Composite material, heat dissipation material, and method for manufacturing heat dissipation material
The composite material with boron nitride particles extending from an inorganic base material addresses the challenge of controlling heat conduction paths, improving thermal conductivity by aligning particles for efficient heat dissipation.
Patent Information
- Application Number
- JP2023001850
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-01-22
- Filing Date
- 2023-01-10
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2041-08-19
AI Technical Summary
Existing methods struggle to effectively control the formation of continuous heat conduction paths in heat dissipation materials using boron nitride particles, which are dispersed in a resin to form a sheet shape, as it is challenging to maintain their alignment and directionality.
A composite material comprising an inorganic base material with boron nitride particles arranged on one surface, where the particles extend from the base material, allowing for the formation of a continuous heat conduction path in the thickness direction by filling resin between and within the particles.
This approach facilitates easy control over the heat conduction paths, enhancing thermal conductivity by maintaining the alignment of boron nitride particles in the heat dissipation material.
Smart Images

Figure 0007555438000004 
Figure 0007555438000002 
Figure 0007555438000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to composite materials, heat dissipating materials, and methods for making heat dissipating materials. [Background technology]
[0002] Boron nitride has lubricating properties, high thermal conductivity, and insulating properties, and is used in a variety of applications, such as as a solid lubricant, a release material, a cosmetic ingredient, a heat dissipation material, and a heat-resistant insulating sintered body.
[0003] For example, Patent Document 1 describes a hexagonal boron nitride powder that can impart high thermal conductivity and high dielectric strength to a resin composition obtained by filling the resin with the powder, which contains aggregated particles made of primary particles of hexagonal boron nitride and has a BET specific surface area of 0.7 to 1.3 m. 2 / g and an oil absorption measured in accordance with JIS K 5101-13-1 of 80 g / 100 g or less is disclosed. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-160134 A Summary of the Invention [Problem to be solved by the invention]
[0005] The boron nitride particles as described above may be used in the form of a heat dissipation material (heat dissipation sheet) that is dispersed in a resin and formed into a sheet shape. In this case, in order to increase the thermal conductivity of the heat dissipation material in the thickness direction, it is desirable to disperse the boron nitride particles in the heat dissipation material so that a continuous heat conduction path is formed in the thickness direction of the heat dissipation material. However, it is not necessarily easy to control the heat conduction path formed by the boron nitride particles in the heat dissipation material.
[0006] An object of the present invention is to facilitate control of the thermal conduction paths formed by boron nitride particles in a heat dissipating material. [Means for solving the problem]
[0007] One aspect of the present invention is a composite material comprising an inorganic substrate and a plurality of boron nitride particles disposed on one surface of the inorganic substrate, the plurality of boron nitride particles extending from the inorganic substrate as a starting point.
[0008] In this composite material, a plurality of boron nitride particles are arranged to extend from the substrate, and thus by filling the spaces between the boron nitride particles of this composite material and the interior of the boron nitride particles with resin, a heat dissipating material can be produced while maintaining the state in which the boron nitride particles extend in the thickness direction of the heat dissipating material. Therefore, in the thickness direction of the obtained heat dissipating material, a continuous heat conduction path is easily formed by the boron nitride particles. In other words, by using this composite material, it is easier to control the heat conduction path formed by the boron nitride particles in the heat dissipating material, compared to, for example, a case in which a powder of boron nitride particles is mixed with a resin.
[0009] The inorganic substrate may comprise one selected from the group consisting of carbon and boron nitride.
[0010] The average length of the plurality of boron nitride particles in the extension direction may be 50 μm or more.
[0011] Another aspect of the present invention is a method for producing a heat dissipating material, comprising the step of filling spaces between a plurality of boron nitride particles of a composite material with a resin. The method for producing a heat dissipating material may further comprise the step of removing the inorganic base material after the above step.
[0012] Another aspect of the present invention is a sheet-shaped heat dissipating material containing a plurality of boron nitride particles and a resin, the plurality of boron nitride particles extending from one surface of the heat dissipating material toward the other surface opposite the one surface, and the average length of the plurality of boron nitride particles in the extending direction may be 50 μm or more. Effect of the Invention
[0013] According to the present invention, it is possible to easily control the heat conduction paths formed by the boron nitride particles in the heat dissipation material. [Brief description of the drawings]
[0014] [Figure 1] 1 is a graph showing the results of X-ray diffraction measurement of the boron nitride particles of Example 1. [Diagram 2] 1 is an SEM image of the composite material of Example 1. [Diagram 3] 1 is an SEM image of the composite material of Example 2. [Figure 4] 1 is a microscope image of a cross section in the thickness direction of the heat dissipation material of Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, an embodiment of the present invention will be described in detail. A composite material according to an embodiment includes an inorganic substrate and a plurality of boron nitride particles disposed on one surface of the inorganic substrate.
