Protective sheet for semiconductor processing and method for manufacturing semiconductor device

The protective sheet for semiconductor processing addresses warping issues by combining a base material with a stress-relaxing intermediate layer and adhesive layer, ensuring effective stress absorption and reduced warpage, enhancing handling and preventing damage.

JP7555908B2Active Publication Date: 2024-09-25LINTEC CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021511490
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-29
Filing Date
2020-03-24
Publication Date
2024-09-25
Estimated Expiration
2040-03-24

AI Technical Summary

Technical Problem

Conventional protective sheets fail to effectively suppress warping of semiconductor wafers due to residual stress generated in both the protective sheet and the semiconductor wafer itself, leading to handling difficulties and damage during processing.

Method used

A protective sheet for semiconductor processing comprising a base material, an intermediate layer, and an adhesive layer, with specific properties such as a tensile storage modulus and thickness product of 8.0×10^5 N/m or less, residual stress of 10,000 Pa or less in the intermediate layer after 65°C for 300 seconds, and a loss tangent of 0.6 or more at 65°C, designed to reduce rigidity and absorb residual stress.

Benefits of technology

The protective sheet effectively suppresses warping of semiconductor wafers with residual stress, facilitating handling and preventing damage during processing, even after thickness reduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555908000002
    Figure 0007555908000002
  • Figure 0007555908000003
    Figure 0007555908000003
  • Figure 0007555908000004
    Figure 0007555908000004
Patent Text Reader

Abstract

This protection sheet for semiconductor processing has, in order, a base material, and upon the base material, an intermediate layer and an adhesive layer. The product of the tensile storage modulus of the base material and the thickness of the base material is 8.0×105 N / m or less, and the residual stress in the intermediate layer after the intermediate layer is kept at 65°C for 300 seconds is 10000 Pa or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a protective sheet for semiconductor processing and a method for manufacturing a semiconductor device. In particular, the present invention relates to a protective sheet for semiconductor processing that is suitably used for suppressing warpage of a semiconductor wafer, and a method for manufacturing a semiconductor device using the protective sheet for semiconductor processing. [Background technology]

[0002] Various electronic devices are equipped with a large number of semiconductor devices mounted with semiconductor chips obtained by dividing a semiconductor wafer on which a circuit is formed. A circuit protection layer such as a passivation film for protecting the circuit from the external environment and a passivation film for bump formation may be formed on the semiconductor wafer on which a circuit is formed. Such a circuit protection layer mechanically and chemically protects the circuit formed on the semiconductor wafer.

[0003] In addition, electronic devices are rapidly becoming smaller and more multifunctional, and semiconductor chips are also required to be smaller, thinner, and more dense. In order to make chips smaller and thinner, it is common to form circuits on the front side of a semiconductor wafer, and then grind the back side of the semiconductor wafer to adjust the thickness of the chip.

[0004] During back grinding of a semiconductor wafer, a protective sheet called a back grind tape is attached to the wafer surface in order to prevent contamination of the wafer surface during grinding and to hold the semiconductor wafer in place. Although the attachment of such a protective sheet improves the grinding quality, the attachment of the protective sheet causes residual stress in the protective sheet.

[0005] The semiconductor wafer before back grinding has high rigidity, so the residual stress in the protective sheet is canceled out. However, when the semiconductor wafer is thinned by back grinding, the rigidity of the semiconductor wafer decreases, so the residual stress in the protective sheet becomes apparent, and the semiconductor wafer with reduced rigidity warps together with the protective sheet.

[0006] Furthermore, in the semiconductor wafer on which the circuit protection layer is formed, residual stress is generated in the semiconductor wafer during the formation of the circuit protection layer, and therefore, after the back grinding, the semiconductor wafer tends to warp significantly due to the residual stress in the protection sheet and the residual stress in the semiconductor wafer. When the semiconductor wafer warps, problems occur such as the semiconductor wafer being easily damaged and being difficult to transport to the next process.

