Insulation coating magnetic core for GMI sensor probe, preparation method of insulation coating magnetic core and sensor probe
By using an insulated plating magnetic core in the GMI sensor, wrapping the Al2O3 insulating layer and Fe20Ni80 permalloy coating, the noise problem caused by the contact between the wire and the soft magnetic material coating is solved, and the sensor sensitivity and signal quality are improved.
Patent Information
- Application Number
- CN202411377266.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-30
AI Technical Summary
Direct contact between metal wire and soft magnetic material plating in existing GMI sensors results in eddy current generation, reducing sensor sensitivity and signal quality and introducing additional noise.
The substrate is made of copper wire with a purity of 4N, and the conductive metal layer of Al2O3, FeNi or Nb, and Fe20Ni80 peroxido plating layer are successively wrapped. The insulated plating magnetic core is prepared by magnetron sputtering and electrochemical deposition to avoid electromagnetics. Coupling and noise.
It significantly reduces the noise level of the GMI sensor, improves the sensitivity and signal quality of the sensor, and enhances the anti-interference ability.
Smart Images

Figure CN119049826A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of weak magnetic measurement elements, and in particular relates to an insulating coated magnetic core for a GMI sensor probe, a preparation method thereof, and a sensor probe. Background Art
[0002] Giant Magneto-Impedance (GMI) sensor is a highly sensitive magnetic field sensor widely used in biomedicine, military, aerospace and industrial automation. Its core principle is based on the impedance change caused by the change in the magnetic permeability of the material under AC excitation. The sensitivity and performance of the GMI sensor depend on the magnetic properties and structural design of the material. When the composite wire used for the GMI sensor is in direct contact with the soft magnetic material coating, the AC current will generate eddy currents in the wire. These eddy currents cause energy loss and heat generation, which not only reduces the sensitivity of the sensor, but also introduces additional noise. At the same time, electrical contact may occur between the wire and the soft magnetic material coating, resulting in electromagnetic coupling. This coupling may cause electrical noise and affect the signal quality of the sensor. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide an insulating coated magnetic core for a GMI sensor probe in view of the shortcomings of the prior art. The present invention comprises a metal copper wire, an insulating Al 2 O 3 Coating and Fe 20 Ni 80 The GMI sensor is composed of a layer of Permalloy soft magnetic material. First, a layer of insulating material is sputtered on the surface of the metal wire, then a conductive material is sputtered, and finally the Permalloy soft magnetic material is deposited by electrochemical deposition, which significantly reduces the noise level of the GMI sensor probe.
[0004] Another object of the present invention is to provide a method for preparing the above-mentioned insulating coated magnetic core for a GMI sensor probe.
[0005] Another object of the present invention is to provide the above-mentioned insulating coated magnetic core sensor probe for GMI sensor probe.
[0006] In order to solve the technical problem of the present invention, the following technical solution is adopted: An insulating coated magnetic core for a GMI sensor probe, with a copper wire with a purity of 4N as a substrate, wherein the copper wire has a diameter of 20-140 μm; Al is sequentially wrapped on the copper wire from the inside to the outside; 2 O 3 Insulating layer, conductive metal layer of FeNi or Nb and Fe 20 Ni 80 Permalloy coating; Al 2 O3 The thickness of the insulating layer is 100-500 nm, the thickness of the conductive metal layer of FeNi or Nb is 100-500 nm, and the thickness of Fe 20 Ni 80 The thickness of the Permalloy coating is 4-14 μm, and it is finally annealed with a direct current, the annealing current is 1.6-2 A, and the annealing time is 10-20 min; the insulating coating core used for the GMI sensor probe is U-shaped.
[0007] The Al 2 O 3 The insulating layer and the conductive metal layer of FeNi or Nb are prepared by a magnetron sputtering method, wherein the vacuum degree of the magnetron sputtering is better than 3×10 -5 Pa, the sputtering gas pressure is 0.1-0.3 Pa, and argon gas with a purity of more than 99.99% is introduced.