[0016] The inorganic substrate may be an inorganic substrate that can withstand (have heat resistance to) heating in the production step of the composite material production method described later. The inorganic substrate may be, for example, an inorganic substrate containing an inorganic material having a melting point or sublimation point of 1500°C or higher. The content of the inorganic material having a melting point or sublimation point of 1500°C or higher may be, for example, 95% by mass or higher, 98% by mass or higher, or 99% by mass or higher based on the total amount of the inorganic substrate. The inorganic substrate may be an inorganic substrate consisting only of an inorganic material having a melting point or sublimation point of 1500°C or higher. The melting point or sublimation point of the inorganic material may be appropriately selected according to the heating temperature in the production step, and may be 1600°C or higher, 1800°C or higher, 2000°C or higher, 2200°C or higher, or 2400°C or higher. Examples of inorganic materials having a melting point or sublimation point of 1500°C or higher include carbon, boron carbide, silicon carbide, silicon nitride, alumina, and boron nitride.
[0017] The inorganic substrate may be an inorganic substrate in which the weight change rate of the inorganic substrate before and after heating is 5% or less when heated at 1500°C and 0.1 MPa for 1 hour in a nitrogen atmosphere (for example, an atmosphere containing 95% or more by volume of nitrogen gas). The weight change rate of the inorganic substrate before and after heating is calculated by the following formula, where W1 is the weight of the inorganic substrate before heating and W2 is the weight of the inorganic substrate after heating. The inorganic substrate used for measuring the weight change rate is one which has been heated at 200°C for 2 hours and dried. Weight change rate = (W1 - W2) / W1 x 100
[0018] The inorganic substrate may be, for example, in the form of a sheet, a plate, a rod, etc. Examples of the inorganic substrate include a carbon sheet (graphite sheet), a carbon plate, a carbon rod, a carbon crucible, a boron nitride sheet, a boron nitride plate, a boron nitride crucible, etc. The thickness of the sheet-like inorganic substrate may be, for example, 100 μm or more and 500 μm or less.
[0019] Each of the boron nitride particles extends from the inorganic substrate as a starting point. The inorganic substrate and the boron nitride particles may be chemically bonded to each other at the starting point. The boron nitride particles may extend linearly or curvedly. The boron nitride particles may extend by branching into two or more directions during the extension. The extension direction of the boron nitride particles may be approximately perpendicular to the surface of the inorganic substrate on which the boron nitride particles are arranged, or may be at an angle from the perpendicular direction. The extension direction of the boron nitride particles means the direction connecting the starting point of the boron nitride particles and the point at which the linear distance from the starting point is the maximum.
[0020] The average length in the extension direction of the boron nitride particles may be 50 μm or more, 80 μm or more, 100 μm or more, 125 μm or more, 150 μm or more, or 200 μm or more, and may be 500 μm or less, 400 μm or less, or 300 μm or less.
[0021] The average length in the extension direction of the boron nitride particles can be measured using a laser microscope (for example, "Optelics HYBRID" manufactured by Lasertec Corporation). Specifically, first, the measurement range is set so as to include the thickness of the inorganic substrate and the maximum length of the boron nitride particles for the composite material, and the surface shape of the composite material is measured. Next, the length in the extension direction of the boron nitride particles is measured from the cross-sectional profile of the measured surface shape of the composite material. This measurement of the length in the extension direction is performed for 20 boron nitride particles, and the average value is taken as the average length in the extension direction of the boron nitride particles.
[0022] The boron nitride particles may have an elongated shape as described above. The average aspect ratio of the boron nitride particles may be, for example, 1.2 or more, 1.3 or more, 1.4 or more, 1.5 or more, 2.0 or more, 3.0 or more, 5.0 or more, or 7.0 or more, and may be 12.0 or less, 9.0 or less, or 8.0 or less.
[0023] The average aspect ratio of a boron nitride particle is defined as the average ratio (L1 / L2) of the length of the boron nitride particle in the stretching direction (L1) to the length of the boron nitride particle in the direction perpendicular to the stretching direction (L2) for 20 boron nitride particles. The length of the boron nitride particle in the direction perpendicular to the stretching direction can be measured from the cross-sectional profile of the surface shape of the composite material in the same manner as the length in the stretching direction.
