Fluororesin modifier, modified fluororesin molded body, and manufacturing method thereof
A block copolymer-based fluororesin modifier addresses the limitations of existing methods by enhancing adhesion and functionality on fluororesins, overcoming shape and environmental challenges.
Patent Information
- Application Number
- JP2020120763
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-22
- Filing Date
- 2020-07-14
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2040-07-14
AI Technical Summary
Existing methods for modifying fluororesins, such as plasma treatment and chemical etching, face challenges in modifying complex shapes, safety concerns, and environmental issues due to the use of harmful compounds like PFOS and PFOA, limiting the design of monomers with fluorinated alkyl groups.
A fluororesin modifier containing a block copolymer with structural units derived from monomers having alkyl groups of 8 or more carbon atoms and polar groups, which is applied to form a functional layer on the fluororesin surface, enhancing adhesion and functionality without environmental hazards.
The modified fluororesin exhibits excellent adhesiveness to other materials and can be applied uniformly to complex shapes, including porous materials, while avoiding harmful compounds, thus expanding its applications.
Smart Images

Figure 0007555565000019 
Figure 0007555565000001 
Figure 0007555565000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a fluororesin modifier and a modified fluororesin molded article and a method for producing the same. [Background technology]
[0002] Fluororesins such as polytetrafluoroethylene (PTFE), a polymer of tetrafluoroethylene, are used in a variety of fields due to their excellent chemical stability, heat resistance, solvent resistance, weather resistance, electrical insulation, etc. However, there are issues such as the inactivity of the fluororesin surface and poor adhesion to other materials, and various modification methods are being investigated to expand the use of fluororesins.
[0003] As a method for modifying fluororesin, physical treatment such as plasma or laser, and a method combining this with chemical treatment are known. For example, Patent Document 1 discloses a surface modification method for a fluororesin molded product, which performs physical modification by injecting ions in the plasma into the molded product surface to roughen the surface and chemical modification by replacing fluorine atoms on the surface of the molded product with atoms other than fluorine atoms by applying a negative voltage to the surface of the fluororesin molded product when irradiating the surface of the fluororesin molded product with plasma, and further discloses a surface modification method for a fluororesin molded product, which includes a step (1) of introducing active sites into the molded product surface by irradiating the surface of the fluororesin molded product with plasma, a step (2) of graft polymerizing the monomer at the active sites on the molded product surface by irradiating the surface of the fluororesin molded product with plasma in an atmosphere gas that essentially contains a water-soluble monomer having an unsaturated bond, and a step (3) of removing the homopolymer derived from the monomer that has accumulated on the surface of the molded product after graft polymerization.
[0004] As a method for chemically modifying fluororesin, chemical etching treatment using agents such as metallic sodium-ammonia solution is also known.
[0005] Furthermore, in Patent Document 3, the present inventors have disclosed a method for modifying a fluororesin using a copolymer having a structural unit derived from a first monomer (A) and a structural unit derived from a second monomer (B), in which the monomer (A) is any monomer selected from the group consisting of (meth)acrylate, (meth)acrylamide, vinyl ether, vinyl ester, siloxane, α-olefin, and substituted styrene, having a fluorinated alkyl group represented by a specific structural formula at its side chain, and the monomer (B) is a monomer having a functional group. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2009-263529 A [Patent Document 2] JP 2009-13310 A [Patent Document 3] JP 2016-79389 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, the methods described in Patent Documents 1 and 2, in which active sites are introduced onto the surface of a fluororesin by plasma treatment and a chemical reaction is caused at these active sites, have problems such as only modifying the surface of the area irradiated with the plasma, making them unsuitable for modifying molded products with complex shapes.
[0008] Chemical etching using chemicals such as metallic sodium-ammonia solution has been problematic in terms of safety and environmental impact because it uses highly reactive metallic sodium.
[0009] The method disclosed in Patent Document 3 does not require the generation of radicals on the surface of the fluororesin by plasma treatment or the like in order to perform chemical modification, and can more easily modify the fluororesin surface. However, organic fluorine compounds such as perfluorooctanesulfonic acid (PFOS, CF3-(CF2)6-SO3H) and its salts, and perfluorooctanoic acid (PFOA, CF3-(CF2)6-COOH) are difficult to decompose and have a high tendency to accumulate, and in recent years, their impact on the environment has become a problem. For this reason, restrictions on the use of polymers having fluorinated alkyl groups in their side chains are also being considered. Specifically, in addition to perfluorooctanesulfonic acid and its salts, and perfluorooctanoic acid, polymers having fluorinated C8-16 side chains, etc., and polymers having a linear or branched perfluoroheptyl group ((C7F 15 Various regulations are being considered for substances that have the fluorinated alkyl group and can release PFOA upon decomposition. As a result, there are concerns that the design of monomers with fluorinated alkyl groups in the side chains may be restricted.
[0010] Under such circumstances, an object of the present invention is to provide a new fluororesin modifier that can be used to modify fluororesin. Another object of the present invention is to provide a modified fluororesin molded article imparted with various desired functionalities and a method for producing the same. [Means for solving the problem]
[0011] As a result of intensive research aimed at solving the above problems, the present inventors discovered that the following invention meets the above object, and thus completed the present invention.
[0012] That is, the present invention relates to the following inventions. <1> A fluororesin modifier comprising a block copolymer including a structural unit (A) derived from any one of monomers (A) selected from the group consisting of (meth)acrylate, (meth)acrylamide, vinyl ether, vinyl ester, siloxane, α-olefin and substituted styrene, the monomer having an alkyl group having 8 or more carbon atoms in the side chain, and a structural unit (B) derived from a monomer (B) having a polar group. <2> The structural unit (B) has at least one group selected from the group consisting of an amino group, a hydroxyl group, and an oxyalkylene group in a side chain. <1> Fluororesin modifier according to claim 1. <3> The block copolymer is a block copolymer solution containing the block copolymer and a solvent. <1> or <2> Fluororesin modifier according to claim 1. <4> A method for producing a modified fluororesin molded product, comprising a surface modification step of contacting a fluororesin modifier with a fluororesin molded product to form a functional layer containing the fluororesin modifier on at least a portion of the surface of the fluororesin molded product, wherein the fluororesin modifier contains a block copolymer comprising a structural unit (A) derived from a monomer (A) selected from the group consisting of (meth)acrylate, (meth)acrylamide, vinyl ether, vinyl ester, siloxane, α-olefin and substituted styrene, the monomer (A) having an alkyl group having 8 or more carbon atoms in its side chain, and a structural unit (B) derived from a monomer (B) having a polar group. <5> The fluororesin molded article is an extruded article. <4> A method for producing the modified fluororesin molded article according to claim 1. <6> The method further comprises a surface roughening step of roughening the surface of the fluororesin molded body prior to the surface modification step. <4> or <5> A method for producing the modified fluororesin molded article according to claim 1. <7> A modified fluororesin molded body having a fluororesin molded body and a functional layer containing a block copolymer formed on at least a portion of the surface of the fluororesin molded body, wherein the block copolymer is a block copolymer containing a structural unit (A) derived from any monomer (A) selected from the group consisting of (meth)acrylate, (meth)acrylamide, vinyl ether, vinyl ester, siloxane, α-olefin and substituted styrene, the monomer having an alkyl group having 8 or more carbon atoms in its side chain, and a structural unit (B) derived from a monomer (B) having a polar group. Effect of the Invention
[0013] According to the present invention, a new fluororesin modifier that can be used to modify a fluororesin molded article is provided. Also, according to the present invention, a modified fluororesin molded article to which various desired functionalities are imparted and a method for producing the same are provided. For example, according to the present invention, a modified fluororesin molded article having excellent adhesion to other materials and a method for producing the same are provided. [Brief description of the drawings]
[0014] [Figure 1] (a) shows an SEM image of the surface of an unstretched PTFE film, and (b) shows an SEM image of the surface of an expanded PTFE film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The following is a detailed description of the embodiments of the present invention, but the following description of the constituent elements is one example (representative example) of the embodiment of the present invention, and the present invention is not limited to the following content as long as the gist of the present invention is not changed. Note that in this specification, when the expression "~" is used, it is used as an expression including the numerical value or physical property value before and after it.
