rounded corner portion and that are located on the side of the rounded corner portion. The notch portion can be a concave shape that is concave toward the opposing side, and the concave shape may be U-shaped or V-shaped. The notch portion may be formed on one side of the square shape or on two or more sides. The notch portion can be provided in an area where at least one of the earpiece, speaker, camera lens, LED lamp, proximity sensor, illuminance sensor, fingerprint authentication sensor, operation button, etc. is installed in a smartphone, for example.

[0021] When the optical laminate 11 has a rectangular shape, the glue chipping portion 5 is preferably formed on at least one side of the rectangular shape, and may be formed on two or more sides, or may be formed on all four sides. The glue chipping portion 5 may be formed continuously or discontinuously over the entire length of the side, or may be formed on a part of the side. The glue chipping portion 5 may be formed on at least a part of the cutout portion, or may be formed on the entire cutout portion.

[0022] The optical laminate 11 may have a hole penetrating the entire optical laminate 11 in the lamination direction. The hole may be circular, elliptical, rectangular, hexagonal, or other polygonal shape, and at least one corner of the polygon may be rounded. A glue chip 5 may be formed around the hole. The glue chip formed in the hole may be formed in at least a part of the periphery of the hole, or may be formed around the entire periphery of the hole. The hole may be provided in an area where a camera lens or the like is installed, for example, in a smartphone or the like.

[0023] When the optical laminate 11 has a square shape, and this square shape is a rectangle having a pair of long sides and a pair of short sides, and the absorption axis direction of the polarizing layer 41 is at an angle of 45°±10° with respect to the long sides, it is preferable that the glue chipping portion 5 is formed on at least one of the pair of long sides and at least one of the pair of short sides. In this specification, the above angle refers to an acute angle between the absorption axis direction and the long side. The glue chipping portion 5 may be formed on both of the pair of long sides, or may be formed on both of the pair of short sides. When the polarizing layer 41 of the optical laminate 11 is exposed to a high temperature environment, it is likely to shrink in the absorption axis direction, so that the shrinkage stress of the polarizing layer 41 is likely to concentrate on the sides located at both ends of the absorption axis direction. Therefore, in the optical laminate 11 in which the absorption axis direction and the long side are in a relationship of 45°±10°, it is considered that the shrinkage stress of the polarizing layer 41 is likely to concentrate on both the long sides and the short sides, and the hue of the reflected light of the first retardation layer 21 is likely to change. As described above, by providing the glue chipping portion 5 on at least one of the pair of long sides and at least one of the pair of short sides, the shrinkage stress of the polarizing layer 41 can be dispersed in the portion where the shrinkage stress is likely to concentrate when the optical laminate 11 is exposed to a high temperature environment. This is believed to effectively prevent the deterioration of the uniformity of the hue of the reflected light in the plane even when the optical laminate 11 is exposed to a high temperature environment. The angle that the absorption axis direction of the polarizing layer 41 makes with the long sides may be 45°±5°, 45°±2°, or 45°.

[0024] When the optical laminate 11 has a square shape, and this square shape is a rectangle having a pair of long sides and a pair of short sides, and the absorption axis direction of the polarizing layer 41 forms an angle of 0°±10° with respect to the long side, it is preferable that the glue chipping portion 5 is formed on at least one of the pair of short sides. In this specification, the above angle refers to an acute angle between the absorption axis direction and the long side. The glue chipping portion 5 may be formed on both of the pair of short sides. In the optical laminate 11 in which the absorption axis direction and the long side are in a relationship of 0°±10°, for the above-mentioned reasons, it is considered that the shrinkage stress of the polarizing layer 41 is likely to concentrate on the short side, and the hue of the reflected light of the first retardation layer 21 is likely to change. Therefore, it is considered that by providing the glue chipping portion 5 on at least one of the pair of short sides, the deterioration of the uniformity of the hue of the reflected light in the plane can be effectively suppressed even when the optical laminate 11 is exposed to a high-temperature environment. The angle that the absorption axis direction of the polarizing layer 41 makes with respect to the long side may be 0°±5°, 0°±2°, or 0°.

[0025] When the optical laminate 11 has a square shape, and this square shape is a rectangle having a pair of long sides and a pair of short sides, and the absorption axis direction of the polarizing layer 41 forms an angle of 0°±10° with respect to the short side, it is preferable that the glue chipping portion 5 is formed on at least one of the pair of long sides. In this specification, the above angle refers to an acute angle between the absorption axis direction and the short side. The glue chipping portion 5 may be formed on both of the pair of long sides. In the optical laminate 11 in which the absorption axis direction and the short side are in a relationship of 0°±10°, for the above-mentioned reasons, it is considered that the shrinkage stress of the polarizing layer 41 is likely to concentrate on the long side, and the hue of the reflected light of the first retardation layer 21 is likely to change. Therefore, it is considered that by providing the glue chipping portion 5 on at least one of the pair of long sides, the deterioration of the uniformity of the hue of the reflected light in the plane can be effectively suppressed even when the optical laminate 11 is exposed to a high-temperature environment. The angle that the absorption axis direction of the polarizing layer 41 makes with respect to the short side may be 0°±5°, 0°±2°, or 0°.

[0026] In the optical laminate 11 shown in Fig. 1, the first retardation layer 21 may be an A plate or a C plate. In addition, in the optical laminate 11 shown in Fig. 1, the first retardation layer 21 can be a quarter-wave plate to serve as a circular polarizing plate.

