Easily-planar high-frequency rare earth soft magnetic material and preparation method thereof

By developing R2 (FexCo1-x)17 rare earth-3d group intermetallic compounds with Th2Zn17 crystal structure, the problem of decreasing permeability of ferrite soft magnetic materials in the GHz band is solved, and high-frequency electromagnetic characteristics and temperature stability are achieved , significantly improves the properties of the material.

CN118919205APending Publication Date: 2024-11-08ZHEJIANG UNIV +1
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411203138.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-08

Smart Images

  • Figure CN118919205A_ABST
    Figure CN118919205A_ABST
Patent Text Reader

Abstract

The invention discloses an easy-to-face type high-frequency rare earth soft magnetic material and a preparation method thereof. The material is a Th2Zn17 type R2 (FexCo1-x) 17 rare earth-3d group intermetallic compound, and has two anisotropic fields along a c axis and in an easily magnetized plane. The preparation method comprises the following steps: reducing Fe and Co acetylacetonate into magnetic iron and cobalt nanoparticles in an organic solvent by using oil phase synthesis and reduction diffusion processes, uniformly coating rare earth oxide in the magnetic nanoparticles through oil phase reaction, and finally obtaining the rare earth soft magnetic material through a reduction diffusion heat treatment process by using calcium hydride as a reducing agent. The rare earth soft magnetic material has high Curie temperature, high-frequency magnetic conductivity and cut-off frequency, can be used in high-frequency and high-temperature environments, can use a large amount of high-abundance light rare earth elements such as yttrium and cerium, and is beneficial to solving the production and marketing balance of rare earth products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a high-frequency rare earth soft magnetic material with easy-surface anisotropy and a preparation method thereof, belonging to the field of new materials and new processes for electronic components. Background Art

[0002] As communication technology develops towards high frequencies, the operating frequencies of electronic components have reached the GHz band. For example, the application frequency of WLAN wireless local area networks is 5.1GHz, the application frequency of IoT settlement systems generally reaches 6.0GHz, and the application frequency of 5G mobile phone communications has reached 40.0GHz. However, the current high-frequency soft magnetic materials, mainly ferrites, have a sharp drop in magnetic permeability in the GHz band due to the constraints of the Snoek limit, which makes them unable to meet the requirements of high-frequency applications. Therefore, it is urgent to develop new soft magnetic materials with high magnetic permeability under high-frequency conditions.

[0003] Rare earth soft magnetic materials are a series of rare earth-3d metal compounds with soft magnetic properties formed by rare earth elements and transition metal elements. Rare earth soft magnetic materials have similar composition to rare earth permanent magnets, but the difference is that the magnetocrystalline anisotropy type of rare earth permanent magnets is easy axis type, while rare earth soft magnetic materials are easy face type, which has multiple easy magnetization axes and are in the same crystal plane. Therefore, rare earth soft magnetic materials are also called rare earth easy face materials. Rare earth soft magnetic materials currently mainly include R2[(Fe,Co) 1-x M x ] 17 Compounds and R2(Fe,Co) with 2:14:1 phase as the main phase 14 B compound, its biggest feature is that it has both high saturation flux and high cutoff frequency, so it has excellent high-frequency soft magnetic properties (XCKou, PHYSICAL REVIEW B.1992,46,10). Experiments have shown that its high-frequency performance is better than the currently widely used hexagonal microwave ferrite, and the operating frequency can reach 1.0-40.0GHz. The outstanding high-frequency characteristics of rare earth soft magnetic materials originate from the strong anisotropy field of the easy magnetization plane. According to the Snoek limit, for a certain soft magnetic material, its magnetic permeability μ i With the cut-off frequency f r The product of (μ i -1)f r is a constant value, so the permeability and cutoff frequency cannot be increased at the same time (JLSnoek, Nature. 1947, 160, 90). However, for rare earth soft magnetic materials, due to the existence of two anisotropic fields along the c-axis and in the easy magnetization plane, (μ i -1)f rIt is no longer a constant and is much higher than that of general soft magnetic materials, so that the magnetic permeability and cut-off frequency under high-frequency conditions can be significantly improved, thus breaking through the Snoek limit.

