Retort manufacturing method, retort and rotary kiln
The plasma welding of Ni-based alloys without fillers in a rotary kiln addresses the weldability issue, enabling retorts with enhanced high-temperature resistance and mechanical strength for large-scale applications.
Patent Information
- Application Number
- JP2024023891
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-02-20
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2044-02-20
AI Technical Summary
Ni-based alloys containing 2.0% or more aluminum by weight are difficult to weld, limiting the availability of retorts with excellent high-temperature oxidation resistance.
A retort manufacturing method using a rotary kiln that plasma welds a Ni-based alloy without a filler, forming a joint portion with controlled crystal grain sizes to enhance mechanical strength and oxidation resistance.
The method enables the production of retorts with improved high-temperature oxidation resistance and mechanical strength, suitable for large-scale applications like sintering lithium-ion battery materials.
Smart Images

Figure 0007555648000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a retort manufacturing method, a retort, and a rotary kiln. [Background technology]
[0002] 2. Description of the Related Art A rotary kiln equipped with a retort (heating furnace) (see, for example, Patent Document 1) is used for heat treatment of various objects to be treated, including powder.
[0003] Among the materials that are heat-treated using a rotary kiln, there are some that are sintered in an oxidizing atmosphere, such as the positive electrode material of lithium-ion batteries, and there is a demand for the development of a retort that has excellent oxidation resistance at high temperatures (hereinafter referred to as "high-temperature oxidation resistance").
[0004] A known material having excellent high-temperature oxidation resistance is a nickel-based alloy (Ni-based alloy) containing, by weight, 2.0 to 5.0% aluminum (Al), 0.1 to 2.5% silicon (Si), 0.8 to 4.0% chromium (Cr), 0.1 to 1.5% manganese (Mn), 0.001 to 0.01% boron (B), 0.001 to 0.1% zirconium (Zr), with the remainder being nickel (Ni) and unavoidable impurities (Patent Document 2).
[0005] Another known material with excellent high-temperature oxidation resistance is a Ni-based alloy containing, by weight, 2.0-5.0% Al, 0.1-2.5% Si, 0.1-1.5% Mn, 0.001-0.01% B, 0.001-0.1% Zr, with the remainder being Ni and unavoidable impurities (Patent Document 3). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2011-080740 A [Patent Document 2] JP 2014-080675 A [Patent Document 3] JP 2015-045035 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, since Al has a lower melting point than other contained components, Ni-based alloys containing a large amount of Al (2.0 wt % or more), such as the Ni-based alloys in Patent Documents 2 and 3, are difficult to weld, and retorts using such Ni-based alloys are not currently available on the market.
[0008] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a method for producing a retort using a Ni-based alloy containing 2.0% by weight or more of Al, a retort using a Ni-based alloy containing 2.0% by weight or more of Al, and a rotary kiln equipped with the retort. [Means for solving the problem]
[0009] [Retort manufacturing method] The retort manufacturing method of the present invention is a method for manufacturing a retort for a rotary kiln, in which a joint of a base material made of a Ni-based alloy containing 90.0% by weight or more of Ni and 2.0% by weight or more of Al (aluminum) is plasma welded without using a filler to produce a retort.
[0010] [retort] The retort of the present invention is a rotary kiln retort, and comprises a base material made of a Ni-based alloy containing 90.0% by weight or more of Ni and 2.0% by weight or more of Al, and a weld metal part generated at a joint of the base material, the base material comprising a heat-affected zone generated around the weld metal part and a base material part which is a part of the base material other than the heat-affected zone, and the value obtained by (Equation 1) (average crystal grain size in the heat-affected zone / average crystal grain size in the base material part)×100 is 100 to 300%, and / or the average crystal grain size in the heat-affected zone is less than 250 μm.
[0011] In the present application, a Ni-based alloy containing 2.0 to 5.0% by weight of Al can be used as the base material.
[0012] In the present application, a Ni-based alloy containing 90.0% or more by weight of Ni, 2.0% or more by weight of Al, as well as 0.1 to 2.5% by weight of Si, 0.1 to 1.5% by weight of Mn, 0.001 to 0.01% by weight of B, and 0.001 to 0.1% by weight of Zr can also be used as the base material.
