RTB permanent magnet and its manufacturing method

A two-step grain boundary diffusion process for R-T-B permanent magnets enhances both residual magnetic flux density and coercive force, addressing the need for improved magnetic properties in smaller, lighter components.

JP7555871B2Active Publication Date: 2024-09-25TDK CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021055189
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-29
Publication Date
2024-09-25
Estimated Expiration
2041-03-29

AI Technical Summary

Technical Problem

Existing R-T-B permanent magnets do not meet the demands for higher residual magnetic flux density and coercive force required in smaller, lighter, and more efficient magnetic components.

Method used

A two-step grain boundary diffusion process is employed, where a first diffusion material containing light rare earth elements is applied to the magnet base material, followed by a second diffusion material containing heavy rare earth elements, to enhance both residual magnetic flux density and coercive force.

Benefits of technology

The process results in an R-T-B permanent magnet with improved magnetic properties, achieving a residual magnetic flux density of 1450 mT or more and coercive force of 1800 kA/m or more, suitable for advanced applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555871000008
    Figure 0007555871000008
  • Figure 0007555871000009
    Figure 0007555871000009
  • Figure 0007555871000010
    Figure 0007555871000010
Patent Text Reader

Abstract

To provide an R-T-B based permanent magnet having both high residual magnetic flux density and high coercive force, and a method for producing the R-T-B based permanent magnet.SOLUTION: A method for producing an R-T-B based permanent magnet includes: a step of preparing a magnet base material 20 including an R-T-B based alloy; a first diffusion step of attaching a first diffusion material sheet 11a, which is formed by mixing a binder and a first diffusion material 11 containing a light rare earth element, to at least part of a surface of the magnet base material and then heating the magnet base material 20 with the first diffusion material 11 attached thereon; and a second diffusion step of, after the first diffusion step, attaching a second diffusion material sheet 12a, which is sheeted by mixing a binder and a second diffusion material 12 containing a heavy rare earth element, to at least part of a surface of the magnet base material and then heating the magnet base material 20 with the second diffusion material 12 attached thereon.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an RTB permanent magnet via a grain boundary diffusion step, and to an RTB permanent magnet produced by said method. [Background technology]

[0002] Rare earth magnets with an RTB composition have better magnetic properties than other permanent magnets, and in recent years, various studies have been conducted with the aim of further improving these magnetic properties. For example, Patent Document 1 discloses a method (grain boundary diffusion method) in which, after producing an RTB permanent magnet, a heavy rare earth element is attached to the surface and heated to diffuse the heavy rare earth element through the grain boundaries. By using this method, it is possible to improve the magnetic properties, particularly the coercive force.

[0003] However, there is currently a demand for many magnetic components (such as motors) to be even smaller, lighter, and with higher performance and efficiency, and in order to meet these demands, it is necessary to further improve both the residual magnetic flux density and coercive force of RTB permanent magnets. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2016 / 121790 Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made in view of the above-mentioned circumstances, and has an object to provide an RTB permanent magnet that combines high residual magnetic flux density and high coercive force, and a method for manufacturing the RTB permanent magnet. [Means for solving the problem]

[0006] In order to achieve the above object, the method for producing an RTB permanent magnet according to the present invention comprises the steps of: providing a magnet substrate comprising an RTB based alloy; a first diffusion step of attaching a first diffusion material containing at least one light rare earth element to at least a part of a surface of the magnet base material, and heating the magnet base material to which the first diffusion material is attached; The method includes a second diffusion step of, after the first diffusion step, attaching a second diffusion material containing at least one heavy rare earth element to at least a portion of the surface of the magnet base material, and heating the magnet base material to which the second diffusion material is attached.

[0007] As described above, by carrying out a two-stage grain boundary diffusion process in which a light rare earth element is diffused first and then a heavy rare earth element is diffused, an RTB permanent magnet having both high residual magnetic flux density and high coercivity can be obtained.

[0008] Preferably, the first diffusing material contains, as the light rare earth element, one or more elements selected from the group consisting of Nd and Pr.

[0009] Also, preferably, the first diffusion material includes an RL-M alloy containing the light rare earth element and M, and in the RL-M alloy, RL is the light rare earth element, and M is an element having a eutectic temperature with RL of 800°C or less.

[0010] Also, preferably, the content of heavy rare earth elements in the first diffusing material is 10 mass % or less, and more preferably, the first diffusing material is substantially free of heavy rare earth elements.

[0011] On the other hand, the second diffusing material preferably contains, as the heavy rare earth element, one or more elements selected from the group consisting of Tb and Dy.

[0012] Preferably, the RTB alloy contained in the magnet base material contains one or more rare earth elements, with Nd as essential, as R, one or more iron group elements, with Fe as essential, as T, boron, and Cu. And, preferably, in the RTB alloy, the total content of R is 27.5 mass% or more and 30.8 mass% or less, the content of Cu is 0.05 mass% or more and 0.5 mass% or less, and the content of B is 0.92 mass% or more and 1.03 mass% or less. When the magnet base material satisfies the above composition, the effects of improving the residual magnetic flux density and the coercive force become more pronounced.

[0013] The RTB permanent magnet according to the present invention can be obtained, for example, by the manufacturing method described above, An RTB permanent magnet in which R is one or more light rare earth elements, essentially Nd, and one or more heavy rare earth elements, T is one or more iron group elements, essentially Fe, and B is boron, The RTB based permanent magnet includes a plurality of core-shell particles, Each of the plurality of core-shell particles has R 2 T 14 a core portion containing B crystals and a shell portion covering the core portion and having a higher content of the heavy rare earth element than the core portion, In a cross section at a depth of 100 μm from the surface of the RTB permanent magnet, the maximum thickness of the shell portion is, on average, 0.5 μm or less, The RTB permanent magnet has a concentration distribution in which the content of the light rare earth element and the content of the heavy rare earth element both decrease in a depth direction from the surface of the RTB permanent magnet.

[0014] Because the RTB permanent magnet has the above characteristics, it is possible to improve both the residual magnetic flux density and the coercive force.

[0015] Preferably, the RTB permanent magnet of the present invention contains an M element having a eutectic temperature with the light rare earth element of 800° C. or lower, The RTB permanent magnet has a concentration distribution in which the content of the M element decreases from the surface toward the depth direction.

[0016] Also, preferably, the RTB permanent magnet further contains Cu, the total R content being 28.4 mass% or more and 32.0 mass% or less, the Cu content being 0.2 mass% or more and 0.7 mass% or less, and the B content being 0.92 mass% or more and 1.03 mass% or less. When the RTB permanent magnet satisfies the above composition, the magnetic properties (particularly the coercive force) are further improved.

[0017] Preferably, the heavy rare earth element contained in the RTB permanent magnet is Tb and / or Dy. Also, preferably, the RTB permanent magnet further contains Pr as the light rare earth element.

[0018] Moreover, the RTB permanent magnet preferably has a residual magnetic flux density of 1450 mT or more and a coercive force of 1800 kA / m or more.

[0019] The RTB permanent magnet of the present invention can be used as a component of motors, generators, compressors, actuators, magnetic sensors, speakers, etc., and is particularly suitable as a component of motors. Furthermore, motors including the RTB permanent magnet of the present invention can be mounted in various electronic devices, industrial equipment, etc., and are particularly suitable for use as automobile motors (EV, HV, PHV, etc.). [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a perspective view showing an example of a magnet substrate. [Diagram 2] FIG. 2 is a schematic diagram illustrating the flow of the first and second diffusion steps. [Figure 3A] FIG. 3A is an enlarged schematic cross-sectional view showing a cross section of the magnet base material. [Figure 3B]FIG. 3B is an enlarged schematic cross-sectional view of the RTB permanent magnet after the second diffusion step. [Figure 4A] FIG. 4A is a perspective view showing an example of an RTB permanent magnet. [Figure 4B] FIG. 4B is a cross-sectional view taken along line VB-VB shown in FIG. 4A. [Diagram 5] FIG. 5 is a schematic diagram showing a cross section of a core-shell particle. [Figure 6] FIG. 6 is a SEM cross-sectional photograph of an RTB permanent magnet according to an example (sample 1). [Figure 7] FIG. 7 is an SEM cross-sectional photograph of the RTB permanent magnet according to Comparative Example 1. [Figure 8] FIG. 8 is a schematic diagram of an IPM motor using the RTB type permanent magnet of the present invention. [Figure 9] FIG. 9 is a schematic diagram showing an automobile utilizing the IPM motor shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, the present invention will be described in detail based on the embodiments shown in the drawings.

[0022] In this embodiment, first, a method for manufacturing an RTB permanent magnet will be described, and then, the features of the RTB permanent magnet obtained by this manufacturing method will be described. The manufacturing method for an RTB permanent magnet of this embodiment includes a step of preparing a magnet base material, a first diffusion step of diffusing a light rare earth element into the magnet base material, and a second diffusion step of further diffusing a heavy rare earth element into the magnet base material after the first diffusion step. Each step will be described in order below.

[0023] (Magnetic substrate preparation process) In this step, the magnet substrate 20 shown in FIG. 1 is manufactured. First, the features of the magnet substrate 20 will be described in detail. The magnet substrate 20 is a sintered body of an RTB alloy, and is a material before the diffusion step described later is performed. In FIG. 1, the magnet substrate 20 is a rectangular parallelepiped having two main surfaces 20a perpendicular to the Z axis and four side surfaces 20b perpendicular to the X axis or the Y axis. However, the shape of the magnet substrate 20 is not particularly limited, and may be, for example, a polygonal shape, a cylindrical shape, a hollow cylindrical shape, or an arc segment shape in which the main surfaces are curved in an arc shape. In the drawings, the X axis, the Y axis, and the Z axis are approximately perpendicular to each other.

