Fluorine adsorbent manufacturing method and fluorine removal and recovery method
The use of alkaline earth metal salts molded with cellulose nanofibers addresses the inefficiencies and costs of existing fluorine removal technologies, providing a cost-effective and reusable adsorbent for efficient fluorine recovery and separation.
Patent Information
- Application Number
- JP2020197221
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-27
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2040-11-27
AI Technical Summary
Existing fluorine removal technologies face challenges such as high costs, low utilization rates, environmental impact from waste generation, and inefficiencies in solid-liquid separation due to the use of rare earth elements, magnesium oxide, zirconium compounds, and hydrophilic organic polymers, which also fail to facilitate the reuse of recovered fluorine.
A fluorine adsorbent composed of alkaline earth metal salts molded with cellulose nanofibers as a binder, allowing for efficient fluorine recovery and reuse by chemical reaction, without high-temperature processing, and maintaining structural integrity for easy recycling.
The adsorbent achieves high adsorption efficiency, low manufacturing costs, and effective solid-liquid separation, enabling the recovery and reuse of fluorine as alkaline earth fluoride, suitable for various industrial applications.
Smart Images

Figure 0007555541000001 
Figure 0007555541000002 
Figure 0007555541000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a fluorine adsorbent used for reducing or recovering fluorine ions contained in wastewater or the like, and a method for removing or recovering fluorine using the same. [Background technology]
[0002] In the fields of metal, semiconductor, and glass manufacturing, chemicals containing fluorine are used in processes such as pickling and etching, and fluoride ions may be present in process water and wastewater. Furthermore, among the fluorocarbon gases that have been used in large quantities as refrigerants for air conditioners and refrigerators, the production of certain fluorocarbons that have a large impact on the ozone layer, as well as alternative fluorocarbons that have a smaller impact on the ozone layer but still contribute to global warming, has been banned, and the transition to new refrigerants is underway. However, in order to prevent the stock of these refrigerants in the market from being released into the atmosphere, they must be completely decomposed using heat or other methods. The hydrogen fluoride gas generated during the decomposition is usually absorbed in water and collected in a smoke scrubber, and the absorbed water contains fluoride ions. Fluorine is also used in a variety of other products, such as fluororesins and lubricants, and when fluorine-containing wastewater generated during the manufacturing process or product disposal is discharged, it is necessary to remove fluoride ions.
[0003] Usually, fluoride ions in wastewater are removed by adding powdered calcium salts such as slaked lime to generate insoluble calcium fluoride, which is then subjected to solid-liquid separation, but the generated calcium fluoride is in the form of fine crystals. For this reason, separation is difficult using solid-liquid separation methods that utilize the difference in specific gravity, such as sedimentation or centrifugation, because the difference in specific gravity between the wastewater and the calcium fluoride is so slight. In addition, when performing solid-liquid separation using methods such as filtering, the filter needs to be finely sized, which causes clogging even with a small amount of processing, resulting in extremely poor efficiency.
[0004] One method currently available for overcoming these difficulties in solid-liquid separation is to generate hydrogen fluoride microcrystals using a calcium salt and at the same time add a flocculant to flocculate the generated hydrogen fluoride microcrystals, thereby increasing their apparent particle size and specific gravity, thereby enabling efficient separation by sedimentation, centrifugation, filtering, or the like.
[0005] As flocculants, aluminum sulfate, PAC (polyaluminum chloride) or polymer flocculants are used. Generally, polymer flocculants are expensive in terms of chemical cost. Although aluminum sulfate and PAC are inexpensive, the recovered calcium fluoride contains a considerable amount of iron salts and aluminum salts, making it difficult to reuse the calcium fluoride. As a result, a large amount of waste is generated, which not only increases disposal costs but also places a heavy burden on the environment.
[0006] For this reason, various proposals have been made to efficiently remove fluorine (see, for example, Patent Documents 1 to 4). Patent Document 1 proposes an adsorbent composed of a composition of a hydrous oxide of a rare earth element prepared by heating and aging the hydrous oxide at 300° C. to 600° C., and a resin.