[0013] In the present application, as the base material, a Ni-based alloy containing 90.0% or more by weight of Ni and 2.0% or more by weight of Al, as well as 0.1 to 2.5% by weight of Si, 0.8 to 4.0% by weight of Cr, 0.1 to 1.5% by weight of Mn, 0.001 to 0.01% by weight of B, and 0.001 to 0.1% by weight of Zr can also be used.
[0014] [Rotary kiln] The rotary kiln of the present invention is equipped with the retort of the present invention. Effect of the Invention
[0015] According to the present invention, it is possible to provide a retort using a Ni-based alloy that has excellent resistance to high-temperature oxidation. [Brief description of the drawings]
[0016] [Figure 1] (a) to (c) show an example of a manufacturing process for a cylindrical part. [Diagram 2] (a) to (d) show an example of the retort manufacturing process. [Diagram 3] This shows an example of a rotary kiln. [Figure 4] Schematic diagram of retort joints. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] (Definitions of terms used in this application) Prior to describing the embodiments of the present invention, definitions of major terms used in the present application will be provided. In the present application, the term "weld" refers to a portion including a weld metal portion and a heat-affected zone. The term "weld metal portion" refers to a molten portion and a welded metal portion, and the term "heat-affected zone" refers to a portion of the unmelted base material where the structure, metallurgical properties, mechanical properties, etc. have been changed by heat from welding, cutting, etc.
[0018] In addition, the term "melted zone" refers to the portion of the base material that has melted, and the term "welded metal zone" refers to the metal that has transferred from the filler metal to the weld zone. In this application, the portion of the base material other than the heat-affected zone is referred to as the "base material zone."
[0019] In addition, in this application, "crystal" refers to a solid substance in which atoms or ions are arranged in a periodic three-dimensional lattice pattern, "crystal grain" refers to an individual crystal in a substance made up of fine crystals such as a crystalline solid such as a metal or ceramic, and "average crystal grain size" refers to the average grain size of the crystal grains contained in a metal. Hereinafter, the embodiments of this application will be described using these terms.
[0020] (Embodiment of retort manufacturing method) First, an example of a retort pouch manufacturing method of the present invention will be described. In the retort pouch manufacturing method of this embodiment, a cylindrical component (hereinafter, referred to as a "cylindrical part") 10a constituting a retort pouch 10 is manufactured as shown in Figs. 1(a) to (c).
[0021] The cylindrical part 10a can be manufactured by bending a plate-shaped base material 11 as a base into a cylindrical shape so that both end faces face each other, and then welding the joints of both end faces that are bent into a cylindrical shape. The bending process of the base material 11 can be performed by a conventional method using a conventional device.
[0022] For the base material 11, a nickel-based alloy (Ni-based alloy) containing 90.0% by weight or more of nickel (Ni) and 2.0% by weight or more of aluminum (Al) can be used.
[0023] Specifically, in addition to 90.0% by weight or more of Ni and 2.0% by weight or more of Al, one or more of silicon (Si), manganese (Mn), boron (B), zirconium (Zr), and chromium (Cr) can be used.
[0024] For example, the alloy may contain 90.0% by weight or more of Ni and 2.0 to 5.0% by weight of Al, as well as 0.1 to 2.5% by weight of Si, 0.1 to 1.5% by weight of Mn, 0.001 to 0.01% by weight of B, and 0.001 to 0.1% by weight of Zr.
[0025] In addition, for example, a material containing 90.0% or more Ni and 2.0-5.0% Al, as well as 0.1-2.5% Si, 0.8-4.0% Cr, 0.1-1.5% Mn, 0.001-0.01% B, and 0.001-0.1% Zr can be used. The components and content ratios of the Ni-based alloy shown here are merely examples, and other components and content ratios may be used.
[0026] The welding of the joints can be performed, for example, by a method using plasma (plasma welding). In general plasma welding, a filler (filler metal) is used during welding, but in the retort manufacturing method of this embodiment, plasma welding is performed without using a filler metal.