[0016] <Fluororesin modifier> The present invention relates to a fluororesin modifier (hereinafter sometimes referred to as the "fluororesin modifier of the present invention") containing a block copolymer comprising a structural unit (A) derived from any monomer (A) selected from the group consisting of (meth)acrylate, (meth)acrylamide, vinyl ether, vinyl ester, siloxane, α-olefin, and substituted styrene, the monomer having an alkyl group having 8 or more carbon atoms in its side chain, and a structural unit (B) derived from a monomer (B) having a polar group.
[0017] As described above, fluororesin has poor adhesion to other materials, and therefore, in general, modifiers for chemically modifying fluororesin are ones that introduce reactive functional groups capable of undergoing radical reaction with fluororesin, or ones that introduce functional groups with the same structure as fluororesin, such as fluorinated alkyl groups. Meanwhile, the present inventors have surprisingly found that a block copolymer containing a structural unit (A) derived from a monomer (A) having an alkyl group with 8 or more carbon atoms in its side chain, which is a structure different from that of a fluororesin, and a structural unit (B) derived from a monomer (B) having a polar group, can be adhered to the surface of a fluororesin. Furthermore, they have found that the use of such a block copolymer can impart functionality derived from the structural unit (B) to the fluororesin, and in particular, can modify the fluororesin to have excellent adhesion to other materials. As described above, there is concern that the polymer having a long-chain fluorinated alkyl group has a structure that can be used from an environmental perspective, but the block copolymer used in the present invention has a low environmental load, a high degree of freedom in design, and can be easily modified in design depending on the structure of the fluororesin to be modified.
[0018] [Block copolymer] The block copolymer contained in the fluororesin modifier of the present invention is a block copolymer containing a structural unit (A) derived from any one monomer (A) selected from the group consisting of (meth)acrylate, (meth)acrylamide, vinyl ether, vinyl ester, siloxane, α-olefin, and substituted styrene, which has an alkyl group having 8 or more carbon atoms in its side chain, and a structural unit (B) derived from a monomer (B) having a polar group. The block copolymer may be composed of the structural unit (A) and the structural unit (B), and may further contain other structural units as long as the object of the present invention is not impaired. The block copolymer is preferably composed substantially of the structural unit (A) and the structural unit (B), and the total content of the structural unit (A) and the structural unit (B) in the block copolymer may be 95% by mass or more, 98% by mass or more, etc.
[0019] Unit The structural unit (A) is derived from any monomer (A) having an alkyl group having 8 or more carbon atoms and selected from the group consisting of (meth)acrylate, (meth)acrylamide, vinyl ether, vinyl ester, siloxane, α-olefin, and substituted styrene. The structural unit (A) has an alkyl group having 8 or more carbon atoms, which serves as a site that exhibits side chain crystallinity. It is presumed that the interaction between this site that exhibits side chain crystallinity and the fluororesin causes the block copolymer to adhere firmly to the fluororesin.
[0020] In the present application, "(meth)acrylate" refers to both acrylate and methacrylate. Similarly, "(meth)acrylamide" refers to both acrylamide and methacrylamide.
[0021] In the structural unit (A), the alkyl group having a side chain length of 8 or more carbon atoms is bonded directly to the main chain of the structural unit (A) or via a linking group (ester bond, amide bond, ether bond, benzene ring, etc.).
[0022] In the structural unit (A), an alkyl group having a length of 8 or more carbon atoms in the side chain can bond the fluororesin and the block copolymer more firmly, so that an alkyl group having 12 or more carbon atoms is preferable, and an alkyl group having 16 or more carbon atoms is more preferable. In addition, the alkyl group is preferably a linear alkyl group. On the other hand, the upper limit can be appropriately set within a range in which the adhesion between the block copolymer and the fluororesin can be maintained, taking into consideration dispersibility in a solvent, etc. As a specific upper limit, in reality, the number of carbon atoms is preferably 50 or less, the number of carbon atoms is more preferably 40 or less, and the number of carbon atoms is further preferably 30 or less. In addition, the number of carbon atoms may be 28 or less or 25 or less. If the number of carbon atoms in the alkyl group is too large, the block copolymer cannot have a proper three-dimensional structure, and the adhesion of the block copolymer to the fluororesin decreases, or the dispersibility in the solvent decreases. In addition, it may be difficult to set the polymerization conditions for producing the block copolymer.
[0023] Specifically, examples of the alkyl group having 8 or more carbon atoms in the side chain contained in the structural unit (A) include a decyl group, a dodecyl group, a tridecyl group, a tetradecyl group, a hexadecyl group, an octadecyl group (stearyl group), and a docosyl group (behenyl group).
[0024] The degree of polymerization of the structural unit (A) is 2 or more. The degree of polymerization of the structural unit (A) may be appropriately selected within a range in which adhesion to the fluororesin can be maintained depending on the structures of the monomers (A) and (B), etc. In order to improve adhesion to the fluororesin, the degree of polymerization of the structural unit (A) is preferably 7 or more, and may be 8 or more or 10 or more. In addition, the degree of polymerization of the structural unit (A) is preferably 1,000 or less, and may be 800 or less, 500 or less, 300 or less, 100 or less, 50 or less, 30 or less, or 20 or less.
[0025] In the block copolymer, the molecular weight (g / mol) corresponding to the structural unit (A) is preferably 3,000 or more. By having the molecular weight corresponding to the structural unit (A) of 3,000 or more, it is possible to more firmly adhere to the fluororesin. The molecular weight corresponding to the structural unit (A) may be 4,000 or more or 5,000 or more. It may also be 20,000 or less, 15,000 or less, 10,000 or less, or 8,000 or less.
[0026] These molecular weights are the values (Mw: weight average molecular weight) that can be calculated in terms of polystyrene from the results obtained by GPC. In addition, the modifying copolymer may be difficult to dissolve in a solvent, making it difficult to measure the molecular weight. In such cases, the molecular weights of each can be calculated by methods such as elemental analysis, IR, and NMR.
[0027] The structural unit (A) is preferably a structural unit derived from a (meth)acrylate or α-olefin monomer having an alkyl group with a length of 8 or more carbon atoms in the side chain. More specifically, the structural unit (A) is preferably any one of those represented by the following general formula (A-1) or (A-2).
[0028] [ka]
[0029] In the general formulas (A-1) and (A-2), R a1represents a hydrogen atom or a methyl group.
[0030] In the general formulas (A-1) and (A-2), R a2 represents an alkyl group having 8 or more carbon atoms. a2 is preferably a linear alkyl group. a2 The number of carbon atoms in the alkyl group represented by the formula (I) is preferably 12 or more, and more preferably 16 or more. The upper limit can be 50 or less, 40 or less, 30 or less, 28 or less, or 25 or less, for example.
[0031] In general formulas (A-1) and (A-2), m is an integer of 2 or more. m is preferably 7 or more, more preferably 8 or more, or 10 or more. m is preferably 1,000 or less, and may be 800 or less, 500 or less, 300 or less, 100 or less, 50 or less, 30 or less, or 20 or less.
[0032] From the viewpoints of ease of obtaining the monomers that are the raw materials for the block copolymer, ease of control of the polymerization conditions, ease of interaction between alkyl groups having 8 or more carbon atoms, etc., it is more preferable that the structural unit (A) is represented by general formula (A-1).
[0033] [Block] The structural unit (B) is derived from a monomer (B) having a polar group. The structural unit (A) exerts a function of adhering to the fluororesin, whereas the structural unit (B) imparts its functionality to the fluororesin and has a function of modifying the fluororesin. For example, the structural unit (B) contributes to improving the adhesion to other materials.
[0034] A polar group is a polar atomic group, and when present in a polymer using a monomer having the group, it forms a structure that exhibits polarity within the polymer. When a polar group is present in a polymer after polymerization, the polarity imparted to the surface of the fluororesin can be used to modify the fluororesin into one that has excellent adhesion to other materials.
[0035] The polar group may be present in the main chain structure of the structural unit (B) or in a side chain thereof. Furthermore, the structural unit (B) may have two or more polar groups. The polarity derived from the polar group of the structural unit (B) is easily expressed on the surface of the modified fluororesin, and the modification effect is large, so the structural unit (B) preferably has a polar group on its side chain. When the side chain has a polar group, the main chain has little effect on the modification of the fluororesin, so the structure of the main chain is not particularly limited. In addition, the polar group of the side chain can be directly bonded to the main chain of the structural unit (B) or bonded via a linking group (ester bond, amide bond, ether bond, benzene ring, etc.). For example, the structural unit (B) can be a structural unit derived from any monomer selected from the group consisting of (meth)acrylate, (meth)acrylamide, vinyl ether, vinyl ester, siloxane, α-olefin, and substituted styrene, which has a polar group on the side chain.