[0027] The optical laminate 11 shown in Fig. 1 can be manufactured, for example, by preparing a polarizing plate 40 and a first retardation layer 21, applying or transferring an adhesive to at least one of the first protective layer 42 side of the polarizing plate 40 and the first retardation layer 21, and bonding the polarizing plate 40 and the first retardation layer 21 via an adhesive layer. When the first retardation layer 21 is a liquid crystal layer, the first retardation layer 21 of the base layer-attached first retardation layer in which the first retardation layer 21 is peelably formed on the first base layer and the polarizing plate 40 may be laminated via an adhesive, and then the first base layer may be peeled off.

[0028] The method for forming the glue missing portion 5 in the optical laminate 11 is not particularly limited, but for example, it can be formed by adjusting the application range or transfer position of the adhesive layer for forming the adhesive layer 31. When forming the adhesive layer 31 by transfer, a portion that becomes the glue missing portion 5 may be formed in the adhesive layer formed on a release film or the like prepared for transfer, and the adhesive layer with the portion that becomes the glue missing portion 5 formed therein may be transferred onto the polarizing plate 40 or the first retardation layer 21.

[0029] In order to form a portion that will become the glue missing portion 5 in an adhesive layer formed on a release film or the like, for example, as shown in Figures 3(a) and (b), an adhesive layer 60 with a release film, in which an adhesive layer 61 is formed on a release film 62, is prepared, and the adhesive layer 60 with a release film is cut from the adhesive layer 61 side with a single-edged cutting blade 65. In the process of cutting the adhesive layer 60 with a release film in this way, the adhesive layer 61 can be pressed into a tapered shape by the side on which the blade is formed, out of both sides of the single-edged cutting blade 65, and an adhesive layer 31 with a tapered end can be formed.

[0030] (Modification) The optical film of the present embodiment may be modified as shown in the following modified examples, and each structure and each step of the embodiment and its modified examples may be combined and implemented.

[0031] (Variation 1) In the above embodiment, the optical laminate 11 including the polarizing plate 40 having the first protective layer 42 and the second protective layer 43 on both sides of the polarizing layer 41 has been described, but is not limited thereto. The polarizing plate may include the polarizing layer 41 and either the first protective layer 42 or the second protective layer 43. In addition, the optical laminate 11 may not include the first protective layer 42 or the second protective layer 43.

[0032] (Variation 2) When the optical laminate 11 shown in Fig. 1 is a circular polarizing plate, this circular polarizing plate can be used, for example, for anti-reflection of an organic electroluminescence (organic EL) display device. In this case, the optical laminate 11 is used by being attached to the viewing side of an optical display element of an organic EL display device. Therefore, the optical laminate 11 may have an adhesive layer for an optical display element on the opposite side of the adhesive layer 31 of the first retardation layer 21 to be attached to the optical display element.

[0033] (Variation 3) In the above embodiment, the optical laminate 11 including the first retardation layer 21 has been described, but is not limited thereto, and may be, for example, the optical laminate shown in FIG. 2. FIG. 2 is a cross-sectional view showing a schematic diagram of another example of the optical laminate of this embodiment. In the following, the same members as those described above are given the same reference numerals, and their description is omitted. The optical laminate 12 shown in FIG. 2 has a polarizing plate 40, a pressure-sensitive adhesive layer 31, a first retardation layer 21, an adhesive layer 35, and a second retardation layer 22 in this order. The adhesive layer 35 may be an adhesive layer formed using an adhesive, or may be an adhesive layer formed using an adhesive. The second retardation layer 22 may be a retardation film, or may be a liquid crystal layer containing a liquid crystal compound such as a polymerizable liquid crystal compound. When the second retardation layer 22 is a liquid crystal layer, the optical laminate 12 may have an alignment layer for aligning the liquid crystal compound constituting the second retardation layer 22 on the opposite side of the adhesive layer 35 of the second retardation layer 22.

[0034] In the optical laminate 12, a circular polarizing plate can be formed by using the first retardation layer 21 as a 1 / 2 wavelength plate and the second retardation layer 22 as a 1 / 4 wavelength plate; using the first retardation layer 21 as a 1 / 4 wavelength plate with reverse wavelength dispersion and the second retardation layer 22 as a positive C plate; using the first retardation layer 21 as a positive C plate and the second retardation layer 22 as a 1 / 4 wavelength plate with reverse wavelength dispersion, etc. When the combination of the first retardation layer 21 and the second retardation layer 22 is a 1 / 2 wavelength plate and a 1 / 4 wavelength plate, the slow axis direction of the 1 / 2 wavelength plate can be 70° to 80° and the slow axis direction of the 1 / 4 wavelength plate can be 10° to 20° with respect to the absorption axis direction of the polarizing layer 41. In addition, when the first retardation layer 21 and the second retardation layer 22 are combined to form a quarter-wave plate with reverse wavelength dispersion and a positive C plate, the slow axis direction of the quarter-wave plate can be set to 40° to 50° with respect to the absorption axis direction of the polarizing layer 41. In cases where the optical laminate 12, which is a circular polarizing plate, is used for antireflection of an organic EL display device, the optical laminate 12 shown in FIG. 2 may have a pressure-sensitive adhesive layer for optical display elements on the side opposite to the adhesive layer 35 of the second retardation layer 22.

