Olefin production process

The described method improves olefin yield by using a sodium-reduced zeolite catalyst with a specific Si/Al ratio and regenerates the catalyst efficiently, addressing the yield limitations of existing olefin production methods.

JP7555418B2Active Publication Date: 2024-09-24SUMITOMO CHEM CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022543915
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-08-20
Filing Date
2021-08-11
Publication Date
2024-09-24
Estimated Expiration
2041-08-11

AI Technical Summary

Technical Problem

The existing methods for producing olefins, particularly those using MFI type zeolite catalysts, do not achieve sufficient yield of olefins with 2 to 3 carbon atoms.

Method used

A method involving catalytic cracking of polyolefins and organic chlorine compounds in the presence of a zeolite catalyst with a sodium content less than 0.1% by mass and a Si/Al ratio of 100 or more, along with a regeneration process using an oxygen-containing atmosphere to restore catalyst performance.

Benefits of technology

This method enhances the yield of olefins with 2 to 3 carbon atoms and allows for the effective regeneration of the zeolite catalyst, maintaining high catalytic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555418000001
    Figure 0007555418000001
Patent Text Reader

Abstract

The present invention aims to improve olefin yield. This olefin production method includes a step in which a raw material that includes at least a polyolefin and an organochlorine compound is catalytically cracked in the presence of a zeolite catalyst having a sodium atom content of less than 0.1% by mass.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a process for producing an olefin and a method for regenerating a catalyst used in the process. [Background technology]

[0002] The main raw materials in the petrochemical industry are lower olefins such as ethylene and propylene obtained by cracking and reforming naphtha, and aromatic hydrocarbons such as benzene, toluene, and xylene. A wide variety of chemical products are synthesized using these as starting materials. Among them, plastics are the most widely produced, and are widely used in a range of products from industrial to everyday use due to their excellent properties as a material, such as being lightweight, highly corrosion-resistant, and easily moldable. As a result, the amount of waste plastic being discharged is also enormous.

[0003] Non-Patent Document 1 describes a chemical recycling technology for efficiently decomposing polyethylene into petrochemical raw materials. Specifically, the method describes catalytic decomposition of polyethylene using MFI-type zeolite containing sodium atoms to obtain olefins having 2 to 5 carbon atoms. [Prior art documents] [Non-patent literature]

[0004] [Non-Patent Document 1] Monthly Fine Chemical (December 2017 issue Vol.46 No.12) Summary of the Invention [Problem to be solved by the invention]

[0005] However, the yield of the olefin having 2 to 3 carbon atoms obtained by the method described in Non-Patent Document 1 is not necessarily sufficient. Therefore, the present invention provides a method for producing an olefin which provides an excellent yield of the olefin having 2 to 3 carbon atoms. [Means for solving the problem]

[0006] The present invention provides the following [1] to

[14] . [1] A method for producing an olefin, comprising the step of catalytically cracking a raw material containing at least a polyolefin and an organic chlorine compound in the presence of a zeolite catalyst having a sodium content of less than 0.1 mass%. [2] The method for producing an olefin according to [1], wherein the zeolite catalyst is an MFI type zeolite catalyst. [3] The method for producing an olefin according to [1] or [2], wherein the Si / Al ratio of the zeolite catalyst is 100 or more. [4] The method for producing an olefin according to [1] or [2], wherein the Si / Al ratio of the zeolite catalyst is 300 or more. [5] The method for producing an olefin according to [1], wherein the olefin is an olefin having 2 to 3 carbon atoms. [6] The method for producing an olefin according to any one of [1] to [5], wherein the sodium content of the zeolite catalyst is less than 0.05 mass %. [7] The method for producing an olefin according to any one of [1] to [6], wherein the organic chlorine compound comprises at least one of polyvinyl chloride and polyvinylidene chloride. [8] The method for producing an olefin according to [7], wherein the content of chlorine atoms in the raw material is 10 mass% or less. [9] The method for producing an olefin according to any one of [1] to [8], further comprising a step of thermally cracking the raw material prior to the step of catalytic cracking.

[10] The method for producing olefins according to any one of [1] to [9], further comprising a step of vaporizing the raw material prior to the catalytic cracking step, wherein the catalytic cracking step is a step of catalytically cracking the raw material in a gaseous state.

[11] The method for producing an olefin according to any one of [1] to

[10] , wherein the catalytic cracking step is carried out at a temperature of 450° C. or higher and 600° C. or lower.

[12] The method for producing an olefin according to any one of [1] to

[11] , wherein the zeolite catalyst is a regenerated catalyst.

[13] A method for regenerating a catalyst, comprising the step of calcining a used zeolite catalyst used in the olefin production method according to any one of [1] to

[11] in an atmosphere containing 1 volume % to 50 volume % oxygen to obtain a regenerated catalyst.

[14] A method for producing olefins, comprising a step of catalytically cracking a feedstock containing polyolefins in the presence of a regenerated catalyst regenerated by the regeneration method according to

[13] . Effect of the Invention

[0007] According to the present invention, it is possible to provide a production method excellent in the yield of olefins having 2 to 3 carbon atoms. Also, according to the present invention, it is possible to provide a catalyst regeneration method capable of simply regenerating a regenerated catalyst having high catalytic performance after regeneration from a spent zeolite catalyst used in the production method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] 1. Olefin production method The method for producing olefins according to the present invention includes a step of catalytically cracking a raw material containing at least a polyolefin and an organic chlorine compound in the presence of a zeolite catalyst having a sodium content of less than 0.1 mass%. The method for producing olefins according to the present embodiment will be specifically described below.

[0009] <Catalytic cracking process (catalytic cracking process)> ·Raw materials The raw material that can be used in the olefin production method of the present embodiment includes at least a polyolefin and an organic chlorine compound.

[0010] Specific examples of polyolefins contained as raw materials include polyolefin-based plastics such as polyethylene, polypropylene, polybutene, ethylene-vinyl acetate copolymer, ethylene-methyl acrylate copolymer, ethylene-methyl methacrylate copolymer, ethylene-propylene copolymer, and ethylene-α-olefin copolymer, as well as mixtures of two or more of these. Among these, polyethylene, polypropylene, and ethylene-propylene copolymer are preferred.

[0011] In addition to the polyolefin plastics, the raw materials may include other components such as polystyrene, polyamide, polycarbonate, polyurethane, polyester, polymethyl methacrylate, acrylonitrile-styrene copolymer, acrylonitrile-butadiene-styrene copolymer, natural rubber, and synthetic rubber.

[0012] Specific examples of organic chlorine compounds contained as raw materials include polyvinyl chloride (PVC) and polyvinylidene chloride (PVDC). The organic chlorine compound preferably contains at least one of polyvinyl chloride and polyvinylidene chloride.

[0013] In the olefin production method of the present embodiment, the upper limit of the content of chlorine atoms that may be contained in the raw material is about 30 mass%, and from the viewpoint of the yield of the target olefin, the content of chlorine atoms in the raw material is preferably 10 mass% or less.

[0014] The raw materials may include, for example, industrial products such as molded articles produced using the above-mentioned polyolefins, organic chlorine compounds, and other components. Specific examples of industrial products include plastic containers and packaging collected under the Container and Packaging Recycling Law.

[0015] The raw material may be in a solid state like the above-mentioned molded body. The raw material may be the above-mentioned solid industrial product that has been changed into a liquid and / or gaseous state, and may be, for example, a liquid and / or gaseous mixture of the above-mentioned polyolefin, organic chlorine compound, and other components.

[0016] Zeolite catalyst The zeolite catalyst used in this embodiment includes beta zeolite, faujasite zeolite, L zeolite, ferrierite zeolite, mordenite zeolite, and MFI zeolite, and is preferably a zeolite catalyst made of MFI zeolite. The zeolite catalyst of this embodiment has a sodium content of less than 0.1% by mass. From the viewpoint of the yield of the target olefin, the sodium content of the zeolite catalyst of this embodiment is more preferably less than 0.05% by mass.

[0017] The zeolite catalyst used in the present embodiment may usually contain silicon atoms, aluminum atoms, oxygen atoms, and hydrogen atoms as atoms other than sodium atoms. The zeolite catalyst may also contain atoms such as titanium atoms, chromium atoms, manganese atoms, iron atoms, cobalt atoms, nickel atoms, copper atoms, ruthenium atoms, rhodium atoms, palladium atoms, silver atoms, iridium atoms, platinum atoms, boron atoms, nitrogen atoms, magnesium atoms, phosphorus atoms, zinc atoms, and gallium atoms.