[0036] Representative polar groups include an amino group, an ammonium group, a carboxyl group, a hydroxyl group, a sulfonic acid group, an alkoxy group, an oxyalkylene group, a carbonyl group, an ether group, a sulfonyl group, an ester group, and an amide group.
[0037] The structural unit (B) preferably has any one selected from the group consisting of an amino group, a hydroxyl group, and an oxyalkylene group. More preferably, the monomer (B) constituting the structural unit (B) is a monomer having any one selected from the group consisting of an amino group, a hydroxyl group, and an oxyalkylene group in its side chain.
[0038] Here, the amino group may be unsubstituted or may have a substituent. The amino group is represented by the general formula "-NR y3 R y4 (However, R y3 and R y4 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms). Examples of such an amino group include -NH2, -N(CH3)2, -N(C2H5)2, and -NH(tert-C4H9).
[0039] Substituents for the amino group include alkyl groups and carboxyalkyl groups.
[0040] In addition, the oxyalkylene group is "-(C p H 2p It is a divalent group represented by the formula (X) (p is an integer of 1 or more). When the monomer (B) has an oxyalkylene group, it is preferably a monomer having a group represented by the following formula (X).
[0041] -(C p H 2p -O) q -R x1 ...Formula (X) (In formula (X), p is an integer of 1 to 10, q is an integer of 1 to 10, R x1 represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms.
[0042] More preferably, in the general formula (X), p is an integer of 1 to 5, q is an integer of 2 to 10, and R x1 is a hydrogen atom or an alkyl group having 1 to 5 carbon atoms. More preferably, p is an integer of 1 to 2, q is an integer of 2 to 10, and R x1 is a hydrogen atom or an alkyl group having 1 to 2 carbon atoms.
[0043] The degree of polymerization of the structural unit (B) is an integer of 2 or more. The degree of polymerization of the structural unit (B) is appropriately determined depending on the structures of the monomer (A) and the monomer (B). The degree of polymerization of the structural unit (B) is preferably 2 to 1,000. In order to exert a more stable modifying effect, it is more preferably 5 or more, or 10 or more. It may also be 20 or more, 30 or more, or 40 or more. The degree of polymerization of the structural unit (B) may also be 800 or less, 500 or less, 300 or less, 100 or less, or 60 or less.
[0044] In the block copolymer, the molecular weight (g / mol) corresponding to the structural unit (B) is preferably 500 or more. By having the molecular weight corresponding to the structural unit (B) of 500 or more, it is possible to obtain a copolymer with even better adhesion to other materials. The molecular weight corresponding to the structural unit (B) is preferably 1,000 or more, more preferably 5,000 or more, and even more preferably 10,000 or more. It may also be 20,000 or less, 15,000 or less, or 12,000 or less.
[0045] The structural unit (B) can have, for example, a structure represented by any one of the following general formulas (B-1) to (B-4).
[0046] [ka]
[0047] In general formulae (B-1) to (B-4), R b1 represents a hydrogen atom or a methyl group.
[0048] In general formulae (B-1) to (B-4), R L represents a single bond or an alkylene group, and is preferably a single bond or an alkylene group having 1 to 4 carbon atoms.
[0049] The alkylene group may be unsubstituted or may have a substituent. Examples of the alkylene group having a substituent include an alkylene group substituted with a hydroxy group or a hydroxyalkyl group.
[0050] In general formulae (B-1) to (B-4), R b2 represents any one selected from the group consisting of a hydrogen atom, an alkyl group, an amino group, an ammonium group, a carboxyl group, a hydroxyl group, a sulfonic acid group, an alkoxy group, and a group represented by the above general formula (X). R b2is preferably any one selected from the group consisting of a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, an amino group, and a group represented by the above general formula (X), more preferably any one selected from the group consisting of a hydrogen atom, an amino group, and a group represented by the above general formula (X), and even more preferably an amino group. The preferred embodiments of the amino group and the group represented by the general formula (X) are as described above.
[0051] In general formula (B-2), R b3 represents a hydrogen atom or an alkyl group, preferably a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, and more preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms.
[0052] In the general formulas (B-1) to (B-4), n is an integer of 2 or more. n is preferably 8 or more, and may be 10 or more, 20 or more, 30 or more, or 40 or more. Moreover, n is preferably 1,000 or less, and may be 800 or less, 500 or less, 300 or less, 100 or less, or 60 or less.
[0053] Moreover, the structural unit (B) can have a structure represented by any of the following general formulas (B-5) to (B-7).
[0054] [ka]
[0055] In general formulae (B-5) to (B-7), R b4 represents a hydrogen atom or a methyl group.
[0056] In general formulae (B-5) to (B-7), R L represents a single bond or an alkylene group, and is preferably a single bond or an alkylene group having 1 to 4 carbon atoms.
[0057] The alkylene group may be unsubstituted or may have a substituent. Examples of the alkylene group having a substituent include an alkylene group substituted with a hydroxy group or a hydroxyalkyl group.
[0058] In general formulae (B-5) to (B-7), R b5 represents any one selected from the group consisting of an amino group, an ammonium group, a carboxyl group, a hydroxyl group, a sulfonic acid group, an alkoxy group, and a group represented by general formula (X). R b5 is preferably an amino group or a group represented by the above general formula (X), and more preferably an amino group. The preferred embodiments of the amino group and the group represented by the general formula (X) are as described above.
[0059] In the general formulas (B-5) to (B-7), n is an integer of 2 or more. n may be 5 or more, 10 or more, 20 or more, 30 or more, or 40 or more. Moreover, n is preferably 1,000 or less, and may be 800 or less, 500 or less, 300 or less, 100 or less, or 60 or less.
[0060] The structural unit (B) is preferably one represented by general formula (B-1) from the viewpoints of ease of availability of the raw material monomers and ease of control of the polymerization conditions.
[0061] More specific examples of suitable structural units (B) include those represented by the general formula (B-1): b1 is a hydrogen atom or a methyl group, and R L is an alkylene group, and R b2 is an amino group. b1 is a hydrogen atom or a methyl group, and R L is a single bond, and R b2 is a group represented by general formula (X). In addition, the structural unit derived from (meth)acrylic acid (in general formula (B-1), R b1 is hydrogen or a methyl group, and R L is a single bond, and R b2 is a hydrogen atom).
[0062] A preferred block copolymer is a copolymer containing a structural unit (A) represented by general formula (A-1) and a structural unit (B) represented by general formula (B-1). By using such a block copolymer, the structural unit (A) and the fluororesin are firmly bonded to each other, and the function of the structural unit (B) can be easily and strongly expressed.
[0063] The polymerization method for the block copolymer is not particularly limited, and the polymerization can be performed by known techniques such as various living polymerization methods (radical, anionic, cationic). As the living radical polymerization method, the NMP method, the ATRP method, the RAFT method, etc. can be used.
[0064] For example, a monomer (A) mixed solution preparation step is performed in which the monomer (A) mixed solution is prepared by mixing the monomer (A) with an initiator in a polymerization solvent. Next, the monomer (A) mixed solution prepared in this mixed solution preparation step is subjected to a monomer (A) polymerization step based on the polymerization mechanism of the initiator, such as living radical polymerization, under a nitrogen atmosphere or the like while being appropriately stirred in a reactor at an appropriate polymerization temperature (for example, about 90 to 120°C), to obtain a monomer (A) block polymer. Furthermore, a monomer (B) polymerization step is performed in which the monomer (B) is mixed into the solution in which the monomer (A) block polymer is mixed, and the monomer (B) is further polymerized by radicals or the like in the solution. This makes it possible to obtain a block copolymer having a monomer (A)-derived block and a monomer (B)-derived block. The order in which the monomer (A) and the monomer (B) are polymerized can be changed depending on the type and molecular weight of the monomers to be polymerized, the polymerization conditions for each, and the like.
[0065] When the other structural unit is contained, it may be polymerized with the monomer (A) and the monomer (B) as a third monomer.