[0035] The optical laminate 12 shown in FIG. 2 can be formed, for example, by preparing a retardation layer laminate in which the first retardation layer 21 and the second retardation layer 22 are laminated via an adhesive layer 35, and a polarizing plate 40, applying or transferring an adhesive to at least one of the first protective layer 42 side of the polarizing plate 40 and the first retardation layer 21 side of the retardation layer laminate, and bonding the polarizing plate 40 and the retardation layer laminate via an adhesive. When the first retardation layer 21 and the second retardation layer 22 are both liquid crystal layers, the optical laminate 12 can be obtained, for example, as follows. First, the first retardation layer 21 of the base layer-attached first retardation layer in which the first retardation layer 21 is peelably formed on the first base layer, and the second retardation layer 22 of the base layer-attached second retardation layer in which the second retardation layer 22 is peelably formed on the second base layer are laminated via an adhesive layer to obtain a retardation layer laminate. Next, the first base layer is peeled off from this retardation layer laminate, and the first retardation layer 21 side and the first protective layer 42 side of the polarizing plate 40 are laminated together via an adhesive, and then the second base layer is peeled off to obtain the optical laminate 12 shown in FIG. 2.

[0036] Hereinafter, the common features of the above-described embodiment and its modified examples will be described in detail.

[0037] (polarizing layer) The polarizing layer 41 may be a PVA-based resin film having a dichroic dye such as iodine adsorbed and oriented therein, or may be a layer in which a liquid crystal compound is hardened and the dichroic dye is oriented therein.

[0038] The PVA-based resin film is a film formed using a polyvinyl alcohol-based resin. The polyvinyl alcohol-based resin refers to a resin containing 50% by mass or more of a structural unit derived from vinyl alcohol. As the polyvinyl alcohol-based resin, a saponified polyvinyl acetate-based resin can be used. The saponification degree of the polyvinyl acetate-based resin can be determined in accordance with JIS K 6727 (1994), and can be, for example, in the range of 80.0 to 100.0 mol%.

[0039] Examples of polyvinyl acetate resins include polyvinyl acetate, which is a homopolymer of vinyl acetate, and copolymers of vinyl acetate and other monomers copolymerizable therewith. Examples of other monomers copolymerizable with vinyl acetate include unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfonic acids, and (meth)acrylamides having an ammonium group. In this specification, "(meth)acrylic" refers to at least one selected from the group consisting of acrylic and methacrylic. The same applies to other terms with "(meth)" added.

[0040] An example of the PVA-based resin film may be an unstretched film formed by forming a film of a polyvinyl alcohol-based resin, or a stretched film obtained by stretching this unstretched film. When the PVA-based resin film is a stretched film, it is preferably a stretched film that is longitudinally uniaxially stretched, and is preferably a stretched film that is dry-stretched. When the PVA-based resin film is a stretched film, the stretching ratio is usually 1.1 to 8 times.

[0041] Examples of the dichroic dye adsorbed and oriented on the PVA-based resin film include iodine and organic dyes. Examples of the organic dye include Red BR, Red LR, Red R, Pink LB, Rubin BL, Bordeaux GS, Sky Blue LG, Lemon Yellow, Blue BR, Blue 2R, Navy RY, Green LG, Violet LB, Violet B, Black H, Black B, Black GSP, Yellow 3G, Yellow R, Orange LR, Orange 3R, Scarlet GL, Scarlet KGL, Congo Red, Brilliant Violet BK, Spra Blue G, Spra Blue GL, Spra Orange GL, Direct Sky Blue, Direct Fast Orange S, Fast Black, etc. The dichroic dye may be used alone or in combination of two or more kinds.

[0042] As an example of a polarizing layer in which a dichroic dye is oriented in a layer in which a liquid crystal compound is hardened, a dichroic dye is oriented in a polymerizable liquid crystal compound, and the polymerizable liquid crystal compound is polymerized to form a hardened layer. Such a polarizing layer can be formed by applying a polarizing layer forming composition containing a liquid crystal compound and a dichroic dye onto a substrate film, and polymerizing and hardening the liquid crystal compound while maintaining the liquid crystal state. The polarizing layer thus obtained is in a state in which it is laminated on a substrate film, and the substrate film may be used as it is as a protective layer for the polarizing layer. Alternatively, a polarizing layer with a substrate film in which the substrate film is peelable from the polarizing layer may be laminated on the first retardation layer via a pressure-sensitive adhesive layer 31, and then the substrate film may be peeled off.

[0043] The liquid crystal compound may have a property of exhibiting a liquid crystal state, and is preferably in a highly oriented state such as a smectic phase, since it can exhibit high polarization performance. It is also preferable that the liquid crystal compound has a polymerizable functional group. The dichroic dye is a dye that exhibits dichroism by being oriented together with the liquid crystal compound, and the dichroic dye itself may have liquid crystal properties or may have a polymerizable functional group. Any compound in the composition for forming a polarizing layer containing a liquid crystal compound has a polymerizable functional group.

[0044] Examples of dichroic dyes that can be used in the polarizing layer using a liquid crystal compound include acridine dyes, oxazine dyes, cyanine dyes, naphthalene dyes, azo dyes, and anthraquinone dyes, among which azo dyes are preferred. Examples of azo dyes include monoazo dyes, bisazo dyes, trisazo dyes, tetrakisazo dyes, and stilbene azo dyes, among which bisazo dyes and trisazo dyes are more preferred. The dichroic dyes may be used alone or in combination of two or more.

[0045] The composition for forming the polarizing layer may contain a solvent, a polymerization initiator such as a photopolymerization initiator, a photosensitizer, a polymerization inhibitor, a dispersant, a leveling agent, a stabilizer, a surfactant, a crosslinking agent, a silane coupling agent, etc. The polymerizable liquid crystal compound, dichroic dye, solvent, polymerization initiator, photosensitizer, polymerization inhibitor, etc. contained in the composition for forming the polarizing layer may be a known one. In addition, the polymerizable liquid crystal compound may be the same as the compound exemplified as the polymerizable liquid crystal compound used to obtain the first retardation layer and the second retardation layer described later.