[0027] When a filler is used, the filler needs to be melted, and the output becomes larger and the spraying time becomes longer. When the output becomes larger and the spraying time becomes longer, the crystal grains in the heat-affected zone 11a become thicker, and the difference in the average crystal grain size between the base material 11 and the heat-affected zone 11a becomes larger. When the difference in the average crystal grain size between the base material 11 and the heat-affected zone 11a becomes larger, the mechanical strength decreases and cracks may occur when the material is bent.
[0028] In this regard, when plasma welding is performed without using a filler as in the present embodiment, the output can be reduced and the spraying time can be shortened, thereby suppressing the enlargement of the crystal grains in the heat-affected zone 11a and minimizing the difference in average crystal grain size between the base material 11 and the heat-affected zone 11a. As a result, the occurrence of cracks during bending can be suppressed.
[0029] In addition, unlike electron beam welding, plasma welding does not require a chamber to hold the workpiece to be welded. This has the advantage that it can weld large objects that cannot be welded with electron beam welding (for example, a retort 10 with a diameter of 1700 mm and a length of 2000 mm).
[0030] After welding, the joint can be reinforced. The welding material (welding rod) for the reinforcement can be the same as the base material 11 or a different material. An example of a material different from the base material 11 is TIG617 (JIS SNi6617). It is preferable to use a welding rod that has excellent strength at high temperatures and high-temperature oxidation resistance. The reinforcement can be performed as necessary, and can be omitted if not required.
[0031] After manufacturing a plurality of cylindrical parts 10a in the above manner, they are used to complete a retort 10 of a desired length. Specifically, as shown in Figures 2(a) to 2(d), two or more cylindrical parts 10a are arranged so that their internal spaces communicate with each other and their end faces face each other, and the joints of the end faces of the butted cylindrical parts 10a are welded.
[0032] The tubular parts 10a can be welded together in the same manner as the welding method used to manufacture the tubular parts 10a described above. As in the case of manufacturing the tubular parts 10a, in this case too, the molten parts can be overfilled as necessary. Thereafter, multiple tubular parts 10a are joined in the same manner as above to complete the retort 10 of the desired length.
[0033] The retort manufacturing method of the present embodiment is merely an example, and the retort manufacturing method of the present invention is not limited to this embodiment. The retort manufacturing method of the present invention can be modified, such as by replacing, adding, or omitting steps, within the scope of achieving the intended purpose.
[0034] (Retort and rotary kiln embodiments) Next, an example of the retort 10 and rotary kiln 100 of the present invention will be described. As an example, the rotary kiln 100 shown in Fig. 3 is a so-called externally heated rotary kiln 100, and includes, as its main components, the retort 10, an outer cylinder 20 provided on the outer periphery of the retort 10, a supply section 30 provided on one end side in the longitudinal direction of the retort 10, and a discharge section 40 provided on the other end side.
[0035] The outer cylinder 20 is a part that heats the retort 10, the supply unit 30 is a part that supplies the object to be heat-treated into the retort 10, and the discharge unit 40 is a part that discharges the object after heat treatment and the gas generated during the heat treatment to the outside. The outer cylinder 20, the supply unit 30, and the discharge unit 40 can be existing parts.
[0036] The retort 10 is a furnace (heating furnace) for heating an object to be heat-treated. The retort 10 is rotatably supported by a support device 50. The retort 10 includes a plurality of tubular parts 10a that are aligned in the longitudinal direction and welded together. The tubular parts 10a can be manufactured, for example, by the method described in the embodiment of the manufacturing method of the retort above (the method of plasma welding without using a filler).
[0037] The retort 10 of this embodiment uses the above-mentioned Ni-based alloy as the base material 11. The Ni-based alloy has already been described in the embodiment of the method for producing a retort, and therefore a description thereof will be omitted here.
[0038] 4 is a conceptual diagram of the joints of the retort 10. The joints referred to here include both end face portions that are opposed to each other when the tubular part 10a is bent into a cylindrical shape during production, as well as the end face portions where two adjacent tubular parts 10a are butted together.
[0039] 4, the joining portion of the tubular part 10a in this embodiment includes a base material 11 and a weld metal portion 12, and a heat-affected zone 11a exists in the region of the base material 11 adjacent to the weld metal portion 12. In addition, a reinforcement portion 13 is formed on the upper surface side of the weld metal portion 12.