[0007] Patent Document 2 proposes magnesium oxide with a BET specific surface area of 10 m2 / g or more, and states that in order to obtain magnesium oxide with a high BET specific surface area, it is calcined at 400 to 1000°C, and then sieved to use granules with a particle size of 100 μm to 1 mm. In the examples, 0.2 g of magnesium oxide is added to 100 ml of an aqueous solution containing 500 ppm fluorine, and the result of adsorption at 25°C for 24 hours is shown, with the lowest fluorine content being 53 ppm.
[0008] In Patent Document 3, a zirconium hydrate compound is used as a fluorine-adsorbing element compound, and an adsorbent composed of a composition of this compound and a hydrophilic organic polymer is given a specific spherical structure to provide a durable adsorbent.
[0009] Patent Document 4 proposes an adsorbent comprising a composite granule of iron oxide hydroxide particles and / or iron oxide particles containing zirconium and an organic polymer resin. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] JP 2005-28312 A [Patent Document 2] JP 2005-342578 A [Patent Document 3] Patent No. 4854999 [Patent Document 4] Patent No. 5637708 Summary of the Invention [Problem to be solved by the invention]
[0011] However, the invention described in Patent Document 1 has problems such as high costs due to the use of scarce rare earth elements, the need for a high-temperature heating process, and the use of resin to maintain the shape. In the invention described in Patent Document 2, it is calculated that 44.7 mg of F in the liquid reacted with magnesium oxide. However, this is smaller than the theoretical value of 188.7 mg when 0.2 g of magnesium oxide is completely converted into MgF2, and there is an issue that the utilization rate of the material is low. The inventions described in Patent Documents 3 and 4 have a problem of high cost due to the use of expensive zirconium and a hydrophilic organic polymer. Furthermore, Patent Documents 1 to 4 do not mention any treatment after fluorine adsorption, and there is also a problem in that the adsorbent is not designed to reuse the recovered fluorine. The present invention has been made in view of the above problems, and an object of the present invention is to provide a fluorine adsorbent which can be produced at low cost, efficiently removes and recovers fluorine from fluorine-containing wastewater, facilitates solid-liquid separation after the recovery, and enables the reuse of fluorine. [Means for solving the problem]
[0012] The present invention has been made to solve at least some of the problems described above, and can be realized as the following application examples. Note that the reference symbols and supplementary explanations in parentheses in this section indicate the corresponding relationship with the embodiments described later in order to aid in understanding the present invention, and do not limit the present invention in any way.
[0013] [Application example 1] The invention described in Application Example 1 is a fluorine adsorbent comprising one or more inorganic powders made of alkaline earth metal salts molded into any shape using cellulose nanofibers as a binder. In this type of fluorine adsorbent, a composite molded body made by adding a small amount of cellulose nanofiber (hereinafter referred to as CNF) as a binder to alkaline earth metal salts that easily react with fluorine to form fluorides has both moderate water permeability and strength that does not collapse in fluorine-containing aqueous solutions. Therefore, by contacting this composite molded body with a fluorine-containing liquid, fluorine can be efficiently recovered.
[0014] In addition, it can be produced inexpensively because it uses common alkaline earth metal salts, does not require special high-temperature firing, etc., and has low production costs. Furthermore, fluorine adsorption is not physical, but utilizes a chemical reaction between alkaline earth metals, which have a high affinity for fluorine, and fluorine, so the adsorption efficiency is high.
[0015] In addition, since the fluorine adsorbed is not broken down, it can be easily recovered and reused as a fluoride.
[0016] [Application example 2] The fluorine adsorbent according to application example 2 is the fluorine adsorbent according to application example 1, wherein the inorganic powder is one or more selected from the group consisting of magnesium salts, calcium salts, strontium salts, and barium salts.
[0017] [Application example 3] The fluorine adsorbent according to the third aspect of the present invention is characterized in that the inorganic powder is one or more of magnesium hydroxide, calcium hydroxide, calcium phosphate, and calcium carbonate.