[0046] The thickness of the polarizing layer 41 is usually 2 to 40 μm, and from the viewpoint of making the polarizing layer thinner, it is preferably 30 μm or less, and more preferably 20 μm or less. A polarizing layer in which a dichroic dye is oriented in a layer in which a liquid crystal compound is cured can be formed to have a smaller thickness than a polarizing layer in which a dichroic dye such as iodine is adsorbed and oriented in a PVA-based resin film. The thickness of the polarizing layer using a liquid crystal compound may be, for example, 0.5 to 5 μm, and preferably 1 to 4 μm.

[0047] Furthermore, the luminosity-corrected single transmittance Ty of the polarizing layer 41 is preferably 40 to 47%, and more preferably 41 to 45%, taking into consideration the balance with the luminosity-corrected polarization degree Py. The luminosity-corrected polarization degree Py is preferably 99.9% or more, and more preferably 99.95% or more. Ty and Py can be determined by performing luminosity correction on the obtained transmittance and polarization degree using an integrating sphere spectrophotometer with a 2-degree visual field (C light source) according to JIS Z 8701.

[0048] (Polarizing plate) The polarizing plate is a plate in which protective layers (first protective layer, second protective layer) are laminated on one or both sides of a polarizing layer via a known pressure-sensitive adhesive layer or adhesive layer. The thickness of the polarizing plate can be, for example, 2 μm or more and 300 μm or less, and may be 10 μm or more, 150 μm or less, 120 μm or less, or 80 μm or less.

[0049] As the protective layer, for example, a film formed from a thermoplastic resin having excellent transparency, mechanical strength, thermal stability, moisture blocking properties, isotropy, stretchability, etc. is used. Specific examples of such thermoplastic resins include cellulose resins such as triacetyl cellulose; polyester resins such as polyethylene terephthalate and polyethylene naphthalate; polyethersulfone resins; polysulfone resins; polycarbonate resins; polyamide resins such as nylon and aromatic polyamide; polyimide resins; polyolefin resins such as polyethylene, polypropylene, and ethylene-propylene copolymers; cyclic polyolefin resins having cyclo- and norbornene structures (also called norbornene-based resins); (meth)acrylic resins; polyarylate resins; polystyrene resins; polyvinyl alcohol resins, and mixtures thereof. When protective layers are laminated on both sides of the polarizing layer, the resin compositions of the two protective layers may be the same or different. The film formed from the thermoplastic resin may be surface-treated (for example, corona treatment, etc.) to improve adhesion to the polarizing layer, and a thin layer such as a primer layer (also called an undercoat layer) may be formed.

[0050] The protective layer may be, for example, the above-mentioned thermoplastic resin that has been stretched, or may not be stretched (hereinafter, may be referred to as "unstretched resin"). Examples of the stretching treatment include uniaxial stretching and biaxial stretching.

[0051] The thickness of the protective layer is preferably 3 μm or more, more preferably 5 μm or more. The thickness of the protective layer is preferably 50 μm or less, more preferably 35 μm or less. The above upper limit and lower limit can be arbitrarily combined. The thinner the polarizing plate, the lower the rigidity, and the more susceptible it is to the shrinkage stress of the polarizing layer. Therefore, in an optical laminate in which the polarizing plate has a thin protective layer, the polarizing plate is more susceptible to the shrinkage stress of the polarizing layer at its end, and the uniformity of the hue of the reflected light in the plane tends to deteriorate in a high temperature environment. Therefore, in such an optical laminate, as described above, by setting the distance L1 of the glue chipping amount to 3 μm or more, it is considered that the deterioration of the uniformity of the hue of the reflected light in the plane can be effectively suppressed even in a high temperature environment.

[0052] The surface of the protective layer opposite to the polarizing layer may have a surface treatment layer, such as a hard coat layer, an antireflection layer, an anti-sticking layer, an anti-glare layer, a diffusion layer, etc. The surface treatment layer may be a separate layer laminated on the protective layer, or may be formed by applying a surface treatment to the surface of the protective layer.

[0053] (First Retardation Layer and Second Retardation Layer) The first retardation layer and the second retardation layer (hereinafter, both may be collectively referred to as "retardation layers") may be retardation films or liquid crystal layers. The retardation film may be any film that exhibits optical anisotropy, and examples thereof include stretched films obtained by stretching a film formed of polyvinyl alcohol, polycarbonate, polyester, polyarylate, polyimide, polyolefin, polycycloolefin, polystyrene, polysulfone, polyethersulfone, polyvinylidene fluoride / polymethyl methacrylate, acetyl cellulose, saponified ethylene-vinyl acetate copolymer, polyvinyl chloride, etc., by about 1.01 to 6 times.

[0054] When the retardation layer is a liquid crystal layer, the type of liquid crystal compound constituting the liquid crystal layer is not particularly limited, and a rod-shaped liquid crystal compound, a discotic liquid crystal compound, and a mixture thereof can be used. The liquid crystal layer is formed by applying a liquid crystal layer forming composition containing a liquid crystal compound, a solvent, and various additives as necessary, onto an alignment layer to form a coating film, and solidifying (curing) this coating film to form a liquid crystal layer that is a cured layer of the liquid crystal compound. Alternatively, the liquid crystal layer may be formed by applying a liquid crystal layer forming composition onto a substrate layer to form a coating film, and stretching this coating film together with the substrate layer. The liquid crystal layer forming composition may contain a polymerization initiator, a reactive additive, a leveling agent, a polymerization inhibitor, and the like, in addition to the above-mentioned liquid crystal compound and solvent. The liquid crystal compound, the solvent, the polymerization initiator, the reactive additive, the leveling agent, the polymerization inhibitor, and the like can be appropriately used as the liquid crystal compound, the solvent, the polymerization initiator, the reactive additive, the leveling agent, the polymerization inhibitor, and the like that are known in the art.