[0024] In this embodiment, the two main surfaces 20a of the magnet base material 20 are magnetic pole surfaces. A magnetic pole surface is a surface through which magnetic flux mainly passes, and is a positive pole (N pole) or a negative pole (S pole) of a permanent magnet. When the RTB permanent magnet to be manufactured is an anisotropic magnet, the magnetic pole surface can be determined by the direction of the magnetic field applied in the molding process described below. It should be noted that which surface of the magnet base material 20 is to be the magnetic pole surface is not particularly limited, and one main surface 20a and one side surface 20b may be the magnetic pole surface, or two opposing side surfaces 20b may be the magnetic pole surfaces.

[0025] In the RTB alloy constituting the magnet base material 20, R is one or more rare earth elements essentially consisting of Nd (neodymium), T is one or more iron group elements essentially consisting of Fe (iron), and B is boron. Here, the rare earth elements refer to Sc, Y, and lanthanoid elements belonging to Group 3 of the long periodic table, and among the rare earth elements, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu are referred to as heavy rare earth elements (RH), and rare earth elements other than RH are referred to as light rare earth elements (RL). In addition, the iron group elements refer to Fe, Co, and Ni.

[0026] The total content of R in the magnet base material 20 can be 25% by mass to 35% by mass, and is preferably 27.5% by mass or more and 30.8% by mass or less. When the total content of R satisfies the above composition range, precipitation of α-Fe and the like that exhibits soft magnetism is suppressed, and R 2 T 14B crystals are more likely to be produced. Here, in this embodiment, "the content of the predetermined element contained in the magnet base material 20" refers to the content per unit mass of the magnet base material 20, and means the ratio of the predetermined element to 100% by mass of the magnet base material. In other words, the total content of R described above is calculated as the ratio of the total mass of rare earth elements to 100% by mass of the magnet base material. The content of the predetermined element in the permanent magnet 2 described later will also be expressed in the same manner as above.

[0027] When multiple rare earth elements are included as R, the content of Nd included in the magnet base material 20 is not particularly limited, but is preferably 22 mass% or more. In this case, Pr, Tb, and Dy are preferably included in the magnet base material 20 as rare earth elements other than Nd. When a heavy rare earth element (RH) such as Tb or Dy is added as R other than Nd, the total content of RH included in the magnet base material 20 is preferably 2.5 mass% or less.

[0028] The content of B in the magnet base material 20 can be set to 0.5 mass % to 1.5 mass %, and is preferably set to 0.92 mass % to 1.03 mass %.

[0029] Meanwhile, the content of T contained in the magnet base material 20 is expressed as the balance and may be appropriately determined according to the contents of other elements. T may be Fe alone, or Fe may be partially substituted with Co. In this case, the content of Co is not particularly limited, and may be, for example, 4 mass% or less, and preferably 1 mass% or less.

[0030] Furthermore, the magnet base material 20 preferably contains one or more m elements selected from the group consisting of Cu, Ga, Al, and Zr, in addition to the above-mentioned R, T, and B. Of the above, it is more preferable that the m element contains Cu.

[0031] The content of Cu contained in the magnet base material 20 is preferably 0.05% by mass or more and 0.50% by mass or less. Furthermore, when Ga, Al, and Zr are contained as the m elements, the contents of these elements are not particularly limited, and for example, it is preferable that the Ga content be 0.08% by mass or more and 0.30% by mass or less, the Al content be 0.10% by mass or more and 0.30% by mass or less, and the Zr content be 0.10% by mass or more and 0.30% by mass or less.

[0032] The magnet base material 20 may also contain carbon (C), nitrogen (N), and oxygen (O). The carbon content in the magnet base material 20 is preferably 1100 ppm by mass or less, and more preferably 900 ppm by mass or less. The nitrogen content in the magnet base material 20 is preferably 1000 ppm by mass or less, and more preferably 600 ppm by mass or less. The oxygen content in the magnet base material 20 is preferably 1200 ppm by mass or less, and more preferably 800 ppm by mass or less.

[0033] Furthermore, in addition to the above-mentioned elements, the magnet base material 20 may contain inevitable impurities such as Mn, Ca, Cl, S, and F, and the total content of the inevitable impurities is, for example, about 0.001% to 1.0% by mass.

[0034] The composition of the magnet substrate 20 can be analyzed by a method generally known in the art. For example, the content of various elements such as R, T, and B can be measured by X-ray fluorescence analysis (XRF) or inductively coupled plasma emission spectrometry (ICP). For example, the oxygen content can be measured by inert gas fusion-non-dispersive infrared absorption method, the carbon content can be measured by combustion in oxygen flow-infrared absorption method, and the nitrogen content can be measured by inert gas fusion-thermal conductivity method.

[0035] As shown in FIG. 3A, the magnet base material 20 is R 2 T 14 It contains main phase grains 4 made of B crystals and grain boundaries 6 located between the main phase grains 4, and may also contain other subphases to the extent that they do not impair the magnetic properties.

[0036] The average particle size of the main phase particles 4 is not particularly limited, and may be, for example, 1.0 μm to 10 μm, and preferably 2.5 μm to 6.0 μm, calculated as the equivalent circle diameter. The average particle size of the main phase particles 4 can be measured by observing a cross section of the magnet substrate 20 as shown in Fig. 3A with various electron microscopes (SEM, STEM, TEM), and measuring the equivalent circle diameters of at least 20 main phase particles 4 contained in the cross section.

[0037] In addition, R constituting the main phase particle 4 2 T 14 In the B crystal, a part of the iron group element T may be substituted with a transition metal element such as an m element.

[0038] The grain boundaries 6 include two-particle boundaries 6a located between two adjacent main phase particles 4, and grain boundary multiple points 6b surrounded by three or more main phase particles 4. The grain boundaries 6 are also formed by connecting other phases (i.e., R 2 T 14 The grain boundaries 6 are composed of a phase other than the B crystal phase, and the type and ratio of the phases constituting the grain boundaries 6 are not particularly limited. Examples of the other phases constituting the grain boundaries 6 include a phase (R-rich layer) having a higher concentration of R than the main phase particles 4, a phase having a high concentration of transition metal elements such as T (iron group elements) and Ga, an oxide layer of rare earth elements, and an ROC phase.

[0039] The magnet base material 20 having the above-mentioned characteristics can be manufactured through a process including a raw material alloy production process, a process of pulverizing the raw material alloy (pulverizing process), a process of molding the raw material alloy powder (molding process), and a process of sintering the molded body (sintering process).

[0040] First, a raw material metal corresponding to the composition of the RTB alloy described above is prepared, and the prepared raw material metal is melted in a vacuum or in an inert gas atmosphere such as Ar gas. The molten raw material metal is then cast to obtain a raw material alloy.

[0041] In this case, the type of raw material metal is not particularly limited, and for example, rare earth metals or rare earth alloys, pure iron, pure cobalt, ferroboron, and further alloys and compounds thereof can be used. In addition, the method for casting the raw material metal is also not particularly limited, and for example, ingot casting, strip casting, book molding, centrifugal casting, etc. can be mentioned. In addition, if the raw material alloy after casting has solidification segregation, it may be subjected to homogenization treatment (solution treatment) as necessary.

[0042] Next, the raw alloy obtained in the above steps is pulverized. From the viewpoint of obtaining high magnetic properties, it is preferable that the atmosphere in each step from the pulverization step to the sintering step is an atmosphere with a low oxygen concentration. An atmosphere with a low oxygen concentration is, for example, an atmosphere with an oxygen concentration of 200 ppm or less. By controlling the oxygen concentration in each step, it is possible to control the amount of oxygen contained in the magnet base material 20 and the final permanent magnet 2 obtained.

[0043] The pulverization step is carried out in two stages, namely, coarse pulverization and fine pulverization, although the raw alloy may be pulverized in a single stage, namely, the fine pulverization step alone.

[0044] In the coarse pulverization step, the material is coarsely pulverized until the particle size is about several hundred μm to several mm, to obtain a coarsely pulverized powder. The method of coarse pulverization is not particularly limited, and for example, a method of performing hydrogen absorption pulverization or a method using a coarse pulverizer can be adopted. When performing hydrogen absorption pulverization, the amount of nitrogen contained in the magnet base material 20 and the final permanent magnet 2 can be controlled by controlling the nitrogen gas concentration in the atmosphere during the dehydrogenation process.

[0045] Next, the obtained coarsely pulverized powder is pulverized until the average particle size is about several μm to obtain a pulverized powder (raw alloy powder). The average particle size of the pulverized powder is not particularly limited, but can be, for example, 1 μm to 10 μm, and preferably 2 μm to 6 μm. In the pulverization process, the nitrogen gas concentration in the atmosphere is controlled to control the amount of nitrogen contained in the magnet base material 20 and the final permanent magnet 2.

[0046] The method of pulverization is not particularly limited, and various types of pulverizers can be used. In addition, it is preferable to add a pulverization aid during pulverization, and examples of the pulverization aid include lauric acid amide and oleic acid amide. By using the pulverization aid, it is possible to obtain a pulverized powder with high orientation during molding. It is possible to control the amount of carbon contained in the magnet base material 20 and the final permanent magnet 2 by changing the amount of pulverization aid added.

[0047] In the above steps (from the step of preparing the raw alloy to the step of crushing), the raw alloy powder was obtained by the one-alloy method, but a two-alloy method may also be used in which two alloys, a first alloy and a second alloy, are mixed to produce the raw alloy powder.

[0048] Next, the obtained raw alloy powder is molded into a predetermined shape. The molding method is not particularly limited, and may be dry molding or wet molding. In this embodiment, the raw alloy powder is filled into a die and compressed in a magnetic field (dry molding).