[0066] More specific examples of the monomer (A) include dodecyl acrylate (lauryl acrylate), dodecyl methacrylate (lauryl methacrylate), octadecyl acrylate (stearyl acrylate), octadecyl methacrylate (stearyl methacrylate), docosyl acrylate (behenyl acrylate), docosyl methacrylate (behenyl methacrylate), and the like.
[0067] Specific examples of the monomer (B) include monomers having an amino group, such as 2-(dimethylamino) ethyl methacrylate (DMAEMA), 2-(dimethylamino) ethyl acrylate (DMAEA), 2-(diethylamino) ethyl methacrylate (DEAEMA), 2-(diethylamino) ethyl acrylate (DEAEA), 2-(tert-butylamino) ethyl methacrylate (TBAEMA), N,N-dimethylacrylamide (DMAA), N,N-dimethylaminopropyl acrylamide (DMAPAA), and N,N-diethylacrylamide (DEAA).
[0068] As the monomer (B), methoxy-polyethylene glycol-acrylate (CH2=CH(CO)O(CH2-CH2-O-) q CH3) (q=2-9), ethoxy-polyethylene glycol-acrylate (CH2=CH(CO)O(CH2-CH2-O-) q C2H5) (q=2-9), polyethylene glycol monoacrylate (CH2=CH(CO)O(CH2-CH2-O-) qExamples of monomers having an oxyalkylene group include di(ethylene glycol) ethyl ether acrylate (CH2=CH(CO)O(CH2-CH2-O-)2C2H5, Diethylen Glycol Monoethyl Ether Acrylate, DEEA) and deca(ethylene glycol) ethyl ether acrylate (CH2=CH(CO)O(CH2-CH2-O-) 10 C2H5) and other monomers. Also included are (meth)acrylic acid and the like.
[0069] In addition, a precursor polymer can be synthesized by polymerizing monomer (A) with monomer (B) having a reactive group such as an oxiranyl group on its side chain, and then reacting it with an amino group or the like to obtain a block copolymer.
[0070] Specifically, as described above, the monomer (A) is mixed with an initiator in a polymerization solvent, and the monomer (A) polymerization step based on the polymerization mechanism of the initiator, such as living radical polymerization, is carried out in a reactor at an appropriate polymerization temperature (for example, about 90 to 120°C) under a nitrogen atmosphere while being appropriately stirred, to obtain a monomer (A) block polymer. The solution in which the monomer (A) block polymer is mixed is mixed with a monomer (B) having an oxiranyl group (for example, any monomer selected from the group consisting of (meth)acrylate, (meth)acrylamide, vinyl ether, vinyl ester, siloxane, α-olefin, and substituted styrene having an oxiranyl group), and the monomer (B) polymerization step is carried out to further polymerize the monomer (B) by radicals in the solution. This results in a solution in which a precursor polymer having a block derived from the monomer (A) and a block derived from the monomer (B) is mixed. Next, when this precursor polymer is reacted with iminodiacetic acid, the oxiranyl group reacts with the iminodiacetic acid to obtain a block copolymer having an amine structure derived from iminodiacetic acid (a structure having a carboxyalkyl group-substituted amino group in the side chain).
[0071] Examples of the monomer (B) capable of introducing an amino group or the like into the side chain after polymerization include glycidyl acrylate and glycidyl methacrylate.
[0072] [Block copolymer solution] The fluororesin modifier of the present invention may contain other components other than the block copolymer. For example, the fluororesin modifier of the present invention may be a block copolymer solution containing a block copolymer and a solvent. By preparing a block copolymer solution containing a block copolymer and a solvent, it is easy to impart desired properties such as adhesiveness to a desired range of the fluororesin molded article by adjusting the viscosity and concentration to any desired value.
[0073] In the present application, the concept of a block copolymer solution includes not only a homogeneous solution in which the block copolymer is completely dissolved in a solvent, but also a suspension or dispersion. Depending on the structure of the block copolymer, it may be difficult to completely dissolve the block copolymer in a solvent, so the block copolymer may be suspended or dispersed in a solvent in the form of a suspension or dispersion.
[0074] (solvent) In the fluororesin modifier containing a block copolymer and a solvent, the solvent is not particularly limited and examples thereof include toluene, xylene, hexane, butyl acetate, acetonitrile, ethanol, dimethyl sulfoxide, tetrahydrofuran, etc. The solvent may be a single solvent consisting of only one type of solvent, or a mixed solvent consisting of two or more types of solvents. Preferably, the solvent contains one or more selected from the group consisting of toluene, butyl acetate, xylene, and tetrahydrofuran. When the fluororesin modifier contains a mixed solvent, it is preferable that the main solvent is one or more selected from the group consisting of toluene, butyl acetate, xylene, and tetrahydrofuran. Specifically, any one selected from the group consisting of toluene, butyl acetate, xylene, and tetrahydrofuran occupies preferably 50% by volume or more of the total volume of the solvent, and may occupy 70% by volume or more, 90% by volume or more, or 95% by volume or more.
[0075] (concentration) In the fluororesin modifier containing a block copolymer and a solvent, the concentration of the block copolymer in the fluororesin modifier can be appropriately set according to the type of block copolymer, the method of using the fluororesin modifier, etc. The concentration of the block copolymer in the fluororesin modifier is preferably 0.01 to 2.0% by mass. The lower limit of the concentration of the block copolymer is preferably 0.02% by mass or more, more preferably 0.05% by mass or more. If the concentration of the block copolymer is too low, the modifying effect on the fluororesin may be insufficient. The upper limit of the concentration of the block copolymer is preferably 1.5% by mass or less, more preferably 1.0% by mass or less. It can also be 0.8% by mass or less, 0.6% by mass or less, or 0.5% by mass or less. Even if the concentration of the block copolymer is increased, the modifying effect on the fluororesin may be saturated. In addition, if the concentration of the block copolymer is too high, micellization due to self-assembly of the block copolymer itself may occur, and the block copolymer may not function sufficiently as a modifier for the fluororesin.
[0076] By using the fluororesin modifier of the present invention, it is possible to modify a fluororesin molded article to have various desired functionalities (for example, excellent adhesion). That is, the present invention can also be a method for modifying a fluororesin molded article, which includes a surface modification step of contacting the fluororesin molded article with a fluororesin modifier to form a functional layer containing the fluororesin modifier on at least a part of the surface of the fluororesin molded article, and the fluororesin modifier contains a block copolymer containing a constituent unit (A) derived from any monomer (A) selected from the group consisting of (meth)acrylate, (meth)acrylamide, vinyl ether, vinyl ester, siloxane, α-olefin, and substituted styrene, which has an alkyl group having 8 or more carbon atoms in the side chain, and a constituent unit (B) derived from a monomer (B) having a polar group. By utilizing the method for modifying a fluororesin molded article of the present invention, it is possible to produce a modified fluororesin molded article described below.
[0077] <Method for producing modified fluororesin molded product> The present invention relates to a method for producing a modified fluororesin molded product (hereinafter, sometimes referred to as the "method for producing the modified fluororesin molded product of the present invention"), which comprises a surface modification step of contacting the fluororesin modifier of the present invention with a fluororesin molded product and forming a functional layer containing the fluororesin modifier on at least a portion of the surface of the fluororesin molded product. The method for producing a modified fluororesin molded article of the present invention is a method for obtaining a modified fluororesin molded article by modifying a fluororesin molded article with the above-mentioned fluororesin modifier of the present invention. By producing a modified fluororesin molded article using such a production method, it is possible to easily obtain a modified fluororesin molded article having various desired functionalities imparted to desired portions, regardless of the shape, etc. of the fluororesin molded article. In particular, by using such a production method, it is possible to easily obtain a modified fluororesin molded article having excellent adhesion to other materials.
[0078] The method for producing a fluororesin molded article of the present invention allows even molded articles having complex shapes to be treated uniformly with the fluororesin modifier by adjusting the viscosity, etc., of the fluororesin modifier of the present invention, making it possible to modify the article regardless of its shape. Furthermore, physical techniques such as plasma treatment may damage the fluororesin molded article and reduce its mechanical strength depending on its shape, such as a thin film. The method for producing a modified fluororesin molded article of the present invention is a chemical technique, and it is possible to modify molded articles that are susceptible to damage or loss of mechanical strength caused by physical techniques while suppressing damage to the molded article or loss of mechanical strength. Furthermore, while it has been difficult to modify the interior of a porous material using conventional modification methods such as plasma treatment, the method for producing a modified fluororesin molded product of the present invention makes it possible to easily modify the entire porous material by penetrating the fluororesin modifier into the interior, such as the pores, of the molded product.
