Protective sheet for semiconductor processing and method for manufacturing semiconductor device
The protective sheet for semiconductor processing addresses warping and peeling issues by using a base material with high rigidity and an intermediate layer with specific stress relaxation properties, ensuring stable wafer handling and reduced damage during back grinding.
Patent Information
- Application Number
- JP2021511489
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-29
- Filing Date
- 2020-03-24
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2040-03-24
AI Technical Summary
Existing protective sheets for semiconductor processing fail to adequately suppress warping of thin semiconductor wafers due to reduced rigidity, leading to damage and transportation issues during back grinding, and poor peeling of the adhesive tape.
A protective sheet comprising a base material, an intermediate layer with residual stress of 300 Pa or less, and an adhesive layer, where the intermediate layer has a shear storage modulus of 25000 Pa or less and a loss tangent of 1.0 or more, designed to absorb residual stress and maintain wafer rigidity.
The solution effectively suppresses warpage of semiconductor wafers after processing, allowing for thinner materials and easier handling, reducing damage and improving peeling efficiency.
Smart Images

Figure 0007555907000002 
Figure 0007555907000003 
Figure 0007555907000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a protective sheet for semiconductor processing and a method for manufacturing a semiconductor device. In particular, the present invention relates to a protective sheet for semiconductor processing that is suitably used for suppressing warpage of a semiconductor wafer, and a method for manufacturing a semiconductor device using the protective sheet for semiconductor processing. [Background technology]
[0002] Various electronic devices are equipped with a large number of semiconductor devices mounted with semiconductor chips obtained by dividing a semiconductor wafer on which a circuit is formed. Electronic devices are rapidly becoming smaller and more multifunctional, and semiconductor chips are also required to be smaller, thinner, and more dense. In order to make chips smaller and thinner, it is common to form circuits on the front surface of a semiconductor wafer, and then grind the back surface of the semiconductor wafer to adjust the thickness of the chip.
[0003] During back grinding of a semiconductor wafer, a protective sheet called back grind tape is applied to the wafer surface to protect the circuits on the wafer surface and to hold the semiconductor wafer. However, the semiconductor wafer after back grinding is very thin and tends to warp together with the adhesive tape. When the semiconductor wafer warps, it becomes more likely to be damaged and it becomes difficult to transport the semiconductor wafer to the next process, causing other problems.
[0004] For example, Patent Document 1 discloses a surface protection sheet in which high stress relaxation properties are imparted to the base material in order to suppress warping of semiconductor wafers. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2016 / 063827 Summary of the Invention [Problem to be solved by the invention]
[0006] In Patent Document 1, the rigidity of the substrate is reduced in order to impart stress relaxation properties to the substrate. However, when the rigidity of the substrate is low, the rigidity of the entire protective sheet is reduced, and there is a problem that the semiconductor wafer cannot be held sufficiently when the semiconductor wafer is thinned by back grinding of the semiconductor wafer. In addition, there is a problem that the substrate stretches when the tape is peeled off after grinding, which causes peeling failure.
[0007] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a protective sheet for semiconductor processing that can suppress warping after thinning a semiconductor wafer, and a method for manufacturing a semiconductor device using the protective sheet for semiconductor processing. [Means for solving the problem]
[0008] An aspect of the present invention is [1] A protective sheet for semiconductor processing having a substrate, an intermediate layer and a pressure-sensitive adhesive layer on the substrate in this order, This is a protective sheet for semiconductor processing, in which the residual stress of the intermediate layer after being held at 65°C for 300 seconds is 300 Pa or less.
[0009] [2] The product of the tensile storage modulus of the substrate and its thickness is 3.5 × 10 4 The protective sheet for semiconductor processing according to [1], wherein the strength is N / m or more.
[0010] [3] The protective sheet for semiconductor processing according to [1] or [2], wherein the shear storage modulus of the intermediate layer at 65°C is 25,000 Pa or less.
[0011] [4] The protective sheet for semiconductor processing according to any one of [1] to [3], wherein the loss tangent of the intermediate layer at 65° C. is 1.0 or more.
[0012] [5] A step of attaching the semiconductor processing protection sheet according to any one of [1] to [4] to a semiconductor wafer; and reducing the rigidity of the semiconductor wafer to which the protective sheet for semiconductor processing is attached. Effect of the Invention
[0013] According to the present invention, it is possible to provide a protective sheet for semiconductor processing that can suppress warping after processing a semiconductor wafer to make it thinner, and a method for manufacturing a semiconductor device using the protective sheet for semiconductor processing. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of the protective sheet for semiconductor processing according to this embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing a state in which the protective sheet for semiconductor processing according to this embodiment is attached to the circuit surface of a semiconductor wafer. [Figure 3A] FIG. 3A is a schematic cross-sectional view showing a semiconductor wafer after back grinding to which a conventional protective sheet for semiconductor processing has been attached. [Figure 3B] FIG. 3B is a schematic cross-sectional view showing a semiconductor wafer after backside grinding to which the protective sheet for semiconductor processing according to this embodiment has been attached. [Figure 4] FIG. 4 is a schematic cross-sectional view for explaining that the residual stress of the intermediate layer is low in the protective sheet for semiconductor processing according to this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention will now be described in detail based on specific embodiments in the following order.
[0016] (1. Protective sheet for semiconductor processing) The semiconductor processing protective sheet 1 according to this embodiment has a structure in which an intermediate layer 20 and an adhesive layer 30 are laminated in this order on a substrate 10, as shown in Fig. 1. The semiconductor processing protective sheet is not limited to the structure shown in Fig. 1, and may have other layers as long as the effects of the present invention can be obtained. For example, a release sheet may be formed on the main surface 30a of the adhesive layer 30 in order to protect the adhesive layer 30 until the adhesive layer 30 is attached to an adherend.