[0018] Here, the ratio of the number of moles of silicon atoms to the number of moles of aluminum atoms in the zeolite catalyst (Si / Al ratio) is preferably 100 or more, and more preferably 300 or more, from the viewpoint of improving the yield of the target olefin.

[0019] The sodium content and Si / Al ratio of the zeolite catalyst can be calculated by analyzing the zeolite catalyst according to a conventionally known ICP emission spectrometry method.

[0020] Here, MFI type zeolite means a crystalline aluminosilicate having an MFI structure according to the structure code of the International Zeolite Association (IZA). Specific examples of MFI type zeolite include H + -ZSM-5, NH4 + -ZSM-5, Na + -ZSM-5, Ca 2+ The MFI type zeolite can be prepared by any suitable method known in the art. + -ZSM-5 may also be used. The identification of MFI type zeolite can be carried out by analysis using X-ray diffraction analysis.

[0021] The method for producing the zeolite catalyst used in this embodiment will be described below. The zeolite catalyst used in this embodiment can be produced by a production method including the steps of preparing a mixture containing a silicon source, an aluminum source, a template, and an alkali metal source, and crystallizing the mixture to obtain a zeolite. Here, the "template" refers to a substance for imparting a pore structure to the zeolite.

[0022] As the silicon source, a conventionally known silicon source used in the production of various zeolites can be used, and specific examples of the silicon source include tetraethyl orthosilicate, colloidal silica, silica gel dry powder, silica hydrogel, and sodium silicate.

[0023] As the aluminum source, a conventionally known aluminum source used in the production of various zeolites can be used. Specific examples of the aluminum source include aluminum nitrate, aluminum chloride, sodium aluminate, aluminum hydroxide, and aluminum alkoxide. Among these aluminum sources, aluminum nitrate or sodium aluminate is preferred.

[0024] The type of template that can be used in the present embodiment is not particularly limited. As the template, conventionally known templates such as organic ammonium salts and amines that are generally used in the synthesis of zeolites can be used.

[0025] Specific examples of the template include tetrapropylammonium salt, tetraethylammonium salt, tetramethylammonium salt, benzyltrimethylammonium salt, tetrabutylammonium salt, propanolamine, ethanolamine, n-propylamine, morpholine, 1,5-diaminopentane, 1,6-diaminohexane, dipropylenetetramine, and triethylenetetramine. Among these templates, tetrapropylammonium salt (tetrapropylammonium hydroxide) is preferred.

[0026] Examples of alkali metal sources include alkali metal hydroxides, alkali metal chlorides, alkali metal bromides, and alkali metal sulfides. Specific examples of alkali metals include sodium and potassium.

[0027] When the alkali metal is sodium, specific examples of the sodium source include sodium hydroxide, sodium nitrate, sodium chloride, sodium bromide, sodium sulfate, sodium silicate, sodium aluminate, and compounds containing sodium as a counter cation.

[0028] When the alkali metal is potassium, specific examples of the potassium source include potassium hydroxide, potassium nitrate, potassium chloride, potassium bromide, potassium sulfate, potassium silicate, potassium aluminate, and compounds containing potassium as a counter cation.

[0029] In the above mixture, the ratio of the number of moles of silicon atoms to the number of moles of aluminum atoms (Si / Al ratio) is preferably at least 100, more preferably at least 300. The ratio may be at most 10,000, and is preferably at most 2,500.

[0030] It is also preferable that the ratio of the number of moles of each component in the mixture to the number of moles of silicon atoms satisfies the following requirements. Molding agent: 0.02 or more, 5.0 or less Alkaline metal source: 0.01 or more, 0.2 or less Water: 2 or more, 100 or less

[0031] Furthermore, it is more preferable that the ratio of the number of moles of each component in the mixture to the number of moles of silicon atoms satisfies the following requirement. Molding agent: 0.05 or more, 2.0 or less Alkaline metal source: 0.04 or more, 0.3 or less Water: 5 or more, 50 or less

[0032] The specific steps will be described below. First, the above components (mixture) are stirred at room temperature for 1 hour to 48 hours (e.g., 18 hours), and the mixture is placed in a sealed pressure vessel (autoclave), and the mixture is treated in the autoclave at a temperature of 100°C to 200°C for 1 hour to 120 hours, thereby preparing a zeolite precursor.

[0033] After the crystallization is completed, the mixture (suspension) containing the prepared zeolite precursor is sufficiently cooled with ice water or the like, and after cooling is completed, the mixture is subjected to solid-liquid separation (e.g., centrifugation) to remove the supernatant, and the solid-liquid separation process by washing with a sufficient amount of pure water is repeated until the pH of the removed supernatant becomes 8 or less.

[0034] Next, it is dried at a temperature of 100° C. to 150° C. (for example, 120° C.) for 1 hour to 48 hours (for example, 8 hours), and then may be fired at a temperature of about 400° C. to 700° C. (for example, 550° C.) for 1 hour to 48 hours (for example, 7 hours). By the above steps, a zeolite (eg, MFI type zeolite) can be obtained.

[0035] The zeolite prepared as described above contains a relatively large amount of sodium or potassium contained in the alkali metal source, and therefore, in order to obtain the zeolite catalyst used in the present embodiment, it is usually necessary to remove the alkali metal from the zeolite.

[0036] As a method for removing the alkali metal from the zeolite, there is mentioned a method for contacting the zeolite with an aqueous solution of an ammonium salt.

[0037] Examples of ammonium salts include ammonium salts of inorganic acids such as ammonium sulfate, ammonium hydrogen sulfate, ammonium carbonate, ammonium hydrogen carbonate, diammonium hydrogen phosphate, ammonium dihydrogen phosphate, ammonium phosphate, ammonium hydrogen pyrophosphate, ammonium pyrophosphate, ammonium chloride, and ammonium nitrate, and ammonium salts of organic acids such as ammonium acetate, etc. Among these, it is preferable to use ammonium sulfate, ammonium chloride, and ammonium nitrate.

[0038] Specifically, this step involves mixing an aqueous solution of an ammonium salt with zeolite and contacting them at a temperature of 50°C to 200°C for 1 to 48 hours, and repeating this step one or more times as necessary, thereby adjusting (reducing) the alkali metal content (e.g., the sodium atom content) to a desired content.

[0039] Next, the solid is sufficiently cooled to separate the solid and liquid, washed with a sufficient amount of pure water, and dried at any temperature between 60°C and 150°C.

[0040] Thereafter, it is preferable to perform firing at a temperature of about 400° C. to 700° C. (for example, 550° C.) for 1 hour to 48 hours (for example, 5 hours).

[0041] By preparing as described above, it is possible to obtain the zeolite catalyst of the present embodiment having a sodium content of less than 0.1 mass % by reducing sodium atoms, which is an alkali metal.

[0042] The temperature in the catalytic cracking process (contact temperature T 2 ) is usually 400° C. to 700° C., and preferably 450° C. to 600° C. (450° C. or higher and 600° C. or lower).

[0043] The pressure in the catalytic cracking process (contact pressure P 2) is usually 0 MPaG to 5 MPaG, preferably 0 MPaG to 0.5 MPaG.

[0044] In the catalytic cracking step, steam or an inert gas such as nitrogen gas or CO2 gas may be allowed to coexist.

[0045] The catalytic cracking step can be carried out using any suitable conventionally known reaction vessel, examples of which include quartz glass, carbon steel, stainless steel, Inconel alloy, Hastelloy alloy, Incoloy alloy, and Monel alloy.

[0046] The olefin obtained in the catalytic cracking step is usually an olefin having 2 to 5 carbon atoms, such as ethylene, propylene, or butene, and preferably an olefin having 2 to 3 carbon atoms.

[0047] The zeolite catalyst used in the catalytic cracking step may be a regenerated catalyst (details will be described later). That is, the olefin production method of the present embodiment may include a step of catalytically cracking a raw material containing polyolefin in the presence of a regenerated catalyst.

[0048] <Thermal decomposition process (thermal decomposition process)> In the olefin production method of this embodiment, from the viewpoint of further improving the olefin yield, it is preferable to further include a step of thermally cracking the raw material prior to the catalytic cracking step already described, and to make the catalytic cracking step a step of catalytically cracking a raw material in a gaseous state, a liquid state or a mixture thereof.

[0049] The thermal cracking step in the olefin production method of this embodiment can be carried out using any suitable conventionally known device, adopting conditions appropriate for the selected raw material and the components contained in the raw material.