[0079] [Fluororesin molded body] The fluororesin molded article used in the manufacturing method of the modified fluororesin molded article of the present invention is obtained by molding a fluororesin into an arbitrary shape according to the application. The fluororesin is not particularly limited, and a homopolymer of a monomer containing fluorine or a copolymer with another monomer can be used. Specific examples include polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride (THV), polyvinylidene fluoride (PVDF), polychlorotrifluoroethylene (PCTFE), chlorotrifluoroethylene-ethylene (ECTFE), tetrafluoroethylene-ethylene (ETFE), tetrafluoroethylene-hexafluoropropylene (FEP), and tetrafluoroethylene-perfluoroalkyl vinyl ether (PFA).
[0080] Among them, the fluororesin molded article is preferably a molded article containing polytetrafluoroethylene, which is obtained by processing a polytetrafluoroethylene homopolymer, copolymer, or mixture with other resin into any desired shape.
[0081] The shape of the fluororesin molded article is not particularly limited, and examples thereof include molded articles such as sheets, films, particles, plates, porous materials, and various members.
[0082] Also, a stretched product such as a stretched sheet or film may be used. In particular, polytetrafluoroethylene is preferred because it can be made porous by stretching, and the block copolymers interact more strongly with each other, resulting in a higher modification effect. The stretching method is not particularly limited, and may be any method such as longitudinal uniaxial stretching, transverse uniaxial stretching, sequential biaxial stretching, simultaneous biaxial stretching, multiaxial stretching, etc., but biaxial stretching such as sequential biaxial stretching and simultaneous biaxial stretching is preferred. For stretching, a roll stretching machine, a tenter stretching machine, a tubular stretching machine, a tensile tester, etc. can be used depending on the stretching method. The stretching ratio is not particularly limited, but may be, for example, 1.05 to 10 times and 2 to 5 times in the longitudinal and transverse directions, respectively.
[0083] [Surface modification process] The surface modification step is a step of contacting the fluororesin modifier of the present invention with a fluororesin molded article to form a functional layer containing the fluororesin modifier on at least a portion of the surface of the fluororesin molded article.
[0084] The fluororesin modifier of the present invention used in the method for producing the modified fluororesin molded body of the present invention is as described above, and may be a block copolymer or may contain components other than the block copolymer, such as a block copolymer solution containing a block copolymer and a solvent. From the viewpoint of the modification effect of the obtained modified fluororesin molded body, it is preferable to use a block copolymer solution containing a block copolymer and a solvent as the fluororesin modifier of the present invention. By making it a block copolymer solution, it is easy to adjust the viscosity to an arbitrary value, and it is possible to contact the fluororesin molded body more uniformly. This makes it possible to impart functionality more uniformly to the desired part of the obtained modified fluororesin molded body, and the functionality imparted is likely to be improved overall. For example, it is easy to improve the adhesion to other materials more uniformly and overall at the desired part of the obtained modified fluororesin molded body. Furthermore, since the degree of freedom of the block copolymer when contacting with the fluororesin molded body is improved, the block copolymer is likely to have a structure that easily interacts with the fluororesin molded body, and the block copolymer and the fluororesin molded body can act more firmly. In addition, since the structural unit (B) of the block copolymer is easily present on the outermost surface of the fluororesin molded article, the functionality (e.g., adhesion to other materials) imparted to the surface of the modified fluororesin molded article is more excellent, and the thickness of the functional layer formed on the fluororesin molded article is also easily controlled.
[0085] The method of contacting the fluororesin modifier of the present invention with a fluororesin molded article is not particularly limited as long as it is possible to form a functional layer containing the fluororesin modifier of the present invention on at least a part of the surface of the fluororesin molded article. Examples of the contact method include immersion such as dip coating, coating (applying) such as spin coating, applicator application, slit coating, die coating, bar coating, screen printing, inkjet printing, and gravure printing, and spraying such as spray coating.
[0086] The contact of the copolymer solution with the fluororesin molded article may be by any method that can bring the copolymer solution into contact with the portion of the fluororesin molded article to be modified, and may be appropriately selected depending on the shape of the fluororesin molded article, the area to be modified, etc.
[0087] In the surface modification step, the treatment temperature when the fluororesin modifier is brought into contact with the fluororesin molded product may be appropriately determined depending on the contact method, the composition of the fluororesin modifier, the type of fluororesin molded product, etc. The treatment temperature may be room temperature, or may be higher than room temperature, taking safety and other factors into consideration. For example, the treatment temperature may be 20°C or higher or 25°C or higher. If the treatment temperature is too high, the fluororesin molded product may be deformed or decomposed, so the upper limit may be 200°C or lower or 150°C or lower.
[0088] When the treatment temperature is set to a temperature higher than room temperature, the fluororesin modifier and the fluororesin molded product may be heated to a preset temperature depending on the contacting method, etc., and then the fluororesin modifier and the fluororesin molded product may be contacted with each other, or the fluororesin modifier and the fluororesin molded product may be contacted with each other and then the temperature may be raised to the set temperature.
[0089] When the contact method is immersion, the treatment time for contacting the fluororesin modifier with the fluororesin molded product can be appropriately determined depending on the composition of the fluororesin modifier, the type of the fluororesin molded product, etc. For example, when the treatment is performed in a state where the reactivity of the fluororesin modifier or the fluororesin molded product is increased by increasing the treatment temperature, the treatment time may be relatively short, such as 1 second or more or 30 seconds or more. In addition, in order to sufficiently form a functional layer, the treatment time may be 1 minute or more or 5 minutes or more. As long as the deformation of the fluororesin molded product does not occur, the treatment time may be long, and may be 60 minutes or less or 40 minutes or less. In addition, since the modification effect is saturated when the contact time is longer than a certain time, the treatment time may be 30 minutes or less or 20 minutes or less depending on conditions such as the treatment temperature.
[0090] When the contact method is coating or spraying, the amount of the fluororesin modifier applied is not particularly limited as long as it is an amount that can be uniformly applied to the part of the fluororesin molded article to be modified. For example, the amount of application is 10 to 300 g / m 2 50~250g / m 2 , 100~250g / m 2 etc.
[0091] In the method for producing a modified fluororesin molded article of the present invention, when a surface modification step is carried out using a block copolymer solution as a fluororesin modifier, a solvent removal step for removing the solvent is usually carried out after the surface modification step to form a functional layer. The method for removing the solvent may be drying at about room temperature in a well-ventilated environment, drying under reduced pressure, drying by heating, etc. Also, these drying methods may be used in combination.
[0092] Furthermore, the method for producing a fluororesin molded article of the present invention may include a step of roughening the surface of the fluororesin molded article prior to the surface modification step, depending on the shape of the fluororesin molded article, to the extent that the mechanical strength of the fluororesin molded article is not significantly impaired.
[0093] [Surface roughening process] The surface roughening step is a step carried out before the surface modification step, and is a step for roughening the surface of the fluororesin molded article. The method for roughening the surface is not particularly limited, and any conventional method such as filing, blasting, or etching can be used.
[0094] Moreover, if the surface of the fluororesin molded article is roughened too much in the roughening step, the mechanical properties of the resulting modified fluororesin molded article may be impaired and the modification effect may become uneven. Therefore, the degree of roughening may be appropriately determined in consideration of the mechanical properties and purpose of the resulting fluororesin molded article depending on the roughening method and the shape of the fluororesin molded article. For example, in the surface roughening step, the surface of the fluororesin molded article can be roughened so that the surface roughness in maximum height (Rz) is 80 μm or less or 60 μm or less. The lower limit of the surface roughness in maximum height (Rz) of the fluororesin molded article can be 10 μm or more or 20 μm or more. The surface of the fluororesin molded article can be roughened to have an arithmetic mean roughness (Ra) of 15 μm or less, 10 μm or less, or 8 μm or less. The lower limit of the arithmetic mean roughness (Ra) of the surface of the fluororesin molded article can be 1 μm or more, or 3 μm or more. The maximum height roughness (Rz) and arithmetic mean roughness (Ra) of the surface are surface roughness defined in JIS B 0633 (2001).