[0008] The FeNi or Nb conductive metal layer is sputtered by direct current with a power of 10-20 W and a sputtering time of 2500 s-5000 s; 2 O 3 The insulating layer is sputtered by radio frequency with a power of 80-100 W and a sputtering time of 4000 s-8500 s.
[0009] The Al 2 O 3 The distance between the target and the substrate during magnetron sputtering of the insulating layer and the conductive metal layer of FeNi or Nb is 1-6 cm.
[0010] The Fe 20 Ni 80 The Permalloy coating is prepared by electrochemical deposition, specifically: the electrolyte composition is 0.01 M / L FeSO 4 7H 2 O, 0.1 M / L NiSO 4 7H 2 O, 0.3 M / L H 3 BO 3 , 5 g / L ascorbic acid, 1 g / L glycine, 2 g / L saccharin; During electrochemical deposition, the electrolyte temperature is 45℃-65℃, the pH is 2-4, the deposition time is 2500-5000 s, and the deposition current density is 1.5-4A / dm 2 .
[0011] The method for preparing the insulating coated magnetic core for the GMI sensor probe has the following specific steps: Step a: fold a copper wire substrate with a purity of 4N into a U shape, and the diameter of the copper wire is 20-140 μm; Step b: pre-treating the copper wire substrate, specifically: washing with deionized water for 5-10 min → washing with 40-45 g / L sodium carbonate weak base solution for 10-15 min → washing with deionized water for 5-10 min → washing with 2 ml / 50 ml hydrochloric acid solution for 10-15 min → washing with deionized water for 5-10 min, taking out and drying with dry nitrogen; Step c: Al is plated on the pretreated copper wire substrate by magnetron sputtering 2 O 3 Insulating layer and FeNi or Nb conductive metal layer, first Al 2 O 3 The target and FeNi or Nb target are placed in the sputtering chamber and evacuated until the background vacuum reaches 3×10 -5 Pa or less; then the pretreated copper wire substrate is transferred from the sample feeding chamber to the sputtering chamber, the distance between the target and the substrate is 1-6 cm, argon gas with a purity of more than 99.99% is introduced into the sputtering chamber, and the gas pressure is adjusted to 0.1-0.3 Pa, the conductive metal layer of FeNi or Nb is formed by direct current sputtering, the power is 10-20 W, the sputtering time is 1500 s-4000 s, and the thickness of the conductive metal layer of FeNi or Nb is 100-500 nm; the Al 2 O 3 The insulating layer is sputtered by radio frequency with a power of 80-100 W and a sputtering time of 4500 s-9000 s. 2 O 3 The thickness of the insulating layer is 100-500 nm; Step d: Prepare electrolyte to deposit Fe 20 Ni 80 Permalloy coating, the electrolyte composition is 0.01 M / L FeSO 4 7H 2 O, 0.1 M / L NiSO 4 7H 2 O, 0.3 M / L H 3 BO 3 , 5 g / L ascorbic acid, 1 g / L glycine, 2 g / L saccharin; Step e: Deposition by three-electrode method, during electrodeposition, pH value is 2-4, deposition current density is 1.5-4 A / dm 2 ; The electrolyte temperature is 45℃-65℃, the deposition time is 2500-5000 s, Fe 20 Ni 80 The thickness of the Permalloy coating is 4-14 μm; Step f: After electrochemical deposition, take out the U-shaped insulating coated magnetic core for the GMI sensor probe, wipe off the surface solution, and then anneal with a direct current. The annealing current is 1.6-2 A and the annealing time is 10-20 min.
[0012] The sensor probe made of the insulating coated magnetic core for the GMI sensor probe comprises a U-shaped insulating coated magnetic core for the GMI sensor probe, a voltage signal pickup coil, a second glass tube and a first glass tube, and a PCB printed circuit board; one side of the U-shaped insulating coated magnetic core for the GMI sensor probe penetrates into the second glass tube, the second glass tube is sleeved in the first glass tube, the other side of the U-shaped insulating coated magnetic core for the GMI sensor probe penetrates into the interlayer between the first glass tube and the second glass tube, and the U-shaped insulating coated magnetic core for the GMI sensor probe avoids mutual conduction by penetrating into different glass tubes; the voltage signal pickup coil is wound on the first glass tube, and the voltage signal pickup coil and the U-shaped insulating coated magnetic core for the GMI sensor probe are welded to the PCB printed circuit board.