[0040] One of the features of the retort shell 10 of this embodiment is that the value obtained by the following formula 1 is 100 to 300%. (average grain size in heat-affected zone / average grain size in base material) × 100 (Equation 1)
[0041] According to a comparative test described later, the value obtained by the above formula 1 was 335% when plasma welding was performed using a filler, whereas it was 237% when plasma welding was performed without using a filler.
[0042] In the former, the value obtained by the above formula 1 was 335%, and numerous cracks were confirmed in the bending test, whereas in the latter, the value obtained by the above formula 1 was 237%, and no cracks were confirmed in the bending test.
[0043] For this reason, when the value obtained by formula 1 is in the range of 100 to 300%, as in the case of the retort 10 of this embodiment, there is significance at least in bending strength in comparison with retorts outside that range.
[0044] In the present application, the average grain size of the base material 11 and the heat-affected zone 11a was measured by the following method. This measurement method is based on JIS G 0551, Appendix A (evaluation of grain size) except that the number of grains captured in the circular area observed in the micrograph was set to 10. The specific measurement method is as follows.
[0045] (1) An area including the joint and base material 11 is photographed using an electron microscope to obtain a micrograph including the heat-affected zone 11a and base material portion 11b of base material 11. (2) Set an observation circle on the 100x magnification micrograph obtained in (1) above, and define the number of grains in the observation circle as n1 and the number of grains intersecting the circumference as n2. The equivalent number of crystal grains, n 100 The equivalent number of grains n is calculated using the following formula (2). 100 The calculation is performed for each of the heat-affected zone 11a and the base material zone 11b. n 100 =n1+n2 / 2...(Formula 2) (3) Next, a 1 mm sample on the surface of the test piece at a magnification of 100 times was taken. 2 The number of crystal grains per unit area, m, is calculated using the following formula (3). m = 2 × n 100 ...(Formula 3) (4) Using the values obtained in (2) and (3) above, the average crystal grain size d is calculated by the following formula (4). d=1 / √m (Equation 4)
[0046] The method for measuring the average crystal grain size described here is merely an example, and the average crystal grain size can also be measured by other methods.
[0047] In addition to the above features, another feature of the retort 10 of this embodiment is that the average crystal grain size of the heat-affected zone 11a is less than 250 μm, preferably less than 200 μm.
[0048] According to a comparative test described later, the average crystal grain size of the heat-affected zone 11a when plasma welding was performed using a filler was 277 μm, whereas the average crystal grain size of the heat-affected zone 11a when plasma welding was performed without using a filler was 158 μm.
[0049] In the former, in which the average crystal grain size in the heat-affected zone 11a was 277 μm, numerous cracks were confirmed in the bending test, whereas in the latter, in which the average crystal grain size in the heat-affected zone 11a was 158 μm, no cracks were confirmed in the bending test.
[0050] For this reason, when the average crystal grain size of the heat-affected zone 11a is less than 250 μm, preferably less than 200 μm, as in the retort 10 of this embodiment, there is significance at least in bending strength compared to those that do not satisfy this numerical value.
[0051] The retort 10 and the rotary kiln 100 of the present embodiment are merely examples, and the retort 10 and the rotary kiln 100 of the present invention are not limited to the present embodiment. The retort 10 and the rotary kiln 100 of the present invention can be modified, such as by appropriately replacing, adding, or omitting, the configuration, as long as the intended purpose can be achieved.
[0052] (Experimental Example) The applicant of the present invention conducted comparative tests using a number of test pieces in order to verify the effects of the retort pouch 10 produced by the retort pouch production method of the present invention. The outline and results of the comparative tests are as follows.
[0053] -Comparative test overview- Three test pieces shown in Table 1 were prepared, and a tensile test, a bending test, and a micro test were performed on each test piece. [Table 1]
[0054] As shown in Table 1, the examples are test pieces welded in the same manner as the retort manufacturing method, in which Ni-based alloy (Ni-2Cr-4Al-1.5Si-0.5Mn) was plasma welded without using a filler, and the fusion zone was reinforced. A TIG617 (JIS SNi6617 equivalent) welding rod was used for the reinforcement.