[0024] Each boron nitride particle may be solid or hollow. When the boron nitride particle is hollow, the boron nitride particle may have an outer shell formed by boron nitride and a hollow portion surrounded by the outer shell. The hollow portion may be formed along the extension direction of the boron nitride particle, and may have a shape approximately similar to the external shape of the boron nitride particle. When the boron nitride particle is hollow, the tip of the boron nitride particle may be an open end, and the open end may be connected to the above-mentioned hollow portion.
[0025] The number of boron nitride particles arranged per unit area of the inorganic substrate is, for example, 10 particles / mm 2 More than 20 pieces / mm2 or more than 30 pieces / mm 2 or more, and 2 Below 200 pieces / mm 2 or less than 100 pieces / mm 2 It may be the following:
[0026] Next, a method for producing the above-mentioned composite material will be described below. The composite material can be produced by a production method including a step (arrangement step) of arranging a mixture containing boron carbide and boric acid and an inorganic substrate in a container made of a carbon material, and a step (production step) of generating boron nitride particles on the inorganic substrate by heating and pressurizing the container in a nitrogen atmosphere. Another embodiment of the present invention is a method for producing such a composite material.
[0027] The container made of a carbon material is a container capable of housing the mixture and the inorganic base material. The container may be, for example, a carbon crucible. The container is preferably a container whose airtightness can be enhanced by covering the opening. In the arrangement step, for example, the mixture may be arranged at the bottom of the container, and the inorganic base material may be arranged so as to be fixed to the side wall surface or the inside of the lid of the container. Details of the inorganic base material are the same as those described in the above embodiment (composite material).
[0028] The boron carbide in the mixture may be, for example, in powder form (boron carbide powder). The boric acid in the mixture may be, for example, in powder form (boric acid powder). The mixture may be obtained, for example, by mixing boron carbide powder and boric acid powder by a known method.
[0029] The boron carbide powder can be produced by a known production method. For example, the method for producing the boron carbide powder includes mixing boric acid with acetylene black, and then heating the mixture at 1800 to 2400°C for 1 to 10 hours in an inert gas (e.g., nitrogen gas) atmosphere to obtain aggregated boron carbide particles. The aggregated boron carbide particles obtained by this method can be crushed, sieved, washed, impurity removed, dried, etc., to obtain boron carbide powder.
[0030] The average particle size of the boron carbide powder can be adjusted by adjusting the grinding time of the aggregated boron carbon particles. The average particle size of the boron carbide powder may be 5 μm or more, 7 μm or more, or 10 μm or more, and may be 100 μm or less, 90 μm or less, 80 μm or less, or 70 μm or less. The average particle size of the boron carbide powder can be measured by a laser diffraction scattering method.
[0031] The mixing ratio of boron carbide and boric acid can be appropriately selected. The content of boric acid in the mixture is preferably 2 parts by mass or more, more preferably 5 parts by mass or more, and even more preferably 8 parts by mass or more, relative to 100 parts by mass of boron carbide, from the viewpoint that boron nitride particles tend to become large, and may be 100 parts by mass or less, 90 parts by mass or less, 80 parts by mass or less, or 70 parts by mass or less.
[0032] The mixture containing boron carbide and boric acid may further contain other components, such as silicon carbide, carbon, iron oxide, etc. When the mixture containing boron carbide and boric acid further contains silicon carbide, it becomes easier to obtain boron nitride particles that do not have open ends.
[0033] The inside of the container is a nitrogen atmosphere containing, for example, 95% by volume or more of nitrogen gas. The content of nitrogen gas in the nitrogen atmosphere is preferably 95% by volume or more, more preferably 99.9% by volume or more, and may be substantially 100% by volume. In addition to nitrogen gas, the nitrogen atmosphere may contain ammonia gas, etc.
[0034] From the viewpoint that boron nitride particles tend to grow large, the heating temperature is preferably 1450° C. or higher, more preferably 1600° C. or higher, and even more preferably 1800° C. or higher. The heating temperature may be 2400° C. or lower, 2300° C. or lower, or 2200° C. or lower.
[0035] The pressure during pressing is preferably 0.3 MPa or more, more preferably 0.6 MPa or more, from the viewpoint that boron nitride particles tend to become large. The pressure during pressing may be 1.0 MPa or less, or 0.9 MPa or less.