[0017] As shown in Fig. 2, the protective sheet for semiconductor processing 1 according to this embodiment is used by attaching the main surface 30a of the adhesive layer 30 to the circuit surface 50a of the semiconductor wafer 50. When the protective sheet for semiconductor processing 1 is attached to the semiconductor wafer 50, it is attached while applying tension to the protective sheet for semiconductor processing 1 (while stretching the protective sheet for semiconductor processing 1). As a result, residual stress RS occurs in the attached protective sheet for semiconductor processing 1. The substrate is usually more rigid than components other than the substrate and resists tension, so residual stress occurs mainly in the substrate.
[0018] Since the substrate is pulled during application, the residual stress generated in the substrate acts in the direction of shrinkage of the substrate. This residual stress is canceled by the rigidity of the semiconductor wafer before grinding the semiconductor wafer. However, after grinding the semiconductor wafer, the thickness of the semiconductor wafer is reduced, and the rigidity of the semiconductor wafer is reduced. As a result, as shown in FIG. 3A, after grinding the semiconductor wafer to which the conventional semiconductor processing protective sheet 100 is applied, the residual stress becomes apparent, and the semiconductor wafer 50 is warped.
[0019] In contrast, the semiconductor processing protective sheet 1 according to this embodiment has the characteristics described below, so that the semiconductor wafer 50 to which the semiconductor processing protective sheet 1 is attached is prevented from warping even if the thickness is reduced by grinding, as shown in Fig. 3B. The components of the semiconductor processing protective sheet 1 will be described in detail below.
[0020] (2. Base material) The substrate is not limited as long as it is made of a material capable of supporting a semiconductor wafer. For example, various resin films used as substrates for backgrinding tapes are exemplified. The substrate may be made of a single-layer film made of one resin film, or may be made of a multi-layer film made of a plurality of resin films laminated together.
[0021] (2.1 Physical properties of the substrate) In this embodiment, the substrate preferably has high rigidity. The substrate has high rigidity, so that the semiconductor wafer can be held without being damaged even if the thickness of the wafer is reduced by grinding. In addition, the substrate can be prevented from stretching during tape peeling after grinding, which can cause peeling failure.
[0022] In this embodiment, the rigidity of the substrate is evaluated by the product of the tensile storage modulus of the substrate and the thickness of the substrate. The product of the tensile storage modulus of the substrate and the thickness of the substrate is 3.5×10 4 In order to prevent peel failure, it is preferable that the product of the tensile storage modulus of the substrate and the thickness of the substrate is 8.0×10 5 It is preferable that the resistance be less than N / m.
[0023] The preferred thickness range of the substrate varies depending on the tensile storage modulus of the substrate, but in this embodiment, the thickness is preferably 15 μm or more and 200 μm or less, and more preferably 40 μm or more and 150 μm or less.
[0024] (2.2 Substrate material) As the material of the substrate, when the thickness of the substrate is within the above range, a material in which the product of the tensile storage modulus of the substrate and the thickness of the substrate is within the above range is preferable. In this embodiment, for example, polyesters such as polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, wholly aromatic polyester, polyamide, polycarbonate, polyacetal, modified polyphenylene oxide, polyphenylene sulfide, polysulfone, polyether ketone, biaxially oriented polypropylene, etc. can be mentioned. Among these, polyesters are preferable, and polyethylene terephthalate is more preferable.
[0025] (3. Middle Class) The intermediate layer is a layer disposed between the substrate and the adhesive layer. In this embodiment, the intermediate layer is a layer having high stress relaxation properties that can take on the residual stress of the substrate and relax the residual stress within the intermediate layer. As shown in FIG. 4, the substrate 10 shrinks due to the residual stress after the semiconductor processing protection sheet 1 is attached, but most of the residual stress is relaxed in the intermediate layer, so that warpage of the semiconductor wafer 50 is suppressed. The intermediate layer may be composed of one layer (single layer) or may be composed of two or more layers.
[0026] The thickness of the intermediate layer 20 is set arbitrarily within a range in which the effects of the present invention can be obtained. In this embodiment, the thickness of the intermediate layer 20 is preferably 30 μm or more and 600 μm or less, and more preferably 50 μm or more and 400 μm or less. The thickness of the intermediate layer means the thickness of the entire intermediate layer. For example, the thickness of an intermediate layer composed of multiple layers means the total thickness of all layers constituting the intermediate layer.
[0027] In this embodiment, the intermediate layer has the following physical properties.
[0028] (3.1 Residual stress after holding at 65℃ for 300 seconds) In this embodiment, the residual stress of the intermediate layer after holding at 65°C for 300 seconds is 300 Pa or less. The residual stress taken from the substrate is rapidly relaxed in the intermediate layer and is almost stable after 300 seconds. In addition, the semiconductor processing protection sheet is usually attached to the semiconductor wafer at a temperature of about 65°C.
[0029] Therefore, by keeping the stress remaining in the intermediate layer after holding at 65°C for 300 seconds within the above range, the residual stress assumed from the attached substrate is sufficiently alleviated within the intermediate layer. Note that "residual stress in the intermediate layer after holding at 65°C for 300 seconds" refers to the residual stress in the intermediate layer measured after the temperature of the intermediate layer is maintained at 65°C for 300 seconds.
[0030] The residual stress of the intermediate layer after being held at 65° C. for 300 seconds is preferably 250 Pa or less, and more preferably 200 Pa or less. In addition, the residual stress of the intermediate layer after being held at 65° C. for 300 seconds is preferably 0.1 Pa or more.
[0031] In this embodiment, the residual stress of the intermediate layer after being held at 65°C for 300 seconds can be measured as follows: The material constituting the intermediate layer is prepared as a sample of a predetermined size, and the sample at a temperature of 65°C is twisted using a dynamic viscoelasticity measuring device to apply shear strain to the sample. The shear stress 300 seconds after the strain is applied is measured, and the measured shear stress is regarded as the residual stress of the intermediate layer after being held at 65°C for 300 seconds.