[0055] The substrate layer (first substrate layer, second substrate layer) on which the liquid crystal layer is formed is preferably a film formed of a resin material. For example, a resin material having excellent transparency, mechanical strength, thermal stability, stretchability, etc. is used as the resin material. Specifically, polyolefin resins such as polyethylene and polypropylene; cyclic polyolefin resins such as norbornene polymers; polyester resins such as polyethylene terephthalate and polyethylene naphthalate; (meth)acrylic acid resins such as (meth)acrylic acid and polymethyl (meth)acrylate; cellulose ester resins such as triacetyl cellulose, diacetyl cellulose, and cellulose acetate propionate; vinyl alcohol resins such as polyvinyl alcohol and polyvinyl acetate; polycarbonate resins; polystyrene resins; polyarylate resins; polysulfone resins; polyethersulfone resins; polyamide resins; polyimide resins; polyether ketone resins; polyphenylene sulfide resins; polyphenylene oxide resins, and mixtures and copolymers thereof can be mentioned. Of these resins, it is preferable to use any one of cyclic polyolefin resins, polyester resins, cellulose ester resins and (meth)acrylic acid resins, or a mixture of these.

[0056] The substrate layer may be a single layer or may have a multi-layer structure of two or more layers. When the substrate layer has a multi-layer structure, the types of resins constituting each layer may be the same or different. The thickness of the substrate layer is not particularly limited, but is generally preferably 1 to 300 μm, more preferably 10 to 200 μm, and even more preferably 30 to 120 μm, from the viewpoint of workability such as strength and handling.

[0057] The above-mentioned alignment layer has an alignment regulating force that aligns liquid crystal compounds such as polymerizable liquid crystal compounds contained in the liquid crystal layer formed thereon in a desired direction. Examples of the alignment layer include an alignment polymer layer formed from an alignment polymer, a photoalignment polymer layer formed from a photoalignment polymer, and a groove alignment layer having a concave-convex pattern or a plurality of grooves on the layer surface. The thickness of the alignment layer is usually 10 to 500 nm, and preferably 10 to 200 nm.

[0058] (Adhesive layer) The adhesive layer is a layer formed using an adhesive. In this specification, the adhesive is a material that exerts adhesive properties by attaching itself to an adherend such as an optical film or a liquid crystal layer, and is called a pressure-sensitive adhesive. As the adhesive, any conventionally known adhesive having excellent optical transparency can be used without any particular limitation, and for example, an adhesive having a base polymer such as an acrylic, urethane, silicone, or polyvinyl ether can be used. The thickness of the adhesive layer may be 3 μm or more, 5 μm or more, or 35 μm or less, or 30 μm or less.

[0059] The adhesive layer may contain additives such as an ultraviolet absorber, an antistatic agent using an ionic compound or the like, a solvent, a crosslinking catalyst, a tackifier resin (tackifier), a plasticizer, a softener, a dye, a pigment, an inorganic filler, etc. In particular, when the first retardation layer is a liquid crystal layer, the adhesive layer contains an ultraviolet absorber, so that the liquid crystal compound contained in the liquid crystal layer can be prevented from being deteriorated by the influence of external light or the like.

[0060] (Adhesive layer) The adhesive layer can be formed by a pressure-sensitive adhesive layer, an adhesive layer formed using an adhesive, or a combination thereof, and is usually one layer, but may be two or more layers. When the adhesive layer is composed of two or more layers, each layer may be formed of the same material or different materials. The pressure-sensitive adhesive layer can be formed by using the pressure-sensitive adhesive described above.

[0061] The adhesive that can be used in the adhesive layer can be, for example, a water-based adhesive, an active energy ray curing adhesive, or any other conventionally known adhesive, without any particular limitation. Examples of the water-based adhesive include a polyvinyl alcohol-based resin aqueous solution, a water-based two-liquid urethane-based emulsion adhesive, and the like. Examples of the active energy ray curing adhesive include an adhesive that is cured by irradiation with active energy rays such as ultraviolet rays, and include, for example, those containing a polymerizable compound and a photopolymerization initiator, those containing a photoreactive resin, and those containing a binder resin and a photoreactive crosslinking agent. Examples of the polymerizable compound include photopolymerizable monomers such as photocurable epoxy monomers, photocurable acrylic monomers, and photocurable urethane monomers, and oligomers derived from these monomers. Examples of the photopolymerization initiator include those containing a substance that generates active species such as neutral radicals, anion radicals, and cation radicals when irradiated with active energy rays such as ultraviolet rays. EXAMPLES

[0062] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. In the examples and comparative examples, "%" and "parts" are by mass % and parts by mass unless otherwise specified.

[0063] [Preparation of polarizing plate] A 20 μm-thick triacetyl cellulose film was prepared as the first protective layer. A 29 μm-thick norbornene-based resin film with a hard coat layer formed on one surface was prepared as the second protective layer. A PVA-based resin film with iodine, a dichroic dye, adsorbed and aligned was prepared as the polarizing layer. The polarizing layer had a thickness of 8 μm.