[0036] The time for which the heating and pressure are applied is preferably 3 hours or more, more preferably 5 hours or more, from the viewpoint that boron nitride particles tend to become large. The time for which the heating and pressure are applied may be 40 hours or less, or 30 hours or less.
[0037] In this manner, the above-mentioned boron nitride particles are formed on the inorganic substrate, and a composite material is obtained in which a plurality of boron nitride particles extend from the inorganic substrate as the starting point. The fact that the particles formed on the inorganic substrate are boron nitride particles can be confirmed by recovering a portion of the particles from the inorganic substrate, performing X-ray diffraction measurement on the recovered particles, and detecting a peak derived from boron nitride.
[0038] The composite material obtained as described above can be used as a heat dissipation material by filling the spaces between the boron nitride particles of the composite material with resin. That is, another embodiment of the present invention is a method for producing a heat dissipation material, comprising a step of filling the spaces between the boron nitride particles of the composite material with resin (filling step).
[0039] Examples of resins include epoxy resin, silicone resin, silicone rubber, acrylic resin, phenolic resin, melamine resin, urea resin, unsaturated polyester, fluororesin, polyimide, polyamideimide, polyetherimide, polybutylene terephthalate, polyethylene terephthalate, polyphenylene ether, polyphenylene sulfide, wholly aromatic polyester, polysulfone, liquid crystal polymer, polyethersulfone, polycarbonate, maleimide-modified resin, ABS (acrylonitrile-butadiene-styrene) resin, AAS (acrylonitrile-acrylic rubber-styrene) resin, and AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resin.
[0040] The viscosity of the resin at 25°C may be 0.1 Pa·s or more, 0.3 Pa·s or more, or 0.5 Pa·s or more, and may be 200 Pa·s or less, 150 Pa·s or less, or 120 Pa·s or less. In this specification, the viscosity refers to the viscosity measured using a rotational viscometer at a shear rate of 10 (1 / sec).
[0041] In the filling step, the amount of resin to be filled may be appropriately adjusted depending on the form of use of the heat dissipation material, the required characteristics, etc. The amount of resin to be filled may be, for example, 15 vol% or more, 20 vol% or more, 30 vol% or more, 40 vol% or more, 50 vol% or more, or 60 vol% or more based on the total volume of the heat dissipation material, and may be 70 vol% or less, 60 vol% or less, 50 vol% or less, or 40 vol% or less.
[0042] In the filling step, the spaces between the boron nitride particles of the composite material may be filled with only resin, or may be filled with a mixture containing resin and other components. Examples of other components include a curing agent. The curing agent may be any agent that can cure the resin, and is appropriately selected according to the type of resin. Examples of curing agents used together with the epoxy resin include phenol novolac compounds, acid anhydrides, amino compounds, and imidazole compounds. The amount of the curing agent added may be, for example, 0.5 parts by mass or more or 1.0 parts by mass or more, and 15 parts by mass or less or 10 parts by mass or less, relative to 100 parts by mass of the resin.
[0043] The other components may be an inorganic filler, a curing accelerator (curing catalyst), a coupling agent, a wetting and dispersing agent, a surface conditioner, and the like.
[0044] The inorganic filler may be a thermally conductive filler such as aluminum oxide, magnesium oxide, silicon oxide, zinc oxide, boron nitride, silicon nitride, aluminum nitride, or graphite.
[0045] In the filling step, the amount of inorganic filler to be filled may be appropriately adjusted depending on the form of use of the heat dissipation material, the required characteristics, etc. The amount of inorganic filler to be filled may be, for example, vol% or more, 3 vol% or more, 5 vol% or more, 10 vol% or more, 12 vol% or more, or 15 vol% or more, and 40 vol% or less, 35 vol% or less, 30 vol% or less, or 20 vol% or less, based on the total volume of the heat dissipation material.
[0046] Examples of the curing accelerator (curing catalyst) include phosphorus-based curing accelerators such as tetraphenylphosphonium tetraphenylborate and triphenyl phosphate, imidazole-based curing accelerators such as 2-phenyl-4,5-dihydroxymethylimidazole, and amine-based curing accelerators such as boron trifluoride monoethylamine.
[0047] Examples of the coupling agent include a silane-based coupling agent, a titanate-based coupling agent, and an aluminate-based coupling agent, etc. Examples of the chemical bonding group contained in these coupling agents include a vinyl group, an epoxy group, an amino group, a methacryl group, and a mercapto group.