[0095] <Modified fluororesin molded body> The present invention also relates to a modified fluororesin molded product having a fluororesin molded product and a functional layer containing a block copolymer formed on at least a part of the surface of the fluororesin molded product, wherein the block copolymer is a block copolymer containing structural unit (A) derived from any monomer (A) selected from the group consisting of (meth)acrylate, (meth)acrylamide, vinyl ether, vinyl ester, siloxane, α-olefin and substituted styrene, the monomer having an alkyl group having 8 or more carbon atoms in its side chain, and structural unit (B) derived from monomer (B) having a polar group (hereinafter sometimes referred to as the "modified fluororesin molded product of the present invention").
[0096] By forming such a modified fluororesin molded article, it is possible to obtain a molded article having various functionalities due to the polar groups of the structural unit (B), and in particular, excellent adhesion to other materials.
[0097] The modified fluororesin molded article of the present invention can be suitably produced by the method for producing the modified fluororesin molded article of the present invention, and the block copolymer contained in the functional layer of the modified fluororesin molded article of the present invention has the same structure as the block copolymer contained in the fluororesin modifier of the present invention. The preferred embodiments of the block copolymer are also the same as those described above. The formation of a functional layer on the surface of a fluororesin molded article can be confirmed by methods such as component analysis of each layer using FT-IR or component analysis of a cut section.
[0098] In addition, the modified fluororesin molded article may have a structure having a functional layer containing a block copolymer on at least a part of the surface thereof, and the functional layer may be formed in a desired area of the fluororesin molded article depending on the purpose. For example, the entire surface layer of the sheet-like or particulate molded article may have a functional layer, or the surface layer may have a functional layer in a spotted or striped pattern. In addition, the modified fluororesin molded article may have a functional layer in the pores of a porous membrane or the like.
[0099] The functional layer may be a layer made of a block copolymer, or may contain other components different from the block copolymer. In order to improve the adhesion of the modified fluororesin molded article to other members, it is preferable that the functional layer contains a block copolymer as a main component. The content of the block copolymer in the functional layer may be 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, etc.
[0100] The shape of the fluororesin molded article is not particularly limited, and examples thereof include molded articles such as sheets, films, particles, plates, porous materials, and various members. EXAMPLES
[0101] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples unless the gist of the present invention is changed.
[0102] [1] Production of block copolymers (1-1) Preparation of copolymer (BHA-TBAEMA) 5.0g of butyl acetate and 5.0g of behenyl acrylate (BHA) were placed in a separable flask, and the butyl acetate and BHA were mixed, then degassed and replaced with nitrogen. Under a nitrogen atmosphere, the mixture of butyl acetate and BHA was stirred to dissolve BHA in the butyl acetate, and 0.38g of initiator (Blocbuilder MA) was added. Under a nitrogen atmosphere, BHA was polymerized at 110°C for 24 hours to obtain a BHA polymer solution. 5.0g of 2-(tert-butylamino)ethyl methacrylate (TBAEMA) and 5.0g of butyl acetate were added to the BHA polymer solution, and polymerization was further carried out under a nitrogen atmosphere at 110°C for 24 hours. Methanol was added to cause reprecipitation, and a block copolymer of BHA and TBAEMA (BHA-TBAEMA) was obtained.
[0103] The structural formula of the obtained BHA-TBAEMA is shown below as general formula (I).
[0104] [ka]
[0105] (1-2) Preparation of copolymer (STA-TBAEMA) A block copolymer of STA and TBAEMA (STA-TBAEMA) was obtained in the same manner as in (1-1) above, except that 5.0 g of stearyl acrylate (STA) was used instead of 5.0 g of behenyl acrylate (BHA).
[0106] The structural formula of the obtained STA-TBAEMA is shown below as general formula (II).
[0107] [ka]
[0108] (1-3) Preparation of copolymer (STA-DEEA) 3.0g of butyl acetate and 3.0g of diethylene glycol monoethyl ether acrylate (DEEA) were placed in a separable flask, and the butyl acetate and DEEA were mixed, followed by degassing and nitrogen replacement. Under a nitrogen atmosphere, the mixture of butyl acetate and DEEA was stirred, and the DEEA was dissolved in the butyl acetate, after which 0.29g of an initiator (Blocbuilder MA) was added. DEEA was polymerized under a nitrogen atmosphere at 105°C for 4 hours to obtain a solution of DEEA polymer. 5.8g of stearyl acrylate (STA) and 4.9g of butyl acetate were added to the solution of DEEA polymer, and polymerization was further carried out under a nitrogen atmosphere at 105°C for 4 hours. Methanol was added to cause reprecipitation, and a block copolymer of STA and DEEA (STA-DEEA) was obtained. The weight average molecular weight (Mw) of the obtained STA-DEEA was determined in polystyrene equivalent using GPC, and the weight average molecular weight of the STA-derived constituent unit was found to be approximately 5,000, and the weight average molecular weight of the DEEA-derived constituent unit was found to be approximately 10,000.
[0109] The structural formula of the obtained STA-DEEA is shown below as general formula (III).
[0110] [ka]
[0111] (1-4) Preparation of copolymer (STA-AA) 6.6g of butyl acetate and 6.6g of stearyl acrylate (STA) were placed in a separable flask, and the butyl acetate and STA were mixed, then degassed and replaced with nitrogen. Under a nitrogen atmosphere, the mixture of butyl acetate and STA was stirred to dissolve STA in the butyl acetate, and 0.386g of initiator (Blocbuilder MA) was added. Under a nitrogen atmosphere, STA was polymerized at 105°C for 4.5 hours to obtain a solution of STA polymer. 3.42g of acrylic acid (AA) and 3.42g of butyl acetate were added to the solution of STA polymer, and polymerization was further carried out under a nitrogen atmosphere at 105°C for 27 hours. Methanol was added to cause reprecipitation, and a block copolymer of STA and AA (STA-AA) was obtained. The weight average molecular weight (Mw) of the obtained STA-AA was determined in terms of polystyrene using GPC, and the weight average molecular weight of the constituent units derived from STA was approximately 4,500, and the weight average molecular weight of the constituent units derived from AA was approximately 3,400.
[0112] The structural formula of the obtained STA-AA is shown below as general formula (IV).
[0113] [ka]
[0114] [2] Preparation of block copolymer solution (fluororesin modifier) (2-1) Preparation of block copolymer solution (1) The block copolymer used was BHA-TBAEMA, and the solvent used was tetrahydrofuran (THF). BHA-TBAEMA was added to THF and mixed so that the concentration of the block copolymer was 0.1 wt %, to prepare 100 g of block copolymer solution (1).
[0115] (2-2) Preparation of block copolymers (2) to (11) Block copolymer solutions (2) to (11) were prepared in the same manner as for block copolymer solution (1), except that the block copolymer, solvent, and amount of block copolymer added were changed so as to obtain the compositions shown in Table 1.
[0116] [Table 1]
[0117] [3] Preparation of PTFE film Film (F1-a): A PTFE film (manufactured by Sanplatec Co., Ltd.) having a thickness of 100 μm was cut into a size of 12.5±0.5 mm×100 mm to prepare film (F1-a). Film (F1-b): A 500 μm thick PTFE film (manufactured by Sanplatec Co., Ltd.) was cut into a size of 12.5±0.5 mm×100 mm to prepare film (F1-b). Film (F2-a): A PTFE film (manufactured by Sanplatec Co., Ltd.) having a thickness of 100 μm was cut into a size of 130 mm×200 mm to prepare film (F2-a). Film (F2-b): A PTFE film (manufactured by Sanplatec Co., Ltd.) having a thickness of 500 μm was cut into a size of 130 mm×200 mm to prepare film (F2-b).
[0118] [Example 1] Production of modified fluororesin molded body (immersion) (Example 1-1) The block copolymer solution (1) (100 g) was placed in a separable flask and heated to 60°C (modification temperature) in an oil bath. When the temperature reached 60°C, 10 sheets of film (F1-a) were suspended by wire and immersed. After 10 minutes, all the films were removed from the block copolymer solution (1). The films treated with the block copolymer solution (1) were vacuum dried (45°C, 30 min) to obtain 10 sheets of modified film (A1).