[0007] To address such problems, for example, Patent Document 1 discloses a surface protection sheet in which high stress relaxation properties are imparted to the base material in order to suppress warping of the semiconductor wafer. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] International Publication No. 2016 / 063827 Summary of the Invention [Problem to be solved by the invention]

[0009] In Patent Document 1, the warpage of the semiconductor wafer is suppressed by imparting stress relaxation properties to the substrate and eliminating the residual stress generated in the substrate. However, the protective sheet described in Patent Document 1 cannot eliminate the residual stress generated in the semiconductor wafer itself, such as a semiconductor wafer on which a circuit protection layer is formed. As a result, there is a problem that when residual stress is generated in the semiconductor wafer itself, the warpage of the semiconductor wafer cannot be suppressed.

[0010] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a protective sheet for semiconductor processing that can suppress warping of a semiconductor wafer when applied to a semiconductor wafer in which residual stress occurs, and a method for manufacturing a semiconductor device using the protective sheet for semiconductor processing. [Means for solving the problem]

[0011] An aspect of the present invention is [1] A protective sheet for semiconductor processing having a substrate, an intermediate layer and a pressure-sensitive adhesive layer on the substrate in this order, The product of the tensile storage modulus of the substrate and the thickness of the substrate is 8.0 × 10 5 N / m or less, This is a protective sheet for semiconductor processing, in which the residual stress of the intermediate layer after being held at 65°C for 300 seconds is 10,000 Pa or less.

[0012] [2] The protective sheet for semiconductor processing according to [1], wherein the loss tangent of the intermediate layer at 65° C. is 0.6 or more.

[0013] [3] A step of attaching the protective sheet for semiconductor processing according to [1] or [2] to a semiconductor wafer in which residual stress has occurred; and reducing the rigidity of the semiconductor wafer to which the protective sheet for semiconductor processing is attached. Effect of the Invention

[0014] According to the present invention, it is possible to provide a protective sheet for semiconductor processing that, when applied to a semiconductor wafer having residual stress, can suppress warping of the semiconductor wafer more than conventional protective sheets, and a method for manufacturing a semiconductor device using the protective sheet for semiconductor processing. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of the protective sheet for semiconductor processing according to this embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing a state in which the protective sheet for semiconductor processing according to this embodiment is attached to the circuit surface of a semiconductor wafer. [Figure 3A] FIG. 3A is a schematic cross-sectional view showing a semiconductor wafer after back grinding, to which a protective sheet for semiconductor processing is not attached. [Figure 3B] FIG. 3B is a schematic cross-sectional view showing a semiconductor wafer after back grinding to which a conventional protective sheet for semiconductor processing has been attached. [Figure 3C]FIG. 3C is a schematic cross-sectional view showing a semiconductor wafer after backside grinding to which the protective sheet for semiconductor processing according to this embodiment has been attached. [Figure 3D] FIG. 3D is a schematic cross-sectional view showing a semiconductor wafer after backside grinding to which the protective sheet for semiconductor processing according to this embodiment has been attached. [Figure 4] FIG. 4 is a schematic cross-sectional view for explaining that the residual stress of the intermediate layer is low in the protective sheet for semiconductor processing according to this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present invention will now be described in detail based on specific embodiments in the following order.

[0017] (1. Protective sheet for semiconductor processing) The semiconductor processing protective sheet 1 according to this embodiment has a structure in which an intermediate layer 20 and an adhesive layer 30 are laminated in this order on a substrate 10, as shown in Fig. 1. The semiconductor processing protective sheet is not limited to the structure shown in Fig. 1, and may have other layers as long as the effects of the present invention can be obtained. For example, a release sheet may be formed on the main surface 30a of the adhesive layer 30 in order to protect the adhesive layer 30 until the adhesive layer 30 is attached to an adherend.

[0018] The semiconductor processing protective sheet according to this embodiment is preferably used for a semiconductor wafer in which residual stress occurs before the semiconductor processing protective sheet is attached. Examples of such a semiconductor wafer include a semiconductor wafer on which a circuit protection layer such as various passivation films is formed.