[0048] Examples of the wetting and dispersing agent include phosphate salts, carboxylate esters, polyesters, acrylic copolymers, and block copolymers.
[0049] Examples of the surface conditioner include an acrylic surface conditioner, a silicone surface conditioner, a vinyl surface conditioner, and a fluorine surface conditioner.
[0050] The viscosity of the mixture at 25° C. may be 0.1 Pa·s or more, 0.3 Pa·s or more, or 0.5 Pa·s or more, and may be 200 Pa·s or less, 150 Pa·s or less, or 120 Pa·s or less. The filling amount of the mixture, based on the total volume of the heat dissipating material, may be, for example, 15 vol% or more, 20 vol% or more, 30 vol% or more, 40 vol% or more, 50 vol% or more, or 60 vol% or more, and may be 70 vol% or less, 60 vol% or less, 50 vol% or less, or 40 vol% or less.
[0051] The method for producing a heat dissipating material may further include a step of removing the inorganic base material (removal step) after the filling step. In the removal step, the method for removing the inorganic base material may include peeling off the inorganic base material.
[0052] The method for producing a heat dissipation material may further include a step of curing the resin (curing step) after the filling step. The method for curing the resin is appropriately selected depending on the type of resin (and the curing agent used as necessary). For example, when the resin is an epoxy resin and the above-mentioned curing agent is used together, the resin can be cured by heating in the curing step.
[0053] The method for producing a heat dissipating material may further include a processing step of processing the obtained heat dissipating material into a desired shape after the filling step and the curing step. For example, when the composite material is in a sheet form, the processing step may be a step of polishing the surface of the composite material opposite to the inorganic substrate to adjust the thickness of the obtained heat dissipating material. The method for producing a heat dissipating material may include a processing step before and / or after the above-mentioned removal step.
[0054] In this manner, a heat dissipating material containing a plurality of boron nitride particles and a resin can be obtained. In the heat dissipating material obtained by the above-mentioned manufacturing method, since a plurality of boron nitride particles extend from the inorganic substrate as a starting point in the composite material, a plurality of boron nitride particles also extend in a specific direction in the heat dissipating material. For example, when the heat dissipating material is in a sheet form, a plurality of boron nitride particles may extend from one surface (a surface that was in contact with the inorganic substrate) of the heat dissipating material as a starting point toward the other surface (a surface parallel to the one surface) opposite to the one surface. That is, another embodiment of the present invention is a sheet-shaped heat dissipating material containing a plurality of boron nitride particles and a resin, in which a plurality of boron nitride particles extend from one surface (one main surface) of the heat dissipating material as a starting point toward the other surface (the other main surface) opposite to the one surface.
[0055] In a sheet-like heat dissipation material, it can be confirmed by microscopic observation of a cross-section of the heat dissipation material in the thickness direction that multiple boron nitride particles extend from one side of the heat dissipation material toward the opposite side.
[0056] The phrase "extending toward the other surface opposite to one surface" includes not only the case where the extension direction of the boron nitride particles coincides with the direction of the perpendicular line connecting the one surface and the other surface (i.e., the thickness direction of the sheet-like heat dissipating material), but also the case where the extension direction is inclined with respect to the perpendicular line direction. The extension direction of the boron nitride particles may be inclined at an angle of 45° or less, 40° or less, 30° or less, 20° or less, or 10° or less with respect to the perpendicular line direction. The extension directions of the boron nitride particles may be the same or different from each other. In addition, the phrase "extending toward the other surface opposite to one surface" includes both the case where the boron nitride particles reach the other surface and the case where they do not reach the other surface (i.e., it is sufficient that the boron nitride particles extend in the above-mentioned extension direction).
[0057] The average length in the extension direction of the boron nitride particles may be 50 μm or more, 80 μm or more, 100 μm or more, 125 μm or more, 150 μm or more, or 200 μm or more, and may be 500 μm or less, 400 μm or less, or 300 μm or less.
[0058] The average length of the boron nitride particles in the extension direction can be measured by observing the cross section of the heat dissipation material in the thickness direction with a microscope. Specifically, the cross section of the heat dissipation material in the thickness direction is observed with a microscope, and the length of the boron nitride particles from the starting point in the extension direction is measured. This measurement of the extension length is performed for 20 boron nitride particles, and the average value is taken as the average length of the boron nitride particles in the extension direction.