[0004] The excellent high-frequency characteristics of rare earth soft magnetic materials make them have extremely high application value and broad market prospects in the development of high-frequency high-power devices, high-frequency low temperature coefficient devices, and high-frequency miniaturized devices. In the past 20 years, the average consumption growth rate of electronic components has remained at around 20%. The demand for soft magnetic materials in photovoltaic power generation, new energy vehicles, smart grids, consumer electronics, data centers and other fields is bound to continue to increase, and the market prosperity will continue to improve, with great potential. Summary of the invention

[0005] The purpose of the present invention is to provide a high-frequency rare earth soft magnetic material with easy-surface anisotropy and a preparation method thereof in view of the shortcomings of soft magnetic materials such as ferrite.

[0006] The rare earth soft magnetic material of the present invention is Th2Zn 17 R2(Fe x Co 1-x ) 17 Rare earth-3d group metal compounds, wherein 0<x≤1, and R is one or more of Y, Ce, Pr, Nd, Gd, Dy, Er, Tm, and Yb.

[0007] The rare earth soft magnetic material of the invention has an easy magnetization plane (easy face), and the easy magnetization plane is perpendicular to the c-axis, and there are two anisotropic fields along the c-axis and in the easy magnetization plane.

[0008] The rare earth soft magnetic material of the present invention has high-frequency electromagnetic characteristics, an initial magnetic permeability of more than 2.0, and a resonance frequency of more than 2.0 GHz.

[0009] The present invention provides a surface-changeable high-frequency rare earth soft magnetic material and a preparation method thereof, the preparation method comprising the following steps:

[0010] 1) Put oleic acid, dioctylamine and tetralin into a container and heat and activate them under the protection of inert gas;

[0011] 2) According to the general formula of the soft magnetic material to be prepared, R2(Fe x Co 1-x ) 17 Weighing Fe and Co acetylacetonate in the ratio of Fe to Co, adding them into the container, and heating and reducing them under the protection of inert gas to obtain Fe and Co magnetic nanoparticles;

[0012] 3) adding ethanol to the container to perform a coagulation reaction, centrifuging the precipitate, washing it several times, and then dispersing it in an organic protective solvent;

[0013] 4) Weigh the acetylacetonate of rare earth element R and add it to the container containing oleic acid and oleylamine, and then prepare the soft magnetic material according to the general formula R2(Fe x Co 1-x ) 17 The rare earth element R is added to the Fe and Co magnetic nanoparticles dispersed in the organic protective solvent obtained in step 3) in a proportion thereof and heated under the protection of an inert gas to perform an oil phase reaction to obtain magnetic particles uniformly coated with rare earth oxides;

[0014] 5) adding ethanol to carry out coagulation reaction, centrifuging the precipitate, washing it several times and then vacuum drying it to obtain magnetic powder;

[0015] 6) Weigh CaH2 and add it to a stainless steel crucible containing magnetic powder, and then obtain rare earth soft magnetic material through reduction diffusion heat treatment.

[0016] Compared with the existing high-frequency soft magnetic materials, the present invention has the following gain effects: 1) the rare earth soft magnetic material of the present invention has an easy magnetization plane, a stronger anisotropy field, a high-frequency magnetic permeability and a cut-off frequency, and can be used in the microwave frequency band of 1.0-40.0 GHz; 2) the rare earth soft magnetic material of the present invention has a higher Curie temperature and temperature stability, and can be used in a higher temperature service environment; 3) the rare earth soft magnetic material of the present invention is nano-sized, and there is a strong exchange coupling effect between the magnetic particles, which can significantly improve the saturation magnetic flux density and initial magnetic permeability of the material; 4) the rare earth soft magnetic material of the present invention can use a large amount of high-abundance light rare earth elements such as yttrium and cerium, which is conducive to solving the production and marketing balance of rare earth products. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The complex magnetic permeability of the easy-to-surface high-frequency rare earth soft magnetic material prepared in Example 1 of the present invention at 2.0-18.0 GHz.

[0018] Figure 2 The complex magnetic permeability of the easy-to-surface high-frequency rare earth soft magnetic material prepared in Example 2 of the present invention at 2.0-18.0 GHz.

[0019] Figure 3 The complex magnetic permeability of the easy-to-surface high-frequency rare earth soft magnetic material prepared in Example 3 of the present invention at 2.0-18.0 GHz. DETAILED DESCRIPTION

[0020] The present invention is further described and illustrated below in conjunction with specific embodiments. The embodiments are merely exemplary of the present disclosure and do not define the scope of limitation. The technical features of each embodiment of the present invention may be combined accordingly without conflicting with each other.