[0064] In addition, 3 parts by weight of carboxyl-modified polyvinyl alcohol (available from Kuraray Co., Ltd. under the trade name "KL-318") was dissolved in 100 parts by weight of water, and 1.5 parts by weight of a polyamide epoxy-based additive, which is a water-soluble epoxy resin (available from Taoka Chemical Co., Ltd. under the trade name "Sumirez Resin (registered trademark) 650 (30)", an aqueous solution with a solids concentration of 30% by weight) was added to the resulting aqueous solution to prepare a water-based adhesive.

[0065] The first protective layer was subjected to a saponification treatment, and the surface of the second protective layer facing the norbornene-based resin film and both sides of the polarizing layer were subjected to a corona treatment. The first protective layer was attached to one side of the polarizing layer via the aqueous adhesive obtained above, and the side of the second protective layer opposite the hard coat layer (the norbornene-based resin film side) was attached to the other side of the polarizing layer via the same aqueous adhesive as above, and a drying treatment was performed to produce a polarizing plate. The obtained polarizing plate was cut into a rectangular shape so that the absorption axis of the polarizing layer was at 45° to the long side direction.

[0066] [Preparation of the first retardation layer] (Preparation of composition for forming horizontal alignment layer) The following components were mixed, and the resulting mixture was stirred at a temperature of 80° C. for 1 hour to obtain a composition for forming a horizontal alignment layer. ·Photoalignable material (5 parts) (weight average molecular weight: 30000): [ka] Solvent (95 parts): Cyclopentanone

[0067] (Preparation of composition for forming horizontally aligned liquid crystal layer) The following components were mixed, N-methyl-2-pyrrolidone (NMP) was further added so that the solid content concentration became 13%, and the mixture was stirred at 80° C. for 1 hour to obtain a composition for forming a horizontally aligned liquid crystal layer. The following polymerizable liquid crystal compound A was synthesized by the method described in JP-A-2010-31223, and the following polymerizable liquid crystal compound B was synthesized according to the method described in JP-A-2009-173893. ·Polymerizable liquid crystal compound A (90 parts): [ka] ·Polymerizable liquid crystal compound B (10 parts): [ka] Polymerization initiator (6 parts): 2-Dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (Irgacure 369, manufactured by BASF Japan Ltd.)

[0068] (Preparation of the first retardation layer) A cyclic olefin resin (COP) film (ZF-14-50, manufactured by Zeon Corporation) was subjected to a corona treatment. The composition for forming a horizontal alignment layer obtained above was applied to the corona-treated surface of the COP film using a bar coater, and dried at 80°C for 1 minute. A polarized UV irradiation device ("SPOT CURE SP-9", manufactured by Ushio Inc.) was used to irradiate the coating film with an integrated light amount of 100 mJ / cm at a wavelength of 313 nm. 2 The film was exposed to polarized UV light at an axial angle of 45° to obtain a horizontal alignment layer.

[0069] Next, the composition for forming a horizontally aligned liquid crystal layer obtained above was applied to this horizontal alignment layer using a bar coater, and dried for 1 minute at 120° C. The coating film was irradiated with ultraviolet light (under a nitrogen atmosphere, cumulative light amount at a wavelength of 365 nm: 500 mJ / cm ) using a high-pressure mercury lamp ("Unicur VB-15201BY-A", manufactured by Ushio Inc.). 2By doing so, a first retardation layer that is a horizontally aligned liquid crystal layer was formed. The first retardation layer was a quarter-wave plate exhibiting inverse wavelength dispersion.

[0070] [Fabrication of the second retardation layer] (Preparation of the composition for forming the vertical alignment layer) Sunever SE610 (manufactured by Nissan Chemical Industries, Ltd.) was prepared as the composition for forming the vertical alignment layer.

[0071] (Preparation of the composition for forming the vertically aligned liquid crystal layer) The following components were mixed, and cyclopentanone was further added so that the solid content concentration became 13% to obtain a composition for forming a vertically aligned liquid crystal layer. · Polymerizable liquid crystal compound C (100 parts): Paliocolor (registered trademark) LC242 (manufactured by BASF) · Levelling agent (0.1 part): F-556 (manufactured by DIC) · Photoinitiator (3 parts): Irgacure 369 (manufactured by Ciba Specialty Chemicals)

[0072] (Fabrication of the second retardation layer) Corona treatment was performed on a cyclic olefin-based resin (COP) film (ZF-14-50, manufactured by Nippon Zeon Co., Ltd.). The composition for forming the vertical alignment layer obtained above was coated on the corona-treated surface of this COP film with a bar coater and dried at 80 °C for 1 minute to obtain a vertical alignment layer. Subsequently, the composition for forming the vertically aligned liquid crystal layer obtained above was coated on the vertical alignment layer using a bar coater and dried at 90 °C for 120 seconds. Ultraviolet rays were irradiated on this coating film (under a nitrogen atmosphere, integrated light quantity at a wavelength of 365 nm: 500 mJ / cm 2 ) By doing so, a second retardation layer that is a vertically aligned liquid crystal layer was formed. The second retardation layer was a positive C-plate satisfying the relationship of nx ≒ ny < nz.

[0073] [Fabrication of the retardation layer laminate] The surface of the first retardation layer prepared above opposite to the COP film and the surface of the second retardation layer prepared above opposite to the COP film were subjected to corona treatment. The corona-treated surfaces (the first retardation layer surface and the second retardation layer surface) were bonded together via an ultraviolet-curable adhesive, and then the ultraviolet-curable adhesive was cured by irradiating ultraviolet light to obtain a retardation layer laminate in which the first retardation layer and the second retardation layer were laminated via an adhesive layer. The obtained retardation layer laminate was cut into a rectangular shape so that the slow axis of the first retardation layer (1 / 4 wavelength plate) was parallel to the long side direction.