[0050] The thermal cracking step of this embodiment can be carried out using a vessel separate from the vessel in which the catalytic cracking step described above is carried out. Also, the thermal cracking step and the catalytic cracking step of this embodiment may be carried out continuously using the same reaction vessel.

[0051] The pyrolysis temperature T in the pyrolysis process of this embodiment 1 and the contact temperature T in the catalytic cracking process. 2 It is preferable that the condition represented by the following formula is satisfied. 0℃≦T 2 -T 1 ≦200℃

[0052] Thermal decomposition temperature T in the thermal decomposition process 1 The heating temperature is usually 350°C to 550°C, and preferably 400°C to 500°C.

[0053] Pyrolysis pressure P in the pyrolysis process 1 is usually 0 MPaG to 5 MPaG, preferably 0 MPaG to 0.5 MPaG. 1 and contact pressure P 2 The relationship between 1 ≧P 2 It is preferable that:

[0054] In the thermal decomposition step, water vapor or an inert gas such as nitrogen gas or CO2 gas may be allowed to coexist.

[0055] The pyrolysis step can be carried out using any suitable reaction vessel known in the art, and examples of the material for the reaction vessel include quartz glass, carbon steel, stainless steel, Inconel alloy, Hastelloy alloy, Incoloy alloy, and Monel alloy.

[0056] The pyrolysis product of the raw material obtained in the pyrolysis step usually contains hydrocarbons having about 1 to 50 carbon atoms, hydrogen, etc., in a liquid, gaseous state, or a mixture thereof.

[0057] <Process for vaporizing raw materials (vaporization process)> In the olefin production method of this embodiment, it is preferable to further include a vaporization step prior to the catalytic cracking step, and to make the catalytic cracking step a step of catalytically cracking a gaseous raw material.

[0058] The vaporization step in the olefin production method of this embodiment can be carried out using any suitable conventionally known device, adopting conditions corresponding to the selected raw material and the components contained in the raw material.

[0059] The vaporization step of this embodiment can be carried out using the vessel in which the catalytic cracking step described above is carried out. The vaporization step and the catalytic cracking step of this embodiment may be carried out continuously using the same reaction vessel.

[0060] Temperature T in the vaporization process 3 The heating temperature is usually 350°C to 550°C, and preferably 400°C to 500°C.

[0061] Pressure P during the vaporization process 3 is usually 0 MPaG to 5 MPaG, and preferably 0 MPaG to 0.5 MPaG. By setting the pressure in this range, the raw material can be efficiently converted into a gaseous state.

[0062] In the vaporization step, water vapor or an inert gas such as nitrogen gas or CO2 gas may be allowed to coexist.

[0063] The vaporization step can be carried out using any suitable reaction vessel known in the art, and examples of the material for the reaction vessel include quartz glass, carbon steel, stainless steel, Inconel alloy, Hastelloy alloy, Incoloy alloy, and Monel alloy.

[0064] The decomposition products of the raw material obtained in the vaporization step contain gaseous hydrocarbons having about 1 to 50 carbon atoms, hydrogen, and the like.

[0065] In the olefin production process of this embodiment, the thermal cracking step, the vaporization step, and the catalytic cracking step already described may be carried out integrally and continuously in this order.

[0066] According to the olefin production method of the present embodiment, in the case of using raw materials containing organic chlorine compounds, which are inevitably contained in raw materials containing polyolefins such as food packaging containers and which have conventionally had to be removed in advance because they can be catalyst poisons, it is possible to efficiently produce olefins without removing the organic chlorine compounds in advance. Note that, when carrying out the olefin production method of the present embodiment, the organic chlorine compounds may be removed in advance from the raw materials.

[0067] 2. Catalyst regeneration method The zeolite catalyst used in the catalytic cracking step of this embodiment may be a regenerated catalyst. That is, the olefin production method of this embodiment can be carried out by applying a raw material containing polyolefin (which may further contain an organic chlorine compound) to the catalytic cracking step in the presence of a regenerated catalyst obtained by regenerating the used zeolite catalyst used in the olefin production method already described.

[0068] The catalyst regeneration method of this embodiment will now be described in detail. The method for regenerating a catalyst according to the present embodiment includes a step of calcining the catalyst in an atmosphere containing 1% by volume to 50% by volume of oxygen to obtain a regenerated catalyst.

[0069] The step of obtaining the regenerated catalyst is preferably carried out in an atmosphere containing oxygen in the range of 1 volume % to 50 volume %, and more preferably in an atmosphere containing oxygen in the range of 5 volume % to 30 volume %.

[0070] The process for obtaining the regenerated catalyst can be carried out, for example, in an air atmosphere, a nitrogen gas atmosphere, an argon gas atmosphere, a carbon dioxide gas atmosphere, or a mixed gas atmosphere thereof, while adjusting the oxygen concentration in the atmosphere by any suitable method known in the art.

[0071] The temperature in the step of obtaining the regenerated catalyst is preferably in the range of 400°C to 700°C (for example, 550°C), and more preferably in the range of 450°C to 600°C.

[0072] The treatment time in the step of obtaining the regenerated catalyst is preferably 30 minutes to 48 hours (for example, 5 hours), and more preferably 1 hour to 24 hours.

[0073] The regenerated catalyst obtained by the above-mentioned catalyst regeneration method can be used in the olefin production method of this embodiment in the same manner as an unused "zeolite catalyst" for the catalytic cracking reaction of polyolefins, without any particular adjustment of conditions such as temperature, treatment time, and atmosphere. [Example]

[0074] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following examples.

[0075] <Reference example 1> Preparation of zeolite catalyst A Aluminum nitrate nonahydrate (0.29 g), 20.3 mass% tetrapropylammonium hydroxide aqueous solution (76.8 g), sodium hydroxide (0.77 g), and tetraethyl orthosilicate (64.0 g) were added to a 400 mL PTFE container equipped with a stirrer, and the mixture was stirred at room temperature for 18 hours to obtain a mixture. After that, ion-exchanged water (56.6 g) was added to this mixture, and the entire amount was transferred to a stainless steel (SUS) autoclave equipped with a 200 mL PTFE inner cylinder.

[0076] In the mixture, the ratio of the number of moles of silicon atoms to the number of moles of aluminum atoms was 400, the ratio of the number of moles of tetrapropylammonium hydroxide to the number of moles of silicon atoms was 0.56, the ratio of the number of moles of sodium atoms to the number of moles of silicon atoms was 0.06, and the ratio of the number of moles of water to the number of moles of silicon atoms was 13.

[0077] The mixture was heated in an autoclave at 170°C for 24 hours and then cooled with ice water. After cooling, the mixture (suspension) in the cylindrical container was centrifuged and the supernatant was removed to obtain a zeolite precursor.

[0078] Water was added to the obtained zeolite precursor to form a suspension again, and the suspension was then centrifuged and the supernatant was removed. This procedure was repeated until the pH of the supernatant became 8 or less, thereby forming a solid again.

[0079] The obtained solid was dried at 120° C. for 8 hours. The dried solid was pulverized in a mortar and further calcined at 550° C. for 7 hours in a muffle furnace to obtain zeolite 1 (14.1 g).

[0080] Zeolite 1 (6.6 g) and 0.5 M ammonium nitrate aqueous solution (300 mL) were added to a 500 mL resin container and allowed to stand for 6 hours at a temperature of 60° C. The resulting mixture was then subjected to suction filtration using a Buchner funnel to recover the solid.

[0081] The collected solid and 0.5 M aqueous ammonium nitrate solution (330 mL) were added to a flask, and the mixture was allowed to stand for 12 hours at 60° C. After that, the resulting mixture was subjected to suction filtration using a Buchner funnel to collect the solid.

[0082] Next, the collected solid and 0.5M ammonium nitrate aqueous solution (330 mL) were added to the flask, and the mixture was allowed to stand at 60° C. for 6 hours. The mixture was then suction filtered using a Buchner funnel to collect the solid. The collected solid was washed with water (500 mL) and dried at 90° C. for 6 hours to obtain a solid.

[0083] The obtained solid was calcined in an air atmosphere at a temperature of 550° C. for 5 hours using a muffle furnace to obtain a powdered zeolite catalyst A (5.1 g).

[0084] Zeolite catalyst A was analyzed by ICP atomic emission spectrometry, and the sodium atom content was less than 0.01 mass%, which is the detection limit, and the ratio of the number of moles of silicon atoms to the number of moles of aluminum atoms (Si / Al ratio) was 349. Furthermore, as a result of analyzing zeolite catalyst A by X-ray diffraction analysis, it was confirmed that the catalyst had an MFI structure.