[0049] The pressure during compaction can be, for example, 20 MPa to 300 MPa, and the applied magnetic field can be 950 kA / m to 1600 kA / m. The applied magnetic field is not limited to a static magnetic field, and can be a pulsed magnetic field, or a static magnetic field and a pulsed magnetic field can be used in combination. When wet compaction is employed, the raw alloy powder is dispersed in a solvent such as oil to form a slurry, and the slurry is used for press compaction in the same manner as above.

[0050] Next, the above-mentioned compact is sintered in a vacuum or in an inert gas to obtain a sintered body. The sintering conditions may be appropriately determined depending on various conditions such as the composition, the crushing method, and the particle size of the raw alloy powder. For example, the compact can be sintered by holding it in a vacuum or in an inert gas at a temperature of 1000°C to 1200°C for 1 hour to 10 hours.

[0051] After the sintering step, the sintered body may be subjected to a decarbonization treatment as necessary. The method of the decarbonization treatment is not particularly limited, and any known method may be used. For example, the carbon content in the sintered body can be reduced by attaching a predetermined metal S to the sintered body and heat treating it. In the above, the predetermined metal S is a metal whose standard Gibbs energy of formation for generating metal carbide from the metal is lower than that of the rare earth elements (especially Nd) in the sintered body. By attaching the metal S to the sintered body and heat treating it, the carbon in the sintered body reacts with the metal S to become a carbide. The attached metal S hardly penetrates into the sintered body and remains on the surface of the sintered body. By carrying out the decarbonization treatment as described above, the amount of carbon contained in the magnet base material 20 and the permanent magnet 2 finally obtained can be reduced.

[0052] Furthermore, the sintered body may be subjected to shaping such as cutting or grinding, chamfering such as barrel polishing, etc., as necessary. These processes are carried out before the diffusion step described below.

[0053] By the above method, the magnet substrate 20 shown in FIG. 1 and FIG. 3A is obtained.

[0054] (Grain boundary diffusion process) Next, the grain boundary diffusion process (first diffusion process and second diffusion process) will be described. As described above, in this embodiment, the first diffusion process is performed to diffuse mainly light rare earth elements into the magnet base material 20, and the second diffusion process is performed to diffuse mainly heavy rare earth elements into the magnet base material 20 (see FIG. 2).

[0055] Preparation of diffusion material First, the first diffusion material 11 used in the first diffusion step and the second diffusion material 12 used in the second diffusion step are prepared.

[0056] The first diffusing material 11 contains at least one light rare earth element (RL), and the added RL is preferably one or more elements selected from the group consisting of Nd and Pr. The first diffusing material 11 can be a pure metal, an alloy, or a compound containing an RL, such as a hydride, and is particularly preferably an RL-M alloy containing an RL and a predetermined M element.

[0057] In the above, the M element is an element having a eutectic temperature of 800° C. or less with respect to M and RL, and specifically, may be one or more elements selected from the group consisting of Al, Mg, Fe, Mn, Co, Ni, Cu, Zn, Ga, Ge, Ru, Rh, Pd, Ag, Sn, Sb, Pt, Au, Hg, Bi, Si, and Cl. Preferably, the M element is an element having a eutectic temperature of 700° C. or less with respect to M and RL, and specifically, may be one or more elements selected from the group consisting of Al, Mg, Fe, Mn, Co, Ni, Cu, Zn, Ga, Ag, Au, Hg, Si, and Cl. More preferably, the M element is an element having a eutectic temperature of 600° C. or less with respect to Mg, Co, Ni, Cu, or Cl. More preferably, the M element is Cu or Co.

[0058] In addition, if the sum of the contents of the rare earth element R and the M element contained in the first diffusion material 11 (i.e., R+M or RH+RL+M) is taken as 100 mass%, the total content of the M element in the first diffusion material 11 (RL-M alloy) is preferably, for example, 5 mass% to 20 mass%, depending on the type of the M element selected. In particular, when Cu is added as the M element, the content of Cu in the first diffusion material 11 (RL-M alloy) is preferably 10 mass% to 15 mass%. Note that the above content is the ratio of the M element to 100 mass% of the first diffusion material. By including the above M element in the first diffusion material 11, the melting point of the first diffusion material 11 is lowered, and RL is easily diffused into the magnet base material 20.

[0059] The first diffusing material 11 may contain a heavy rare earth element (RH), but the content of RH is preferably 10 mass% or less relative to 100 mass% of the sum of the contents of R and M elements in the first diffusing material. However, it is more preferable that the first diffusing material 11 does not substantially contain RH. More specifically, "substantially does not contain RH" means that the content of RH is less than 0.5 mass%.

[0060] On the other hand, the second diffusion material 12 contains at least one heavy rare earth element RH, and the added RH is preferably one or more elements selected from the group consisting of Tb and Dy. The second diffusion material 12 is a pure metal, an alloy, or TbH 2 The M element in the second diffusing material 12 may be the same as the M element in the first diffusing material 11, and the amount of the M element added may be the same as that in the first diffusing material 11. The type of the M element selected for the first diffusing material 11 and the second diffusing material 12 may be different or the same.

[0061] In addition, the second diffusing material 12 may contain RL in addition to the elements RH and M. In this case, the content of RL is preferably 22.5 mass% or less relative to 100 mass% of the sum of the contents of R and M elements contained in the second diffusing material (i.e., R+M or RH+RL+M). In the second diffusing material 12, it is preferable to adjust the amounts of RL and M elements added so that the content of RH is 60 mass% or more.

[0062] First diffusion process In the first diffusion process, the above-mentioned first diffusion material 11 is attached to at least a portion of the surface of the magnet base material 20, and then the magnet base material 20 is heat-treated under predetermined conditions, thereby diffusing the RL and M elements in the first diffusion material 11 into the interior of the magnet base material 20.

[0063] The surface of the magnet base material 20 to which the first diffusion material 11 is attached is preferably at least a part of the main surface 20a serving as the magnetic pole surface. In this case, the first diffusion material 11 may be attached to only one of the pair of main surfaces 20a, or may be attached to both main surfaces 20a. When the thickness of the magnet base material 20 in the Z-axis direction (the distance between the magnetic pole surfaces) is as thin as 2 mm or less, it is preferable to attach the first diffusion material 11 to only one of the main surfaces 20a. In addition, the first diffusion material 11 may be attached to at least a part of the side surface 20b serving as the non-magnetic pole surface. The number of surfaces to which the first diffusion material 11 is attached and the attachment area thereof may be appropriately determined according to the dimensions of the magnet base material 20 and the application of the RTB permanent magnet 2, which is the target object. In this embodiment, as an example, the first diffusion material 11 is attached to the entire surface of the main surface 20a above the Z-axis.

[0064] Furthermore, the method for attaching the first diffusion material 11 to the surface of the magnet base material 20 is not particularly limited, and for example, a vapor deposition method, a sputtering method, an electrodeposition method, a coating method, a printing method (such as screen printing or squeegee printing), a sheet method, etc. can be used.

[0065] When the sheet method is employed, the powdered first diffusion material 11 and a binder are mixed together to prepare a sheet 11a of the first diffusion material as shown in Fig. 2, and the sheet 11a is adhered to the surface of the magnetic substrate 20. When adhering the sheet 11a to the magnetic substrate 20, an organic solvent such as alcohol, aldehyde, or ketone may be applied to the surface of the sheet 11a or the surface of the magnetic substrate 20.

[0066] When the coating method is adopted, a slurry is prepared by dispersing the powdered first diffusion material 11 in an organic solvent such as alcohol, aldehyde, or ketone. Then, the slurry is applied to the surface of the magnet base material 20 using a spray, a brush, a jet dispenser, a nozzle, or the like. A binder may be added to the slurry so that the first diffusion material 11 can easily adhere to the surface of the magnet base material 20. A paste having a higher viscosity than the slurry may be prepared using the first diffusion material 11, and the paste may be applied to the surface of the magnet base material 20. In various printing methods, the above paste may be printed on the surface of the magnet base material 20.

[0067] As described above, the first diffusion material 11 can be attached to the magnet base material 20 by a number of methods, but whichever method is adopted, it is preferable to control the amount of the first diffusion material 11 attached to satisfy a predetermined condition. That is, it is preferable to control the amount of the first diffusion material 11 attached so that the total amount of RL to be attached is 0.1 to 2.0 parts by mass (more preferably 0.4 to 1.5 parts by mass) relative to 100 parts by mass of the magnet base material.

[0068] The conditions for the heat treatment in the first diffusion step are that the heat treatment atmosphere is in a vacuum or in an inert gas, the holding temperature is preferably above 700°C and below 1000°C, and the temperature holding time is preferably 1 hour to 24 hours. After the predetermined holding time has elapsed, the magnet base material 20 is preferably rapidly cooled, and for example, the cooling rate during rapid cooling is preferably 50°C / min or more. By carrying out the heat treatment under the above conditions, the RL contained in the first diffusion material 11 (RL and the M element when the M element is contained) diffuses into the grain boundaries 6 of the magnet base material 20.

[0069] It is believed that by diffusing RL into the magnet base material 20 in the first diffusion step, the grain boundaries 6 (particularly the two-particle grain boundaries 6a) expand, and RH is more likely to diffuse to the center of the magnet base material 20 in the second diffusion step described below. When the magnet base material 20 contains only Nd as R and the first diffusion material 11 contains RL other than Nd, such as Pr, a shell containing RL other than Nd may be formed on the outer periphery of the main phase grains 4 by the first diffusion step. This shell is R 2 T 14 It is believed that this is generated by the replacement of part of R(Nd) in the B crystal with RL other than Nd.