[0032] (3.2 Shear storage modulus at 65℃) In this embodiment, the shear storage modulus (G') of the intermediate layer at 65°C is preferably 25000 Pa or less. The shear storage modulus (G') is one of the indicators of the ease of deformation (hardness) of the intermediate layer. When the shear storage modulus (G') of the intermediate layer at 65°C is within the above range, the intermediate layer can sufficiently follow the contraction of the base material, thereby suppressing warpage of the semiconductor wafer.
[0033] The shear storage modulus of the intermediate layer at 65°C is 2.5×10 4 Pa or less, and more preferably 2.0×10 4 The shear storage modulus of the intermediate layer at 65° C. is preferably 0.3×10 Pa or less. 4 It is preferable that the pressure is 1 Pa or more.
[0034] The shear storage modulus of the intermediate layer at 65° C. may be measured by a known method. For example, the intermediate layer may be used as a sample of a predetermined size, and the sample may be strained at a predetermined frequency within a predetermined temperature range using a dynamic viscoelasticity measuring device to measure the elastic modulus, and the shear storage modulus may be calculated from the measured elastic modulus.
[0035] (3.3 Loss tangent at 65℃) In this embodiment, the loss tangent (tan δ) of the intermediate layer at 65°C is preferably 1.0 or more. The loss tangent is defined as "loss modulus / storage modulus" and is a value measured by the response to stress applied to an object using a dynamic viscoelasticity measuring device. When the loss tangent of the intermediate layer at 65°C is within the above range, the residual stress taken over from the base material is consumed as heat, thereby suppressing warpage of the semiconductor wafer.
[0036] The loss tangent of the intermediate layer at 65° C. is more preferably 1.0 or more, and even more preferably 1.2 or more. Also, the loss tangent of the intermediate layer at 65° C. is preferably 3.0 or less.
[0037] The loss tangent of the intermediate layer at 65° C. may be measured by a known method, similar to the shear storage modulus. For example, the intermediate layer is prepared as a sample of a predetermined size, and a dynamic viscoelasticity measuring device is used to apply a strain to the sample at a predetermined frequency within a predetermined temperature range to measure the elastic modulus, and the loss tangent can be calculated from the measured elastic modulus.
[0038] (3.4 Gel fraction of the intermediate layer) In this embodiment, the gel fraction of the intermediate layer is preferably 55% or less. With a gel fraction within the above range, the intermediate layer has flexibility and can sufficiently follow the contraction of the base material, thereby suppressing warpage of the semiconductor wafer.
[0039] The gel fraction of the intermediate layer is more preferably 50% or less, and even more preferably 45% or less, and is preferably 1% or more.
[0040] (3.5 Composition for intermediate layer) The composition of the intermediate layer is not particularly limited as long as the intermediate layer has the above-mentioned physical properties, but in this embodiment, the intermediate layer is preferably composed of a composition containing a resin (intermediate layer composition). The intermediate layer composition preferably contains the components shown below.
[0041] (3.5.1 Urethane (meth)acrylates) Urethane (meth)acrylate is a compound having at least a (meth)acryloyl group and a urethane bond, and has the property of being polymerized by energy ray irradiation. In this embodiment, urethane (meth)acrylate is a component used to impart flexibility to the intermediate layer and to impart the property of reducing residual stress. In this specification, "(meth)acrylate" is used as a term indicating both "acrylate" and "methacrylate", and the same applies to other similar terms.
[0042] The urethane (meth)acrylate may be a monofunctional type or a multifunctional type. In this embodiment, a multifunctional urethane (meth)acrylate is preferred, and from the viewpoint of keeping the residual stress of the intermediate layer within the above range, a bifunctional urethane (meth)acrylate is preferred.
[0043] The urethane (meth)acrylate may be an oligomer, a polymer, or a mixture thereof. In this embodiment, a urethane (meth)acrylate oligomer is preferred.
[0044] The urethane (meth)acrylate can be obtained, for example, by reacting a polyol compound with a polyisocyanate compound to obtain a terminal isocyanate urethane prepolymer, and then reacting the resulting prepolymer with a hydroxyl group-containing (meth)acrylate. The urethane (meth)acrylate may be used alone or in combination of two or more kinds.
[0045] The content of the urethane (meth)acrylate in the intermediate layer composition is preferably 20% by mass or more, more preferably 25% by mass or more, and even more preferably 30% by mass or more. The content of the urethane (meth)acrylate in the intermediate layer composition is preferably 70% by mass or less, more preferably 65% by mass or less, and even more preferably 50% by mass or less.
[0046] 3.5.2 Polymerizable monomers The polymerizable monomer is preferably a polymerizable compound other than the above-mentioned urethane (meth)acrylate, and is a compound that can be polymerized with other components by irradiation with energy rays. Specifically, the polymerizable monomer is preferably a compound having at least one (meth)acryloyl group.
[0047] Examples of the polymerizable monomer include (meth)acrylates having an alkyl group having 1 to 30 carbon atoms; (meth)acrylates having a functional group such as a hydroxyl group, an amide group, an amino group, or an epoxy group; (meth)acrylates having an alicyclic structure; (meth)acrylates having an aromatic structure; (meth)acrylates having a heterocyclic structure; and vinyl compounds such as styrene, hydroxyethyl vinyl ether, hydroxybutyl vinyl ether, N-vinyl formamide, N-vinyl pyrrolidone, and N-vinyl caprolactam.
[0048] Examples of the (meth)acrylate having an alkyl group having 1 to 30 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, hexadecyl (meth)acrylate, octadecyl (meth)acrylate, and eicosyl (meth)acrylate.
[0049] Examples of the (meth)acrylate having a functional group include hydroxyl group-containing (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N-butyl (meth)acrylamide, and N-methylol (meth)acrylamide. Examples of the amide group-containing compounds include acrylamide, N-methylolpropane (meth)acrylamide, N-methoxymethyl (meth)acrylamide, and N-butoxymethyl (meth)acrylamide; amino group-containing (meth)acrylates such as primary amino group-containing (meth)acrylates, secondary amino group-containing (meth)acrylates, and tertiary amino group-containing (meth)acrylates; and epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, and allyl glycidyl ether.