[0085] <Example 1> Olefin Production The upstream reaction tube of two glass reaction tubes connected in series was filled with a raw material (weight ratio LDPE:PVC=95:5) which was a mixture of polyolefin polyethylene (LDPE) (manufactured by Sumitomo Chemical Co., Ltd., product name: Sumikathene G201F) (1.425 g) and organic chlorine compound polyvinyl chloride (PVC) (manufactured by Shin-Etsu Chemical Co., Ltd., product name: Shin-Etsu PVC Straight Polymer TK-1000) (0.075 g), and the downstream reaction tube was filled with zeolite catalyst A (0.3 g).

[0086] A cooling trap was connected further downstream of the downstream reaction tube, and a 5 L gas bag was connected downstream of the cooling trap.

[0087] Nitrogen gas was passed through the upstream reaction tube at a flow rate of 10 NmL / min, and only the downstream reaction tube was heated at 550°C for 1 hour to pretreat the zeolite catalyst A, and then the temperature of the downstream reaction tube was lowered to 525°C.

[0088] The step of pyrolyzing the raw material was carried out by passing nitrogen gas at a flow rate of 10 NmL / min and setting the electric furnace temperature of the upstream reaction tube at 455°C to obtain a pyrolyzed mixture of the raw material.

[0089] Next, the pyrolyzed raw material was subjected to a catalytic cracking process. Specifically, the pyrolyzed raw material obtained as described above was subjected to catalytic cracking at a temperature T 2 The catalyst was then introduced into the downstream reaction tube at 525°C to contact the raw material with the catalyst. The entire liquid catalytic cracking product obtained 2 hours after the start of heating the raw material was collected in a cooling trap cooled with ice water, and the entire gaseous catalytic cracking product was collected in a gas bag.

[0090] The weights of the recovered liquid catalytic cracking product and the residues adhering to the upstream and downstream reaction tubes were measured using a balance.

[0091] The recovered gaseous catalytic cracking product was analyzed by gas chromatography, and as a result, the yield of olefins having 2 to 3 carbon atoms was 37.1% based on the mass of the charged polyethylene.

[0092] In addition, the analytical values ​​of the gaseous catalytic cracking product were corrected so that the total weight of the gaseous catalytic cracking product, the liquid catalytic cracking product, and the residue was the total weight of the raw polyethylene and PVC. As a result, the yield of olefins having 2 to 3 carbon atoms was calculated to be 34.4% based on the mass of the charged polyethylene. The results are also shown in Table 1.

[0093] Finally, the spent zeolite catalyst (spent zeolite catalyst B) was recovered from the reaction system.

[0094] <Example 2> Regeneration of spent zeolite catalyst B (preparation of regenerated catalyst C) The spent zeolite catalyst B recovered in Example 1 was calcined in a muffle furnace in an air atmosphere (oxygen concentration 21% by volume) at a temperature of 550° C. for 5 hours to obtain a regenerated zeolite catalyst as regenerated catalyst C.

[0095] <Example 3> Olefin production using regenerated catalyst C The upstream reaction tube of two glass reaction tubes connected in series was filled with polyethylene (LDPE) (manufactured by Sumitomo Chemical Co., Ltd., product name: Sumikathene G201F) (1.0 g) as a raw material, and the downstream reaction tube was filled with regenerated catalyst C (0.2 g).

[0096] A cooling trap was connected further downstream of the downstream reaction tube, and a 5 L gas bag was connected downstream of the cooling trap.

[0097] Nitrogen gas was passed through the upstream reaction tube at a flow rate of 10 NmL / min, and only the downstream reaction tube was heated at 550°C for 1 hour to pretreat the regenerated catalyst C, and then the temperature of the downstream reaction tube was lowered to 525°C.

[0098] The step of pyrolyzing the raw material was carried out by passing nitrogen gas at a flow rate of 10 NmL / min and setting the electric furnace temperature of the upstream reaction tube at 455°C to obtain a pyrolyzed raw material.

[0099] Next, the step of catalytically cracking the pyrolyzed feedstock is carried out by subjecting the pyrolyzed feedstock obtained as described above to a temperature T 2 into the downstream reaction tube at 525°C, and the raw material was brought into contact with regenerated catalyst C. Two hours after the start of heating the raw material, the entire amount of the liquid catalytic cracking product obtained was collected in a cooling trap cooled with ice water, and the entire amount of the gaseous catalytic cracking product was collected in a gas bag.

[0100] The weights of the recovered liquid catalytic cracking product and the residues adhering to the upstream and downstream reaction tubes were measured using a balance.

[0101] The recovered gaseous catalytic cracking product was analyzed by gas chromatography, and as a result, the yield of olefins having 2 to 3 carbon atoms was 39.0% based on the mass of the charged polyethylene.

[0102] In addition, the analytical values ​​of the gaseous catalytic cracking product were corrected so that the total weight of the gaseous catalytic cracking product, the liquid catalytic cracking product, and the residue was the total weight of the raw polyethylene and PVC. As a result, the yield of olefins having 2 to 3 carbon atoms was calculated to be 36.8% based on the mass of the charged polyethylene. The results are also shown in Table 1.

[0103] <Reference example 2> Preparation of Zeolite Catalyst D Aluminum nitrate nonahydrate (1.15 g), 20.3 mass% tetrapropylammonium hydroxide aqueous solution (76.8 g), sodium hydroxide (0.77 g), and tetraethyl orthosilicate (64.0 g) were added to a 400 mL PTFE container equipped with a stirrer, and the mixture was stirred at room temperature for 18 hours to obtain a mixture. After that, ion-exchanged water (56.6 g) was added to the obtained mixture, and the entire amount was transferred to a SUS autoclave equipped with a 200 mL PTFE inner cylinder.

[0104] The ratio of the number of moles of silicon atoms to the number of moles of aluminum atoms in the mixture was 100, the ratio of the number of moles of tetrapropylammonium hydroxide to the number of moles of silicon atoms was 0.56, the ratio of the number of moles of sodium atoms to the number of moles of silicon atoms was 0.06, and the ratio of the number of moles of water to the number of moles of silicon atoms was 13.

[0105] The mixture was heat-treated in an autoclave at a temperature of 170° C. for 24 hours, and then cooled with ice water. After cooling, the mixture (suspension) in the cylindrical container was centrifuged, and the supernatant was removed to obtain a zeolite precursor.

[0106] Water was added to the obtained zeolite precursor to form a suspension again, and the supernatant was removed by centrifugation. This procedure was repeated until the pH of the supernatant became 8 or less, to obtain a solid.

[0107] The obtained solid was dried at 120° C. for 8 hours, pulverized in a mortar, and further calcined at 550° C. for 7 hours in a muffle furnace to obtain Zeolite 2 (13.6 g).

[0108] Zeolite 2 (6.0 g) and 0.5 M ammonium nitrate aqueous solution (300 mL) were added to a 500 mL resin container and allowed to stand for 6 hours at a temperature of 60° C. The resulting mixture was then subjected to suction filtration using a Buchner funnel to recover the solid.

[0109] The collected solid and 0.5 M ammonium nitrate aqueous solution (300 mL) were added to a flask, and the mixture was allowed to stand for 12 hours at a temperature of 60° C. After that, the obtained mixture was subjected to suction filtration using a Buchner funnel to collect the solid.

[0110] The collected solid and 0.5 M aqueous ammonium nitrate solution (300 mL) were added to a flask, and the mixture was allowed to stand for 6 hours at a temperature of 60° C. After that, the obtained mixture was subjected to suction filtration using a Buchner funnel to collect the solid.

[0111] The collected solid was washed with water (500 mL) and dried at 90° C. for 6 hours, and then calcined in an air atmosphere at 550° C. for 5 hours in a muffle furnace to obtain zeolite 3 (4.6 g).

[0112] The obtained zeolite 3 (4.5 g) and 0.1 M aqueous sodium nitrate solution (450 mL) were added to a two-necked 500 mL glass recovery flask equipped with a condenser, and the mixture was allowed to stand at 100° C. for 2 hours. The mixture was then subjected to suction filtration using a Buchner funnel to recover the solid.

[0113] The collected solid and 0.1M sodium nitrate aqueous solution (450 mL) were added to the recovery flask, and the mixture was allowed to stand at 100° C. for 2 hours. The mixture was then suction filtered using a Buchner funnel to collect the solid. The collected solid was washed with water (300 mL) and dried at 110° C. for 12 hours.

[0114] The obtained solid was calcined in an air atmosphere at a temperature of 550° C. for 5 hours using a muffle furnace to obtain a powdered zeolite catalyst D (4.1 g).