[0021] The easy-to-surface high-frequency rare earth soft magnetic material provided by the present invention is a Th2Zn17 R2(Fe x Co 1-x ) 17 Rare earth-3d group metal intermetallic compound, wherein 0<x≤1, R is one or more of Y, Ce, Pr, Nd, Gd, Dy, Er, Tm, Yb. According to an embodiment of the present invention, it can be specifically prepared according to the following preparation process:

[0022] 1) Take oleic acid, dioctylamine and tetralin in a certain ratio into a three-necked flask, gradually heat to 100°C under the protection of inert gas Ar, keep warm for 1 hour and then cool to room temperature;

[0023] 2) According to the general formula of the soft magnetic material to be prepared, R2(Fe x Co 1-x ) 17 Acetylacetonate of Fe and Co in the ratio of Fe to Co was weighed and added into a three-necked flask, and the temperature was gradually raised to 110° C. and kept warm for 30 minutes under the protection of inert gas Ar to remove air and moisture in the container, and then the reaction container was continued to be heated to 210° C., and the temperature was kept stable for 30 minutes to obtain Fe and Co magnetic nanoparticles;

[0024] 3) After the reaction container is cooled to room temperature, ethanol is added to perform a coagulation reaction, and the mixture in the collection container is centrifuged and washed several times with ethanol, and then dispersed in an organic protective solvent;

[0025] 4) Weigh the acetylacetonate of rare earth element R and add it to a three-necked flask containing oleic acid and oleylamine. Heat it to 120°C under the protection of inert gas Ar and keep it warm for 60 minutes to remove the air and moisture in the container. Then, prepare the soft magnetic material according to the general formula R2(Fe x Co 1-x ) 17 The rare earth element R is added to the Fe and Co magnetic nanoparticles previously dispersed in the organic protective solvent in the same proportion as Fe and Co, and the reaction vessel is heated to 230°C. After the temperature is kept stable for 4 hours, the magnetic particles uniformly coated with rare earth oxides are obtained;

[0026] 5) After the reaction container is cooled to room temperature, ethanol is added to perform a coagulation reaction, the mixture in the container is collected and centrifuged and washed several times with ethanol and cyclohexane, and then vacuum dried for 24 hours to obtain a magnetic powder;

[0027] 6) Weigh CaH2 in a certain ratio and add it to a stainless steel crucible containing magnetic powder, then heat it to 850°C under the protection of inert gas Ar, with a heating rate of 5°C / min, and keep it warm for 90 minutes after the temperature stabilizes for reduction diffusion heat treatment. The solid powder after heat treatment is soaked in a saturated methanol solution of NH4Cl to remove excess CaH2, and finally washed with deionized water several times and vacuum dried for 12 hours to obtain rare earth soft magnetic nanocrystalline powder.

[0028] According to a preferred embodiment of the present invention, the organic protective solvent is cyclohexane, n-hexane or n-heptane. In step 1), the volume ratio of oleic acid to dioctylamine is 1:1 to 1:10, and the volume ratio of oleic acid to tetralin is 1:40 to 1:100. In step 2), the mass ratio of Fe and Co acetylacetonate to the mixed solvent (i.e., oleic acid, dioctylamine and tetralin) is 1:10 to 1:80. In step 4), the volume ratio of oleic acid to oleylamine is 1:5 to 1:20, and the mass ratio of the total amount of oleic acid and oleylamine to the acetylacetonate of rare earth element R is 100-500:1. In step 6), the mass ratio of CaH2 to the acetylacetonate of rare earth element R is 1:5 to 1:20.

[0029] The present invention adopts the following method to test the magnetic permeability of rare earth soft magnetic materials: the prepared rare earth soft magnetic materials are subjected to static magnetic property test, then mixed with a bonding medium in a mass ratio of 1:9 to 9:1 and pressed into a ring, and then placed in a vector network analyzer to test the magnetic permeability of 2.0-18.0GHz. The bonding medium is paraffin, epoxy resin, polyethylene, polypropylene or methyl silicone rubber; the mass ratio of the rare earth soft magnetic material to the bonding medium is preferably 4:1.