[0070] After the first diffusion step, residues such as an oxide film may remain on the surface of the magnet base material 20. Therefore, it is preferable to carry out a processing step to remove the residues after the first diffusion step. The method for removing the residues is not particularly limited, and may be, for example, chemical removal such as etching, physical cutting, shaping such as grinding, or chamfering such as barrel polishing.

[0071] Second diffusion process Next, a second diffusion step is performed using the above-mentioned second diffusion material 12. In the second diffusion step, the second diffusion material 12 is attached to at least a part of the surface of the magnet base material 20, and then the magnet base material 20 is heat-treated under predetermined conditions, thereby diffusing the RH and M elements in the second diffusion material 12 into the inside of the magnet base material 20.

[0072] The second diffusion material 12 is preferably attached to the surface (principal surface 20a and side surface 20b) of the magnet substrate 20 to which the first diffusion material 11 was attached in the first diffusion step. For example, as shown in FIG. 2, when the first diffusion material 11 is attached to the principal surface 20a (pole surface) above the Z axis, the second diffusion material 12 is preferably attached to the principal surface 20a above the Z axis in the same manner as the first diffusion material 11. The attachment area of ​​the second diffusion material 12 may be larger or smaller than the attachment area of ​​the first diffusion material 11, but is preferably about the same. When the attachment area of ​​the second diffusion material 12 is made smaller, the second diffusion material 12 is preferably attached to a portion of the resulting permanent magnet where it is desired to improve the coercive force HcJ in particular.

[0073] In addition, the method for attaching the second diffusion material 12 is not particularly limited, and similarly to the first diffusion step, vapor deposition, sputtering, electrodeposition, coating, printing (screen printing, squeegee printing, etc.), sheeting, etc. can be used. Fig. 2 shows, as an example, the use of a sheet 12a of the second diffusion material, which is obtained by mixing the powdered second diffusion material 12 with a binder and forming the mixture into a sheet.

[0074] In addition, the amount of the second diffusion material 12 attached is preferably controlled to satisfy a predetermined condition. That is, the amount of the second diffusion material 12 attached is preferably controlled so that the total amount of RH attached is 0.3 to 2.0 parts by mass (more preferably 0.4 to 1.0 parts by mass) relative to 100 parts by mass of the magnet base material.

[0075] The conditions of the heat treatment in the second diffusion step are that the heat treatment atmosphere is in a vacuum or in an inert gas, the holding temperature is preferably more than 700°C and not more than 1000°C, and the temperature holding time is preferably 1 hour or more and not more than 24 hours. After the predetermined holding time has elapsed, it is preferable to rapidly cool the magnet base material 20, and for example, the cooling rate during rapid cooling is preferably 50°C / min or more. By performing the heat treatment under the above conditions, RH (RH and M element when M element is included) contained in the second diffusion material 12 is diffused to the grain boundary 6 of the magnet base material 20. The second diffusion step may include an aging step. The aging step is preferably performed by holding the magnet base material 20 at a temperature of 450°C to 700°C for 0.2 hours to 3 hours in a vacuum or in an inert gas after the above rapid cooling, and it is preferable to rapidly cool the magnet base material 20 after the holding time has elapsed.

[0076] The RH diffused to the grain boundary 6 in the second diffusion step is R 2 T 14 RH reacts with a part of the B crystals and becomes concentrated. That is, after the second diffusion step, as shown in FIG. 3B, a shell portion 42 with a high content of RH is formed in the main phase particle 4 in the region where RH has diffused, and the main phase particle 4 becomes a core-shell particle 4a. The core-shell particle 4a will be described in detail later in the explanation of the RTB permanent magnet 2.

[0077] It is preferable to carry out a process for removing residues after the second diffusion step as in the case of the first diffusion step. The method for removing residues is not particularly limited, and may be, for example, chemical removal such as etching, physical cutting, shaping such as grinding, or chamfering such as barrel polishing.

[0078] By the above method, an RTB permanent magnet 2 (FIG. 4A) that combines high residual magnetic flux density and high coercivity can be obtained. Below, the features of the RTB permanent magnet 2 obtained by the manufacturing method of this embodiment will be described.

[0079] (RTB permanent magnet 2) In the RTB permanent magnet 2 (hereinafter referred to as permanent magnet 2) of this embodiment shown in Fig. 4A, a pair of main surfaces 2a are magnetic pole surfaces, and of the pair of main surfaces 2a, the main surface 2a above the Z axis is the surface to which the first diffusion material 11 and the second diffusion material 12 are attached. Note that in Fig. 4A, the permanent magnet 2 has a rectangular parallelepiped shape in accordance with the shape of the magnet base material 20 in Fig. 1. However, the shape and dimensions of the permanent magnet 2 are not particularly limited, and may be, for example, a polygonal shape, a cylindrical shape, a hollow cylindrical shape, or an arc segment shape in which the main surface is curved in an arc shape.

[0080] The permanent magnet 2 has a composition that is slightly different from the composition of the magnet base material 20 used during production, due to the grain boundary diffusion of RL and RH in this order during the production process.

[0081] Specifically, the permanent magnet 2 contains one or more light rare earth elements (RL) essential for Nd, and one or more heavy rare earth elements (RH) as R. RL other than Nd preferably contains Pr, and RH preferably contains Tb and / or Dy.

[0082] The total content of R relative to 100% by mass of the permanent magnet can be 25% to 35% by mass, and is preferably 28.4% by mass or more and 32.0% by mass or less. The total content of RL relative to 100% by mass of the permanent magnet is preferably 26.0% by mass or more and 31.5% by mass or less, and the total content of RH is preferably 0.3% by mass or more and 3.0% by mass or less. In addition, the content of Nd relative to 100% by mass of the permanent magnet is preferably 22.4% by mass or more and 31.5% by mass or less.

[0083] As described above, in the permanent magnet 2, the R content increases compared to the R content in the magnet base material 20 depending on the amount of RL and RH diffused by the diffusion materials (11, 12). On the other hand, the B content in the permanent magnet 2 can be made approximately the same as the B content in the magnet base material 20. That is, the B content relative to 100 mass% of the permanent magnet can be 0.5 mass% to 1.5 mass%, and is preferably 0.92 mass% to 1.03 mass%. When the B content satisfies the above composition range, the magnetic properties (Br, HcJ, squareness ratio Hk / HcJ, etc.) of the permanent magnet 2 tend to be further improved.

[0084] Moreover, it is preferable that the permanent magnet 2 contains the element M added to the first diffusion material 11 and / or the second diffusion material 12. The content C of the element M resulting from the diffusion materials (11, 12) M is preferably 0.5 mass% or less, and more preferably 0.05 mass% to 0.2 mass% with respect to 100 mass% of the permanent magnet. For example, the element M added to the diffusion material may be an element M that is not substantially contained in the magnet base material 20. NO If you select (Ag, Au, etc.), the above content C M is the element M in permanent magnet 2 NO On the other hand, as the M element to be added to the diffusion material, the element M originally contained in the magnet base material 20 is IN When element M in permanent magnet 2 is selected, IN The content of is the content in the magnet base material 20 plus the above content C M is added to form the range.

[0085] For example, when Fe, Co, or Ni is added to the first diffusion material 11 and / or the second diffusion material 12, the T content in the permanent magnet 2 increases slightly compared to the magnet base material 20 during the manufacturing process (the above content C M(Addition is made to the total content of Co). The content of T in the permanent magnet 2 is expressed as the balance. The T in the permanent magnet 2 may be Fe alone, or a portion of Fe may be substituted with Co. In this case, the content of Co is not particularly limited, and may be, for example, 4 mass % or less, and preferably 1 mass % or less. The inclusion of Co improves the corrosion resistance of the permanent magnet 2.

[0086] Moreover, the permanent magnet 2 preferably contains one or more m elements selected from the group consisting of Cu, Ga, Al, and Zr, and more preferably contains Cu as the m element. The m elements are added to the permanent magnet 2 via the magnet base material 20 and / or the diffusion materials (11, 12). The total content of the m elements relative to 100% by mass of the permanent magnet is preferably 0.05% by mass to 1.5% by mass, and more preferably 0.5% by mass to 1.0% by mass.

[0087] More specifically, the content of Cu relative to 100% by mass of the permanent magnet can be 0.05% by mass or more and 0.70% by mass or less, and preferably 0.20% by mass or more and 0.70% by mass or less. By including Cu in the above ratio, the magnetic properties and corrosion resistance of the permanent magnet 2 are further improved. In addition, when Ga, Al, and Zr are included as the m element, the contents of these elements are not particularly limited. For example, the content of Ga can be 0.08% by mass or more and 0.50% by mass or less, and preferably 0.08% by mass or more and 0.3% by mass or less. The content of Al and the content of Zr can be 0.10% by mass or more and 0.50% by mass or less, and preferably 0.10% by mass or more and 0.30% by mass or less. By including Ga, Al, Zr, etc. in the above-mentioned predetermined amounts, it is possible to further improve the magnetic properties (Br, HcJ, Hk / HcJ, etc.), reduce the variation in properties, and improve the manufacturing stability.

[0088] The permanent magnet 2 may also contain carbon (C), nitrogen (N) and oxygen (O). The carbon content in the permanent magnet 2 is preferably 1100 ppm by mass or less, and more preferably 900 ppm by mass or less. The nitrogen content in the permanent magnet 2 is preferably 1000 ppm by mass or less, and more preferably 600 ppm by mass or less. The lower the carbon content and nitrogen content, the higher the coercive force HcJ tends to be. The oxygen content in the permanent magnet 2 is preferably 1200 ppm by mass or less, and more preferably 800 ppm by mass or less. The lower the oxygen content, the higher the corrosion resistance tends to be.