[0018] The industrial method of producing hydrogen fluoride is to react fluorite, a natural resource, with sulfuric acid at high temperatures to recover the gaseous hydrogen fluoride that is produced. Since fluorite is mostly composed of calcium fluoride, by producing a fluorine adsorbent from a calcium salt, the fluorine adsorbent after fluorine recovery can be a substitute for fluorite.
[0019] In addition, alkaline earth fluorides are used as raw materials for single crystal or halide glass, and are used in optical lenses and optical fibers, taking advantage of their optical properties which are different from those of ordinary oxide glasses such as SiO2. Furthermore, materials in which rare earth elements are added to alkaline earth fluorides have fluorescent properties and are used as luminescent materials and wavelength conversion materials.
[0020] By selecting an alkaline earth metal having a composition required for the fluoride glass or fluorescent material as the inorganic powder used in the fluorine adsorbent according to the present invention, the fluorine adsorbent after absorbing fluorine can be used as a raw material.
[0021] [Application example 4] The method for removing fluoride ions described in Application Example 4 is characterized in that the fluoride adsorbent described in any one of Application Examples 1 to 3 is brought into contact with water containing fluoride ions.
[0022] [Application example 5] The fluorine recovery method described in Application Example 5 is characterized in that the fluorine adsorbent described in any one of Application Examples 1 to 3 is brought into contact with water containing fluoride ions to obtain reusable alkaline earth fluoride. [Brief description of the drawings]
[0023] [Figure 1] FIG. 2 is a schematic diagram showing the internal structure of a fluorine adsorbent. [Diagram 2] FIG. 2 is a graph showing the change over time in fluoride ion concentration in a fluoride-containing liquid measured in Example 1, Comparative Example 1, and Comparative Example 2. [Diagram 3] FIG. 2 is a graph showing changes in pH after the molded bodies in Examples 1 to 4 and Comparative Example 1 are placed in a fluorine-containing solution. [Figure 4] FIG. 1 is a graph showing the change over time in fluoride ion concentration in a fluoride-containing liquid measured in Example 6 and Comparative Example 1. [Diagram 5] FIG. 13 is a diagram showing components in the fluorine adsorbent after calcination in Example 7. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] Hereinafter, examples to which the present invention is applied will be described with reference to the drawings. Note that the embodiment of the present invention is not limited to the following examples, and various forms may be adopted as long as they fall within the technical scope of the present invention.
[0025] [Example 1] The fluorine adsorbent 1 is prepared by molding one or more inorganic powders made of alkaline earth metal salts into a desired shape using cellulose nanofibers (CNF) as a binder.
[0026] The alkaline earth metal salt may be any salt that has low solubility in water, is easily reactive with fluorine, and further has low solubility in water of the fluoride after the reaction. The alkaline earth metal salt is selected from one or more of magnesium hydroxide, magnesium carbonate, magnesium phosphate, calcium hydroxide, calcium carbonate, calcium sulfate, calcium phosphate, strontium hydroxide, strontium carbonate, strontium sulfate, strontium phosphate, barium hydroxide, barium carbonate, barium sulfate, and barium phosphate, preferably one or more of magnesium hydroxide, magnesium carbonate, calcium hydroxide, calcium carbonate, and calcium phosphate, and more preferably one or more of magnesium hydroxide, calcium hydroxide, and calcium phosphate.
[0027] CNF is a biomass-derived material made by breaking down the cellulose contained in wood and other materials to the nano level. Various manufacturing methods have been developed, including physical crushing and chemical processing, and any method that is provided in the form of a 1-10% slurry can be selected.
[0028] (Fluorine adsorbent manufacturing method) The fluorine adsorbent 1 is produced by the following steps (a) to (c). (a) One or more alkaline earth metal salts selected from the above-mentioned alkaline earth metal salts are mixed and stirred with the CNF slurry (mixing and stirring process).
[0029] In this case, if the viscosity is too high with only the water contained in the commercially available CNF slurry and the stirring power is insufficient, any water may be added. Any method for mixing and stirring can be used as long as it suits the purpose, but it is sufficient to use a general stirrer, kneader, mixer, etc. that is used for slurries with relatively high viscosity.