[0019] As shown in Figure 2, the semiconductor processing protective sheet 1 of this embodiment is used by attaching the main surface 30a of the adhesive layer 30 to the main surface 51a of the circuit protection layer 51 formed on the circuit surface 50a of the semiconductor wafer 50.

[0020] In a semiconductor wafer having a circuit protection layer, residual stress occurs in the semiconductor wafer when the applied circuit protection layer composition is thermally cured. However, since the rigidity of the semiconductor wafer before back grinding is high, this residual stress is counteracted by the rigidity of the semiconductor wafer itself.

[0021] However, after grinding the semiconductor wafer, the thickness of the semiconductor wafer is reduced, and the rigidity of the semiconductor wafer is reduced. Therefore, when the semiconductor wafer is ground without a protective sheet for semiconductor processing, a warp Wa occurs due to only the residual stress generated in the semiconductor wafer, as shown in FIG. 3A.

[0022] In backgrinding of semiconductor wafers, in order to ensure uniformity of grinding and to prevent contamination of the circuit surface by grinding debris, etc., a protective sheet for semiconductor processing is attached to the circuit surface as described above to temporarily protect the circuit surface from the effects of grinding. Therefore, there is a great advantage in attaching a protective sheet for semiconductor processing to the circuit surface when grinding the backside of a semiconductor wafer.

[0023] When the protective sheet for semiconductor processing 1 is applied to the semiconductor wafer 50, it is applied while applying tension to the protective sheet for semiconductor processing 1 (stretching the protective sheet for semiconductor processing 1). As a result, residual stress RS occurs in the applied protective sheet for semiconductor processing 1. The substrate is usually more rigid than components other than the substrate and resists tension, so the residual stress occurs mainly in the substrate.

[0024] That is, after the semiconductor wafer is attached with the protective sheet for semiconductor processing, in addition to the residual stress generated in the semiconductor wafer, the substrate of the protective sheet for semiconductor processing also has residual stress. The residual stress generated in the substrate is canceled by the rigidity of the semiconductor wafer, similar to the residual stress generated in the semiconductor wafer.

[0025] However, after grinding a semiconductor wafer with a conventional protective sheet 100 for semiconductor processing attached thereto and residual stress generated, as shown in FIG. 3B, both the residual stress generated in the base material and the residual stress generated in the semiconductor wafer become apparent. Therefore, the warp Wb generated in the semiconductor wafer 50 becomes larger than the warp Wa shown in FIG. 3A.

[0026] If the warp generated in the semiconductor wafer 50 is large, it affects the handleability of the semiconductor wafer during conveyance. Therefore, since the warp Wb shown in FIG. 3B is the combined warp caused by the warp due to the residual stress generated in the semiconductor wafer and the warp due to the residual stress generated in the base material, there is a high possibility of affecting the handleability of the semiconductor wafer. That is, assuming that the warp that does not affect the handleability of the semiconductor wafer is W, Wb > W.

[0027] Since the protective sheet 1 for semiconductor processing according to the present embodiment has the characteristics described later, the semiconductor wafer 50 with the protective sheet 1 for semiconductor processing attached thereto enjoys the above-described advantages due to the attachment of the protective sheet for semiconductor processing, and even if the thickness is reduced by grinding, as shown in FIG. 3C, the combined warp Wc can be reduced to such an extent that it does not affect the handleability of the semiconductor wafer. That is, assuming that the warp that does not affect the handleability of the semiconductor wafer is W, Wc < W.

[0028] Preferably, by eliminating the residual stress generated in the base material and further eliminating a part of the residual stress generated in the semiconductor wafer, the semiconductor wafer 50 with the protective sheet 1 for semiconductor processing attached thereto enjoys the above-described advantages due to the attachment of the protective sheet for semiconductor processing, and as shown in FIG. 3D, the warp of the semiconductor wafer is reduced compared to the warp Wa when the protective sheet for semiconductor processing is not attached. That is, Wd < Wa. Hereinafter, the components of the protective sheet 1 for semiconductor processing will be described in detail.