[0030] The present invention is further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments:

[0031] Embodiment 1:

[0032] 1) 0.3 ml of oleic acid, 0.5 ml of dioctylamine and 20.0 ml of tetralin were weighed into a three-necked flask, and gradually heated to 100°C under the protection of inert gas Ar, kept warm for 1 hour, and then cooled to room temperature;

[0033] 2) Weigh 0.605 g of Co(C5H7O2)3 into a three-necked flask, gradually heat it to 110°C under the protection of inert gas Ar and keep it warm for 30 minutes to remove air and moisture in the container, then continue to heat the reaction container to 210°C, keep the temperature stable and keep it warm for 30 minutes to obtain Co magnetic nanoparticles;

[0034] 3) After the reaction container is cooled to room temperature, 20.0 ml of ethanol is added to perform a coagulation reaction, and the mixture in the collection container is centrifuged and washed twice with ethanol, and then dispersed in 10.0 ml of cyclohexane;

[0035] 4) Weigh 0.111 g of Y(C5H7O2)3 and add it to a three-necked flask containing 2.0 ml of oleic acid and 20.0 ml of oleylamine, heat it to 120°C under the protection of inert gas Ar and keep it warm for 60 minutes to remove air and moisture in the container, then add Co magnetic nanoparticles dispersed in cyclohexane and continue to heat the reaction container to 230°C. After the temperature remains stable, keep it warm for 4 hours to obtain Co magnetic particles uniformly coated with Y2O3;

[0036] 5) After the reaction container is cooled to room temperature, ethanol is added to carry out a coagulation reaction, the mixture in the container is collected and centrifuged and washed 4 times with ethanol and cyclohexane, and then vacuum dried for 24 hours to obtain a magnetic powder;

[0037] 6) Weigh 0.1g CaH2 and add it to the stainless steel crucible containing the magnetic powder, then heat it to 850℃ under the protection of inert gas Ar, the heating rate is 5℃ / min, and after the temperature stabilizes, keep it warm for 90 minutes for reduction diffusion heat treatment. The solid powder after heat treatment is immersed in 50.0ml NH4Cl saturated methanol solution to remove excess CaH2, and finally wash it with deionized water twice and vacuum dry it for 12 hours to obtain Y2Co 17 Rare earth soft magnetic nanocrystalline powder.

[0038] 7) The prepared Y2Co 17 Rare earth soft magnetic materials are tested for static magnetic properties, magnetic flux density B s is 1.1T, Curie temperature T c Reach 910℃. 17 The magnetic powder and paraffin were mixed in a mass ratio of 4:1 and pressed into a ring. The ring was then placed in a vector network analyzer to test the magnetic permeability at 2.0-18.0 GHz. The results are shown in the attached figure. Figure 1 As shown, the initial value of the magnetic permeability at 2.0 GHz can reach 2.5, and the cutoff frequency reaches 8.3 GHz.

[0039] Embodiment 2:

[0040] 1) 0.6 ml of oleic acid, 1.0 ml of dioctylamine and 40.0 ml of tetralin were weighed into a three-necked flask, and gradually heated to 100°C under the protection of inert gas Ar, kept warm for 1 hour, and then cooled to room temperature;

[0041] 2) Weigh 0.606 g of Fe(C5H7O2)3 and 0.606 g of Co(C5H7O2)3 into a three-necked flask, gradually heat to 110°C under the protection of inert gas Ar and keep warm for 30 minutes to remove air and moisture in the container, then continue to heat the reaction container to 210°C, keep the temperature stable and keep warm for 30 minutes to obtain Fe and Co magnetic nanoparticles;

[0042] 3) After the reaction container is cooled to room temperature, 40.0 ml of ethanol is added to perform a coagulation reaction, and the mixture in the collection container is centrifuged and washed 4 times with ethanol, and then dispersed in 20.0 ml of cyclohexane;

[0043] 4) Weigh 0.221 g of Nd(C5H7O2)3 and add it to a three-necked flask containing 4.0 ml of oleic acid and 40.0 ml of oleylamine, heat it to 120°C under the protection of inert gas Ar and keep it warm for 60 minutes to remove air and moisture in the container, then add Fe and Co magnetic nanoparticles dispersed in cyclohexane and continue to heat the reaction container to 230°C. After the temperature remains stable, keep it warm for 4 hours to obtain Fe and Co magnetic particles uniformly coated with Nd2O3;

[0044] 5) After the reaction container is cooled to room temperature, ethanol is added to carry out a coagulation reaction, the mixture in the container is collected and centrifuged and washed 4 times with ethanol and cyclohexane, and then vacuum dried for 24 hours to obtain a magnetic powder;