[0030] (a) The slurry produced in the mixing and stirring process is made into a provisional molded body of any shape and size by a commonly used molding method such as casting, extrusion, injection molding, sheet molding, papermaking, etc. (molding process). In Example 1, casting molding was performed in which the slurry was poured into a mold.
[0031] (c) The provisionally molded body obtained in the molding step is heated and dried under vacuum or normal pressure to obtain a molded fluorine adsorbent (drying step). The heating temperature is up to 120°C, preferably in the range of 20 to 80°C, and more preferably 40 to 60°C. In the case of drying under vacuum, a temperature of 10°C, which is called low vacuum, is used. 5 Pa~10 2 in the range of Pa, preferably 10 4 ~10 3 The degree of vacuum may be in the range of Pa.
[0032] This is because if the drying temperature is high or the degree of vacuum is high, the molded body will suddenly lose water in the early stages of drying, and the pores in the molded body will not be able to keep up with the volume expansion from water to steam, causing localized expansion and resulting in deformation of the molded body.On the other hand, if the drying temperature or degree of vacuum is too low, the drying time will be long and inefficient.
[0033] It was confirmed that the preform after drying under appropriate conditions showed almost no external changes such as expansion or contraction compared to before drying. This is thought to be because the CNF forms a strong three-dimensional network skeleton before drying.
[0034] Furthermore, it is believed that the water remaining in the molded body when the CNF network skeleton is formed becomes steam during the drying process and is discharged outside the system, and the resulting voids become pores. Therefore, by controlling the amount of water remaining in the molded body before drying, the porosity in the molded body after drying can be selected as desired.
[0035] (Features of fluorine adsorbents) 1, the molded body 5 produced by such a method can maintain a suitable strength due to the three-dimensional network of CNFs (CNF network 10) while ensuring water permeability due to its large porosity, so that when it is brought into contact with a liquid containing fluorine ions, the reaction in which the alkaline earth metal salt 20 reacts with fluorine to be converted into an alkaline earth fluoride proceeds efficiently throughout the interior of the molded body 5, and the alkaline earth fluoride after the reaction is held on the CNF network 10, so that the molded body 5 does not collapse. Therefore, the molded body can be used as a fluorine adsorbent that has both strength and water permeability and allows efficient fluorine recovery while facilitating solid-liquid separation.
[0036] In addition, by contacting the fluorine adsorbent with fluorine ions equivalent to or greater than the amount of alkaline earth contained in the fluorine adsorbent, the fluorine adsorbent can be converted into an alkaline earth fluoride containing a small amount of CNF. Since CNF, which is an organic substance, can be relatively easily removed by calcination, it can be reused as a high-purity alkaline earth fluoride.
[0037] (Manufacturing results) The raw materials used were calcium hydroxide slurry and CNF slurry, which were stirred and mixed and poured into a PTFE (polytetrafluoroethylene) beaker, after which the beaker was dried. The molded body taken out after drying showed no signs of deformation.
[0038] The molded product was placed in a column through which a fluorine-containing liquid with a fluorine concentration of 65 ppm was circulated to adsorb fluorine ions. The fluorine ion concentration in the fluorine-containing liquid was measured at regular intervals.
[0039] [Comparative Example 1] A predetermined amount of powdered JIS special grade slaked lime was added while stirring to a beaker containing the same amount of fluorine-containing liquid with a fluorine concentration of 65 ppm as that circulated in Example 1, and then the mixture was held for a certain period of time while stirring.
[0040] [Comparative Example 2] The calcium hydroxide slurry was used as the raw material, poured into a PTFE beaker, and then dried together with the beaker. The molded body after drying was brittle, but could be removed without losing its shape by carefully removing it.
[0041] The above molded body was allowed to adsorb fluoride ions in the same manner as in Example 1. Figure 2 shows the change over time in the fluoride ion concentration in the fluoride-containing liquid measured in Example 1, Comparative Example 1, and Comparative Example 2. In Figure 2, the horizontal axis shows the elapsed time, and the vertical axis shows the fluoride concentration. In Figure 2, the case of powdered slaked lime in Comparative Example 1 is shown by "◯", the case of the molded body without CNF in Comparative Example 2 is shown by "△", and the case of the molded body with CNF in Example 1 is shown by "□".