[0050] Examples of (meth)acrylates having an alicyclic structure include isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxy (meth)acrylate, cyclohexyl (meth)acrylate, trimethylcyclohexyl (meth)acrylate, and adamantane (meth)acrylate.
[0051] Examples of the (meth)acrylate having an aromatic structure include phenylhydroxypropyl (meth)acrylate, benzyl (meth)acrylate, and 2-hydroxy-3-phenoxypropyl (meth)acrylate.
[0052] Examples of the (meth)acrylate having a heterocyclic structure include tetrahydrofurfuryl (meth)acrylate and morpholine (meth)acrylate.
[0053] In this embodiment, the polymerizable monomer preferably includes a (meth)acrylate having an alkyl group with 1 to 30 carbon atoms and a (meth)acrylate having an alicyclic structure. From the viewpoint of keeping the residual stress of the intermediate layer within the above range, a (meth)acrylate having an alkyl group with 4 to 14 carbon atoms is preferred, and as the (meth)acrylate having an alicyclic structure, isobornyl (meth)acrylate and trimethylcyclohexyl (meth)acrylate are preferred.
[0054] In addition, when the intermediate layer composition contains a crosslinking agent, a (meth)acrylate having a functional group capable of reacting with the crosslinking agent is not preferred. This is because the crosslinked structure formed by the crosslinking reaction may increase the residual stress of the intermediate layer. For example, a composition for the intermediate layer containing a polyisocyanate-based crosslinking agent and a (meth)acrylate having a hydroxyl group is not preferred.
[0055] The content of the polymerizable monomer in the intermediate layer composition is preferably 20% by mass or more, more preferably 30% by mass or more, and is preferably 80% by mass or less, more preferably 70% by mass or less.
[0056] In addition, the mass ratio of the urethane (meth)acrylate to the polymerizable monomer (urethane (meth)acrylate / polymerizable monomer) in a total of 100 parts by mass of the urethane (meth)acrylate and the polymerizable monomer is preferably from 20 / 80 to 80 / 20, and more preferably from 30 / 70 to 70 / 30.
[0057] 3.5.3 Photoinitiators When the intermediate layer composition contains the above-mentioned urethane (meth)acrylate and polymerizable monomer, the intermediate layer composition preferably contains a photopolymerization initiator. By containing the photopolymerization initiator, polymerization proceeds reliably, and an intermediate layer having the above-mentioned characteristics can be easily obtained.
[0058] Examples of the photopolymerization initiator include photopolymerization initiators such as benzoin compounds, acetophenone compounds, acylphosphine oxide compounds, titanocene compounds, thioxanthone compounds, and peroxide compounds, and photosensitizers such as amines and quinones.Specific examples include 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and 2,2-dimethoxy-1,2-diphenylethan-1-one.These photopolymerization initiators may be used alone or in combination of two or more.
[0059] The amount of the photopolymerization initiator is preferably 0.05 to 15 parts by mass, and more preferably 0.5 to 10 parts by mass, per 100 parts by mass of the total of the urethane (meth)acrylate and the polymerizable monomer.
[0060] 3.5.4 Chain Transfer Agents The intermediate layer composition preferably contains a chain transfer agent. The chain transfer agent can cause a chain transfer reaction and adjust the progress of the curing reaction of the intermediate layer composition. By containing the chain transfer agent, it becomes possible for components with short molecular chains to remain relatively even after curing, so that the cured polymer has a structure with relatively high flexibility. As a result, the residual stress applied to the intermediate layer can be sufficiently relaxed, and it becomes easy to set the residual stress of the intermediate layer within the above range.
[0061] Examples of the chain transfer agent include thiol group-containing compounds. Examples of the thiol group-containing compounds include nonyl mercaptan, 1-dodecanethiol, 1,2-ethanedithiol, 1,3-propanedithiol, triazine thiol, triazine dithiol, triazine trithiol, 1,2,3-propane trithiol, tetraethylene glycol-bis(3-mercaptopropionate), trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetraki ... Examples of the chain transfer agent include thritol tetrakis thioglucolate, dipentaerythritol hexakis (3-mercaptopropionate), tris [(3-mercaptopropionyloxy)-ethyl]-isocyanurate, 1,4-bis (3-mercaptobutyryloxy) butane, pentaerythritol tetrakis (3-mercaptobutyrate), and 1,3,5-tris (3-mercaptobutyloxyethyl)-1,3,5-triazine-2,4,6- (1H,3H,5H)-trione. The chain transfer agent may be used alone or in combination of two or more.
[0062] The amount of the chain transfer agent is preferably 0.1 to 10 parts by mass, more preferably 0.3 to 5 parts by mass, per 100 parts by mass of the total of the urethane (meth)acrylate and the polymerizable monomer.
[0063] (4. Adhesive Layer) The adhesive layer is attached to the circuit surface of the semiconductor wafer, and protects the circuit surface and supports the semiconductor wafer until it is peeled off from the circuit surface. The adhesive layer may be composed of one layer (single layer), or may be composed of two or more layers. When the adhesive layer has multiple layers, these multiple layers may be the same or different from each other, and the combination of layers constituting these multiple layers is not particularly limited.
[0064] The thickness of the adhesive layer is not particularly limited, but is preferably 1 μm or more and 50 μm or less, more preferably 2 μm or more and 30 μm or less. The thickness of the adhesive layer means the thickness of the entire adhesive layer. For example, the thickness of an adhesive layer composed of multiple layers means the total thickness of all layers constituting the adhesive layer.