[0045] 6) Weigh 0.2g CaH2 and add it to the stainless steel crucible containing magnetic powder, then heat it to 850℃ under the protection of inert gas Ar, the heating rate is 5℃ / min, and after the temperature stabilizes, keep it warm for 90 minutes for reduction diffusion heat treatment. The solid powder after heat treatment is immersed in 80.0ml NH4Cl saturated methanol solution to remove excess CaH2, and finally wash it with deionized water twice and vacuum dry it for 12 hours to obtain Nd2(Fe 0.5 Co 0.5 ) 17 Rare earth soft magnetic nanocrystalline powder.

[0046] 7) The obtained Nd2(Fe 0.5 Co 0.5 ) 17 Rare earth soft magnetic materials are tested for static magnetic properties, magnetic flux density B s is 1.6T, Curie temperature T c Reach 726℃. 0.5 Co 0.5 ) 17 The magnetic powder and paraffin were mixed in a mass ratio of 4:1 and pressed into a ring. The ring was then placed in a vector network analyzer to test the magnetic permeability at 2.0-18.0 GHz. The results are shown in the attached figure. Figure 2As shown, the initial value of the magnetic permeability at 2.0 GHz can reach 3.0, and the cutoff frequency reaches 6.0 GHz.

[0047] Embodiment 3:

[0048] 1) 0.3 ml of oleic acid, 0.5 ml of dioctylamine and 20.0 ml of tetralin were weighed into a three-necked flask, and gradually heated to 100°C under the protection of inert gas Ar, kept warm for 1 hour, and then cooled to room temperature;

[0049] 2) Weigh 0.361 g of Fe(C5H7O2)3 and 0.243 g of Co(C5H7O2)3 into a three-necked flask, gradually heat to 110°C under the protection of inert gas Ar and keep warm for 30 minutes to remove air and moisture in the container, then continue to heat the reaction container to 210°C, keep the temperature stable and keep warm for 30 minutes to obtain Fe and Co magnetic nanoparticles;

[0050] 3) After the reaction container is cooled to room temperature, 20.0 ml of ethanol is added to perform a coagulation reaction, and the mixture in the collection container is centrifuged and washed twice with ethanol, and then dispersed in 10.0 ml of n-hexane;

[0051] 4) Weigh 0.110 g of Ce(C5H7O2)3 and add it to a three-necked flask filled with 2.0 ml of oleic acid and 20.0 ml of oleylamine, heat it to 120°C under the protection of inert gas Ar and keep it warm for 60 minutes to remove air and moisture in the container, then add Fe and Co magnetic nanoparticles dispersed in n-hexane and continue to heat the reaction container to 230°C. After the temperature remains stable, keep it warm for 4 hours to obtain Fe and Co magnetic particles uniformly coated with CeO2;

[0052] 5) After the reaction container is cooled to room temperature, ethanol is added to carry out a coagulation reaction, the mixture in the container is collected and centrifuged and washed 4 times with ethanol and cyclohexane, and then vacuum dried for 24 hours to obtain a magnetic powder;

[0053] 6) Weigh 0.1g CaH2 and add it to the stainless steel crucible containing magnetic powder, then heat it to 850℃ under the protection of inert gas Ar, the heating rate is 5℃ / min, and after the temperature stabilizes, keep it warm for 90 minutes for reduction diffusion heat treatment. The solid powder after heat treatment is immersed in 50.0ml NH4Cl saturated methanol solution to remove excess CaH2, and finally wash it with deionized water twice and vacuum dry it for 12 hours to obtain Ce2(Fe 0.6 Co 0.4 ) 17 Rare earth soft magnetic nanocrystalline powder.

[0054] 7) The obtained Ce2(Fe 0.6 Co 0.4 )17 Rare earth soft magnetic materials are tested for static magnetic properties, magnetic flux density B s is 1.2T, Curie temperature T c Reach 484℃. 0.6 Co 0.4 ) 17 The magnetic powder and epoxy resin were mixed in a mass ratio of 4:1 and pressed into a ring. The ring was then placed in a vector network analyzer to test the magnetic permeability at 2.0-18.0 GHz. The results are shown in the attached figure. Figure 3 As shown, the initial value of the magnetic permeability at 2.0 GHz can reach 3.1, and the cutoff frequency reaches 4.7 GHz.