[0013] The diameters of the first glass tube and the second glass tube are adapted to the diameter of a U-shaped insulating coated magnetic core for a GMI sensor probe.
[0014] The U-shaped bending part of the insulating coated magnetic core for the GMI sensor probe does not deposit Fe 20 Ni 80 Permalloy layer.
[0015] The permalloy-plated magnetic core with an insulating layer in the present invention has a high-purity copper wire as the inner core. When the insulating-plated magnetic core used for the GMI sensor probe is working, all the excitation current passes through the high-purity copper wire and does not pass through the coating. Therefore, the uneven rotation of the magnetic moment caused by the skin effect in the permalloy coating can be avoided. The insulating-plated magnetic core with an insulating layer for the GMI sensor probe is "U"-shaped, and has the advantage that two copper wires are electroplated at the same time, which not only avoids the problem of poor uniformity, but also offsets the interference caused by part of the current when the sensor is working. No permalloy is deposited at the bend of the insulating-plated magnetic core used for the GMI sensor probe, avoiding the noise caused by the stress caused by the bend. Because when the GMI sensor is working, the eddy current caused by the current will generate noise inside the metal wire, reducing the signal-to-noise ratio of the sensor, and the insulating coating can effectively suppress the generation of eddy currents, reduce the electromagnetic noise caused by eddy currents, and thus improve the sensitivity and accuracy of the sensor. At the same time, the insulating layer introduced between the metal copper wire and the Permalloy-plated soft magnetic material coating can effectively prevent the alternating current from forming eddy currents between the metal wire and the coating, because eddy currents will cause additional energy loss and heat, resulting in increased noise. The presence of the insulating layer limits the generation of eddy currents, thereby reducing the electromagnetic noise caused thereby. The insulating layer provides electrical isolation between the metal wire and the soft magnetic material coating. This isolation can prevent direct electrical contact between them, reduce electromagnetic coupling and interference, and thus reduce noise. The insulating layer can inhibit the movement of the magnetic domain wall between the metal wire and the coating, and reduce the noise caused by the hysteresis effect. The hysteresis phenomenon can cause signal instability. Through the isolation of the insulating layer, this phenomenon can be reduced and the signal stability can be improved. The insulating layer usually has a lower thermal conductivity and can suppress the thermal noise caused by temperature changes to a certain extent. This is particularly important for working environments with large temperature fluctuations, and helps to improve the temperature stability and signal quality of the sensor. In general, the present invention introduces an insulating layer between the metal copper wire and the Permalloy-plated soft magnetic material coating, and improves the noise performance, stability and anti-interference ability of the GMI sensor by effectively reducing the noise source, and has a wide range of application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a schematic diagram of a composite structure magnetic core with an insulating layer of the present invention; Figure 2 A schematic diagram of a GMI sensor probe having a composite structure magnetic core with an insulating layer according to the present invention; Figure 3 The noise spectrum of a composite structure magnetic core with an insulating layer of the present invention when used in a GMI sensor probe; Among them: copper wire-1, Al 2 O 3 Insulating layer-2, conductive metal layer of FeNi or Nb-3, Fe 20 Ni 80Permalloy coating-4, second glass tube-5, first glass tube-6, voltage signal pickup coil-7. DETAILED DESCRIPTION
[0017] Embodiment 1: A method for preparing an insulating coated magnetic core for a GMI sensor probe, the specific steps are as follows: Step a: taking a copper wire 1 with a purity of 4N and a length of 11 cm as a substrate, and folding it in half to form a U shape, wherein the diameter of the copper wire 1 is 100 μm; Step b: pre-treating the copper wire 1, specifically: washing with deionized water for 10 min → washing with 40 g / L sodium carbonate weak base for 10 min → washing with deionized water for 10 min → washing with 2 ml / 50 ml hydrochloric acid solution for 15 min → washing with deionized water for 10 min, taking out and drying with dry nitrogen for standby use; Step c: Take Al 2 O 3 The target and Nb target were placed in the sputtering chamber of the magnetron sputtering machine and evacuated until the