[0089] Furthermore, in addition to the above-mentioned elements, permanent magnet 2 may contain inevitable impurities such as Mn, Ca, Cl, S, and F, and the total content of the inevitable impurities is, for example, about 0.001% to 1.0% by mass.

[0090] The composition of the permanent magnet 2 can be measured by XRF, ICP, inert gas fusion-non-dispersive infrared absorption method, oxygen flow combustion-infrared absorption method, inert gas fusion-thermal conductivity method, etc., in the same manner as the composition analysis of the magnet substrate 20.

[0091] In the permanent magnet 2 of this embodiment, a concentration distribution of a predetermined element occurs inside. Specifically, the total content of RL continuously decreases from the main surface 2a (pole surface) in the depth direction (i.e., from the surface of the permanent magnet 2 toward the inside). Such a concentration distribution of RL occurs due to grain boundary diffusion of RL in the first diffusion step. Moreover, in the permanent magnet 2, the total content of RH continuously decreases from the main surface 2a (pole surface) in the depth direction. This concentration distribution of RH occurs due to grain boundary diffusion of RH in the second diffusion step.

[0092] Furthermore, in the permanent magnet 2, it is preferable that the content of the M element (preferably one or more selected from Cu, Al, Fe, and Co) continuously decreases from the main surface 2a (pole surface) toward the depth direction. Such a concentration distribution of the M element is generated by the grain boundary diffusion of the M element in the diffusion material (11, 12) in the first diffusion step and / or the second diffusion step. When an iron-group element (Fe, Co, or Ni) is added as the M element in the diffusion material (11, 12), the above-mentioned concentration distribution of the M element is the concentration distribution of T. Therefore, when an iron-group element is selected as the M element of the diffusion material, it is preferable that the content of T continuously decreases from the main surface 2a (pole surface) toward the depth direction.

[0093] The concentration distribution of each of the above-mentioned elements (RL, RH, M elements) can be confirmed using multiple samples β shown in Fig. 4B. Specifically, samples β of a predetermined width Tβ (width in the Z-axis direction) are continuously collected from the main surface 2a along the depth direction (toward the inside of the permanent magnet 2), and each of the collected multiple samples β is subjected to component analysis using ICP. In this case, it is preferable that the predetermined width Tβ is 1 mm or less, or that Tβ<(1 / 10)×T0.

[0094] In the permanent magnet 2 of this embodiment, the results of the above analysis confirmed that the total content of RL, the total content of RH, and the content of M tended to decrease continuously and gradually as the location of the sample β increased. In particular, the sample β1 on the outermost surface side and the sample β in the center center (sample β taken at a depth of 1 / 2T0 from the main surface 2a) and the difference in the content of a specified element (β1-β center ), the difference in the total content of RL is preferably about 0.1% by mass to 0.5% by mass, the difference in the total content of RH is preferably about 0.1% by mass to 0.5% by mass, and the difference in the content of M element is preferably about 0.1% by mass to 0.3% by mass.

[0095] In addition to the above measurement methods, the concentration distribution of each element (RL, RH, M elements) can also be confirmed by performing line analysis or mapping analysis using EDX or EPMA, or laser ablation-ICP mass spectrometry (LA-ICP-MS) on a cross section such as that shown in Figure 4B.

[0096] 3B is a schematic diagram showing an enlarged cross section of the permanent magnet 2 in this embodiment. As described above, in the permanent magnet 2, the main phase particles 4 are core-shell particles 4a in the region where RH is diffused. The core-shell particles 4a are R 2 T 14 The core-shell particles 4a have a core portion 41 made of B crystals and a shell portion 42 that covers the core portion 41 and has a higher content of heavy rare earth elements than the core portion 41. The average particle size of the core-shell particles 4a is not particularly limited and can be, for example, 1.0 μm to 10 μm, and preferably 2.5 μm to 6.0 μm, in terms of the circle-equivalent diameter.

[0097] It is not necessary for the shell portion 42 to cover the entire periphery of the core portion 41, but it is sufficient for the shell portion 42 to cover at least a portion of the core portion 41. The coverage rate of the core portion 41 by the shell portion 42 is not particularly limited, but for example, it is preferable that the shell portion 42 covers 50% or more of the outer periphery of the core portion 41. In the cross section shown in Fig. 3B, it is not necessary for all the main phase particles 4 to be core-shell particles 4a, and there may be main phase particles 4 that do not have a core-shell structure.

[0098] As described above, the shell portion 42 in which RH is concentrated is formed on the outer periphery of the main phase grain 4, which suppresses the generation of nuclei of magnetization reversal near the grain boundaries, thereby improving the coercive force HcJ.

[0099] In addition, in the permanent magnet 2 of this embodiment, the shell thickness of the core-shell particles 4a in the vicinity of the surface where RH is diffused (in this embodiment, the vicinity of the main surface 2a) can be made thinner than in a conventional permanent magnet in which RH is diffused by only one stage of grain boundary diffusion treatment. In fact, FIG. 6 is a cross-sectional photograph of the permanent magnet 2 of this embodiment in which two stages of grain boundary diffusion treatment have been performed, and FIG. 7 is a cross-sectional photograph of a conventional permanent magnet in which only one stage of grain boundary diffusion treatment has been performed. Note that both FIG. 6 and FIG. 7 are cross sections perpendicular to the surface (main surface 2a) to which the diffusion material is attached, and are cross sections observed in a range from the surface to a predetermined depth. In addition, in FIG. 6 and FIG. 7, the area with the brightest contrast is the grain boundary phase, the area with the darkest contrast is the core portion 41 (main phase particle 4), and the gray contrast surrounding the core portion 41 is the shell portion 42.

[0100] In the conventional permanent magnet shown in Fig. 7, the presence of a gray shell portion around the core portion is clearly visible, and it can be confirmed that a thick shell portion on the order of submicrons to microns is formed near the surface (up to a depth of 100 µm). On the other hand, in the cross section of the permanent magnet 2 of this embodiment shown in Fig. 6, it can be seen that the thickness of the shell portion 42 near the surface is clearly thinner than that of the conventional permanent magnet in Fig. 7.

[0101] More specifically, in the permanent magnet 2 of this embodiment, in the cross section A at a depth of 100 μm from the surface (main surface 2a), the maximum thickness t1 of the shell portion 42 is, on average, 0.5 μm or less, preferably 0.2 μm or less, and more preferably 0.1 μm or less. By controlling the maximum thickness t1 of the shell portion 42 within the above range near the surface of the permanent magnet 2, a higher residual magnetic flux density Br and a higher coercive force HcJ can be obtained than the conventional permanent magnet shown in FIG. 7. The reason why the magnetic properties are improved in this way is not necessarily clear, but it is thought to be related to the RH concentration in the shell portion 42. Specifically, it is thought that by reducing the thickness of the shell portion 42, the RH concentration in the shell portion 42 becomes higher than that of the conventional permanent magnet (FIG. 7). As a result, it is thought that the permanent magnet 2 of this embodiment improves HcJ more efficiently without decreasing Br.

[0102] Furthermore, in the permanent magnet 2 of this embodiment, as described above, the thickness of the shell portion 42 becomes thinner near the surface, and RH diffuses deeper into the interior of the permanent magnet 2. Specifically, even in the case of the permanent magnet 2 where the diffusion material (11, 12) is attached only to the principal surface 2a on one side, it can be confirmed that the core-shell particles 4a are present within a range of 3.5 mm deep from the principal surface 2a, and an improvement in HcJ can be expected up to a depth of 3.5 mm.

[0103] The maximum thickness t1 of the shell portion 42 is calculated based on, for example, an analysis using STEM-EDS. First, a cross section A (for example, the XY plane shown by the dashed line in FIG. 4B) is exposed at a depth of 100 μm from the main surface 2a to which the diffusion materials (11, 12) are attached, and a sample for STEM observation is taken from the cross section. The method for taking the sample may be a microsampling method using FIB processing or the like.

[0104] Then, the main phase particles 4 (core-shell particles 4a) contained in the collected observation sample (observation cross section) are analyzed by STEM-EDS. In this embodiment, the core portion 41 and the shell portion 42 are distinguished based on the concentration difference Dc of the heavy rare earth element and the concentration degree E of the heavy rare earth element. Specifically, in the cross section analysis, a virtual rectangle VR (see FIG. 5) is prepared that contains the main phase particle 4 to be measured and has the smallest area relative to the main phase particle 4, and the intersection of the diagonals of the rectangle VR is set as the particle center 41c. Then, after obtaining the concentration distribution of RH and the concentration distribution of RL in the main phase particle 4 by EDS, the RH concentration (Ch n ) and the RH concentration at the particle center 41c (Ch center ) and the difference (Ch n -Ch center ) is defined as the concentration difference of RH, Dc (unit: wt%). Also, the molar ratio of RH to RL at a given point is M H / L n The molar ratio of RH to RL in the particle center 41c is M H / L center And, M H / L center M H / L n The ratio of these is the RH concentration E (no unit).

[0105] In this embodiment, in the shell portion 42, the concentration difference Dc is 0.7 wt% or more, and the enrichment degree E is 1.25 or more. That is, in the cross-sectional analysis, a region that satisfies these two requirements is recognized as the shell portion 42, and a region of the main phase particle 4 other than the shell portion 42 is recognized as the core portion 41. However, there may be cases where the RH concentration detected in the particle center 41c is less than 0.2 wt%. In this case, in consideration of measurement noise, it is considered that substantially no RH is detected in the particle center 41c (i.e., Ch center ≒0), and the region where the RH concentration is 0.7 wt% or more (i.e., the concentration difference Dc is 0.7 wt% or more) can be identified as the shell portion 42. When the cross-sectional sample is observed using an HAADF image or the like, it is also possible to simply distinguish the core portion 41 from the shell portion 42 based on the difference in contrast.