[0065] The composition of the adhesive layer is not limited as long as it has enough adhesiveness to protect the circuit surface of the semiconductor wafer. In this embodiment, the adhesive layer is preferably composed of, for example, an acrylic adhesive, a urethane adhesive, a rubber adhesive, a silicone adhesive, or the like.
[0066] In addition, the adhesive layer is preferably formed from an energy ray curable adhesive. By forming the adhesive layer of the semiconductor processing protective sheet from an energy ray curable adhesive, when the sheet is attached to the semiconductor wafer, the sheet adheres to the semiconductor wafer with high adhesive strength, and when the sheet is peeled off from the semiconductor wafer, the adhesive strength can be reduced by irradiating the sheet with energy rays. Therefore, while appropriately protecting the circuits of the semiconductor wafer, the circuit on the surface of the semiconductor wafer is prevented from being destroyed and the adhesive is prevented from being transferred onto the semiconductor wafer when the semiconductor processing protective sheet is peeled off.
[0067] In this embodiment, the energy ray curable adhesive is preferably composed of an adhesive composition containing an acrylic adhesive. As the acrylic adhesive, it is preferable to use an acrylic polymer.
[0068] The acrylic polymer may be any known acrylic polymer, but in this embodiment, a functional group-containing acrylic polymer is preferred. The functional group-containing acrylic polymer may be a homopolymer formed from one type of acrylic monomer, a copolymer formed from multiple types of acrylic monomers, or a copolymer formed from one or multiple types of acrylic monomers and a monomer other than the acrylic monomer.
[0069] In this embodiment, the functional group-containing acrylic polymer is preferably an acrylic copolymer obtained by copolymerizing an alkyl (meth)acrylate with a functional group-containing monomer.
[0070] Examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, and n-octyl (meth)acrylate.
[0071] The functional group-containing monomer is a monomer containing a reactive functional group. The reactive functional group is a functional group capable of reacting with other compounds such as a crosslinking agent described later. Examples of the functional group in the functional group-containing monomer include a hydroxyl group, a carboxyl group, and an epoxy group, and a hydroxyl group is preferred.
[0072] Examples of hydroxyl group-containing monomers include hydroxyalkyl (meth)acrylates such as hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; and non-(meth)acrylic unsaturated alcohols (unsaturated alcohols not having a (meth)acryloyl skeleton) such as vinyl alcohol and allyl alcohol.
[0073] The pressure-sensitive adhesive composition preferably further contains an energy ray-curable compound having an energy ray-curable group. The energy ray-curable compound having an energy ray-curable group is preferably a compound having one or more groups selected from an isocyanate group, an epoxy group, and a carboxy group, and more preferably a compound having an isocyanate group.
[0074] Examples of compounds having an isocyanate group include 2-methacryloyloxyethyl isocyanate, meta-isopropenyl-α,α-dimethylbenzyl isocyanate, methacryloyl isocyanate, allyl isocyanate, 1,1-(bisacryloyloxymethyl)ethyl isocyanate; acryloyl monoisocyanate compounds obtained by reacting a diisocyanate compound or a polyisocyanate compound with hydroxyethyl (meth)acrylate; and acryloyl monoisocyanate compounds obtained by reacting a diisocyanate compound or a polyisocyanate compound with a polyol compound and hydroxyethyl (meth)acrylate. The isocyanate group undergoes an addition reaction with the hydroxyl group of the functional group-containing acrylic polymer.
[0075] The pressure-sensitive adhesive composition preferably further contains a crosslinking agent, which reacts with functional groups, for example, to crosslink resins contained in the functional-group-containing acrylic polymer.
[0076] Examples of the crosslinking agent include isocyanate-based crosslinking agents (crosslinking agents having an isocyanate group) such as tolylene diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, and adducts of these diisocyanates; epoxy-based crosslinking agents (crosslinking agents having a glycidyl group) such as ethylene glycol glycidyl ether; aziridine-based crosslinking agents (crosslinking agents having an aziridinyl group) such as hexa[1-(2-methyl)-aziridinyl]triphosphatriazine; metal chelate-based crosslinking agents (crosslinking agents having a metal chelate structure) such as aluminum chelate; and isocyanurate-based crosslinking agents (crosslinking agents having an isocyanuric acid skeleton).
[0077] The crosslinking agent is preferably an isocyanate-based crosslinking agent from the viewpoints of improving the cohesive strength of the pressure-sensitive adhesive and thereby improving the adhesive strength of the pressure-sensitive adhesive layer, and of easy availability.
[0078] The pressure-sensitive adhesive composition may further contain a photopolymerization initiator. When the pressure-sensitive adhesive composition contains a photopolymerization initiator, the curing reaction proceeds sufficiently even when irradiated with relatively low-energy energy rays such as ultraviolet rays.
[0079] Examples of the photopolymerization initiator include photoinitiators such as benzoin compounds, acetophenone compounds, acylphosphine oxide compounds, titanocene compounds, thioxanthone compounds, and peroxide compounds, and photosensitizers such as amines and quinones.Specific examples include α-hydroxycyclohexyl phenyl ketone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzyl diphenyl sulfide, benzyl dimethyl ketal, tetramethylthiuram monosulfide, azobisisobutyronitrile, dibenzyl, diacetyl, β-chloroanthraquinone, and 2,4,6-trimethylbenzoyldiphenylphosphine oxide.
[0080] (5. Manufacturing method of protective sheet for semiconductor processing) The method for producing the semiconductor processing protection sheet according to this embodiment is not particularly limited as long as it is a method capable of laminating an intermediate layer and a pressure-sensitive adhesive layer on one side of a substrate, and any known method may be used.
[0081] First, as a composition for forming an intermediate layer, for example, a composition for intermediate layer containing the above-mentioned components, or a composition obtained by diluting the composition for intermediate layer with a solvent, etc. is prepared. Similarly, as a pressure-sensitive adhesive composition for forming a pressure-sensitive adhesive layer, for example, a pressure-sensitive adhesive composition containing the above-mentioned components, or a composition obtained by diluting the pressure-sensitive adhesive composition with a solvent, etc. is prepared.