background vacuum reached 2.8×10 -5 Pa; argon gas with a purity of more than 99.99% was introduced into the sputtering chamber, and the gas pressure was adjusted to 0.1 Pa, and then the pretreated copper wire 1 was transferred from the injection chamber to the sputtering chamber, the distance between the target and the substrate was 1 cm, the Nb conductive metal layer was DC sputtered, the power was 10 W, the sputtering time was 1800 s, the thickness of the Nb conductive metal layer was 100 nm, and the Al 2 O 3 The insulating layer was sputtered by radio frequency with a power of 100 W and a sputtering time of 7000 s. 2 O 3 The thickness of the insulating layer is 500 nm, wherein the thin film is evenly attached to the surface of the copper wire 1 and needs to be turned over so that the thin film evenly covers the surface of the copper wire 1; Step d: Prepare electrolyte to deposit Fe 20 Ni 80 The specific electrolyte composition is 0.01 M / L FeSO 4 7H 2 O, 0.1 M / L NiSO 4 7H 2 O, 0.3 M / L H 3 BO 3 , 5 g / L ascorbic acid, 1 g / L glycine, 2 g / L saccharin; Step e: Deposition by three-electrode method, during electrodeposition, pH value is 2-4, deposition current density is 2 A / dm 2 ; The electrolyte temperature is 45℃-65℃, the deposition time is 3000 s, Fe 20Ni 80 The thickness of the Permalloy coating is 8 μm. During electrochemical deposition, the U-shaped portion of the sputtered copper wire 1 is covered with a fixture so that Fe is not deposited on the U-shaped bending portion of the insulating coating core used for the GMI sensor probe. 20 Ni 80 Permalloy layer; Step f: After electrochemical deposition, take out the U-shaped insulating coated magnetic core for the GMI sensor probe, wipe the surface solution with degreased cotton, and then anneal with a direct current. The annealing current is 2 A and the annealing time is 10 min. During annealing, a wire is used to keep the U-shaped composite structure magnetic core vertical to release stress and induce circumferential anisotropy.
[0018] Embodiment 2: A method for preparing an insulating coated magnetic core for a GMI sensor probe, the specific steps are as follows: Step a: taking a copper wire 1 with a purity of 4N and a length of 11 cm as a substrate, and folding it in half to form a U shape, wherein the diameter of the copper wire 1 is 140 μm; Step b: pre-treating the copper wire 1, specifically: washing with deionized water for 5 min → washing with 45 g / L sodium carbonate weak base for 10 min → washing with deionized water for 10 min → washing with 2 ml / 50 ml hydrochloric acid solution for 15 min → washing with deionized water for 5 min, taking out and drying with dry nitrogen for standby use; Step c: Take Al 2 O 3 The target and Nb target were placed in the sputtering chamber of the magnetron sputtering machine and evacuated until the background vacuum reached 2.0×10 -5 Pa; argon gas with a purity of more than 99.99% was introduced into the sputtering chamber, and the gas pressure was adjusted to 0.2 Pa, and then the pretreated copper wire 1 was transferred from the injection chamber to the sputtering chamber, the distance between the target and the substrate was 1 cm, the Nb conductive metal layer was DC sputtered, the power was 12 W, the sputtering time was 1500 s, the thickness of the Nb conductive metal layer was 100 nm, and the Al 2 O 3 The insulating layer was sputtered by radio frequency with a power of 85 W and a sputtering time of 9000 s. 2 O 3 The thickness of the insulating layer is 500 nm, wherein the thin film is evenly attached to the surface of the copper wire 1 and needs to be turned over so that the thin film evenly covers the surface of the copper wire 1; Step d: Prepare electrolyte to deposit Fe 20 Ni 80 The specific electrolyte composition is 0.01 M / L FeSO 4 7H 2 O, 0.1 M / L NiSO 4 7H2 O, 0.3 M / L H 3 BO 3 , 5 g / L ascorbic acid, 1 g / L glycine, 2 g / L saccharin; Step e: Deposition by three-electrode method, during electrodeposition, pH value is 4, deposition current density is 1.5 A / dm 2 ; the electrolyte temperature is 65℃, the deposition time is 5000 s, Fe 20 Ni 80 The thickness of the Permalloy coating is 14 μm. During electrochemical deposition, the U-shaped portion of the sputtered copper wire 1 is covered with a fixture so that Fe is not deposited on the U-shaped bending portion of the insulating coating core used for the GMI sensor probe. 20 Ni 80 Permalloy layer; Step f: After electrochemical deposition, take out the U-shaped insulating coated magnetic core for the GMI sensor probe, wipe the surface solution with degreased cotton, and then anneal with a direct current. The annealing current is 1.6 A and the annealing time is 20 min. During annealing, a wire is used to keep the U-shaped composite structure magnetic core vertical to release stress and induce circumferential anisotropy.