[0106] After defining the boundary between the core portion 41 and the shell portion 42 by the above-mentioned method, the thickness of the thickest portion of the shell portion 42 within the unit particle is measured as shown in Fig. 5. This measurement is performed for at least 20 core-shell particles 4a, and the average value is taken as the above-mentioned maximum thickness t1. The shell thickness can also be analyzed using a three-dimensional atom probe (3DAP).

[0107] The diffusion depth of RH can be measured by analyzing samples β (FIG. 4B) taken continuously from the surface (principal surface 2a) of the permanent magnet 2 along the depth direction. For example, by observing the cross sections of multiple samples β with STEM and checking the presence or absence of core-shell particles 4a, it is possible to measure the depth to which RH has diffused. In addition, by measuring the magnetic properties of multiple taken samples β with various BH tracers, it is possible to measure the depth to which an increase in HcJ can be observed.

[0108] Specifically, the magnetic properties of the permanent magnet 2 are preferably Br of 1450 mT or more and HcJ of 1800 kA / m or more. When the permanent magnet 2 satisfies these magnetic properties, the performance and efficiency of a motor having the permanent magnet 2 can be improved.

[0109] (Applications of RTB permanent magnets 2) The RTB permanent magnet 2 of the present embodiment can be used as a component of motors, generators, compressors, actuators, magnetic sensors, speakers, etc., and is particularly suitable as a component of motors.

[0110] An example of a motor using a permanent magnet 2 is an IPM motor 50 as shown in Fig. 8. The IPM motor 50 has a rotor 51 and a stator core 52, and the permanent magnet 2 of this embodiment is embedded in the rotor 51. The permanent magnet 2 in the rotor 51 faces a coil 54 present in the stator via a gap 53. The permanent magnet 2 of this embodiment is not limited to the IPM motor of Fig. 8, and can be applied to various motors such as an SPM motor.

[0111] Furthermore, the motor including the permanent magnet 2 of this embodiment can be mounted on various electronic devices, industrial devices, etc., and is particularly suitable for use as an automobile motor 50 (EV, HV, PHV, etc.) as shown in Fig. 9. In Fig. 9, a typical EV 101 and HV 102 are shown in a simple schematic diagram, but the use of the motor including the permanent magnet 2 is not limited to the embodiment shown in Fig. 9. In Fig. 9, reference numeral 60 denotes an inverter, reference numeral 70 denotes a battery, reference numeral 80 denotes an engine, and reference numeral 90 denotes a generator.

[0112] (Summary of the embodiment) In the manufacturing method of the RTB permanent magnet 2 in this embodiment, a first diffusion step is carried out in a first diffusion material 11 containing a light rare earth element (RL), and then a second diffusion step is carried out in a second diffusion material 12 containing a heavy rare earth element (RH). In other words, a two-stage grain boundary diffusion is carried out in which RL is diffused and then RH is diffused.

[0113] In the RTB permanent magnet 2 obtained by this method, the maximum thickness t1 of the shell portion 42 at a location 100 μm deep from the surface of the magnet is thin, t1≦0.5 μm, preferably t1≦0.2, and more preferably t1≦0.1. In this way, by reducing the thickness of the shell portion 42 near the surface, it is possible to further increase the RH concentration in the shell portion 42, and it is believed that RH is favorably diffused to the inside of the magnet. As a result, in the RTB permanent magnet 2, Br and HcJ are improved more than ever before. In other words, the two-stage grain boundary diffusion treatment of this embodiment provides a permanent magnet 2 that has both a higher residual magnetic flux density Br and a higher coercive force HcJ than the conventional one-stage grain boundary diffusion treatment.

[0114] The reason why the above-mentioned effect is obtained by the two-stage grain boundary diffusion treatment is not necessarily clear, but the following reasons are considered, for example.

[0115] First, R by RH 2 T 14It is believed that the suppression of decomposition of B crystals (main phase) is related to this. In the grain boundary diffusion treatment, RH penetrates along the grain boundaries and becomes R 2 T 14 When it comes into contact with B crystal, R 2 T 14 B crystal (especially Nd 2 Fe 14 The outer edge of the B crystal reacts with RH, forming a crystal phase or liquid phase (e.g., RFe 2 Phase and RFe 4 B 4 The decomposition is thought to result in the formation of different crystalline and liquid phases, which then recrystallize to form the RH-enriched shell.

[0116] When RH is diffused into grain boundaries in a single diffusion process as in the past, high concentration RH is diffused near the surface of the magnet. 2 T 14 B crystal, and the above-mentioned R 2 T 14 It is believed that the decomposition reaction of B crystals occurs actively. As a result, in conventional grain boundary diffusion treatment, a thick shell is formed near the surface of the magnet. Although the shell portion where RH is concentrated has the effect of improving HcJ, the thickness of the shell required to improve HcJ is only required to be on the order of a few nanometers, and it is believed that an excessively thick shell will in turn lead to a decrease in Br. Furthermore, in each conventional process stage, much of the attached RH is consumed near the surface of the magnet, making it difficult for it to diffuse sufficiently into the interior of the magnet, which is believed to weaken the effect of improving HcJ.

[0117] On the other hand, in the two-stage grain boundary diffusion treatment in this embodiment, RL is diffused before RH is diffused. 2 T 14 Between B crystals (specifically, Nd 2 Fe 14 B crystal and Nd or Pr) 2 T 14 Since no metal compound phase other than B is generated, in the first diffusion step of this embodiment, RH and R 2 T 14It is considered that no decomposition reaction of the main phase occurs between the rare earth elements A and B crystals. Therefore, it is considered that after the first diffusion step, RL is enriched at the grain boundaries 6, and the concentration of RL is higher than that before the first diffusion step. It is considered that if RH is diffused in this state (second diffusion step), the ratio of RH to the total rare earth elements at the grain boundaries 6 can be relatively reduced.

[0118] In other words, in the two-stage grain boundary diffusion process of this embodiment, RH is in a low concentration state and R is in a low concentration state compared to the conventional one-stage diffusion. 2 T 14 It is believed that the decomposition reaction of the main phase is suppressed by contacting the B crystals. As a result, in this embodiment, the thickness of the shell portion 42 can be made thinner than in the conventional one-stage diffusion, and the RH concentration in the shell portion 42 can be increased by the reduced thickness, making it possible to maintain a high Br. Furthermore, in this embodiment, the suppression of the decomposition reaction of the main phase is believed to suppress the consumption of RH near the surface of the magnet, making it easier for RH to diffuse into the interior of the magnet. As a result, it is believed that the effect of improving HcJ by the diffusion of RH is enhanced, making it possible to achieve both a high HcJ and a high Br.

[0119] It is believed that the reason why RH is more likely to diffuse to the inside is that the two-particle grain boundary 6a is expanded by the diffusion of RL in the first diffusion step. It is believed that the expansion of the grain boundary 6 by RL makes it easier for RH to penetrate to the inside of the magnet in the second diffusion step, resulting in a higher HcJ than with conventional methods. Furthermore, in the manufacturing method of this embodiment, it is believed that the grain growth of the main phase grains 4 in the second diffusion step is suppressed by diffusing RL before the diffusion of RH, and the effect of suppressing this grain growth is believed to have contributed to the improvement of the magnetic properties.

[0120] It should be noted that the above-mentioned principle regarding the modification of the grain boundary 6 (suppression and expansion of the decomposition reaction) is merely speculation, and the effects of the present invention are not limited to the above. Furthermore, the manufacturing method of this embodiment (two-stage grain boundary diffusion treatment) can reduce the amount of RH required to obtain magnetic properties (particularly HcJ) equivalent to those of conventional permanent magnets. As described above, this is because the two-stage grain boundary diffusion treatment of this embodiment can reduce the shell thickness near the surface and can diffuse RH deeper inside the magnet.

[0121] In addition, when the magnet base material 20 used during manufacturing has a predetermined composition, the above-mentioned effect of improving Br and HcJ becomes more remarkable. That is, in the magnet base material 20 (RTB alloy), the total content of R is 27.5 mass% or more and 30.8 mass% or less, the content of Cu is 0.05 mass% or more and 0.5 mass% or less, and the content of B is 0.92 mass% or more and 1.03 mass% or less. In this composition, the total content of R is lower than the composition range of a general RTB alloy. In this way, by using a magnet base material 20 with a low content of R, the effect of improving Br and HcJ by the two-stage grain boundary diffusion treatment becomes higher.

[0122] Although the embodiment of the present invention has been described above, the present invention is not limited to the above-mentioned embodiment, and various modifications can be made within the scope of the present invention. EXAMPLES

[0123] The present invention will be described in more detail below using examples and comparative examples, although the present invention is not limited to the following examples.

[0124] Experiment 1 In experiment 1, the composition of magnet base material 20 was varied and a two-stage grain boundary diffusion treatment was carried out to produce RTB permanent magnets according to samples 1 to 21, and the magnetic properties of these samples were evaluated.

[0125] (Sample 1 to Sample 21) First, Nd, Pr, Tb, DyFe, electrolytic iron, and low carbon ferroboron alloy were prepared as raw materials. In addition, Al, Ga, Cu, Co, and Zr were prepared in the form of pure metal or alloy with Fe. Then, the above raw materials were weighed so that the composition of the magnet substrate 20 would be the composition shown in Table 2, and a raw material alloy was produced by a strip casting method. The thickness of the raw material alloy obtained here was 0.2 mm to 0.6 mm.