[0042] As shown in Figure 2, in Example 1, the time for the F concentration to decrease is longer than in Comparative Example 1, but the F concentration eventually decreases to approximately the same level of 10 mg / L. In contrast, in Comparative Example 2, the F concentration does not decrease completely compared to Example 1.
[0043] [Example 2] Next, Example 2 will be described. In Example 2, calcium hydroxide slurry and CNF slurry were used as raw materials, which were mixed by stirring, and the mixed slurry was filled into 2 ml centrifuge tubes in an amount of 2 ml each, followed by centrifugation, removal of the supernatant, and drying the tubes at 60°C. After drying was completed, the calcium hydroxide remaining at the bottom of the tube and the CNF mixture were integrated, and a molded body similar to that in Example 1 was produced.
[0044] [Example 3] Next, we will explain Example 3. In Example 3, calcium hydroxide slurry and CNF slurry were used as raw materials, which were stirred and mixed to form a clay-like material, and then extruded from a die with a φ5 hole to form a cylindrical molded body, which was cut into 10 mm lengths and dried at 110°C.
[0045] [Example 4] Next, Example 4 will be described. In Example 4, calcium hydroxide slurry and CNF slurry were used as raw materials, and the slurry obtained by mixing and stirring them was passed through a filter equipped with a φ46 filter paper, and the resulting filtrate layer was dried together with the filter paper at 110°C. After drying, the hydrated lime and CNF were integrated on the filter paper, and a thin film layer with water permeability was formed.
[0046] [Example 5] Next, Example 5 will be described. In Example 5, calcium hydroxide slurry and CNF slurry were used as raw materials, and the slurry obtained by stirring and mixing them was repeatedly passed through a pulp mesh, and the thin film of the mixture of slaked lime and CNF formed on the mesh was dried at 110°C. This thin film had appropriate water permeability and could be used as filter paper, and it was also possible to cut it to an appropriate size, pack it into a column, and pass treated water through it.
[0047] (Comparison with conventional products) FIG. 3 shows a graph comparing the pH change after the powdered slaked lime of Comparative Example 1 was added to a fluorine-containing solution of pH 3.3, the pH change after the CNF / slaked lime composite molded in a beaker of Example 1 was added to a fluorine-containing solution of pH 3.3, the pH change after the CNF / slaked lime composite molded using centrifugal force of Example 2 was added to a fluorine-containing solution of pH 3.3, the pH change after the CNF / slaked lime composite molded by extrusion molding of Example 3 was added to a fluorine-containing solution of pH 3.3, the pH change when a fluorine-containing solution with an initial pH of 3.3 was circulated through a filter paper on which a CNF / slaked lime layer was formed of Example 4, and the pH change when a fluorine-containing solution with an initial pH of 3.3 was circulated through a CNF / slaked lime composite molded membrane prepared by papermaking of Example 5.
[0048] In Fig. 3, the vertical axis indicates the pH value, and the horizontal axis indicates the elapsed time. In Fig. 3, "◯" indicates Comparative Example 1, "△" indicates Example 1, "+" indicates Example 2, "=" indicates Example 3, "×" indicates Example 4, and "□" indicates Example 5.
[0049] The adsorption of fluorine by this material is according to the following chemical formula: Ca(OH)2+2HF→CaF2+2H2O This formula shows that the pH changes from acidic to neutral as the amount of fluorine in the liquid decreases, and the rate of change in pH is nothing other than the rate of fluorine reduction. Therefore, the fluorine adsorption rate can be correlated with the rate of pH change.
[0050] Therefore, the test results shown in FIG. 3 show that there is a difference in the fluorine adsorption rate depending on the production method of each CNF / slaked lime shown in the above Examples, and also show that ultimately, any production method can react with all of the HF in the liquid to neutralize the liquid, in other words, has the ability to sufficiently adsorb fluorine.