[0082] Examples of the solvent include organic solvents such as methyl ethyl ketone, acetone, ethyl acetate, tetrahydrofuran, dioxane, cyclohexane, n-hexane, toluene, xylene, n-propanol, and isopropanol.
[0083] Then, the intermediate layer composition or the like is applied onto the substrate by a known method such as spin coating, spray coating, bar coating, knife coating, roll coating, blade coating, die coating, or gravure coating to form a coating film, and the coating film is cured to form an intermediate layer on the substrate. In this embodiment, the coating film is preferably cured by irradiation with energy rays. Examples of the energy rays include ultraviolet rays and electron beams, and ultraviolet rays are preferred.
[0084] Furthermore, in this embodiment, it is preferable to cure the coating film by irradiating the energy rays multiple times, which makes it possible to control the degree of cure of the intermediate layer and to easily set the residual stress of the intermediate layer within the above range.
[0085] Specifically, it is preferable that the coating film is exposed to oxygen and then irradiated with energy rays, and then the coating film is shielded from oxygen and then irradiated with energy rays again.
[0086] In addition, when the energy rays are ultraviolet rays, the ultraviolet irradiation conditions are preferably such that the illuminance of the ultraviolet rays is 30 to 500 mW / cm 2 , more preferably 50 to 340 mW / cm 2 The amount of ultraviolet light irradiation is preferably 100 to 2500 mJ / cm 2 , more preferably 150 to 2000 mJ / cm 2 It is.
[0087] When irradiation with ultraviolet light is further performed, the irradiation conditions are preferably such that the illuminance and dose are greater than those of the previous irradiation.
[0088] An adhesive composition or the like is applied to the intermediate layer thus cured and formed by a known method, and then heated and dried to produce a protective sheet for semiconductor processing in which an intermediate layer and an adhesive layer are formed in that order on the substrate.
[0089] Alternatively, the protective sheet for semiconductor processing may be produced as follows: That is, the intermediate layer composition or the like is applied to the release-treated surface of one release sheet to form a coating film, which is then cured as described above to form an intermediate layer on the release sheet.
[0090] The release-treated surface of the other release sheet is coated with an adhesive composition or the like, and heated and dried to form an adhesive layer on the release sheet. After that, the intermediate layer on one release sheet is bonded to the substrate, and the release sheet is removed. Then, the intermediate layer and the adhesive layer on the other release sheet are bonded to produce a semiconductor processing protective sheet in which the intermediate layer, adhesive layer, and release sheet are provided in this order on the substrate. The release sheet may be appropriately peeled off and removed before using the semiconductor processing protective sheet.
[0091] (6. Manufacturing method of semiconductor device) A method for manufacturing a semiconductor device using the semiconductor processing protective sheet of this embodiment is not particularly limited, as long as it includes a step of attaching the semiconductor processing protective sheet of this embodiment to a semiconductor wafer, and a step of reducing the rigidity of the semiconductor wafer to which the semiconductor processing protective sheet is attached.
[0092] A preferred process for attaching the protective sheet for semiconductor processing according to this embodiment to a semiconductor wafer is, for example, a process for attaching the protective sheet for semiconductor processing according to this embodiment to the surface of the semiconductor wafer on which circuits are formed.
[0093] An example of a process for reducing the rigidity of a semiconductor wafer is a process for grinding the semiconductor wafer to reduce its thickness.
[0094] Below, as an example of a method for manufacturing a semiconductor device using the semiconductor processing protective sheet of this embodiment, a method for manufacturing a semiconductor chip having a circuit formed thereon as a semiconductor device from a semiconductor wafer will be described with reference to Figures 2 to 4.
[0095] First, as shown in FIG. 2, the protective sheet for semiconductor processing 1 is attached to the surface (surface 50a) on which the circuit of the semiconductor wafer is formed to protect the circuit surface. At this time, the protective sheet for semiconductor processing 1 is attached to the circuit surface while being pulled. Therefore, after attachment, the protective sheet for semiconductor processing 1, particularly the highly rigid substrate, generates a residual stress RS acting in the direction of shrinkage of the substrate. Note that the circuit surface to which the protective sheet for semiconductor processing according to this embodiment is attached may have a convex electrode such as a bump or pillar electrode formed thereon.
[0096] As shown in Fig. 4, the residual stress RS causes the substrate 10 to shrink, and the residual stress generated in the substrate 10 is eliminated, but the deformation of the substrate 10 generates residual stress RS in the intermediate layer 20 formed on the substrate. However, in this embodiment, since the intermediate layer has the above-mentioned characteristics, most of the residual stress is alleviated in the intermediate layer and becomes equal to or less than the above-mentioned value. Furthermore, when a convex electrode is formed on the circuit surface, the intermediate layer can fully conform to the step of the circuit surface while alleviating the residual stress, thereby protecting the convex electrode.
[0097] Thereafter, the back surface of the semiconductor wafer to which the protective sheet for semiconductor processing 1 is attached is ground. As shown in FIG. 3B, even if the semiconductor wafer becomes thinner and the rigidity of the semiconductor wafer decreases, the residual stress of the protective sheet for semiconductor processing 1 is already small, so that the warpage of the semiconductor wafer is suppressed. Therefore, it is possible to further reduce the thickness of the semiconductor wafer. In addition, the semiconductor wafer can be easily transported to the next process, and damage to the semiconductor wafer is prevented.
[0098] After the backside grinding, the semiconductor wafer is diced into individual semiconductor chips by a known method. The resulting semiconductor chips are mounted on a substrate by a prescribed method to obtain a semiconductor device.
[0099] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and may be modified in various aspects within the scope of the present invention. EXAMPLES
[0100] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.
[0101] The measurement and evaluation methods in the present examples are as follows.