[0115] Zeolite catalyst D was analyzed by ICP atomic emission spectrometry, and as a result, the sodium atom content was 0.24 mass % and the ratio of the number of moles of silicon atoms to the number of moles of aluminum atoms (Si / Al ratio) was 85. Furthermore, as a result of analyzing zeolite catalyst D by X-ray diffraction analysis, it was confirmed that the catalyst had an MFI structure.

[0116] <Comparative Example 1> Olefin Production The upstream reaction tube of two glass reaction tubes connected in series was filled with a raw material (weight ratio LDPE:PVC=95:5) which was a mixture of polyolefin polyethylene (LDPE) (manufactured by Sumitomo Chemical Co., Ltd., product name: Sumikathene G201F) (1.425 g) and organic chlorine compound polyvinyl chloride (PVC) (manufactured by Shin-Etsu Chemical Co., Ltd., product name: Shin-Etsu PVC Straight Polymer TK-1000) (0.075 g), and the downstream reaction tube was filled with zeolite catalyst D (0.3 g).

[0117] A cooling trap was connected further downstream of the downstream reaction tube, and a 5 L gas bag was connected downstream of the cooling trap.

[0118] Nitrogen gas was passed through the upstream reaction tube at a flow rate of 10 NmL / min, and only the downstream reaction tube was heated at 550°C for 1 hour to pretreat the zeolite catalyst D, and then the temperature of the downstream reaction tube was lowered to 525°C.

[0119] The step of pyrolyzing the raw material was carried out by passing nitrogen gas at a flow rate of 10 NmL / min and setting the temperature of the electric furnace in the upstream reaction tube to 455°C to obtain a pyrolyzed raw material. The step of catalytically decomposing the pyrolyzed raw material was carried out by subjecting the pyrolyzed raw material obtained as described above to a temperature T 2 The raw material was introduced into the downstream reaction tube heated to 525°C, and the raw material was brought into contact with the zeolite catalyst D.

[0120] Two hours after the start of heating the raw material, the entire amount of the liquid catalytic cracking product obtained was collected in a cooling trap cooled with ice water, and the entire amount of the gaseous catalytic cracking product was collected in a gas bag.

[0121] The weights of the recovered liquid catalytic cracking product and the residues adhering to the upstream and downstream reaction tubes were measured using a balance.

[0122] The recovered gaseous catalytic cracking product was analyzed by gas chromatography, and as a result, the yield of olefins having 2 to 3 carbon atoms was 19.8% based on the mass of the charged polyethylene.

[0123] In addition, the analytical values ​​of the gaseous catalytic cracking product were corrected so that the total weight of the gaseous catalytic cracking product, the liquid catalytic cracking product, and the residue was the total weight of the raw polyethylene and PVC. As a result, the yield of olefins having 2 to 3 carbon atoms was calculated to be 25.2% based on the mass of the charged polyethylene. The results are also shown in Table 1.

[0124] Finally, the spent zeolite catalyst (spent zeolite catalyst E) was recovered.

[0125] <Comparative Example 2> Regeneration of spent zeolite catalyst E (preparation of regenerated catalyst F) The spent zeolite catalyst E was heated in a muffle furnace under air for 55 The catalyst was calcined at 0° C. for 5 hours to obtain regenerated catalyst F.

[0126] <Comparative Example 3> Olefin production with regenerated catalyst F The upstream reaction tube of two glass reaction tubes connected in series was filled with polyolefin polyethylene (LDPE) (manufactured by Sumitomo Chemical, product name: Sumikathene G201F) (1.0 g) as a raw material, and the downstream reaction tube was filled with regenerated catalyst F (0.2 g).

[0127] A cooling trap was connected further downstream of the downstream reaction tube, and a 5 L gas bag was connected downstream of the cooling trap.

[0128] Nitrogen gas was passed through the upstream reaction tube at a flow rate of 10 NmL / min, and only the downstream reaction tube was heated at 550°C for 1 hour to pretreat the regenerated catalyst F, and then the downstream reaction tube was cooled to 525°C. The step of pyrolyzing the raw material was carried out by passing nitrogen gas through the upstream reaction tube at a flow rate of 10 NmL / min and setting the electric furnace temperature of the upstream reaction tube to 455°C to obtain a pyrolyzed raw material. The step of catalytically decomposing the pyrolyzed raw material was carried out by catalytically decomposing the raw material obtained as described above at a temperature T 2 The raw material was introduced into the downstream reaction tube heated to 525°C, and the raw material was brought into contact with the regenerated catalyst F.

[0129] Two hours after the start of heating the raw material, the entire amount of the liquid catalytic cracking product obtained was collected in a cooling trap cooled with ice water, and the entire amount of the gaseous catalytic cracking product was collected in a gas bag.

[0130] The weights of the recovered liquid catalytic cracking product and the residues adhering to the upstream and downstream reaction tubes were measured using a balance.

[0131] The recovered gaseous catalytic cracking product was analyzed by gas chromatography, and as a result, the yield of olefins having 2 to 3 carbon atoms was 26.2% based on the mass of the charged polyethylene.

[0132] In addition, the analytical values ​​of the gaseous catalytic cracking product were corrected so that the total weight of the gaseous catalytic cracking product, the liquid catalytic cracking product, and the residue was the total weight of the raw polyethylene and PVC. As a result, the yield of olefins having 2 to 3 carbon atoms was calculated to be 30.8% based on the mass of the charged polyethylene. The results are also shown in Table 1.

[0133] <Reference Example 3> Preparation of Zeolite Catalyst G Aluminum nitrate nonahydrate (0.30 g), 22.3 mass% tetrapropylammonium hydroxide aqueous solution (76.8 g), sodium hydroxide (0.79 g), and tetraethyl orthosilicate (63.4 g) were added to a 400 mL PTFE container equipped with a stirrer, and the mixture was stirred at room temperature for 18 hours to obtain a mixture. After that, ion-exchanged water (56.4 g) was added to this mixture, and the entire amount was transferred to a stainless steel (SUS) autoclave equipped with a 200 mL PTFE inner cylinder.

[0134] In the mixture, the ratio of the number of moles of silicon atoms to the number of moles of aluminum atoms was 400, the ratio of the number of moles of tetrapropylammonium hydroxide to the number of moles of silicon atoms was 0.56, the ratio of the number of moles of sodium atoms to the number of moles of silicon atoms was 0.06, and the ratio of the number of moles of water to the number of moles of silicon atoms was 13.

[0135] The mixture was heated in an autoclave at 170°C for 24 hours and then cooled with ice water. After cooling, the mixture (suspension) in the cylindrical container was centrifuged and the supernatant was removed to obtain a zeolite precursor.

[0136] Water was added to the obtained zeolite precursor to form a suspension again, and the suspension was then centrifuged and the supernatant was removed. This procedure was repeated until the pH of the supernatant became 8 or less, thereby forming a solid again.

[0137] The obtained solid was dried at 120° C. for 8 hours, pulverized in a mortar, and further calcined at 550° C. for 6 hours in a muffle furnace to obtain zeolite 4 (12.5 g).

[0138] Zeolite 4 (10.0 g) and 0.5 M ammonium nitrate aqueous solution (500 mL) were added to a 500 mL resin container, and the container was allowed to stand for 6 hours at a temperature of 60° C. The resulting mixture was then subjected to suction filtration using a Buchner funnel, and the solid was collected.

[0139] The collected solid and 0.5 M ammonium nitrate aqueous solution (500 mL) were added to a flask, and the mixture was allowed to stand for 6 hours at a temperature of 60° C. After that, the obtained mixture was subjected to suction filtration using a Buchner funnel to collect the solid.

[0140] Next, the collected solid and 0.5M ammonium nitrate aqueous solution (500 mL) were added to a flask and allowed to stand at 60° C. for 6 hours. The mixture was then suction filtered using a Buchner funnel to collect the solid. The collected solid was washed with water (750 mL) and dried at 90° C. for 12 hours to obtain a solid.

[0141] The obtained solid was calcined in an air atmosphere at a temperature of 550° C. for 5 hours using a muffle furnace to obtain a powdered zeolite catalyst G (7.3 g).

[0142] Zeolite catalyst G was analyzed by ICP atomic emission spectrometry, and as a result, the sodium atom content was 0.03 mass % and the ratio of the number of moles of silicon atoms to the number of moles of aluminum atoms (Si / Al ratio) was 576. Furthermore, as a result of analyzing zeolite catalyst G by X-ray diffraction analysis, it was confirmed that the catalyst had an MFI structure.