[0059] The number of boron nitride particles arranged per unit area on one side of the heat dissipation material is, for example, 10 particles / mm 2 More than 20 pieces / mm 2 or more than 30 pieces / mm 2 or more, and 2 Below 200 pieces / mm 2 or less than 100 pieces / mm 2The number of boron nitride particles arranged per unit area on one surface of the heat dissipating material can be measured by observing a cross section along one surface of the heat dissipating material with an SEM.
[0060] The content of boron nitride particles may be, for example, 30 vol.% or more, 40 vol.% or more, 50 vol.% or more, or 60 vol.% or more, and 85 vol.% or less, 80 vol.% or less, 70 vol.% or less, 60 vol.% or less, 50 vol.% or less, or 40 vol.% or less, based on the total volume of the heat dissipation material.
[0061] The resin content, based on the total volume of the heat dissipation material, may be, for example, 15 vol.% or more, 20 vol.% or more, 30 vol.% or more, 40 vol.% or more, 50 vol.% or more, or 60 vol.% or more, and may be 70 vol.% or less, 60 vol.% or less, 50 vol.% or less, or 40 vol.% or less.
[0062] The thickness of the sheet-shaped heat dissipating material may be, for example, 80 μm or more, 100 μm or more, 20 μm or more, or 300 μm or more, and may be 800 μm or less, 600 μm or less, or 400 μm or less.
[0063] The heat dissipating material may further contain other components in addition to the above boron nitride particles and resin. Details of the other components are the same as those described in the above method for producing a heat dissipating material.
[0064] The heat dissipating material may be used alone or in combination with another member. For example, a sheet-shaped heat dissipating material may be used in a state where it is laminated with another sheet-shaped member. That is, another embodiment of the present invention is a laminated sheet comprising a first sheet which is the above-mentioned sheet-shaped heat dissipating material, and a second sheet provided on at least one of the first sheet's one surface (the surface which is the starting point of the extension of the above-mentioned plurality of boron nitride particles) and the other surface. In one embodiment, the laminated sheet may comprise a first sheet, a second sheet provided on one surface of the first sheet, and a third sheet provided on the other surface of the first sheet. These embodiments may be used in a laminated sheet comprising a first sheet which is the above-mentioned sheet-shaped heat dissipating material, and a second sheet provided on at least one of the first sheet's one surface (the surface which is the starting point of the extension of the above-mentioned plurality of boron nitride particles) and the other surface. In one embodiment, the laminated sheet may comprise a first sheet, a second sheet provided on one surface of the first sheet, and a third sheet provided on the other surface of the first sheet. In this embodiment, the second sheet and the third sheet may be laminated directly to the first sheet, or may be laminated via an adhesive or the like.
[0065] The second sheet and the third sheet may be formed of, for example, a resin, a metal, etc. The second sheet and the third sheet may contain a resin and an inorganic filler as described above. When the second sheet and the third sheet contain a resin, the resin may be the same as the resin contained in the first sheet, or may be a different resin. EXAMPLES
[0066] The present invention will be described in detail below with reference to examples, although the present invention is not limited to the following examples.
[0067] (Example 1) Lumped boron carbide particles were pulverized by a pulverizer to obtain boron carbide powder with an average particle size of 10 μm. 100 parts by mass of the obtained boron carbide powder and 9 parts by mass of boric acid were mixed and filled into a carbon crucible, and the opening of the carbon crucible was covered with a carbon sheet (manufactured by NeoGraf, thickness: 130 μm, melting point: 4730° C., weight change rate: 1% or less (weight change rate before and after heating at 1500° C. and 0.1 MPa for 1 hour)), and the carbon sheet was sandwiched between the carbon crucible lid and the carbon crucible to fix the carbon sheet. The carbon crucible with the lid was heated in a resistance heating furnace under a nitrogen gas atmosphere at 2000° C. and 0.85 MPa for 20 hours to obtain a composite material in which a plurality of particles extending from the carbon sheet were generated.
[0068] A portion of the particles formed on the carbon sheet was collected and subjected to X-ray diffraction measurement using an X-ray diffractometer (ULTIMA-IV, manufactured by Rigaku Corporation). Figure 1 shows the results of this X-ray diffraction measurement, as well as the results of an X-ray diffraction measurement of boron nitride powder (GP grade) manufactured by Denka Company Ltd. for comparison. As can be seen from Figure 1, only peaks derived from boron nitride were detected, confirming that boron nitride particles had been formed. Figure 2 shows an SEM image of the obtained composite material. Figure 2 shows that multiple boron nitride particles extend from the carbon sheet as a starting point.