[0102] (residual stress in the middle layer) The intermediate layer composition described below was applied by knife coating onto a PET-based release film (manufactured by Lintec Corporation, SP-PET382150, thickness 38 μm) to a thickness of 400 μm to form an intermediate layer composition layer. Next, the intermediate layer composition layer thus formed was laminated with a PET-based release film (manufactured by Lintec Corporation, SP-PET381130, thickness 38 μm) to insulate the intermediate layer composition layer from oxygen. Next, a high-pressure mercury lamp was used to illuminate the intermediate layer composition layer at an illumination intensity of 80 mW / cm. 2 , irradiation amount 200mJ / cm 2 After ultraviolet irradiation under the conditions of 330 mW / cm, a metal halide lamp was used. 2 , irradiation amount 1260mJ / cm 2 The intermediate layer composition layer was cured by irradiating ultraviolet rays under the conditions of 100° C. to obtain an intermediate layer having a thickness of 400 μm. The intermediate layers were laminated to prepare a measurement sample having a thickness of about 0.8 mm. Residual stress measurement was performed using a rheometer MCR302 manufactured by Anton Paar. The measurement conditions are as follows. The sample was sandwiched from above and below by parallel plates, and shear stress was applied to the sample under the conditions of a measurement temperature of 65° C., a gap of 1 mm, and a strain of 100%, and the sample was maintained for a predetermined time. The shear stress value of the intermediate layer after a relaxation time of 300 seconds was taken as the residual stress value.
[0103] (shear storage modulus and loss tangent of the middle layer) Samples for measuring the shear storage modulus and loss tangent were prepared in the same manner as the samples for measuring residual stress. The shear storage modulus (G') and loss tangent (tan δ) were measured using an Anton Paar rheometer MCR302. The measurement conditions were as follows. The sample was sandwiched from above and below by parallel plates, and shear stress was applied to the sample at a measurement temperature of 0 to 100°C, a gap of 1 mm, a strain of 0.05 to 0.5%, and an angular frequency of 1 Hz. The shear storage modulus (G') and loss tangent (tan δ) at 65°C were calculated from these values.
[0104] (Wafer warpage evaluation) The semiconductor processing protective sheet prepared in the examples and comparative examples was attached to a silicon wafer at 65°C, and the surface opposite to the surface to which the semiconductor processing protective sheet was attached was ground until the thickness of the silicon wafer became 100μm. The surface to which the semiconductor processing protective sheet was attached (the surface of the silicon wafer) was placed on a flat plate, and the maximum distance between the back surface of the silicon wafer and the flat plate was measured to evaluate the warpage of the silicon wafer. In this example, samples with a warpage of 5.0mm or less were judged to be good, and samples with a warpage of more than 5.0mm were judged to be bad.
[0105] (Gel fraction) The intermediate layer having a thickness of 400 μm, which was prepared in the same manner as in each of the Examples and Comparative Examples, was cut to a size of 20 mm × 30 mm, and the intermediate layer was wrapped in a nylon mesh (mesh size 200) of 100 mm × 150 mm. The mass of the intermediate layer and the nylon mesh were weighed on a precision balance, and the mass of the nylon mesh, which had been measured in advance, was subtracted from the weighed mass to obtain the mass of only the intermediate layer. This mass was designated as M1.
[0106] Next, the intermediate layer wrapped in the nylon mesh was immersed in 100 mL of ethyl acetate at 25°C for 24 hours. The intermediate layer was then removed and dried at 120°C for 1 hour, and then left for 1 hour under conditions of a temperature of 23°C and a relative humidity of 50% to adjust the humidity. The masses of the intermediate layer and nylon mesh were then weighed using a precision balance, and the mass of the nylon mesh, which had been measured in advance, was subtracted from the weighed mass to obtain the mass of the intermediate layer alone. The mass at this time was designated M2. The gel fraction (%) was expressed as (M2 / M1)×100.
[0107] Example 1 A composition for an intermediate layer was obtained by blending 65 parts by weight of a urethane acrylate oligomer (CN9021 NS, manufactured by Arkema Co., Ltd.), 25 parts by weight of isobornyl acrylate, and 10 parts by weight of dodecyl acrylate, totaling 100 parts by weight, with 3.4 parts by weight of a photopolymerization initiator (Irgacure 1173, manufactured by BASF Co., Ltd.) and 1.2 parts by weight of a chain transfer agent (Karenz MT PE1, manufactured by Showa Denko K.K.).
[0108] The obtained intermediate layer composition was applied by a knife coating method onto a PET film (manufactured by Toray Industries, Inc., thickness 75 μm) as a substrate to a thickness of 400 μm to form an intermediate layer composition layer, and immediately after coating, the intermediate layer composition layer was irradiated with an illuminance of 80 mW / cm using a high-pressure mercury lamp. 2 , irradiation amount 200mJ / cm 2 Further, the intermediate layer composition layer was laminated with a PET release film (manufactured by Lintec Corporation, SP-PET752150, thickness 75 μm) to insulate the intermediate layer composition layer from oxygen, and then the intermediate layer composition layer was irradiated with ultraviolet light at an illuminance of 330 mW / cm using a metal halide lamp. 2 , irradiation amount 1260mJ / cm 2 The intermediate layer composition layer was cured by irradiating ultraviolet light under the above conditions, thereby forming an intermediate layer having a thickness of 400 μm on the PET film substrate.
[0109] The tensile storage modulus of the substrate PET film is 4.0 × 10 9 N / m 2Therefore, the product of the tensile storage modulus of the substrate and the thickness of the substrate (75 μm) was 3.0 × 10 5 (N / m).
[0110] Next, 1.1 parts by mass of trimethylolpropane adduct tolylene diisocyanate (Tosoh Corporation, Coronate L) as a crosslinking agent and 2.2 parts by mass of 2,2-dimethoxy-2-phenylacetophenone (BASF, Irgacure 651) as a photopolymerization initiator were added to 100 parts by mass of an acrylic copolymer (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., composition: 2EHA / EA / MMA / / HEA-MOI%=60 / 15 / 5 / 20 / / 60%, Mw=800,000), and toluene was further added to adjust the solids concentration to 30%, and the mixture was stirred for 30 minutes to prepare a pressure-sensitive adhesive composition.