[0143] <Example 4> Production of olefins The upstream reaction tube of two glass reaction tubes connected in series was filled with a raw material (weight ratio LDPE:PVC=95:5) which was a mixture of polyolefin polyethylene (LDPE) (manufactured by Sumitomo Chemical Co., Ltd., product name: Sumikathene G201F) (1.425 g) and organic chlorine compound polyvinyl chloride (PVC) (manufactured by Shin-Etsu Chemical Co., Ltd., product name: Shin-Etsu PVC Straight Polymer TK-1000) (0.075 g), and the downstream reaction tube was filled with zeolite catalyst G (0.3 g).

[0144] A cooling trap was connected further downstream of the downstream reaction tube, and a 5 L gas bag was connected downstream of the cooling trap.

[0145] Nitrogen gas was passed through the upstream reaction tube at a flow rate of 10 NmL / min, and only the downstream reaction tube was heated at 550°C for 1 hour to pretreat the zeolite catalyst G, and then the temperature of the downstream reaction tube was lowered to 525°C.

[0146] The step of pyrolyzing the raw material was carried out by passing nitrogen gas at a flow rate of 10 NmL / min and setting the temperature of the electric furnace in the upstream reaction tube to 455°C to obtain a pyrolyzed raw material. The step of catalytically decomposing the pyrolyzed raw material was carried out by subjecting the pyrolyzed raw material obtained as described above to a temperature T 2 The raw material was introduced into the downstream reaction tube heated to 525°C, and the raw material was brought into contact with the zeolite catalyst G.

[0147] Two hours after the start of heating the raw material, the entire amount of the liquid catalytic cracking product obtained was collected in a cooling trap cooled with ice water, and the entire amount of the gaseous catalytic cracking product was collected in a gas bag.

[0148] The weights of the recovered liquid catalytic cracking product and the residues adhering to the upstream and downstream reaction tubes were measured using a balance.

[0149] The recovered gaseous catalytic cracking product was analyzed by gas chromatography, and as a result, the yield of olefins having 2 to 3 carbon atoms was 37.0% based on the mass of the charged polyethylene.

[0150] In addition, the analytical values ​​of the gaseous catalytic cracking product were corrected so that the total weight of the gaseous catalytic cracking product, the liquid catalytic cracking product, and the residue was the total weight of the raw polyethylene and PVC. As a result, the yield of olefins having 2 to 3 carbon atoms was calculated to be 38.8% based on the mass of the charged polyethylene. The results are also shown in Table 1.

[0151] Finally, the spent zeolite catalyst (spent zeolite catalyst H) was recovered.

[0152] <Example 5> Regeneration of used zeolite catalyst H (preparation of regenerated catalyst I) The used zeolite catalyst H was calcined in an air atmosphere at a temperature of 550° C. for 5 hours using a muffle furnace to obtain regenerated catalyst I.

[0153] <Example 6> Production of olefins using regenerated catalyst I The upstream reaction tube of two glass reaction tubes connected in series was filled with polyolefin polyethylene (LDPE) (manufactured by Sumitomo Chemical Co., Ltd., product name: Sumikathene G201F) (1.0 g) as a raw material, and the downstream reaction tube was filled with regenerated catalyst I (0.2 g).

[0154] A cooling trap was connected further downstream of the downstream reaction tube, and a 5 L gas bag was connected downstream of the cooling trap.

[0155] Nitrogen gas was passed through the upstream reaction tube at a flow rate of 10 NmL / min, and only the downstream reaction tube was heated at 550°C for 1 hour to pretreat the regenerated catalyst I, and then the temperature of the downstream reaction tube was lowered to 525°C. The step of pyrolyzing the raw material was carried out by passing nitrogen gas through the upstream reaction tube at a flow rate of 10 NmL / min and setting the electric furnace temperature of the upstream reaction tube to 455°C to obtain a pyrolyzed raw material.

[0156] The step of catalytically cracking the pyrolyzed raw material is carried out by subjecting the raw material obtained as described above to a temperature T 2 The raw material was introduced into the downstream reaction tube at 525°C, and the raw material was brought into contact with the regenerated catalyst I.

[0157] Two hours after the start of heating the raw material, the entire amount of the liquid catalytic cracking product obtained was collected in a cooling trap cooled with ice water, and the entire amount of the gaseous catalytic cracking product was collected in a gas bag.

[0158] The weights of the recovered liquid catalytic cracking product and the residues adhering to the upstream and downstream reaction tubes were measured using a balance.

[0159] The recovered gaseous catalytic cracking product was analyzed by gas chromatography, and as a result, the yield of olefins having 2 to 3 carbon atoms was 37.5% based on the mass of the charged polyethylene.

[0160] In addition, the analytical values ​​of the gaseous catalytic cracking product were corrected so that the total weight of the gaseous catalytic cracking product, the liquid catalytic cracking product, and the residue was the total weight of the raw polyethylene and PVC. As a result, the yield of olefins having 2 to 3 carbon atoms was calculated to be 38.6% based on the mass of the charged polyethylene. The results are also shown in Table 1.

[0161] <Reference Example 4> Preparation of Zeolite Catalyst J Aluminum nitrate nonahydrate (0.122 g), 20.3 mass% tetrapropylammonium hydroxide aqueous solution (76.8 g), sodium hydroxide (0.77 g), and tetraethyl orthosilicate (64.0 g) were added to a 400 mL PTFE container equipped with a stirrer, and the mixture was stirred at room temperature for 18 hours to obtain a mixture. After that, ion-exchanged water (56.6 g) was added to this mixture, and the entire amount was transferred to a stainless steel (SUS) autoclave equipped with a 200 mL PTFE inner cylinder.

[0162] In the mixture, the ratio of the number of moles of silicon atoms to the number of moles of aluminum atoms was 1000, the ratio of the number of moles of tetrapropylammonium hydroxide to the number of moles of silicon atoms was 0.56, the ratio of the number of moles of sodium atoms to the number of moles of silicon atoms was 0.06, and the ratio of the number of moles of water to the number of moles of silicon atoms was 13.

[0163] The mixture was heated in an autoclave at 170°C for 24 hours and then cooled with ice water. After cooling, the mixture (suspension) in the cylindrical container was centrifuged and the supernatant was removed to obtain a zeolite precursor.

[0164] Water was added to the obtained zeolite precursor to form a suspension again, and the suspension was then centrifuged and the supernatant was removed. This procedure was repeated until the pH of the supernatant became 8 or less, thereby forming a solid again.

[0165] The obtained solid was dried at 120° C. for 8 hours, pulverized in a mortar, and further calcined at 550° C. for 7 hours in a muffle furnace to obtain zeolite 5 (14.2 g).

[0166] Zeolite 5 (6.6 g) and 0.5 M ammonium nitrate aqueous solution (300 mL) were added to a 500 mL resin container and allowed to stand for 5 hours at a temperature of 60° C. The resulting mixture was then suction filtered using a Buchner funnel, and the collected solid was dried at 90° C. for 1 hour.

[0167] The dried solid and 0.5 M ammonium nitrate aqueous solution (330 mL) were added to a flask, and the mixture was allowed to stand for 6 hours at a temperature of 60° C. After that, the resulting mixture was subjected to suction filtration using a Buchner funnel to collect the solid.

[0168] Next, the collected solid and 0.5M ammonium nitrate aqueous solution (330 mL) were added to a flask and allowed to stand at 60° C. for 12 hours. The mixture was then suction filtered using a Buchner funnel to collect the solid. The collected solid was washed with water (500 mL) and dried at 90° C. for 6 hours to obtain a solid.

[0169] The obtained solid was calcined in an air atmosphere at 550° C. for 5 hours using a muffle furnace to obtain a powdered zeolite catalyst J (5.5 g).

[0170] Zeolite catalyst J was analyzed by ICP atomic emission spectrometry, and the sodium atom content was found to be less than 0.01 mass%, which is the detection limit, and the ratio of the number of moles of silicon atoms to the number of moles of aluminum atoms (Si / Al ratio) was 1,249. In addition, zeolite catalyst J was analyzed by X-ray diffraction analysis, and it was confirmed that it had an MFI structure.

[0171] <Example 7> Production of olefins The upstream reaction tube of two glass reaction tubes connected in series was filled with a raw material (weight ratio LDPE:PVC=95:5) which was a mixture of polyolefin polyethylene (LDPE) (manufactured by Sumitomo Chemical Co., Ltd., product name: Sumikathene G201F) (1.425 g) and organic chlorine compound polyvinyl chloride (PVC) (manufactured by Shin-Etsu Chemical Co., Ltd., product name: Shin-Etsu PVC Straight Polymer TK-1000) (0.075 g), and the downstream reaction tube was filled with zeolite catalyst J (0.3 g).