[0126] Next, hydrogen gas was flowed through the raw alloy at room temperature for 1 hour to absorb hydrogen. After that, the atmosphere was switched from hydrogen gas to Ar gas, and dehydrogenation was performed at 450°C for 1 hour, and the raw alloy was hydrogen-pulverized. The pulverized raw alloy was cooled and then classified using a sieve to obtain a powder (coarsely pulverized material) with a particle size of 400 μm or less. In the manufacture of the samples other than sample 20, the process from this hydrogen absorption and pulverization to the sintering process described later was always performed in a low-oxygen atmosphere with an oxygen concentration of 200 ppm or less. Meanwhile, for sample 20, the oxygen concentration in each process was adjusted so that the oxygen content of the magnet base material 20 was a predetermined amount.

[0127] Next, oleic acid amide was added as a grinding aid to the coarsely ground material and mixed. Then, this coarsely ground material was finely ground in a nitrogen gas flow using a collision plate type jet mill device to obtain fine powder (raw alloy powder) with an average particle size of about 3.9 μm to 4.2 μm. In this fine grinding process, the amount of oleic acid amide added was adjusted so that the carbon content in the magnet base material 20 was within a desired range. The above average particle size is the average particle size D50 measured by a laser diffraction type particle size distribution meter.

[0128] Next, the raw alloy powder was molded in a magnetic field to produce a compact. In this case, the applied magnetic field was a static magnetic field of 1200 kA / m, the pressure during molding was 120 MPa, and the magnetic field application direction and the pressure direction were perpendicular to each other. When the density of the compacts obtained in this molding process was measured, the density of all the compacts was 4.10 Mg / m 3 More than 4.25Mg / m 3 It was within the following range.

[0129] Next, the compact was sintered to obtain a sintered body made of an RTB alloy. The sintering conditions, which differed slightly depending on the composition, were maintained in a vacuum atmosphere at a temperature of 1040°C to 1100°C for 4 hours. The sintered density obtained in this sintering process was 7.45 Mg / m for all samples. 3 ~7.55Mg / m 3 The range was as follows: After that, the sintered body was vertically machined to a size of 15 mm×10 mm×5 mm (thickness in the direction of easy magnetization: 5 mm) to obtain a magnet base material 20.

[0130] Here, the average composition of the magnet base material 20 in each sample was measured. The samples for analysis were obtained by crushing each sample to a size of about 1 mm in average particle diameter using a stamp mill and randomly selecting the crushed material. The contents of various metal elements were measured using XRF and ICP. The oxygen content was measured by inert gas fusion-non-dispersive infrared absorption method, the carbon content was measured by combustion in oxygen gas flow-infrared absorption method, and the nitrogen content was measured by inert gas fusion-thermal conductivity method. The measurement results of each sample are shown in Table 2. The Fe content is the remainder, which means that the contents of elements not listed in Table 2 are included in the Fe content, and the total of R, T, B, and m is 100 mass%.

[0131] Next, a two-stage grain boundary diffusion treatment was performed on the magnet base material 20 in the following manner. First, a first diffusion material 1A containing Nd(RL) and a second diffusion material 2K containing Tb(RH) were prepared with the compositions shown in Table 1. Both of these diffusion materials were alloy powders.

[0132] Next, as a pretreatment for grain boundary diffusion, the magnet base material 20 was subjected to an etching treatment. Specifically, a mixed solution of 100% by mass of ethanol and 3% by mass of nitric acid was prepared, and the magnet base material 20 was immersed in the mixed solution for 3 minutes for etching, and then immersed in ethanol for 1 minute for cleaning. The above etching was performed twice for each sample.

[0133] Next, 75 parts by mass of the first diffusion material 1A containing Nd, 23 parts by mass of alcohol, and 2 parts by mass of acrylic resin were kneaded to obtain a first paste. The alcohol used at this time was a solvent, and the acrylic resin was a binder. Then, the first paste was applied to both of the pair of magnetic pole faces of the magnet base material 20. At this time, the application amount of the first paste was adjusted so that the total amount of Nd attached to the magnet base material 20 was 1.0 part by mass with respect to 100 parts by mass of the magnet base material. After application of the first diffusion material 1A, the magnet base material 20 was held at 900°C for 10 hours in an Ar atmosphere at atmospheric pressure, and then quenched (first diffusion step). After the first diffusion step, the magnet base material 20 was polished using 1200 grit abrasive paper until the residue present on the surface of the magnet base material 20 was removed.

[0134] Next, 75 parts by mass of the second diffusion material 2K containing Tb, 23 parts by mass of alcohol (solvent), and 2 parts by mass of acrylic resin (binder) were kneaded to obtain a second paste. Then, the second paste was applied to both of the pair of magnetic pole faces of the magnet base material 20. At this time, the amount of the second paste applied was adjusted so that the total amount of Tb attached to the magnet base material 20 was 0.5 parts by mass with respect to 100 parts by mass of the magnet base material. After applying the second diffusion material 2K, the magnet base material 20 was held at 900°C for 10 hours in an Ar atmosphere at atmospheric pressure, and then quenched (second diffusion step). Then, after the above heat treatment, the magnet base material 20 was heat treated at 600°C for 1 hour in an Ar atmosphere at atmospheric pressure, and then quenched (aging step). After the aging step, the magnet base material 20 was polished using 1200 grit abrasive paper until the residue present on the surface of the magnet base material 20 was removed.

[0135] Through the above steps, RTB permanent magnets 2 relating to samples 1 to 21 were obtained. The average composition of the RTB permanent magnets 2 was measured in the same manner as for the average composition of the above-mentioned magnet substrate 20. The measurement results are shown in Table 4.

[0136] Furthermore, the maximum thickness t1 (average value of the results of measuring 20 particles) of the shell portion 42 at a cross section 100 μm deep from the magnetic pole face was measured by the method described in the embodiment. The measurement results are shown in Table 4.

[0137] Furthermore, the obtained RTB permanent magnet 2 was magnetized by a pulse magnetic field of 4000 kA / m, and then the residual magnetic flux density Br (mT), coercive force HcJ (kA / m), and squareness ratio Hk / HcJ (%) of each sample were measured using a BH tracer. In this embodiment, Hk / HcJ was measured by taking the magnitude of the magnetic field Hk (kA / m) when the magnetization J was 90% of Br. Br was judged to be particularly good when it was 1450 mT or more, HcJ was judged to be particularly good when it was 1800 or more, and Hk / HcJ was judged to be particularly good when it was 95% or more. The measurement results of each sample 1 to 21 are shown in Table 4.

[0138] Although not shown in Table 4, the presence or absence of concentration distribution of RH (Tb), RL (Nd), and M (Cu) inside each sample was investigated. As a result, it was confirmed that the Nd content, Tb content, and Cu content gradually decreased from the pole surface toward the depth direction in all samples 1 to 21.

[0139] (Comparative Example) In experiment 1, as shown in Tables 3 and 4, RTB permanent magnets according to comparative examples 1, 2, 6, 7, 10, 11, 14, 16, 17, 20, 21, and 22 were manufactured. Specifically, in comparative examples 1, 2, 6, 7, 10, 11, 14, 16, 17, 20, and 21, magnet base materials were manufactured with the same compositions as the above-mentioned samples 1, 2, 6, 7, 10, 11, 14, 16, 17, 20, and 21, respectively, and the magnet base materials were subjected to a single-stage grain boundary diffusion treatment using only the diffusion material 2K containing Tb. Note that numbers correspond to comparative examples 1 to 21 and samples 1 to 21, and the compositions of the magnet base materials of the samples and comparative examples with the same numbers are approximately the same.

[0140] In Comparative Example 22, a magnet base material having the same composition A as Sample 1 was produced, and then a diffusion material 2K containing Tb(RH) was diffused in the first diffusion step, and a diffusion material 1A containing Nd(RL) was diffused in the second diffusion step. That is, in Comparative Example 22, the diffusion order of RH and RL is reversed from that of Sample 1.

[0141] In the above comparative example, the experimental conditions other than those mentioned above were the same as those of samples 1 to 21, and evaluations were performed in the same manner as samples 1 to 21. The evaluation results of the comparative example are shown in Tables 3 and 5.

[0142] [Table 1]

[0143] [Table 2]

[0144] [Table 3]

[0145] [Table 4]

[0146] [Table 5]

[0147] As shown in the results of Tables 4 and 5, when comparing Samples 1 to 21 with Comparative Examples 1 to 21 with the corresponding numbers, it can be confirmed that Samples 1 to 21, which underwent two-stage grain boundary diffusion treatment, have improved magnetic properties compared to the Comparative Examples with the corresponding numbers, and in particular that HcJ is improved while maintaining Br. From these results, it can be confirmed that high Br and high HcJ can be obtained by the two-stage grain boundary diffusion treatment.

[0148] Furthermore, it was confirmed that in Comparative Examples 1 to 21, in which only one stage of grain boundary diffusion treatment was performed, the maximum thickness t1 of the shell portion near the surface exceeded 0.5 μm, while in Samples 1 to 21, in which two stages of grain boundary diffusion treatment were performed, t1 was 0.5 μm or less. In fact, Figure 6 is an SEM photograph of the RTB permanent magnet 2 obtained from Sample 1, and Figure 7 is an SEM photograph of the RTB permanent magnet obtained in Comparative Example 1.

[0149] In the SEM photograph of Comparative Example 1 in Fig. 7, it can be seen that a thicker shell is formed than in the SEM photograph of Fig. 6, and that the shell is particularly thick on the surface side. In contrast, in the SEM photograph of Sample 1 shown in Fig. 6, it can be seen that the thickness of shell portion 42 is clearly thinner than that of Comparative Example 1. From this result, it was found that the thickness of shell portion 42 where RH is concentrated can be thinned by the two-stage grain boundary diffusion treatment, and that by setting the thickness of shell portion 42 near the surface to a predetermined thickness or less (t1 ≦ 0.5 μm), it is possible to achieve both high Br and high HcJ.