[0111] Next, the prepared solution of the adhesive composition was applied to a PET-based release film (SP-PET382150, manufactured by Lintec Corporation, thickness 38 μm) and dried to form an adhesive layer with a thickness of 10 μm, thereby producing an adhesive sheet.
[0112] The release film on the substrate having the intermediate layer obtained above was removed, and the intermediate layer and the adhesive layer of the adhesive sheet were attached to each other to prepare a protective sheet for semiconductor processing.
[0113] Example 2 A semiconductor processing protective sheet was prepared in the same manner as in Example 1, except that a composition was used for the intermediate layer, which was a mixture of 65 parts by weight of a urethane acrylate oligomer (CN9021 NS, manufactured by Arkema Co., Ltd.), 25 parts by weight of isobornyl acrylate, and 10 parts by weight of dodecyl acrylate, for a total of 100 parts by weight, with 3.4 parts by weight of a photopolymerization initiator (Irgacure 1173, manufactured by BASF Co., Ltd.) and 1.0 part by weight of a chain transfer agent (Kalends MT PE1, manufactured by Showa Denko K.K.).
[0114] Example 3 A semiconductor processing protective sheet was prepared in the same manner as in Example 1, except that a composition was used for the intermediate layer, which was a mixture of 65 parts by weight of a urethane acrylate oligomer (CN9021 NS, manufactured by Arkema Co., Ltd.), 25 parts by weight of isobornyl acrylate, and 10 parts by weight of dodecyl acrylate, for a total of 100 parts by weight, with 3.4 parts by weight of a photopolymerization initiator (Irgacure 1173, manufactured by BASF Co., Ltd.) and 0.5 parts by weight of a chain transfer agent (Kalends MT PE1, manufactured by Showa Denko K.K.).
[0115] Example 4 A semiconductor processing protective sheet was prepared in the same manner as in Example 1, except that a composition was used for the intermediate layer, which was a mixture of 65 parts by weight of a urethane acrylate oligomer (CN9021 NS, manufactured by Arkema Co., Ltd.), 25 parts by weight of isobornyl acrylate, and 10 parts by weight of dodecyl acrylate, for a total of 100 parts by weight, with 3.4 parts by weight of a photopolymerization initiator (Irgacure 1173, manufactured by BASF Co., Ltd.) and 0.7 parts by weight of a chain transfer agent (Karenz MT BD1, manufactured by Showa Denko K.K.).
[0116] Comparative Example 1 A protective sheet for semiconductor processing was prepared in the same manner as in Example 1, except that a composition was used for the intermediate layer, which was a mixture of 65 parts by weight of a urethane acrylate oligomer (CN9021 NS, manufactured by Arkema Co., Ltd.), 25 parts by weight of isobornyl acrylate, and 10 parts by weight of dodecyl acrylate, totaling 100 parts by weight, and 3.4 parts by weight of a photopolymerization initiator (Irgacure 1173, manufactured by BASF Co., Ltd.).
[0117] Comparative Example 2 A semiconductor processing protective sheet was prepared in the same manner as in Example 1, except that a composition was used for the intermediate layer, which was a mixture of 65 parts by weight of a urethane acrylate oligomer (CN9021 NS, manufactured by Arkema Co., Ltd.), 25 parts by weight of isobornyl acrylate, and 10 parts by weight of dodecyl acrylate, for a total of 100 parts by weight, with 3.4 parts by weight of a photopolymerization initiator (Irgacure 1173, manufactured by BASF Co., Ltd.) and 0.5 parts by weight of a chain transfer agent (Karenz MT BD1, manufactured by Showa Denko K.K.).
[0118] The above measurements and evaluations were carried out on the obtained samples (Examples 1 to 4 and Comparative Examples 1 and 2). The results are shown in Table 1.
[0119] [Table 1]
[0120] From Table 1, it was confirmed that when the residual stress of the intermediate layer after holding at 65° C. for 300 seconds is within the above-mentioned range, warpage of the wafer can be suppressed. [Explanation of symbols]
[0121] 1...Semiconductor processing protection sheet 10...Base material 20. Middle class 30...Adhesive layer
Claims
1. A semiconductor processing protection sheet having a substrate, an intermediate layer and a pressure-sensitive adhesive layer on the substrate in this order, the intermediate layer composition for forming the intermediate layer contains urethane (meth)acrylate, the residual stress of the intermediate layer after being held at 65° C. for 300 seconds is 300 Pa or less; A protective sheet for semiconductor processing, wherein the loss tangent of the intermediate layer at 65°C is 1.0 or more.
2. The product of the tensile storage modulus of the substrate and the thickness of the substrate is 3.5×10 4 2. The protective sheet for semiconductor processing according to claim 1, wherein the hardness is N / m or more.
3. 3. The protective sheet for semiconductor processing according to claim 1, wherein the intermediate layer has a shear storage modulus of 25,000 Pa or less at 65°C.
4. A step of attaching the semiconductor processing protection sheet according to any one of claims 1 to 3 to a semiconductor wafer; and reducing the rigidity of the semiconductor wafer to which the protective sheet for semiconductor processing is attached.
Citation Information
Patent Citations
Gaibudenkyokugatagasuhodenpaneruno adoresuhoshiki
JP1976017629A
Pressure sensitive adhesive sheet for processing, and method for producing the same
JP2004107644A
Protecting method of semiconductor wafer and semiconductor wafer protective adhesive film
JP2005244206A
Pressure-sensitive adhesive sheet and method of processing product using the pressure-sensitive adhesive sheet
JP2007070432A
Adhesive tape for semiconductor wafer processing, and manufacturing method therefor
JP2010287819A