[0172] A cooling trap was connected further downstream of the downstream reaction tube, and a 5 L gas bag was connected downstream of the cooling trap.

[0173] Nitrogen gas was passed through the upstream reaction tube at a flow rate of 10 NmL / min, and only the downstream reaction tube was heated at 550°C for 1 hour to pretreat the zeolite catalyst J, and then the temperature of the downstream reaction tube was lowered to 525°C.

[0174] The step of pyrolyzing the raw material was carried out by passing nitrogen gas at a flow rate of 10 NmL / min and setting the temperature of the electric furnace in the upstream reaction tube to 455°C to obtain a pyrolyzed raw material. The step of catalytically decomposing the pyrolyzed raw material was carried out by subjecting the pyrolyzed raw material obtained as described above to a temperature T 2 The raw material was introduced into the downstream reaction tube heated to 525°C, and the raw material was brought into contact with zeolite catalyst J.

[0175] Two hours after the start of heating the raw material, the entire amount of the liquid catalytic cracking product obtained was collected in a cooling trap cooled with ice water, and the entire amount of the gaseous catalytic cracking product was collected in a gas bag.

[0176] The weights of the recovered liquid catalytic cracking product and the residues adhering to the upstream and downstream reaction tubes were measured using a balance.

[0177] The recovered gaseous catalytic cracking product was analyzed by gas chromatography, and as a result, the yield of olefins having 2 to 3 carbon atoms was 31.2% based on the mass of the charged polyethylene.

[0178] In addition, the analytical values ​​of the gaseous catalytic cracking product were corrected so that the total weight of the gaseous catalytic cracking product, the liquid catalytic cracking product, and the residue was the total weight of the raw polyethylene and PVC. As a result, the yield of olefins having 2 to 3 carbon atoms was calculated to be 34.5% based on the mass of the charged polyethylene. The results are also shown in Table 1.

[0179] Finally, the spent zeolite catalyst (spent zeolite catalyst K) was recovered.

[0180] <Example 8> Regeneration of used zeolite catalyst K (preparation of regenerated catalyst L) The used zeolite catalyst K was calcined in an air atmosphere at a temperature of 550° C. for 5 hours using a muffle furnace to obtain a regenerated catalyst L.

[0181] <Example 9> Production of olefins using regenerated catalyst L The upstream reaction tube of two glass reaction tubes connected in series was filled with polyolefin polyethylene (LDPE) (manufactured by Sumitomo Chemical Co., Ltd., product name: Sumikathene G201F) (1.0 g) as a raw material, and the downstream reaction tube was filled with regenerated catalyst L (0.2 g).

[0182] A cooling trap was connected further downstream of the downstream reaction tube, and a 5 L gas bag was connected downstream of the cooling trap.

[0183] Nitrogen gas was passed through the upstream reaction tube at a flow rate of 10 NmL / min, and only the downstream reaction tube was heated at 550°C for 1 hour to pretreat the regenerated catalyst L, and then the downstream reaction tube was cooled to 525°C. The process of pyrolyzing the raw material was carried out by passing nitrogen gas through the upstream reaction tube at a flow rate of 10 NmL / min and setting the electric furnace temperature of the upstream reaction tube to 455°C to obtain a pyrolyzed raw material.

[0184] The step of catalytically cracking the pyrolyzed raw material is carried out by subjecting the raw material obtained as described above to a temperature T 2 The raw material was introduced into the downstream reaction tube heated to 525°C, and the raw material was brought into contact with the regenerated catalyst L.

[0185] Two hours after the start of heating the raw material, the entire amount of the liquid catalytic cracking product obtained was collected in a cooling trap cooled with ice water, and the entire amount of the gaseous catalytic cracking product was collected in a gas bag.

[0186] The weights of the recovered liquid catalytic cracking product and the residues adhering to the upstream and downstream reaction tubes were measured using a balance.

[0187] The recovered gaseous catalytic cracking product was analyzed by gas chromatography, and as a result, the yield of olefins having 2 to 3 carbon atoms was 29.8% based on the mass of the charged polyethylene.

[0188] In addition, the analytical value of the gaseous catalytic cracking product was corrected so that the total weight of the gaseous catalytic cracking product, the liquid catalytic cracking product, and the residue was the total weight of the raw polyethylene and PVC. As a result, the yield of olefins having 2 to 3 carbon atoms was calculated to be 33.2% based on the mass of the charged polyethylene. The results are also shown in Table 1.

[0189] <Example 10> Production of olefins The upstream reaction tube of two glass reaction tubes connected in series was filled with a raw material (weight ratio LDPE:PVC=99.5:0.5) which was a mixture of polyolefin polyethylene (LDPE) (manufactured by Sumitomo Chemical Co., Ltd., product name: Sumikathene G201F) (0.9805 g) and organic chlorine compound polyvinyl chloride (PVC) (manufactured by Shin-Etsu Chemical Co., Ltd., product name: Shin-Etsu PVC Straight Polymer TK-1000) (0.0052 g), and the downstream reaction tube was filled with zeolite catalyst A (0.2 g).

[0190] A cooling trap was connected further downstream of the downstream reaction tube, and a 5 L gas bag was connected downstream of the cooling trap.

[0191] Nitrogen gas was passed through the upstream reaction tube at a flow rate of 10 NmL / min, and only the downstream reaction tube was heated at 550°C for 1 hour to pretreat the zeolite catalyst A, and then the temperature of the downstream reaction tube was lowered to 525°C.

[0192] The step of pyrolyzing the raw material was carried out by passing nitrogen gas at a flow rate of 10 NmL / min and setting the temperature of the electric furnace in the upstream reaction tube to 455°C to obtain a pyrolyzed raw material. The step of catalytically decomposing the pyrolyzed raw material was carried out by subjecting the pyrolyzed raw material obtained as described above to a temperature T 2 The raw material was introduced into the downstream reaction tube heated to 525° C., and the raw material was brought into contact with the zeolite catalyst A.

[0193] Two hours after the start of heating the raw material, the entire amount of the liquid catalytic cracking product obtained was collected in a cooling trap cooled with ice water, and the entire amount of the gaseous catalytic cracking product was collected in a gas bag.

[0194] The weights of the recovered liquid catalytic cracking product and the residues adhering to the upstream and downstream reaction tubes were measured using a balance.

[0195] The recovered gaseous catalytic cracking product was analyzed by gas chromatography, and as a result, the yield of olefins having 2 to 3 carbon atoms was 34.3% based on the mass of the charged polyethylene.

[0196] In addition, the analytical values ​​of the gaseous catalytic cracking product were corrected so that the total weight of the gaseous catalytic cracking product, the liquid catalytic cracking product, and the residue was the total weight of the raw polyethylene and PVC. As a result, the yield of olefins having 2 to 3 carbon atoms was calculated to be 40.5% based on the mass of the charged polyethylene. The results are also shown in Table 1.

[0197] Finally, the spent zeolite catalyst (spent zeolite catalyst M) was recovered.

[0198] <Example 11> Regeneration of used zeolite catalyst M (preparation of regenerated catalyst N) The used zeolite catalyst M was calcined in an air atmosphere at a temperature of 550° C. for 5 hours using a muffle furnace to obtain a regenerated catalyst N.

[0199] <Example 12> Production of olefins using regenerated catalyst N The upstream reaction tube of two glass reaction tubes connected in series was filled with polyolefin polyethylene (LDPE) (manufactured by Sumitomo Chemical Co., Ltd., product name: Sumikathene G201F) (0.82 g) as a raw material, and the downstream reaction tube was filled with regenerated catalyst N (0.16 g).

[0200] A cooling trap was connected further downstream of the downstream reaction tube, and a 5 L gas bag was connected downstream of the cooling trap.

[0201] Nitrogen gas was passed through the upstream reaction tube at a flow rate of 10 NmL / min, and only the downstream reaction tube was heated at 550°C for 1 hour to pretreat the regenerated catalyst N, and then the downstream reaction tube was cooled to 525°C. The process of pyrolyzing the raw material was carried out by passing nitrogen gas through the upstream reaction tube at a flow rate of 10 NmL / min and setting the electric furnace temperature of the upstream reaction tube to 455°C to obtain pyrolyzed raw material.

[0202] The step of catalytically cracking the pyrolyzed raw material is carried out by subjecting the raw material obtained as described above to a temperature T 2 The raw material was introduced into the downstream reaction tube at 525°C, and the raw material was brought into contact with the regenerated catalyst N.