[0150] Furthermore, comparing the evaluation results of samples 1 to 21, when the magnet substrate 20 and the RTB permanent magnet 2 were within a specified composition range, 1450 mT≦Br and 1800 kA / m≦HcJ were satisfied, and Br and HcJ tended to be improved.

[0151] In other words, it was found that, as the average composition of the magnet base material 20, the total content of R is preferably 27.5 mass% or more and 30.8 mass% or less, the Cu content is preferably 0.05 mass% or more and 0.5 mass% or less, and the B content is preferably 0.92 mass% or more and 1.03 mass% or less.

[0152] It was also found that, as the average composition of the RTB permanent magnet 2 after grain boundary diffusion, the total R content is preferably 28.4 mass% or more and 31.9 mass% or less, the Cu content is preferably 0.2 mass% or more and 0.7 mass% or less, and the B content is preferably 0.92 mass% or more and 1.03 mass% or less.

[0153] In Comparative Example 22, the maximum thickness of the shell portion near the surface exceeded 0.5 μm, resulting in insufficient improvement in magnetic properties. From this result, it was found that even if RH and RL are diffused at grain boundaries in two stages, when RL is diffused at grain boundaries after RH, the generation of a thick shell portion cannot be suppressed and sufficient magnetic properties cannot be obtained.

[0154] The reason why sufficient improvement in magnetic properties was not obtained when RH was diffused before RL as in Comparative Example 22 is not necessarily clear, but the following reasons are considered. First, when RH was diffused before RL diffusion as in the case of the one-stage grain boundary diffusion (Comparative Example 1), a high concentration of RH was diffused into R 2 T 14 B crystal and R 2 T 14 It is believed that the decomposition reaction of B crystals occurred actively. This is believed to have formed a thick shell near the surface, leading to a decrease in Br. In addition, by diffusing RL after RH diffusion, the shell containing RH formed in the first diffusion step was partially destroyed, weakening the effect of improving HcJ. Furthermore, it is believed that the diffusion of RL increased the thickness of the shell containing RH and reduced the RH concentration in the shell, weakening the effect of improving HcJ.

[0155] As described above, in the two-stage diffusion (Comparative Example 22) in which RH is diffused first, the thickness of the shell increases and the RH concentration in the shell decreases. As a result, Br decreases and HcJ cannot be sufficiently improved.

[0156] (Experiment 2) In experiment 2, several types of diffusion materials shown in Table 6 were prepared, and a two-stage grain boundary diffusion process was carried out using the combinations of diffusion materials shown in Table 7. In experiment 2, the composition of magnet base material 20 was the same as composition A of sample 1 in experiment 1, and RTB permanent magnet 2 was prepared under the same conditions as in experiment 1, except that the composition of the diffusion material was changed. The evaluation results of samples 25 to 36 in experiment 2 are shown in Table 7.

[0157] [Table 6]

[0158] [Table 7]

[0159] As shown in Table 7, in all of Samples 25 to 36 in Experiment 2, the maximum thickness t1 of the shell portion 42 was as thin as 0.2 μm or less, and 1450 mT≦Br and 1800 kA / m≦HcJ. From this result, it was found that when the diffusing materials (11, 12) are within the composition ranges shown in Table 6, it is possible to improve both Br and HcJ. Although not shown in Table 7, it was confirmed that in all of Samples 25 to 36 in Experiment 2, the RL content, RH content, and M element content gradually decreased from the pole face toward the depth direction.

[0160] In addition, comparing Sample 35 and Sample 36, it was found that Tb was more effective than Dy as the RH to be diffused. Note that Sample 36, in which Dy was diffused, had a lower HcJ than the other samples (25 to 35) in which Tb was diffused, but it was confirmed that a higher HcJ could be obtained than when Dy was diffused by only one grain boundary diffusion process. [Explanation of symbols]

[0161] 2...RTB permanent magnet 2a … Main surface (magnetic pole surface) 2b…side 4 … Main phase particles 4a … Core-shell particles 41 ... Core section 42 … Shell part 6 … Grain boundary 6a … Two-grain grain boundary 6b … Grain boundary multiple points 20 ... Magnet substrate 20a…Main surface 20b…side 50 … IPM motor 51 ... Rotor 52 ... Stator core 53 ... Gap 54 ... Coil 101 … Electric vehicle 102…HV vehicle 60 … Inverter 70 … Battery 80 ... Engine 90 ... Generator

Claims

1. preparing a magnet substrate containing an R-T-B based alloy; a first diffusion step of attaching a first diffusion material containing at least one light rare earth element to at least a part of a surface of the magnet base material, and heating the magnet base material to which the first diffusion material is attached; a second diffusion step of adhering a second diffusion material containing at least one heavy rare earth element to at least a part of the surface of the magnet base material after the first diffusion step, and heating the magnet base material to which the second diffusion material is adhered, The R-T-B based alloy contained in the magnet base material contains one or more rare earth elements as R, with Nd being essential, one or more iron group elements as T, with Fe being essential, boron, and Cu; In the R-T-B based alloy, The total content of R is 27.5 mass% or more and 30.8 mass% or less, The Cu content is 0.05 mass% or more and 0.5 mass% or less, The content of B is 0.92 mass% or more and 1.03 mass% or less, The first diffusing material contains one or more elements selected from the group consisting of Nd and Pr as the light rare earth element, the second diffusible material is an RH-M alloy containing the heavy rare earth element and M, The M is an element having a eutectic temperature with the light rare earth element of 800° C. or less, the second diffusive material includes one or more elements having a eutectic temperature with the light rare earth element of 800° C. or less selected from the group consisting of Mg, Co, Ni, Cu, and Cl; The method for producing an RTB system permanent magnet, in which the content of the light rare earth element contained in the RH-M alloy is 0% by mass or more and 22.5% by mass or less.

2. 2. The method for producing an R-T-B system permanent magnet according to claim 1, wherein the second diffusion material contains, as the heavy rare earth element, one or more elements selected from the group consisting of Tb and Dy.

3. the first diffusible material includes an RL-M alloy containing the light rare earth element and the M, In the RL-M alloy, 3. The method for producing an RTB system permanent magnet according to claim 1, wherein RL is the light rare earth element.

4. preparing a magnet substrate containing an R-T-B based alloy; a first diffusion step of attaching a first diffusion material containing at least one light rare earth element to at least a part of a surface of the magnet base material, and heating the magnet base material to which the first diffusion material is attached; a second diffusion step of adhering a second diffusion material containing at least one heavy rare earth element to at least a part of the surface of the magnet base material after the first diffusion step, and heating the magnet base material to which the second diffusion material is adhered, The R-T-B based alloy contained in the magnet base material contains one or more rare earth elements as R, with Nd being essential, one or more iron group elements as T, with Fe being essential, boron, and Cu; In the R-T-B based alloy, The total content of R is 27.5 mass% or more and 30.8 mass% or less, The Cu content is 0.05 mass% or more and 0.5 mass% or less, The content of B is 0.92 mass% or more and 1.03 mass% or less, the first diffusible material includes an RL-M alloy containing the light rare earth element and M, In the RL-M alloy, R is the light rare earth element, The M is an element having a eutectic temperature with the RL of 800° C. or less, The first diffusing material contains one or more elements selected from the group consisting of Nd and Pr as the light rare earth element, The second diffusing material is TbH 2 The present invention relates to a method for producing an RTB system permanent magnet, which is made of pure metal Tb or pure metal Dy.

5. The method for producing an RTB system permanent magnet according to any one of claims 1 to 4, wherein the first diffusion material does not substantially contain a heavy rare earth element.

6. An R-T-B system permanent magnet in which R is one or more light rare earth elements, essentially Nd, and one or more heavy rare earth elements, T is one or more iron group elements, essentially Fe, and B is boron, The R-T-B based permanent magnet includes a plurality of core-shell particles, Each of the core-shell particles has R 2 T 14 a core portion containing B crystals and a shell portion covering the core portion and having a higher content of the heavy rare earth element than the core portion, In a cross section at a depth of 100 μm from the surface of the R-T-B system permanent magnet, the maximum thickness of the shell portion is, on average, 0.5 μm or less, the R-T-B system permanent magnet has a concentration distribution in which the content of the light rare earth element and the content of the heavy rare earth element both decrease from the surface toward the depth direction, An RTB system permanent magnet having a residual magnetic flux density of 1450 mT or more and a coercive force of 1800 kA / m or more.

7. M having a eutectic temperature with the light rare earth element of 800° C. or less is included, 7. The R-T-B system permanent magnet according to claim 6, having a concentration distribution in which the M content decreases from the surface toward the depth direction of the R-T-B system permanent magnet.

8. The R-T-B system permanent magnet further contains Cu, The total content of R is 28.4 mass% or more and 32.0 mass% or less, The Cu content is 0.2 mass% or more and 0.7 mass% or less, 8. The R-T-B system permanent magnet according to claim 6, wherein the B content is 0.92 mass % or more and 1.03 mass % or less.

9. 9. The RTB system permanent magnet according to claim 6, wherein the heavy rare earth element is Tb and / or Dy.

10. 10. The RTB system permanent magnet according to claim 6, further comprising Pr as the light rare earth element.

11. A motor having the RTB system permanent magnet according to any one of claims 6 to 10.

12. A motor vehicle comprising the motor according to claim 11.

Citation Information

Patent Citations

  • Permanent magnet and method for manufacturing the same

    JP2012039100A

  • R-t-b based permanent magnet

    JP2019176140A

  • Manufacturing method of rare-earth magnet

    JP2020136343A

  • Rare earth magnet and production method thereof

    JP2021174818A

  • Method for producing r-t-b sintered magnet

    WO2016121790A1