[0019] Embodiment 3: A method for preparing an insulating coated magnetic core for a GMI sensor probe, the specific steps are as follows: Step a: Take a copper wire 1 with a purity of 4N and a length of 11 cm as a substrate, and fold it in half to form a U shape, wherein the diameter of the copper wire 1 is 20 μm; Step b: pre-treating the copper wire 1, specifically: washing with deionized water for 10 min → washing with 40 g / L sodium carbonate weak base for 15 min → washing with deionized water for 5 min → washing with 2 ml / 50 ml hydrochloric acid solution for 10 min → washing with deionized water for 10 min, taking out and drying with dry nitrogen; Step c: Take Al 2 O 3 The target and FeNi target were placed in the sputtering chamber of the magnetron sputtering machine and evacuated until the background vacuum reached 2.0×10 -5 Pa; argon gas with a purity of more than 99.99% was introduced into the sputtering chamber, and the gas pressure was adjusted to 0.2 Pa, and then the pretreated copper wire 1 was transferred from the injection chamber to the sputtering chamber, the distance between the target and the substrate was 6 cm, the conductive metal layer of FeNi was sputtered by DC, the power was 20 W, the sputtering time was 4000 s, the thickness of the conductive metal layer of FeNi was 500 nm, and the Al 2 O 3 The insulating layer was sputtered by radio frequency with a power of 80 W and a sputtering time of 4500 s. 2 O 3The thickness of the insulating layer is 100 nm, wherein the thin film is evenly attached to the surface of the copper wire 1 and needs to be turned over so that the thin film evenly covers the surface of the copper wire 1; Step d: Prepare electrolyte to deposit Fe 20 Ni 80 The specific electrolyte composition is 0.01 M / L FeSO 4 7H 2 O, 0.1 M / L NiSO 4 7H 2 O, 0.3 M / L H 3 BO 3 , 5 g / L ascorbic acid, 1 g / L glycine, 2 g / L saccharin; Step e: Deposition by three-electrode method, during electrodeposition, pH value is 2, deposition current density is 4 A / dm 2 ; the electrolyte temperature is 45℃, the deposition time is 2500 s, Fe 20 Ni 80 The thickness of the Permalloy coating is 5 μm. During electrochemical deposition, the U-shaped portion of the sputtered copper wire 1 is covered with a fixture so that Fe is not deposited on the U-shaped bending portion of the insulating coating core used for the GMI sensor probe. 20 Ni 80 Permalloy layer; Step f: After electrochemical deposition, take out the U-shaped insulating coated magnetic core for the GMI sensor probe, wipe the surface solution with degreased cotton, and anneal it with a direct current. The annealing current is 2 A and the annealing time is 10 min. During annealing, a wire is used to keep the U-shaped composite structure magnetic core vertical to release stress and induce circumferential anisotropy.