[0119] (Examples 1-2 to 1-13) Modified films (A2) to (A13) were obtained in the same manner as in Example 1-1, except that the block copolymer solution and the modification temperature were changed as shown in Table 2.
[0120] [Table 2]
[0121] [Evaluation of Adhesion of Modified Film Obtained in Example 1] - Preparation of test specimens Using the obtained modified film, test pieces for T-peel tests were prepared in accordance with JIS K6854-3 (1999). Five test pieces were prepared under the same manufacturing conditions using ten sheets of modified film obtained under the same manufacturing conditions. First, two sheets of the modified film were bonded together using Aron Alpha (registered trademark), then dried at 100°C for 20 minutes to obtain a test piece. As a comparative example, a test piece was also obtained by similarly bonding two unmodified films (F1-a) together with Aron Alpha.
[0122] T-type peel test Using the five test pieces thus prepared, a T-peel test was performed in accordance with K6854-3 (1999), and the maximum test force and the average test force of the five test pieces were calculated. The results are shown in Table 2.
[0123] As shown in Table 2, compared to the unmodified film (F1-a), the modified films A1 to A13 are superior in average test force and maximum test force, and show improved adhesion.
[0124] [Example 2] Production of modified fluororesin molded body (coating) The film (F2-a) was placed on the glass plate of a tabletop coater with the short side (130 mm side) horizontal and the long side (200 mm side) vertical. The slit width (distance between the glass plate and the applicator) was set to 1.1 mm so that the distance between the applicator spreading the solution and the film was 1 mm. After dropping the block copolymer solution (6) (about 3 mL) onto the film (F2-a), the block copolymer solution (6) was spread and applied onto the film (F2-a) at a coating speed of 10 mm / min. The film (F2-a) coated with the block copolymer solution (6) was then vacuum dried (45°C, 30 min) to obtain a modified film (b1). The obtained modified film (b1) was cut into a size of 12.5 ± 0.5 mm × 100 mm to obtain a total of 10 modified films (B1).
[0125] [Example 3] Production of modified fluororesin molded product (spraying) (Example 3-1) The block copolymer solution (6) was filled into a spray container, and the block copolymer solution was sprayed onto the surface of the film (F1-a). The film (F1-a) onto which the block copolymer solution (6) had been sprayed was then vacuum dried (45°C, 30 min) to obtain a modified film (C1). The same operation was repeated to obtain a total of 10 modified films (C1). The amount of the block copolymer solution used to produce the 10 modified films was approximately 3 mL.
[0126] (Example 3-2) Ten modified films (C2) were obtained in the same manner as in Example 3-1, except that the block copolymer solution (3) was used instead of the block copolymer solution (6) and the film (F2-a) was used instead of the film (F1-a).
[0127] [Evaluation of Adhesion of Modified Films Obtained in Examples 2 and 3] The average values of the maximum test force and the average test force of the modified film (B1), the modified film (C1), and the modified film (C2) were calculated in the same manner as in the evaluation of the adhesiveness of Example 1. Table 3 shows the results of Example 2, Example 3-1, and Example 3-2 together with the results of Examples 1-5.
[0128] [Table 3]
[0129] As shown in Table 3, the modified films modified by coating or spraying with the block copolymer solution also showed improved adhesion.
[0130] [Example 4] Production of modified fluororesin molded body (production method including surface roughening step) (Example 4-1) The film (F1-b) was roughened by polishing the film surface with sandpaper #180 five times in approximately the same direction to obtain film (f1-b). The same procedure was repeated to prepare 10 sheets of film (f1-b). The degree of roughness of this film (f1-b) was measured in accordance with JIS B 0663 (2001) using a 3D measuring laser microscope OLS4100 (manufactured by SIMADZU) (cutoff wavelength: 80 μm, objective lens: MPLFLN10x, image size: 1280 × 1280 μm), and the maximum height roughness (Rz) was 43 μm and the arithmetic mean roughness (Ra) was 6.5 μm. Next, the same operation as in Example 1-5 was carried out except that the film (f1-b) was used instead of the film (F1-a), to obtain 10 sheets of modified film (A5-R).
[0131] (Example 4-2) The surface of film (F2-b) was roughened by polishing the film surface five times in approximately the same direction with sandpaper #180 to obtain film (f2-b). Next, the same operation as in Example 2 was performed except that film (f2-b) was used instead of film (F2-a) and the slit width (the distance between the glass plate and the applicator) was set to 1.5 mm, thereby obtaining 10 modified films (B1-R) (12.5±0.5 mm×100 mm).
[0132] (Example 4-3) Ten sheets of film (f1-b) were prepared in the same manner as in Example 4-1. Next, the same operation as in Example 3-1 was carried out except that the film (f1-b) was used instead of the film (F1-a), to obtain 10 sheets of each modified film (C1-R).
[0133] (Examples 4-4 to 4-6) Ten sheets of film (f1-b) were prepared in the same manner as in Example 4-1. Next, the same operation as in Example 3-1 was carried out except that film (f1-b) was used instead of film (F1-a) and the block copolymer solution shown in Table 4 was used instead of block copolymer solution (6), thereby obtaining 10 sheets each of modified films (C2-R) to (C4-R).
[0134] [Evaluation of Adhesion of Modified Film Obtained in Example 4] The average values of the maximum test force and the average test force were calculated for the modified films (A5-R), (B1-R), and (C1-R) to (C4-R) in the same manner as in the evaluation of adhesion in Example 1. The results are shown in Table 4.
[0135] [Table 4]
[0136] As shown in Table 4, by roughening the PTFE film and then treating it with the block copolymer solution, a film with excellent adhesion was obtained.
[0137] [Example 5] Production of modified fluororesin molded body (use of expanded PTFE film) (PTFE film stretching) As the fluororesin molded body, a stretched PTFE film was used, which was obtained by sequentially biaxially stretching a PTFE film (manufactured by Sanplatec Co., Ltd.) having a thickness of 800 μm. The stretching of the PTFE film was carried out using a small tabletop tester (EZ-LX-5Z, manufactured by Shimadzu Corporation). First, the film cut to 120 mm x 60 mm (length x width) was stretched so that the length became 120 mm to 240 mm. Then, the film cut to 60 mm x 40 mm (length x width) was stretched again so that the width became 40 mm to 100 mm, to obtain a stretched PTFE film. This expanded PTFE film was appropriately cut out and used for producing a modified PTFE film.
[0138] (Surface observation of expanded PTFE film) The surfaces of the stretched PTFE film and the unstretched PTFE film were observed using an SEM (Hitachi High-Technologies Corporation, TM4000plus scanning electron microscope). Figure 1(a) shows an SEM image of the surface of the unstretched PTFE film, and Figure 1(b) shows an SEM image of the surface of the stretched PTFE film. As shown in Figure 1, the occurrence of pores was confirmed on the surface of the expanded PTFE film, whereas no pores were confirmed on the surface of the unexpanded PTFE film.
[0139] (Example 5-1) A solution (block copolymer solution (7)) in which BHA-TBAEMA was dissolved in toluene so that the concentration of BHA-TBAEMA was 0.5 wt % was used as the block copolymer solution. The block copolymer solution (7) (100 g) was placed in a separable flask and heated to 30°C (modification temperature) in an oil bath. When the temperature reached 30°C, 10 stretched PTFE films (10±0.5 mm x 60 mm) were suspended by wire and immersed in the solution. After 10 minutes, all of the films were removed from the block copolymer solution (7). The films treated with the block copolymer solution (7) were vacuum dried (45°C, 30 min) to obtain 10 modified films (E1).
[0140] (Example 5-2 to Example 5-6) Except for changing the block copolymer solution and the modification temperature as shown in Table 5, the same procedure as in Example 5-1 was carried out to obtain modified films (E2) to (E6).
[0141] [Table 5]
[0142] [Evaluation of Adhesion of Modified Film Obtained in Example 5] Except for changing the area of the adhesive joint from 12.5±0.5 mm×75 mm to 10±0.5 mm×50 mm, five test pieces were prepared in the same manner as in Example 1, and a T-peel test was carried out. The average value of the average peel force (average test force / test piece width) of the five test pieces was calculated. Table 5 shows the results of Examples 5-1 to 5-6.