[0029] (2. Substrate) The substrate is not limited as long as it is made of a material capable of supporting a semiconductor wafer. For example, various resin films used as substrates for backgrinding tapes are exemplified. The substrate may be made of a single-layer film made of one resin film, or may be made of a multi-layer film made of a plurality of resin films laminated together.

[0030] (2.1 Physical properties of the substrate) In this embodiment, it is preferable that the rigidity of the substrate is equal to or less than a predetermined value. If the rigidity of the substrate is too high, the residual stress generated in the substrate cannot be fully alleviated in the intermediate layer described later, and the residual stress of the intermediate layer tends to exceed the above-mentioned range. As a result, in addition to the warp caused by the residual stress generated in the semiconductor wafer itself, the warp caused by the residual stress of the intermediate layer occurs. Therefore, problems such as the semiconductor wafer being easily damaged and the handling property of the semiconductor wafer being deteriorated during transportation occur.

[0031] In this embodiment, the rigidity of the substrate is evaluated by the product of the tensile storage modulus of the substrate and the thickness of the substrate. The product of the tensile storage modulus of the substrate and the thickness of the substrate is 8.0×10 5 N / m or less. The product of the tensile storage modulus of the substrate and the thickness of the substrate is 7.5×10 5 It is more preferable that the resistance is less than or equal to N / m.

[0032] On the other hand, the product of the tensile storage modulus of the substrate and the thickness of the substrate is 5.0 × 10 3 N / m or more is preferable, and 1.2×10 5 When the rigidity of the substrate is equal to or greater than a predetermined value, the residual stress in the substrate can be eliminated by the intermediate layer, and warpage caused by the residual stress in the semiconductor wafer can be suppressed by the rigidity of the substrate.

[0033] In other words, by controlling the stress relaxation ability of the intermediate layer and the stress resistance ability exhibited by the rigidity of the base material, warping of the semiconductor wafer after back grinding can be suppressed even if residual stress occurs in the semiconductor wafer.

[0034] The preferred thickness range of the substrate varies depending on the tensile storage modulus of the substrate, but in this embodiment, the thickness is preferably 15 μm or more and 200 μm or less, and more preferably 40 μm or more and 150 μm or less.

[0035] (2.2 Substrate material) As the material of the substrate, when the thickness of the substrate is within the above range, a material in which the product of the tensile storage modulus of the substrate and the thickness of the substrate is within the above range is preferable. In this embodiment, for example, polyesters such as polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, wholly aromatic polyester, polyamide, polycarbonate, polyacetal, modified polyphenylene oxide, polyphenylene sulfide, polysulfone, polyether ketone, biaxially oriented polypropylene, etc. can be mentioned. Among these, polyesters are preferable, and polyethylene terephthalate is more preferable.

[0036] (3. Middle Class) The intermediate layer is a layer disposed between the substrate and the adhesive layer. In this embodiment, the intermediate layer is a layer having high stress relaxation properties that can take on the residual stress of the substrate and relax the residual stress within the intermediate layer. As shown in FIG. 4, the substrate 10 shrinks due to the residual stress after the semiconductor processing protection sheet 1 is attached, but most of the residual stress is relaxed in the intermediate layer, so that warpage of the semiconductor wafer 50 is suppressed. The intermediate layer may be composed of one layer (single layer) or may be composed of two or more layers.

[0037] The thickness of the intermediate layer 20 is set arbitrarily within a range in which the effects of the present invention can be obtained. In this embodiment, the thickness of the intermediate layer 20 is preferably 50 μm or more and 500 μm or less. The thickness of the intermediate layer means the thickness of the entire intermediate layer. For example, the thickness of an intermediate layer composed of multiple layers means the total thickness of all layers constituting the intermediate layer.

[0038] In this embodiment, the intermediate layer has the following physical properties.

[0039] (3.1 Residual stress after holding at 65℃ for 300 seconds) In this embodiment, the residual stress of the intermediate layer after holding at 65°C for 300 seconds is 10,000 Pa or less. The residual stress taken from the substrate is rapidly relaxed in the intermediate layer and is almost stable after 300 seconds. In addition, the semiconductor processing protection sheet is usually attached to the semiconductor wafer at a temperature of about 65°C.