[0203] Two hours after the start of heating the raw material, the entire amount of the liquid catalytic cracking product obtained was collected in a cooling trap cooled with ice water, and the entire amount of the gaseous catalytic cracking product was collected in a gas bag.

[0204] The weights of the recovered liquid catalytic cracking product and the residues adhering to the upstream and downstream reaction tubes were measured using a balance.

[0205] The recovered gaseous catalytic cracking product was analyzed by gas chromatography, and as a result, the yield of olefins having 2 to 3 carbon atoms was 35.0% based on the mass of the charged polyethylene.

[0206] In addition, the analytical values ​​of the gaseous catalytic cracking product were corrected so that the total weight of the gaseous catalytic cracking product, the liquid catalytic cracking product, and the residue was the total weight of the raw polyethylene and PVC. As a result, the yield of olefins having 2 to 3 carbon atoms was calculated to be 41.5% based on the mass of the charged polyethylene. The results are also shown in Table 1.

[0207] <Example 13> Production of olefins The upstream reaction tube of two glass reaction tubes connected in series was filled with a raw material (weight ratio LDPE:PVC=90:10) which was a mixture of polyolefin polyethylene (LDPE) (manufactured by Sumitomo Chemical Co., Ltd., product name: Sumikathene G201F) (0.135 g) and organic chlorine compound polyvinyl chloride (PVC) (manufactured by Shin-Etsu Chemical Co., Ltd., product name: Shin-Etsu PVC Straight Polymer TK-1000) (0.015 g), and the downstream reaction tube was filled with zeolite catalyst A (0.3 g).

[0208] A cooling trap was connected further downstream of the downstream reaction tube, and a 5 L gas bag was connected downstream of the cooling trap.

[0209] Nitrogen gas was passed through the upstream reaction tube at a flow rate of 10 NmL / min, and only the downstream reaction tube was heated at 550°C for 1 hour to pretreat the zeolite catalyst A, and then the temperature of the downstream reaction tube was lowered to 525°C.

[0210] The step of pyrolyzing the raw material was carried out by passing nitrogen gas at a flow rate of 10 NmL / min and setting the temperature of the electric furnace in the upstream reaction tube to 455°C to obtain a pyrolyzed raw material. The step of catalytically decomposing the pyrolyzed raw material was carried out by subjecting the pyrolyzed raw material obtained as described above to a temperature T 2 The raw material was introduced into the downstream reaction tube heated to 525° C., and the raw material was brought into contact with the zeolite catalyst A.

[0211] Two hours after the start of heating the raw material, the entire amount of the liquid catalytic cracking product obtained was collected in a cooling trap cooled with ice water, and the entire amount of the gaseous catalytic cracking product was collected in a gas bag.

[0212] The weights of the recovered liquid catalytic cracking product and the residues adhering to the upstream and downstream reaction tubes were measured using a balance.

[0213] The recovered gaseous catalytic cracking product was analyzed by gas chromatography, and as a result, the yield of olefins having 2 to 3 carbon atoms was 30.3% based on the mass of the charged polyethylene.

[0214] In addition, the analytical values ​​of the gaseous catalytic cracking product were corrected so that the total weight of the gaseous catalytic cracking product, the liquid catalytic cracking product, and the residue was the total weight of the raw polyethylene and PVC. As a result, the yield of olefins having 2 to 3 carbon atoms was calculated to be 39.7% based on the mass of the charged polyethylene. The results are also shown in Table 1.

[0215] Finally, the spent zeolite catalyst (spent zeolite catalyst O) was recovered.

[0216] <Example 14> Regeneration of used zeolite catalyst O (preparation of regenerated catalyst P) The used zeolite catalyst O was calcined in an air atmosphere at a temperature of 550° C. for 5 hours using a muffle furnace to obtain a regenerated catalyst P.

[0217] <Example 15> Production of olefins using regenerated catalyst P The upstream reaction tube of two glass reaction tubes connected in series was filled with polyolefin polyethylene (LDPE) (manufactured by Sumitomo Chemical Co., Ltd., product name: Sumikathene G201F) (1.0 g) as a raw material, and the downstream reaction tube was filled with regenerated catalyst P (0.2 g).

[0218] A cooling trap was connected further downstream of the downstream reaction tube, and a 5 L gas bag was connected downstream of the cooling trap.

[0219] Nitrogen gas was passed through the upstream reaction tube at a flow rate of 10 NmL / min, and only the downstream reaction tube was heated at 550°C for 1 hour to pretreat the regenerated catalyst P, and then the downstream reaction tube was cooled to 525°C. The process of pyrolyzing the raw material was carried out by passing nitrogen gas through the upstream reaction tube at a flow rate of 10 NmL / min and setting the electric furnace temperature of the upstream reaction tube to 455°C to obtain a pyrolyzed raw material.

[0220] The step of catalytically cracking the pyrolyzed raw material is carried out by subjecting the raw material obtained as described above to a temperature T 2 The raw material was introduced into the downstream reaction tube at 525°C, and the raw material was brought into contact with the regenerated catalyst P.

[0221] Two hours after the start of heating the raw material, the entire amount of the liquid catalytic cracking product obtained was collected in a cooling trap cooled with ice water, and the entire amount of the gaseous catalytic cracking product was collected in a gas bag.

[0222] The weights of the recovered liquid catalytic cracking product and the residues adhering to the upstream and downstream reaction tubes were measured using a balance.

[0223] The recovered gaseous catalytic cracking product was analyzed by gas chromatography, and as a result, the yield of olefins having 2 to 3 carbon atoms was 32.8% based on the mass of the charged polyethylene.

[0224] In addition, the analytical values ​​of the gaseous catalytic cracking product were corrected so that the total weight of the gaseous catalytic cracking product, the liquid catalytic cracking product, and the residue was the total weight of the raw polyethylene and PVC. As a result, the yield of olefins having 2 to 3 carbon atoms was calculated to be 42.8% based on the mass of the charged polyethylene. The results are also shown in Table 1.

[0225] [Table 1]

Claims

1. The method for producing an olefin having 2 to 3 carbon atoms includes a step of catalytically cracking a raw material containing at least a polyolefin and an organic chlorine compound, the organic chlorine compound including at least one of polyvinyl chloride and polyvinylidene chloride, and having a chlorine atom content of 10 mass% or less, in the presence of a zeolite catalyst having a sodium atom content of less than 0.1 mass%, at 400°C or more and 700°C or less.

2. The method for producing an olefin according to claim 1, wherein the zeolite catalyst is an MFI type zeolite catalyst.

3. The process for producing an olefin according to claim 1 or 2, wherein the zeolite catalyst has a Si / Al ratio of 100 or more.

4. The process for producing an olefin according to claim 1 or 2, wherein the Si / Al ratio of the zeolite catalyst is 300 or more.

5. The method for producing an olefin according to any one of claims 1 to 4, wherein the content of the sodium atoms in the zeolite catalyst is less than 0.05 mass%.

6. The method for producing an olefin according to any one of claims 1 to 5, further comprising a step of thermally cracking the feedstock prior to the step of catalytic cracking.

7. The method for producing an olefin according to any one of claims 1 to 5, further comprising a step of vaporizing the raw material before the catalytic cracking step, and the catalytic cracking step is a step of catalytically cracking the gaseous raw material.

8. The process for producing an olefin according to any one of claims 1 to 7, wherein the catalytic cracking step is carried out at a temperature of 450°C or higher and 600°C or lower.

9. The method for producing an olefin according to any one of claims 1 to 8, wherein the zeolite catalyst is a regenerated catalyst.

10. A method for regenerating a catalyst, comprising a step of calcining a used zeolite catalyst used in the olefin production method according to any one of claims 1 to 9 in an atmosphere containing 1 volume % to 50 volume % of oxygen to obtain a regenerated catalyst.

11. A method for producing an olefin, comprising a step of catalytically cracking a feedstock containing a polyolefin in the presence of a regenerated catalyst regenerated by the regeneration method according to claim 10.

Citation Information

Patent Citations

  • Method and apparatus for chemical recycling of waste plastic

    JP2002121318A

  • System and method for producing intermediate distillate products and lower olefins from hydrocarbon feedstocks

    JP2010526179A

  • Conversion of plastics to olefinic and aromatic products

    JP2016513147A

  • Conversion of plastics to olefinic and aromatic products through product recycling

    JP2016514170A

  • Conversion of plastic to olefin and aromatic product

    JP2017137347A