[0055] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. For ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A surface-changeable high-frequency rare earth soft magnetic material, characterized in that: The soft magnetic material is prepared by oil phase synthesis and reduction diffusion process, which is Th2Zn 17 Rare earth-3d group intermetallic compounds R2(Fe x Co 1-x ) 17 , wherein 0<x≤1, Fe is iron element, Co is cobalt element, R is rare earth element, and R is one or more of Y, Ce, Pr, Nd, Gd, Dy, Er, Tm, and Yb elements.

2. The easy-to-surface high-frequency rare earth soft magnetic material according to claim 1, characterized in that: The soft magnetic material has an easy magnetization plane, and the easy magnetization plane is perpendicular to the c-axis, and there are two anisotropic fields along the c-axis and in the easy magnetization plane.

3. The easy-to-surface high-frequency rare earth soft magnetic material according to claim 1, characterized in that: The soft magnetic material has high-frequency electromagnetic characteristics, an initial magnetic permeability of more than 2.0, and a resonance frequency of more than 2.0 GHz.

4. A method for preparing the easy-to-surface high-frequency rare earth soft magnetic material according to any one of claims 1 to 3, characterized in that: The steps include: 1) oleic acid, dioctylamine and tetralin are added to a container to prepare a mixed solvent, and heated under the protection of an inert gas for activation; 2) According to the general formula of the soft magnetic material to be prepared, R2(Fe x Co 1-x ) 17 Weighing Fe and Co acetylacetonate in the ratio of Fe to Co, adding them into the container, and heating and reducing them under the protection of inert gas to obtain Fe and Co magnetic nanoparticles; 3) adding ethanol to the container to perform a coagulation reaction, centrifuging the precipitate, washing it several times, and then dispersing it in an organic protective solvent; 4) Weigh the acetylacetonate of rare earth element R and add it to the container containing oleic acid and oleylamine, and then prepare the soft magnetic material according to the general formula R2(Fe x Co 1-x ) 17 The rare earth element R is added to the Fe and Co magnetic nanoparticles dispersed in the organic protective solvent obtained in step 3) in a proportion thereof and heated under the protection of an inert gas to perform an oil phase reaction to obtain magnetic particles uniformly coated with rare earth oxides; 5) adding ethanol to carry out coagulation reaction, centrifuging the precipitate, washing it several times and then vacuum drying it to obtain magnetic powder; 6) Weigh CaH2 and add it to a stainless steel crucible containing magnetic powder, and then obtain rare earth soft magnetic material through reduction diffusion heat treatment.

5. The method for preparing the easy-to-surface high-frequency rare earth soft magnetic material according to claim 4, characterized in that: The organic protective solvent is cyclohexane, n-hexane or n-heptane.

6. The method for preparing the easy-to-surface high-frequency rare earth soft magnetic material according to claim 4, characterized in that: In step 1), the volume ratio of oleic acid to dioctylamine is 1:1 to 1:10, and the volume ratio of oleic acid to tetralin is 1:40 to 1:

100.

7. The method for preparing the easy-to-surface high-frequency rare earth soft magnetic material according to claim 4, characterized in that: In step 2), the mass ratio of the acetylacetonate of Fe and Co to the mixed solvent is 1:10 to 1:

80.

8. The method for preparing the easy-to-surface high-frequency rare earth soft magnetic material according to claim 4, characterized in that: In step 4), the volume ratio of oleic acid to oleylamine is 1:5-1:20, and the mass ratio of the total amount of oleic acid and oleylamine to the acetylacetonate of rare earth element R is 100-500:

1.

9. The method for preparing the easy-to-surface high-frequency rare earth soft magnetic material according to claim 4, characterized in that: In step 6), the mass ratio of CaH2 to the acetylacetonate of the rare earth element R is 1:5 to 1:20.

Citation Information

Cited By

  • Rare earth intermetallic nitride non-spherical nano soft magnetic particle and preparation method and application thereof

    CN119407184A

  • A rare earth metal internitride non-spherical nano soft magnetic particle and its preparation method and application

    CN119407184B

  • 2 / 17 type rare earth soft magnetic composite material based on high-abundance rare earth resources and preparation method of 2 / 17 type rare earth soft magnetic composite material

    CN121204551A

  • 2:17 type rare earth soft magnetic composite material based on high-abundance rare earth resources and preparation method thereof

    CN121204551B