[0020] Embodiment 4: A method for preparing an insulating coated magnetic core for a GMI sensor probe, the specific steps are as follows: Step a: Take a copper wire 1 with a purity of 4N and a length of 11 cm as a substrate, and fold it in half to form a U shape, wherein the diameter of the copper wire 1 is 20 μm; Step b: pre-treating the copper wire 1, specifically: washing with deionized water for 10 min → washing with 40 g / L sodium carbonate weak base for 15 min → washing with deionized water for 5 min → washing with 2 ml / 50 ml hydrochloric acid solution for 10 min → washing with deionized water for 10 min, taking out and drying with dry nitrogen; Step c: Take Al 2 O 3 The target and FeNi target were placed in the sputtering chamber of the magnetron sputtering machine, and the distance between the target and the substrate was adjusted to 3 cm, and then vacuum was started. When the background vacuum reached 2.0×10 -5Pa, the pretreated copper wire 1 is transferred from the sample chamber to the sputtering chamber, and then argon gas with a purity of more than 99.99% is introduced into the sputtering chamber, and the gas pressure is adjusted to 0.1 Pa. The conductive metal layer FeNi is sputtered by DC sputtering with a power of 20 W, a sputtering time of 4000 s, and a thickness of 500 nm. 2 O 3 The insulating layer was sputtered by radio frequency with a power of 80 W and a sputtering time of 4500 s. 2 O 3 The thickness of the insulating layer is 100 nm. In order to ensure that the thin film is evenly attached to the surface of the copper wire 1, the copper wire 1 needs to be turned over so that the thin film is evenly covered on its surface.
[0021] Step d: Prepare electrolyte to deposit Fe 20 Ni 80 The specific electrolyte composition is 0.01 M / L FeSO 4 7H 2 O, 0.1 M / L NiSO 4 7H 2 O, 0.3 M / L H 3 BO 3 , 5 g / L ascorbic acid, 1 g / L glycine, 2 g / L saccharin; Step e: Deposition by three-electrode method, during electrodeposition, pH value is 2, deposition current density is 4 A / dm 2 ; The electrolyte temperature is 45℃, the deposition time is 2000 s, Fe 20 Ni 80 The thickness of the Permalloy coating is 4 μm. During electrochemical deposition, the U-shaped portion of the sputtered copper wire 1 is covered with a fixture so that Fe is not deposited on the U-shaped bending portion of the insulating coating core used for the GMI sensor probe. 20 Ni 80 Permalloy layer; Step f: After electrochemical deposition, take out the U-shaped insulating coated magnetic core for the GMI sensor probe, wipe the surface solution with degreased cotton, and anneal it with a direct current. The annealing current is 2 A and the annealing time is 10 min. During annealing, a wire is used to keep the U-shaped composite structure magnetic core vertical to release stress and induce circumferential anisotropy.
[0022] Embodiment 5: A sensor probe made of an insulating coated magnetic core for a GMI sensor probe, comprising a U-shaped insulating coated magnetic core for a GMI sensor probe, a voltage signal pickup coil 7, a second glass tube 5 and a first glass tube 6, and a PCB printed circuit board; wherein the U-shaped bending portion of the U-shaped insulating coated magnetic core for the GMI sensor probe is not deposited with Fe 20Ni 80 Permalloy layer. A copper wire 1 with a purity of 4N is used as the substrate, and the diameter of the copper wire 1 is 20-140 μm; Al 2 O 3 Insulating layer 2, conductive metal layer 3 of FeNi or Nb and Fe 20 Ni 80 Permalloy coating 4; wherein Al 2 O 3 The thickness of the insulating layer 2 is 100-500 nm, the thickness of the conductive metal layer 3 of FeNi or Nb is 100-500 nm, and the thickness of the Fe 20 Ni 80 The thickness of the Permalloy coating 4 is 4-14 μm. One side of the U-shaped insulating coating magnetic core for the GMI sensor probe penetrates into the second glass tube 5, and the second glass tube 5 is sleeved in the first glass tube 6. The other side of the U-shaped insulating coating magnetic core for the GMI sensor probe penetrates into the interlayer between the first glass tube 6 and the second glass tube 5. The U-shaped insulating coating magnetic core for the GMI sensor probe avoids mutual conduction by penetrating different glass tubes; the diameters of the first glass tube 6 and the second glass tube 5 are adapted to the diameter of the U-shaped insulating coating magnetic core for the GMI sensor probe. The voltage signal pickup coil 7 is wound on the first glass tube 6, and the voltage signal pickup coil 7 and the U-shaped insulating coating magnetic core for the GMI sensor probe are welded to the PCB printed circuit board.