[0074] [Measurement of distance L1 of glue chipping area] An acrylic adhesive layer having a thickness of 20 μm provided on a release film was laminated on the second retardation layer side of the optical laminate obtained in each example and each comparative example to obtain an optical laminate with an adhesive layer. The side on which the glue chipping was formed of this optical laminate with an adhesive layer was confirmed, and the cross section of the optical laminate with an adhesive layer was cut along a direction perpendicular to the side at the position where the glue chipping was formed, and the profile was measured using a laser microscope. Based on the measured profile, the distance L1 between the position of the innermost end at the end of the adhesive layer 61 and the position of the outermost end at the end of the polarizing layer was measured.

[0075] [High temperature test] An acrylic adhesive layer having a thickness of 20 μm was laminated on the second retardation layer side of the optical laminate obtained in each Example and Comparative Example, and this acrylic adhesive layer was attached to a glass plate to prepare an evaluation sample. The obtained evaluation sample was subjected to a high temperature test in which it was placed in an oven at a temperature of 80° C. for 200 hours. The evaluation sample after the high temperature test was placed on a reflector (MIRO5 5011GP, manufactured by Alanod) with the glass plate facing downward, and the hue of the reflected light was measured using a spectrophotometer (CM2600d, Konica Minolta, Inc.). The measurement was performed by attaching a mask with an opening diameter φ of 1.5 mm when light enters an integrating sphere from the evaluation sample, and the hue of the reflected light (a * b * ) and the hue of the reflected light at the center of the evaluation sample (the intersection of the diagonals of the rectangle) (a * b* ) and the average difference between them is Δa * b * It was calculated as: Δa * b * =(Δa *2 +Δb *2 ) 1 / 2

[0076] In addition, the evaluation sample after the high temperature test was placed on a reflector (MIRO5 5011GP, manufactured by Alanod), and the reflected light was observed visually from the optical laminate side to evaluate the visibility of the color unevenness of the optical laminate. When the color unevenness was weakly visible, it was evaluated as A, and when it was strongly visible, it was evaluated as B.

[0077] Example 1 3(a) and (b) are schematic diagrams for explaining a method for preparing a pressure-sensitive adhesive layer in an embodiment. As shown in FIG. 3(a), a pressure-sensitive adhesive layer 60 with a release film was prepared, which had a pressure-sensitive adhesive layer 61 formed on a release film 62 using an acrylic pressure-sensitive adhesive having a thickness of 20 μm. The pressure-sensitive adhesive layer 61 contained an ultraviolet absorber. As shown in FIG. 3(a), a cutting blade 65 with an angle θ at a tip portion 65a was cut from the pressure-sensitive adhesive layer 61 side along a direction parallel to the lamination direction of the pressure-sensitive adhesive layer 60 with a release film (the direction of the arrow in the figure), to cut the pressure-sensitive adhesive layer 60 with a release film into a rectangular shape. A single-edged cutting blade 65 was used as the cutting blade. The cut surface of the rectangular pressure-sensitive adhesive layer 60 with a release film after cutting was the surface that contacted the surface on which the blade was formed, among both surfaces of the single-edged cutting blade 65.

[0078] The adhesive layer 61 of the obtained rectangular adhesive layer 60 with release film was attached to the first protective layer side (triacetyl cellulose film side) of the polarizing plate prepared above, and then the release film 62 was peeled off. The surface exposed by peeling off the COP film on the first retardation layer side of the retardation layer laminate prepared above was attached to the surface of the adhesive layer 61 exposed by peeling off the release film 62, and then the COP film on the second retardation layer side was peeled off to obtain an optical laminate (circular polarizing plate) having a layer structure of second protective layer / polarizing layer / first protective layer / adhesive layer 61 / first retardation layer / adhesive layer / second retardation layer. In the preparation of the optical laminate, when each layer was attached, a corona treatment was performed on the attachment surface, and when the layers were attached, the long and short sides were aligned, and the absorption axis direction of the polarizing layer was set to 45° with respect to the slow axis direction of the first retardation layer.

[0079] The obtained optical laminate had a glue chip formed around its entire circumference. The distance L1 was measured for the glue chip at any position on each side of the optical laminate using the procedure described above, and the average value was calculated. In addition, a high-temperature test was performed on the obtained optical laminate, and the change in the hue of the reflected light was measured, and a visibility evaluation was performed to confirm the state of color unevenness. These results are shown in Table 1. From the measurement results of the distance L1 on each side, it was found that the distance L1 of the glue chip around the entire circumference of the optical laminate of this example was approximately the same as the value shown in Table 1.

[0080] [Example 2 and Comparative Example 1] An optical laminate was obtained in the same manner as in Example 1, except that a rectangular adhesive layer 60 with a release film was obtained using a cutting blade (single-edged) with a smaller angle θ of the tip portion 65a than that used in Example 1 as the cutting blade used to cut the adhesive layer 60 with a release film (FIG. 3(a)). The obtained optical laminate had glue chipping formed on its entire circumference. The distance L1 was measured for glue chipping at any position on each side of the optical laminate using the above-mentioned procedure, and the average value was calculated. In addition, a high-temperature test was performed on the obtained optical laminate, and the change in the hue of the reflected light was measured, and the visibility was evaluated to confirm the state of color unevenness. These results are shown in Table 1. It should be noted that, from the measurement results of the distance L1 on each side, it was recognized that the distance L1 of the glue chipping was approximately the same as the value shown in Table 1 on the entire circumference of the optical laminate of this example.