[0069] In addition, the length (L1) of the boron nitride particles in the extension direction and the length (L2) in the direction perpendicular to the extension direction were measured using a laser microscope ("Optelics HYBRID" manufactured by Lasertec Corporation). Specifically, the measurement range was set so as to include the thickness of the carbon sheet and the maximum height of the boron nitride particles for the composite material, and the surface shape of the composite material was measured. Next, the length (L1) of the boron nitride particles in the extension direction was measured from the cross-sectional profile of the measured surface shape of the composite material. In addition, the length (L2) in the direction perpendicular to the extension direction was also measured. These length measurements were performed for 20 boron nitride particles. The average length in the extension direction of the boron nitride particles was 254 μm, and the average aspect ratio was 3.4.
[0070] Example 2 In Example 1, the carbon sheet was changed to a boron nitride plate (p-BN plate, thickness: 500 μm, sublimation point: 2400° C.), the boron nitride plate was placed at the opening of the carbon crucible, and the boron nitride plate was fixed by sandwiching it between the carbon crucible lid and the carbon crucible. The carbon crucible with the lid was heated in a resistance heating furnace under nitrogen gas atmosphere at 1600° C. and 0.85 MPa for 5 hours, to obtain a composite material in which multiple particles extending from the boron nitride plate were generated.
[0071] Some of the particles formed on the boron nitride plate were collected and subjected to X-ray diffraction measurement using an X-ray diffractometer (Rigaku Corporation, "ULTIMA-IV"), confirming that boron nitride particles had been formed. Figure 3 shows an SEM image of the resulting composite material. Figure 3 confirms that multiple boron nitride particles extend from the boron nitride plate as a starting point.
[0072] In addition, the length (L1) of the boron nitride particles in the extension direction and the length (L2) in the direction perpendicular to the extension direction were measured in the same manner as in Example 1. The average length of the boron nitride particles in the extension direction was 139 μm, and the average aspect ratio was 1.5.
[0073] Example 3 A cylindrical jig (inner diameter 20 mm) was prepared, and the composite material obtained in Example 1 was placed inside the jig with the carbon sheet on the bottom and the boron nitride particles on the top. A mixture (viscosity at 25°C: 150 Pa·s) of 41.5 parts of epoxy resin (manufactured by DIC Corporation, product name: HP4032D), 5.1 parts of hardener (manufactured by DIC Corporation, product name: VH4150), 0.3 parts by volume of hardener (hardener catalyst) A (manufactured by Hokko Chemical Industry Co., Ltd., product name: TPP) and 0.5 parts by volume of hardener B (manufactured by Shikoku Kasei Kogyo Co., Ltd., product name: 2PHZ-PW) was poured into the inside of the jig, and the resin was filled between the multiple boron nitride particles of the composite material. The resin was hardened by heating at a temperature of 150°C for 60 minutes, and then the jig was removed. The surface of the cured resin obtained on the side opposite to the inorganic substrate was ground with a surface grinder to adjust the thickness of the cured resin to 200 μm. The cured resin was then peeled off from the carbon sheet to obtain a sheet-like heat dissipation material having a thickness of 200 μm and a diameter of 20 mm. The amount of boron nitride particles filled in the obtained heat dissipation material was 9 volume % based on the total volume of the heat dissipation material.
[0074] Figure 4 shows a microscopic image of a cross section in the thickness direction of the obtained heat dissipation material. From Figure 4, it was confirmed that multiple boron nitride particles extend from one surface of the heat dissipation material toward the opposite surface. The average length of the multiple boron nitride particles in the extension direction of the heat dissipation material was 174 μm. In addition, the thermal resistance of the obtained heat dissipation material was measured by the method described below and was found to be 1.1°C / W.
[0075] (Reference Example 1) Boron nitride particles were recovered from the composite material obtained in Example 1. The recovered boron nitride particles were mixed with a mixture (viscosity at 25°C: 150 Pa·s) of 41.5 parts of epoxy resin (manufactured by DIC Corporation, product name: HP4032D), 5.1 parts of curing agent (manufactured by DIC Corporation, product name: VH4150), 0.3 parts by volume of curing accelerator (curing catalyst) A (manufactured by Hokko Chemical Industry Co., Ltd., product name: TPP) and 0.5 parts by volume of curing accelerator B (manufactured by Shikoku Chemical Industry Co., Ltd., product name: 2PHZ-PW), and then cured by heating for 60 minutes under a temperature condition of 150°C to obtain a sheet-shaped heat dissipation material with a thickness of 200 μm and a diameter of 20 mm. The filling amount of boron nitride particles in the obtained heat dissipation material was 10% by volume based on the total volume of the heat dissipation material. The thermal resistance of the obtained heat dissipation material was measured by the method described below and was 1.82°C / W.