[0023] The sensor noise of the GMI sensor probe of the present invention is significantly reduced at 1 Hz when AC excitation and DC bias are applied to the sensor probe, compared with the composite structure magnetic core without an insulating layer. Figure 3 The noise power spectral density shows that at a frequency of 1 Hz, the noise value drops from 59 pT / √Hz to 42 pT / √Hz.
Claims
1. An insulating coated magnetic core for a GMI sensor probe, characterized in that: A copper wire (1) with a purity of 4N is used as a substrate, wherein the diameter of the copper wire (1) is 20-140 μm; an Al2O3 insulating layer (2), a FeNi or Nb conductive metal layer (3) and a Fe 20 Ni 80 Permalloy coating (4); wherein the thickness of the Al2O3 insulating layer is 100-500 nm, the thickness of the FeNi or Nb conductive metal layer is 100-500 nm, and the Fe 20 Ni 80 The thickness of the Permalloy coating is 4-14 μm, and it is finally annealed with a direct current, the annealing current is 1.6-2 A, and the annealing time is 10-20 min; the insulating coating core used for the GMI sensor probe is U-shaped.
2. The insulating coated magnetic core for a GMI sensor probe according to claim 1, characterized in that: The Al2O3 insulating layer (2) and the FeNi or Nb conductive metal layer (3) are prepared by a magnetron sputtering method, wherein the vacuum degree of the magnetron sputtering is better than 3×10 -5 Pa, the sputtering gas pressure is 0.1-0.3 Pa, and argon gas with a purity of more than 99.99% is introduced.
3. The insulating coated magnetic core for a GMI sensor probe according to claim 2, characterized in that: The FeNi or Nb conductive metal layer is formed by direct current sputtering with a power of 10-20 W and a sputtering time of 1500 s-4000 s; the Al2O3 insulating layer is formed by radio frequency sputtering with a power of 80-100 W and a sputtering time of 4500 s-9000 s.
4. The insulating coated magnetic core for a GMI sensor probe according to claim 3, characterized in that: During magnetron sputtering of the Al2O3 insulating layer and the FeNi or Nb conductive metal layer, the distance between the target and the substrate is 1-6 cm.
5. The insulating coated magnetic core for a GMI sensor probe according to claim 4, characterized in that: The Fe 20 Ni 80 The Permalloy coating (4) is prepared by electrochemical deposition, specifically: the electrolyte composition is 0.01 M / L FeSO4·7H2O, 0.1 M / L NiSO4·7H2O, 0.3 M / L H3BO3, 5 g / L ascorbic acid, 1 g / L glycine, and 2 g / L saccharin; during electrochemical deposition, the electrolyte temperature is 45°C-65°C, the pH is 2-4, the deposition time is 2500 s-5000 s, and the deposition current density is 1.5-4A / dm 2 .