[0051] [Example 6] Next, Example 6 will be described. In Example 6, calcium hydroxide slurry and CNF slurry were used as raw materials, and water was further added to these to prepare a dilute slurry, which was then circulated by a liquid pump. A cylindrical filter made of polypropylene (PP) with a mesh size of 1 μm was inserted into the filter housing and placed midway along the circulation line so that the solid content in the dilute slurry could be filtered by the cylindrical filter.
[0052] Immediately after starting circulation, a considerable amount of solid matter passed through the cylindrical filter, but as the thickness of the filtered material on the filter increased, the amount passing through decreased, and by continuing circulation for a certain period of time, a calcium hydroxide / CNF composite layer of a certain thickness was able to be formed on the PP filtration filter.
[0053] After the circulation was completed, the liquid remaining in the filter housing was removed with compressed air, and the cylindrical filter was then removed from the filter housing and dried at 110° C. Even after drying, no peeling was observed in the calcium hydroxide / CNF composite layer on the PP filter, and the PP filter surface was coated with a constant thickness.
[0054] When the PP filter on which the calcium hydroxide / CNF composite layer was produced by the above method was inserted into a filter housing installed in a circulation line of a fluoride ion-containing liquid and allowed to adsorb fluorine, the fluoride ion concentration in the liquid decreased, similar to the molded bodies produced in Examples 1 and 2, and showed a fluoride concentration reduction rate equivalent to that of Comparative Example 1, as shown in Figure 4. Furthermore, no collapse or peeling was observed even after the reaction with fluorine, confirming that the calcium hydroxide / CNF composite layer produced by this method also functions as a fluoride adsorbent.
[0055] In Fig. 4, the horizontal axis indicates the elapsed time, and the vertical axis indicates the fluorine concentration. In Fig. 4, the powdered slaked lime of Comparative Example 1 is indicated by "◯", and the PP filter molded body of Example 6 is indicated by "□".
[0056] Example 7 Next, a description will be given of Example 7. In Example 7, a fluorine adsorbent prepared by the same method as in Example 1 was brought into contact with an aqueous solution containing fluorine ions in an amount twice the equivalent of calcium hydroxide contained in the fluorine adsorbent, to remove fluorine ions from the aqueous solution.
[0057] After the removal was completed, the fluorine adsorbent was taken out of the aqueous solution and dried at 110°C for 24 hours to remove moisture, and then calcined in an electric furnace at 400°C for 2 hours. Figure 5 shows the results of X-ray diffraction analysis of the fluorine adsorbent before and after calcination. As shown in FIG. 5, the diffraction peak of the calcined fluorine adsorbent (indicated by "A" in FIG. 5) completely coincides with the diffraction peak of CaF2 (multiple diffraction peaks indicated by "B" in FIG. 5), indicating that the product is calcium fluoride with high purity. In FIG. 5, the vertical axis indicates the X-ray diffraction intensity, and the horizontal axis indicates the energy of the X-ray spectrum. [Explanation of symbols]
[0058] 5... Molded body 10... CNF network 20... Alkaline earth metal salt.
Claims
1. A fluorine adsorbent characterized in that one or more inorganic powders made of alkaline earth metal salts are molded into any shape using cellulose nanofibers as a binder.
2. 2. The fluorine adsorbent according to claim 1, wherein the inorganic powder is one or more of a magnesium salt, a calcium salt, a strontium salt, and a barium salt.
3. 2. The fluorine adsorbent according to claim 1, wherein the inorganic powder is one or more of magnesium hydroxide, calcium hydroxide, calcium phosphate, and calcium carbonate.
4. A method for removing fluoride ions, comprising contacting water containing fluoride ions with the fluoride adsorbent according to any one of claims 1 to 3.
5. A method for recovering fluorine, comprising contacting water containing fluoride ions with the fluorine adsorbent according to any one of claims 1 to 3 to obtain reusable alkaline earth fluorides.
Citation Information
Patent Citations
JP1973054999A
Antenna device
JP1981037708A
Fluorine adsorbent and its manufacturing method
JP2005028312A
Method and apparatus for retreating chemical, and method for producing fluorite
JP2005097083A
Fluorine adsorbent and production method
JP2005342578A