[0081] [Table 1] [Explanation of symbols]

[0082] 5 glue chipping portion, 11 optical laminate, 12 optical laminate, 21 first retardation layer, 22 second retardation layer, 31 adhesive layer, 35 bonding layer, 40 polarizing plate, 41 polarizing layer, 42 first protective layer, 43 second protective layer, 60 adhesive layer with release film, 61 adhesive layer, 62 release film, 65 cutting blade, 65a blade tip portion.

Claims

1. A circular polarizing plate having a polarizing plate including a polarizing layer, a pressure-sensitive adhesive layer, and a first retardation layer in this order, Further, a second retardation layer is provided on the opposite side of the first retardation layer from the pressure-sensitive adhesive layer, The thickness of the polarizing plate is 2 μm or more and 150 μm or less, the first retardation layer and the second retardation layer are liquid crystal layers which are hardened layers of a liquid crystal compound, The polarizing layer is a polyvinyl alcohol-based resin film having a dichroic dye adsorbed and oriented thereon, the circularly polarizing plate has a glue-defective portion at an end portion in a planar direction thereof, and has a rectangular shape or a rectangular shape having a notch portion on at least one side thereof; The rectangular shape has a pair of long sides and a pair of short sides, The absorption axis direction of the polarizing layer forms an angle of 45°±10° with respect to the long side, The glue missing portion is At least one of the pair of long sides and at least one of the pair of short sides are formed, and A circular polarizing plate formed such that, in a cross section passing through the portion where the polarizing layer and the pressure-sensitive adhesive layer overlap in the stacking direction, the position of the innermost end of the end of the pressure-sensitive adhesive layer is located 3 μm or more and 50 μm or less inside from the position of the outermost end of the end of the polarizing layer.

2. A circularly polarizing plate having a polarizing plate including a polarizing layer, a pressure-sensitive adhesive layer, and a first retardation layer in this order, Further, a second retardation layer is provided on the opposite side of the first retardation layer from the pressure-sensitive adhesive layer, The thickness of the polarizing plate is 2 μm or more and 150 μm or less, the first retardation layer and the second retardation layer are liquid crystal layers which are hardened layers of a liquid crystal compound, The polarizing layer is a polyvinyl alcohol-based resin film having a dichroic dye adsorbed and oriented thereon, the circularly polarizing plate has a glue-defective portion at an end portion in a planar direction thereof, and has a rectangular shape or a rectangular shape having a notch portion on at least one side thereof; The rectangular shape has a pair of long sides and a pair of short sides, The absorption axis direction of the polarizing layer forms an angle of 0°±10° with respect to the long side, The glue missing portion is At least one of the pair of short sides is formed, and A circular polarizing plate formed such that, in a cross section passing through the portion where the polarizing layer and the pressure-sensitive adhesive layer overlap in the stacking direction, the position of the innermost end of the end of the pressure-sensitive adhesive layer is located 3 μm or more and 50 μm or less inside from the position of the outermost end of the end of the polarizing layer.

3. A circularly polarizing plate having a polarizing plate including a polarizing layer, a pressure-sensitive adhesive layer, and a first retardation layer in this order, Further, a second retardation layer is provided on the opposite side of the first retardation layer from the pressure-sensitive adhesive layer, The thickness of the polarizing plate is 2 μm or more and 150 μm or less, the first retardation layer and the second retardation layer are liquid crystal layers which are hardened layers of a liquid crystal compound, The polarizing layer is a polyvinyl alcohol-based resin film having a dichroic dye adsorbed and oriented thereon, the circularly polarizing plate has a glue-defective portion at an end portion in a planar direction thereof, and has a rectangular shape or a rectangular shape having a notch portion on at least one side thereof; The rectangular shape has a pair of long sides and a pair of short sides, The absorption axis direction of the polarizing layer forms an angle of 0°±10° with respect to the short side, The glue missing portion is At least one of the pair of long sides is formed, and A circular polarizing plate formed such that, in a cross section passing through the portion where the polarizing layer and the pressure-sensitive adhesive layer overlap in the stacking direction, the position of the innermost end of the end of the pressure-sensitive adhesive layer is located 3 μm or more and 50 μm or less inside from the position of the outermost end of the end of the polarizing layer.

4. A circular polarizing plate described in any one of claims 1 to 3, wherein the polarizing plate has a protective layer on one or both sides of the polarizing layer.

5. The polarizing plate has a protective layer on both sides of the polarizing layer, the protective layer on the surface of the polarizing layer facing the first retardation layer is a triacetyl cellulose film, The circular polarizing plate according to claim 4 , wherein the protective layer on the surface of the polarizing layer opposite to the first retardation layer side is a norbornene-based resin film.

6. 6. The circular polarizing plate according to claim 1, wherein the second retardation layer is provided on the first retardation layer via an adhesive layer.

Citation Information

Patent Citations

  • Polarizing plate having adhesive layer

    JP1996194116A

  • Optical member

    JP2001235626A

  • Adhesion type optical film, method for manufacturing adhesion type optical film, and image display device

    JP2004170907A

  • Combined polarizing plate, liquid crystal display device, and method for manufacturing combined polarizing plate

    JP2008009237A

  • Method for manufacturing adhesive optical film, adhesive optical film and image display device

    JP2009086452A