6. A method for preparing an insulating coated magnetic core for a GMI sensor probe according to any one of claims 1 to 5, characterized in that The specific steps are as follows: Step a: folding a copper wire substrate with a purity of 4N into a U shape, wherein the diameter of the copper wire (1) is 20-140 μm; Step b: pre-treating the copper wire substrate, specifically: washing with deionized water for 5-10 min → washing with 40-45 g / L sodium carbonate weak base solution for 10-15 min → washing with deionized water for 5-10 min → washing with 2 ml / 50 ml hydrochloric acid solution for 10-15 min → washing with deionized water for 5-10 min, taking out and drying with dry nitrogen; Step c: Using magnetron sputtering, the Al2O3 insulating layer (2) and the FeNi or Nb conductive metal layer (3) are sequentially plated on the pretreated copper wire substrate. First, the Al2O3 target and the FeNi or Nb target are placed in a sputtering chamber and evacuated until the background vacuum reaches 3×10 -5 Pa or less; then the pretreated copper wire substrate is transferred from the injection chamber to the sputtering chamber, the distance between the target and the substrate is 1-6 cm, argon gas with a purity of more than 99.99% is introduced into the sputtering chamber, and the gas pressure is adjusted to 0.1-0.3 Pa, the conductive metal layer of FeNi or Nb is DC sputtered, the power is 10-20 W, the sputtering time is 1500 s-4000 s, and the thickness of the conductive metal layer of FeNi or Nb is 100-500 nm; the Al2O3 insulating layer is radio frequency sputtered, the power is 80-100 W, the sputtering time is 4500 s-9000 s, and the thickness of the Al2O3 insulating layer is 100-500 nm; Step d: Prepare electrolyte to deposit Fe 20 Ni 80 Permalloy coating, the electrolyte composition of which is 0.01 M / L FeSO4·7H2O, 0.1 M / L NiSO4·7H2O, 0.3 M / L H3BO3, 5 g / L ascorbic acid, 1 g / L glycine, and 2 g / L saccharin; Step e: Deposition by three-electrode method, during electrodeposition, pH value is 2-4, deposition current density is 1.5-4 A / dm 2 ; The electrolyte temperature is 45℃-65℃, the deposition time is 2500 s-5000 s, Fe 20 Ni 80 The thickness of the Permalloy coating is 4-14 μm; Step f: After electrochemical deposition, take out the U-shaped insulating coated magnetic core for the GMI sensor probe, wipe off the surface solution, and then anneal with a direct current. The annealing current is 1.6-2 A and the annealing time is 10-20 min.
7. A sensor probe made of an insulating coated magnetic core for a GMI sensor probe according to any one of claims 1 to 5, characterized in that: The invention comprises a U-shaped insulating coated magnetic core for a GMI sensor probe, a voltage signal pickup coil (7), a second glass tube (5), a first glass tube (6), and a PCB printed circuit board; one side of the U-shaped insulating coated magnetic core for a GMI sensor probe is inserted into the second glass tube (5), the second glass tube (5) is sleeved in the first glass tube (6), the other side of the U-shaped insulating coated magnetic core for a GMI sensor probe is inserted into the interlayer between the first glass tube (6) and the second glass tube (5), and the U-shaped insulating coated magnetic core for a GMI sensor probe is prevented from being connected to each other by being inserted into different glass tubes; the voltage signal pickup coil (7) is wound on the first glass tube (6), and the voltage signal pickup coil (7) and the U-shaped insulating coated magnetic core for a GMI sensor probe are welded to the PCB printed circuit board.
8. The sensor probe made of an insulating coated magnetic core for a GMI sensor probe according to claim 7, characterized in that: The diameters of the first glass tube (6) and the second glass tube (5) are adapted to the diameter of a U-shaped insulating coated magnetic core for a GMI sensor probe.
9. The sensor probe made of an insulating coated magnetic core for a GMI sensor probe according to claim 8, characterized in that: The U-shaped bending part of the insulating coated magnetic core for the GMI sensor probe does not deposit Fe 20 Ni 80 Permalloy layer.
Citation Information
Patent Citations
Method for improving thermostability of anisotropic magnetoresistance permalloy film
CN102867645A
Fluxgate sensor and manufacturing method thereof
CN106772142A
GMI sensor probe, U-shaped composite structure magnetic core thereof and preparation method of U-shaped composite structure magnetic core
CN117316617A
Thin-film magnetic head and its produciton
JP1994203326A
Common mode filter and method of manufacturing the same
US20140203900A1
Cited By
Two-phase composite structure magnetic core and preparation method thereof, orthogonal fluxgate probe, magnetic sensing test system and molecular test method
CN121718945A