[0143] As shown in Table 5, from the results of Examples 5-1 to 5-4, when the stretched PTFE film was used, it was possible to modify the film with the block copolymer solution, similarly to the case of using the unstretched PTFE film. Furthermore, the higher the modification temperature, the more the adhesive strength improved. In addition, the results of Examples 5-4 to 5-6 show that the stretched PTFE film could be modified even when the concentration of the block copolymer was changed. In particular, the modified film (E6) modified using a solution with a block copolymer concentration of 0.7 wt% showed such strong adhesion that the film itself was destroyed during the T-peel test. The average peel force of the unmodified stretched PTFE film was similar to that of the unmodified unstretched PTFE film.
[0144] [FT-IR measurement of modified film (E4)] When the surface of the modified film (E4) was observed by FT-IR, a peak derived from CH (2950 cm -1 , 2850cm -1 ), C=O peak (1700cm -1 ) were confirmed. On the other hand, these peaks were not confirmed in the unmodified expanded PTFE film. From this result, it was confirmed that BHA-TBAEMA exists on the surface of the expanded PTFE in the modified film (E4).
[0145] [Contact angle of modified film (E4)] The contact angle of the surface was measured using a water contact angle measuring device (Kyowa Interface Science Co., Ltd. "Dropmaster100"). The contact angle of the stretched PTFE film (unmodified) was 137°, and that of the modified film (E4) was 116°, confirming that the hydrophilicity of the film could be improved by modifying it with BHA-TBAEMA.
[0146] [Reference Example 1] Preparation of copolymer (4) A block copolymer of DFHA and TBAEMA (DFHA-TBAEMA) was obtained in the same manner as in the production of BHA-TBAEMA (1-1), except that 5.0 g of 2,2,3,3,4,4,5,5,6,6,7,7-dodecafluoroheptyl acrylate (DFHA) was used instead of 5.0 g of behenyl acrylate (BHA).
[0147] [Reference Example 2] Production of modified film and evaluation of adhesion DFHA-TBAEMA was added to toluene and mixed so that the concentration of DFHA-TBAEMA was 0.1 wt %, to prepare 100 g of a DFHA-TBAEMA solution. Modified films (D1) and (D2) were obtained in the same manner as in Example 3-1 and Example 4-3, except that the DFHA-TBAEMA solution was used instead of the block copolymer solution (6). In the same manner as in the evaluation of adhesion in Example 1, the average values of the maximum test force and the average test force of the obtained modified film (D1) were calculated, and the maximum test force was 1.5 [N] and the average test force was 0.8 [N]. In addition, when the average values of the maximum test force and the average test force of the modified film (D2) were calculated, the maximum test force was 9.8 [N] and the average test force was 5.6 [N].
[0148] A comparison of the modified films of Examples 3-1 and 4-3 with the modified film of Reference Example 2 shows that the block copolymer (BHA-TBAEMA) in the fluororesin modifier of the present invention, although it does not have a similar structure to the PTFE to be modified, can impart adhesive strength equal to or greater than that achieved by treatment with a block copolymer solution (DFHA-TBAEMA) having a similar structure to the PTFE to be modified. [Industrial Applicability]
[0149] According to the present invention, the fluororesin modifier of the present invention can be used to produce modified fluororesin molded articles imparted with desired functionality, such as PTFE, which has excellent adhesion to other materials, thereby expanding the range of uses for fluororesins.
Claims
1. A block composed of a structural unit (A) represented by the following general formula (A-1) or general formula (A-2), A fluororesin modifier comprising a block copolymer including a block composed of a structural unit (B) represented by the following general formula (B-1), (B-2), (B-3), (B-4), (B-6) or (B-7): 【Chemistry 1】 In the general formulae (A-1) and (A-2), R a1 represents a hydrogen atom or a methyl group; R a2 represents an alkyl group having 8 or more carbon atoms; m is 2 to 1,000. 【Chemistry 2】 In the general formulae (B-1) to (B-4), R b1 represents a hydrogen atom or a methyl group; R L represents a single bond or an alkylene group having 1 to 4 carbon atoms; R b2 represents any one selected from the group consisting of a hydrogen atom, an amino group, an ammonium group, a carboxyl group, a hydroxyl group, a sulfonic acid group, an alkoxy group, and -(C p H 2p -O) q -R x1 (p is an integer of 1 to 10, q is an integer of 1 to 10, and R x1 represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms); R b3 represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms; n is 2 to 1,000. 【Chemistry 3】 In the general formulae (B-6) and (B-7), R b4 represents a hydrogen atom or a methyl group; R L represents a single bond or an alkylene group having 1 to 4 carbon atoms; R b5 represents any one selected from the group consisting of an amino group, an ammonium group, a carboxyl group, a hydroxyl group, a sulfonic acid group, an alkoxy group, and -(C p H 2p -O) q -R x1 (p is an integer of 1 to 10, q is an integer of 1 to 10, and R x1 represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms); n is 2 to 1,000.
2. In the general formulae (B-1) to (B-4), R b2 represents any one selected from the group consisting of a hydrogen atom, an amino group, and -(C p H 2p -O) q -R x1 (p is an integer of 1 to 10, q is an integer of 1 to 10, and R x1 represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms); The fluororesin modifier according to claim 1, wherein in the general formulas (B-6) and (B-7), R b5 represents an amino group or -(C p H 2p -O) q -R x1 (p is an integer of 1 to 10, q is an integer of 1 to 10, and R x1 represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms).
3. The fluororesin modifier according to claim 1 or 2, which is a block copolymer solution containing the block copolymer and a solvent.
4. A method for producing a modified fluororesin molded body, comprising a surface modification step of contacting a fluororesin modifier described in any one of claims 1 to 3 with a fluororesin molded body and forming a functional layer containing the fluororesin modifier on at least a portion of the surface of the fluororesin molded body.
5. The method for producing a modified fluororesin molded article according to claim 4, wherein the fluororesin molded article is an extruded article.
6. The method for producing a modified fluororesin molded article according to claim 4 or 5, further comprising a surface roughening step of roughening the surface of the fluororesin molded article prior to the surface modification step.
7. A modified fluororesin molded product having a fluororesin molded product and a functional layer containing a block copolymer formed on at least a part of a surface of the fluororesin molded product, The block copolymer is a block copolymer comprising a block composed of a structural unit (A) represented by the following general formula (A-1) or general formula (A-2) and a block composed of a structural unit (B) represented by the following general formula (B-1), (B-2), (B-3), (B-4), (B-6) or (B-7). A modified fluororesin molded article. 【Chemistry 4】 In the general formulae (A-1) and (A-2), R a1 represents a hydrogen atom or a methyl group; R a2 represents an alkyl group having 8 or more carbon atoms; m is 2 to 1,000. 【Chemistry 5】 In the general formulae (B-1) to (B-4), R b1 represents a hydrogen atom or a methyl group; R L represents a single bond or an alkylene group having 1 to 4 carbon atoms; R b2 represents any one selected from the group consisting of a hydrogen atom, an amino group, an ammonium group, a carboxyl group, a hydroxyl group, a sulfonic acid group, an alkoxy group, and -(C p H 2p -O) q -R x1 (p is an integer of 1 to 10, q is an integer of 1 to 10, and R x1 represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms); R b3 represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms; n is 2 to 1,000. 【Chemistry 6】 In the general formulae (B-6) and (B-7), R b4 represents a hydrogen atom or a methyl group; R L represents a single bond or an alkylene group having 1 to 4 carbon atoms; R b5 represents any one selected from the group consisting of an amino group, an ammonium group, a carboxyl group, a hydroxyl group, a sulfonic acid group, an alkoxy group, and -(C p H 2p -O) q -R x1 (p is an integer of 1 to 10, q is an integer of 1 to 10, and R x1 represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms); n is 2 to 1,000.
Citation Information
Patent Citations
Method for modifying surface of fluororesin molding
JP2009013310A
Method for modifying surface of fluororesin-based molding
JP2009263529A
Surface-modified material, composition for surface modification, and restoration method
JP2015229725A
Copolymer, modifier for fluororesin, modification method of fluororesin, and method for producing copolymer for modification of fluororesin
JP2016079389A
Method for modifying molded product of polyethylene-based resin, modifier of polyethylene-based resin, and molded product of polyethylene-based resin
JP2018030927A