[0055] In Comparative Example 1, the same Ni-based alloy (Ni-2Cr-4Al-1.5Si-0.5Mn) as in the Example was plasma welded using a filler, and the welded part was overfilled. The filler was the same Ni-based alloy (Ni-2Cr-4Al-1.5Si-0.5Mn) as the base material, and the welding rod for overfilling was the same Ni-based alloy (Ni-2Cr-4Al-1.5Si-0.5Mn) as the base material.
[0056] In Comparative Example 2, the same Ni-based alloy (Ni-2Cr-4Al-1.5Si-0.5Mn) as in the Example was welded by electron beam welding without using a filler, and the welded part was reinforced. The same Ni-based alloy (Ni-2Cr-4Al-1.5Si-0.5Mn) as the base material was used as the welding rod for the reinforcement.
[0057] In the tensile test, the tensile strength (N / mm 2 The tensile test was performed according to JIS Z3121 using JIS Z3121 No. 1A test pieces.
[0058] In the bending test, cracks during bending on the front side and during bending on the back side were measured, and photographs were taken during bending on the front side and during bending on the back side. The bending test was performed according to JIS Z3122 using a JIS Z3122 No. 1A test piece.
[0059] In the micro test, the average crystal grain size (μm) of the heat-affected zone and the average crystal grain size (μm) of the base material were measured, and the values were calculated by applying these values to the above formula 1. The micro test was performed according to JIS Z3122 using a JIS Z3122 No. 1A test piece.
[0060] -Results of the comparative test- The results of the comparative test are shown in Table 2. [Table 2]
[0061] [About tensile testing] As shown in Table 2, the tensile strength of the example is 643 N / mm 2 The tensile strength of Comparative Example 1 is 811 N / mm 2 , and the tensile strength of Comparative Example 2 is 670N / mm 2 The joint efficiency of the example was 95.3%, the joint efficiency of the comparative example 1 was 120.1%, and the joint efficiency of the comparative example 2 was 99.3%.
[0062] [About bending tests] As shown in Table 2, no cracks occurred in either front bending or back bending in Example and Comparative Example 2. On the other hand, in Comparative Example 1, many cracks were observed during front bending.
[0063] [About micro testing] As shown in Table 2, in the example, the average crystal grain size in the heat-affected zone was 158 μm, and the average crystal grain size in the base material was 67 μm. Furthermore, the value obtained by applying these values to the above formula 1 was 237%, which was within the range of 100 to 300%.
[0064] In Comparative Example 1, the heat-affected zone had an average crystal grain size of 277 μm, and the base material had an average crystal grain size of 83 μm. Furthermore, the value obtained by applying these values to the above formula 1 was 335%, which did not fall within the range of 100 to 300%.
[0065] In Comparative Example 2, the heat-affected zone had an average crystal grain size of 69 μm, and the base material had an average crystal grain size of 68 μm. The value obtained by applying these values to the formula 1 was 102%, which was within the range of 100 to 300%.
[0066] From the results of this comparative test, it was confirmed that in the test piece (Comparative Example 1) that was plasma welded using a filler, the crystal grains in the heat-affected zone 11a became enlarged, the difference in average crystal grain size between the heat-affected zone 11a and the base material portion 11b became larger, and the difference in average crystal grain size between the heat-affected zone 11a and the base material portion 11b became larger, which resulted in the occurrence of cracks in the bending test.
[0067] On the other hand, in the test piece (embodiment) in which plasma welding was performed without using a filler, it was confirmed that no cracks occurred in the bending test because the enlargement of the crystal grains in the heat-affected zone 11a was suppressed, the difference in average crystal grain size between the heat-affected zone 11a and the base material portion 11b did not become large, and the difference in average crystal grain size between the heat-affected zone 11a and the base material portion 11b did not become large.
[0068] The same results as in the examples were obtained with a test piece (Comparative Example 2) that was electron beam welded without using a filler. However, electron beam welding requires a chamber to hold the workpiece, and it is not realistic to prepare a chamber to hold a large retort. Therefore, for the manufacture of large retorts, a method of plasma welding without using a filler is preferable. [Industrial Applicability]
[0069] The retort 10 and its manufacturing method of the present invention can be used for various applications, but can be particularly suitably used as a retort 10 and its manufacturing method for use in sintering a positive electrode material for a lithium ion battery. In particular, a retort 10 using a Ni-based alloy that does not contain Cr can be suitably used as a retort 10 for sintering a positive electrode material for a lithium ion battery.