[0040] Therefore, by keeping the stress remaining in the intermediate layer after holding at 65°C for 300 seconds within the above range, the residual stress assumed from the attached substrate is sufficiently alleviated within the intermediate layer. Note that "residual stress in the intermediate layer after holding at 65°C for 300 seconds" refers to the residual stress in the intermediate layer measured after the temperature of the intermediate layer is maintained at 65°C for 300 seconds.

[0041] The residual stress of the intermediate layer after being held at 65° C. for 300 seconds is preferably 6000 Pa or less, and more preferably 5000 Pa or less. In addition, the residual stress of the intermediate layer after being held at 65° C. for 300 seconds is preferably 1 Pa or more.

[0042] In this embodiment, the residual stress of the intermediate layer after being held at 65°C for 300 seconds can be measured as follows: The material constituting the intermediate layer is prepared as a sample of a predetermined size, and the sample at a temperature of 65°C is twisted using a dynamic viscoelasticity measuring device to apply shear strain to the sample. The shear stress 300 seconds after the strain is applied is measured, and the measured shear stress is regarded as the residual stress of the intermediate layer after being held at 65°C for 300 seconds.

[0043] (3.2 Loss tangent at 65℃) In this embodiment, the loss tangent (tan δ) of the intermediate layer at 65° C. is preferably 0.6 or more. The loss tangent is defined as "loss modulus / storage modulus" and is a value measured by the response to stress applied to an object using a dynamic viscoelasticity measuring device. When the loss tangent of the intermediate layer at 65° C. is within the above range, the residual stress taken over from the base material is consumed as heat, thereby suppressing warpage of the semiconductor wafer.

[0044] The loss tangent of the intermediate layer at 65° C. is more preferably 0.8 or more, and even more preferably 1.0 or more. Also, the loss tangent of the intermediate layer at 65° C. is preferably 3.0 or less.

[0045] The loss tangent of the intermediate layer at 65° C. may be measured by a known method. For example, the intermediate layer may be prepared as a sample of a predetermined size, and a dynamic viscoelasticity measuring device may be used to apply a strain to the sample at a predetermined frequency within a predetermined temperature range to measure the elastic modulus, and the loss tangent may be calculated from the measured elastic modulus.

[0046] (3.3 Composition for intermediate layer) The composition of the intermediate layer is not particularly limited as long as the intermediate layer has the above-mentioned physical properties, but in this embodiment, the intermediate layer is preferably composed of a composition containing a resin (intermediate layer composition). The intermediate layer composition preferably contains the components shown below.

[0047] (3.3.1 Urethane (meth)acrylates) Urethane (meth)acrylate is a compound having at least a (meth)acryloyl group and a urethane bond, and has the property of being polymerized by energy ray irradiation. In this embodiment, urethane (meth)acrylate is a component used to impart flexibility to the intermediate layer and to impart the property of reducing residual stress. In this specification, "(meth)acrylate" is used as a term indicating both "acrylate" and "methacrylate", and the same applies to other similar terms.

[0048] The urethane (meth)acrylate may be a monofunctional type or a multifunctional type. In this embodiment, a multifunctional urethane (meth)acrylate is preferred, and from the viewpoint of keeping the residual stress of the intermediate layer within the above range, a bifunctional urethane (meth)acrylate is preferred.

[0049] The urethane (meth)acrylate may be an oligomer, a polymer, or a mixture thereof. In this embodiment, a urethane (meth)acrylate oligomer is preferred.

[0050] The urethane (meth)acrylate can be obtained, for example, by reacting a polyol compound with a polyisocyanate compound to obtain a terminal isocyanate urethane prepolymer, and then reacting the resulting prepolymer with a hydroxyl group-containing (meth)acrylate. The urethane (meth)acrylate may be used alone or in combination of two or more kinds.

[0051] The content of the urethane (meth)acrylate in the intermediate layer composition is preferably 20% by mass or more, more preferably 25% by mass or more, and even more preferably 30% by mass or more. The content of the urethane (meth)acrylate in the intermediate layer composition is preferably 70% by mass or less, more preferably 65% ​​by mass or less, and even more preferably 50% by mass or less.