[0076] [Method of measuring thermal resistance] The thermal resistance of the obtained heat dissipation material was measured in accordance with ASTM D5470 using a resin material thermal resistance measuring device (manufactured by Hitachi Technology and Services Co., Ltd.) The obtained heat dissipation material was cut into 10 mm x 10 mm pieces, and the heat dissipation material with grease applied to both sides was placed between a thermocouple and heated and pressurized under conditions of a sample temperature of 50°C, a heat source output of 10 W, and a load of 1 MPa. The thermal resistance value A was calculated from the temperature difference ΔT between the front and back of the test piece and the heat source output Q, using A = ΔT / Q.
[0077] (Reference example 2) A heat dissipating material was produced in the same manner as in Reference Example 1, except that the boron nitride particles were changed to boron nitride ("GP" manufactured by Denka).
[0078] (Reference example 3) A heat dissipating material was produced in the same manner as in Reference Example 1, except that boron nitride particles were not used.
[0079] [Method of measuring dielectric constant] In order to evaluate the dielectric properties of the heat dissipation materials of Example 3 and Reference Examples 1 to 3, an impedance analyzer (IWATSU PSM3750+IAI2) was used at a frequency of 10 -1 ~10 7The capacitance (C) of the heat dissipation material was measured in the range of 500 Hz. In this measurement, the applied voltage was 10 V, and the evaluation temperature was room temperature of 25°C. One side of the heat dissipation material was gold sputtered to provide an electrode over the entire surface, and the other side was gold sputtered to provide a circular electrode with a diameter of 15 mm. The dielectric properties of the heat dissipation material were evaluated by comparing the relative dielectric constant ε of the heat dissipation material at a frequency of 1 kHz. The relative dielectric constant ε of the heat dissipation material was calculated from the following relational expression. C = ε × ε0 × S / d (C: capacitance of heat sink, S: area of circular electrode, d: thickness of heat sink, ε0: dielectric constant of vacuum)
[0080] The relative dielectric constants of the heat dissipating materials of Example 3 and Reference Examples 1 to 3 were as follows. Example 3: 4.58 Reference example 1:5.10 Reference example 2: 4.83 Reference example 3: 4.50 From these results, it was confirmed that the dielectric properties of the heat dissipation material of Example 3 did not decrease, and exhibited dielectric properties at or above a certain level.
Claims
1. An inorganic substrate; a plurality of boron nitride particles disposed on one surface of the inorganic substrate; the plurality of boron nitride particles extend from the inorganic substrate; The average length of the plurality of boron nitride particles in the extension direction is 50 μm or more, The composite material, wherein the plurality of boron nitride particles have an average aspect ratio of 12.0 or less.
2. 2. The composite material of claim 1, wherein the inorganic substrate comprises one selected from the group consisting of carbon and boron nitride.
3. A method for producing a heat dissipation material, comprising the step of filling spaces between the plurality of boron nitride particles of the composite material according to claim 1 or 2 with a resin.
4. The method for producing a heat dissipation material according to claim 3 , further comprising the step of removing the inorganic base material after the step.
5. A sheet-shaped heat dissipation material containing a plurality of boron nitride particles and a resin, A heat dissipation material in which the plurality of boron nitride particles extend from one surface of the heat dissipation material toward the other surface opposite the one surface (however, this does not include a laminate comprising a metal composite and an insulating material part, the metal composite having a metal body and a plurality of boron nitride nanotubes arranged on a surface of the metal body, the metal composite being arranged on the surface of the insulating material part from the boron nitride nanotube side, and the insulating material part including a cured portion of a thermosetting component containing a thermosetting compound and a thermosetting agent, and an insulating filler which is not a nanotube).
6. The heat dissipation material according to claim 5 , wherein the average length of the plurality of boron nitride particles in the extension direction is 50 μm or more.
Citation Information
Patent Citations
Heat dissipating sheet, interface, electronic parts, and manufacturing method of heat dissipating sheet
JP2006147801A
Manufacturing method
JP2013505194A
Method of manufacturing electronic apparatus and electronic apparatus
JP2014003144A
Hexagonal boron nitride powder and method for producing the same
JP2016160134A
Laminate
JP2017094542A