[0070] In the case of an alloy containing a large amount of Cr (for example, an alloy containing 20% or more by weight of Cr), the Cr in the alloy may react with lithium (Li), and the Cr may be incorporated into the positive electrode material, causing malfunctions. However, in the case of a retort 10 using a Ni-based alloy with a low Cr content, such a risk can be reduced. [Explanation of symbols]
[0071] 10 Retort 10a Cylindrical parts 11 Base material 11a Heat affected zone 11b Base material (part other than the heat-affected part of the base material) 12 Welded metal parts 13 Excess fill 20 Outer cylinder 30 Supply section 40 Discharge section 50 Support device 100 Rotary Kiln
Claims
1. In a method for producing retorts in a rotary kiln, A joint portion of a base material made of a Ni-based alloy containing Ni: 90.0 wt. % or more and Al: 2.0 wt. % or more is plasma welded without using a filler, A metal filler is applied to the outside of the weld metal portion formed at the joint by the plasma welding using a material different from the base metal. A retort manufacturing method comprising the steps of:
2. In the retort manufacturing method according to claim 1, A material that satisfies JIS SNi6617 is used as a material different from the base material. A retort manufacturing method comprising the steps of:
3. In the retort of a rotary kiln, The present invention comprises a base material made of a Ni-based alloy containing 90.0% by weight or more of Ni and 2.0% by weight or more of Al, a weld metal part formed at a joining portion of the base material by plasma welding, and a reinforcement part made of a material different from the base material and provided on the outside of the weld metal part, The base material includes a heat-affected zone generated around the weld metal portion and a base material portion which is a portion of the base material other than the heat-affected zone, (Equation 1) (average crystal grain size in the heat-affected zone / average crystal grain size in the base material)×100 is 100 to 300%, or / and the average crystal grain size in the heat-affected zone is less than 250 μm. A retort pouch characterized in that
4. In the retort according to claim 3, The reinforcement portion is made of a material that satisfies JIS SNi6617. A retort pouch characterized in that
5. The retort according to claim 3, The content of Al is 2.0 to 5.0 wt.%. A retort pouch characterized in that
6. The retort according to claim 3, The Ni-based alloy contains Ni: 90.0% by weight or more and Al: 2.0% by weight or more, Si: 0.1 to 2.5% by weight, Mn: 0.1 to 1.5% by weight, B: 0.001 to 0.01% by weight, Zr: 0.001 to 0.1 wt %; A retort pouch characterized in that
7. The retort according to claim 3, The Ni-based alloy contains Ni: 90.0% by weight or more and Al: 2.0% by weight or more, Si: 0.1 to 2.5% by weight, Cr: 0.8 to 4.0% by weight, Mn: 0.1 to 1.5% by weight, B: 0.001 to 0.01% by weight, Zr: 0.001 to 0.1 wt %; A retort pouch characterized in that
8. In rotary kilns, The retort according to any one of claims 3 to 7 is provided as a retort. A rotary kiln characterized by the above.
Citation Information
Patent Citations
Method for welding high-temperature resisting alloy furnace tubes by adopting plasma arc
CN101648314A
Groove provided in thick parent metal members for plasmaaarc welding
JP1978046452A
Rotary kiln and product
JP2011080740A
Ni-BASED ALLOY EXCELLENT IN HOT FORGING PROPERTY, HIGH TEMPERATURE OXIDATION RESISTANCE AND HIGH TEMPERATURE HALOGEN GAS CORROSION PROPERTY AND MEMBER USING Ni-BASED ALLOY
JP2014080675A
Ni-BASED ALLOY EXCELLENT IN HOT FORGEABILITY, HIGH-TEMPERATURE OXIDATION RESISTANCE AND RESISTANCE TO HIGH-TEMPERATURE HALOGEN GAS CORROSION AND MEMBER USING THE SAME
JP2015045035A