[0052] (3.3.2 Polymerizable monomers) The polymerizable monomer is preferably a polymerizable compound other than the above-mentioned urethane (meth)acrylate, and is a compound that can be polymerized with other components by irradiation with energy rays. Specifically, the polymerizable monomer is preferably a compound having at least one (meth)acryloyl group.

[0053] Examples of the polymerizable monomer include (meth)acrylates having an alkyl group having 1 to 30 carbon atoms; (meth)acrylates having a functional group such as a hydroxyl group, an amide group, an amino group, or an epoxy group; (meth)acrylates having an alicyclic structure; (meth)acrylates having an aromatic structure; (meth)acrylates having a heterocyclic structure; and vinyl compounds such as styrene, hydroxyethyl vinyl ether, hydroxybutyl vinyl ether, N-vinyl formamide, N-vinyl pyrrolidone, and N-vinyl caprolactam.

[0054] Examples of the (meth)acrylate having an alkyl group having 1 to 30 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, hexadecyl (meth)acrylate, octadecyl (meth)acrylate, and eicosyl (meth)acrylate.

[0055] Examples of the (meth)acrylate having a functional group include hydroxyl group-containing (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N-butyl (meth)acrylamide, and N-methylol (meth)acrylamide. Examples of the amide group-containing compounds include acrylamide, N-methylolpropane (meth)acrylamide, N-methoxymethyl (meth)acrylamide, and N-butoxymethyl (meth)acrylamide; amino group-containing (meth)acrylates such as primary amino group-containing (meth)acrylates, secondary amino group-containing (meth)acrylates, and tertiary amino group-containing (meth)acrylates; and epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, and allyl glycidyl ether.

[0056] Examples of (meth)acrylates having an alicyclic structure include isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxy (meth)acrylate, cyclohexyl (meth)acrylate, trimethylcyclohexyl (meth)acrylate, and adamantane (meth)acrylate.

[0057] Examples of the (meth)acrylate having an aromatic structure include phenylhydroxypropyl (meth)acrylate, benzyl (meth)acrylate, and 2-hydroxy-3-phenoxypropyl (meth)acrylate.

[0058] Examples of the (meth)acrylate having a heterocyclic structure include tetrahydrofurfuryl (meth)acrylate and morpholine (meth)acrylate.

[0059] In this embodiment, the polymerizable monomer preferably includes a (meth)acrylate having an alkyl group with 1 to 30 carbon atoms and a (meth)acrylate having an alicyclic structure. From the viewpoint of keeping the residual stress of the intermediate layer within the above range, a (meth)acrylate having an alkyl group with 4 to 14 carbon atoms is preferred, and as the (meth)acrylate having an alicyclic structure, isobornyl (meth)acrylate and trimethylcyclohexyl (meth)acrylate are preferred.

[0060] In addition, when the intermediate layer composition contains a crosslinking agent, a (meth)acrylate having a functional group capable of reacting with the crosslinking agent is not preferred. This is because the crosslinked structure formed by the crosslinking reaction may increase the residual stress of the intermediate layer. For example, a composition for the intermediate layer containing a polyisocyanate-based crosslinking agent and a (meth)acrylate having a hydroxyl group is not preferred.

[0061] The content of the polymerizable monomer in the intermediate layer composition is preferably 20% by mass or more, more preferably 30% by mass or more, and is preferably 80% by mass or less, more preferably 70% by mass or less.

[0062] In addition, the mass ratio of the urethane (meth)acrylate to the polymerizable monomer (urethane (meth)acrylate / polymerizable monomer) in a total of 100 parts by mass of the urethane (meth)acrylate and the polymerizable monomer is preferably from 20 / 80 to 80 / 20, and more preferably from 30 / 70 to 70 / 30.

[0063] (3.3.3 Photoinitiators) When the intermediate layer composition contains the above-mentioned urethane (meth)acrylate and polymerizable monomer, the intermediate layer composition preferably contains a photopolymerization initiator. By containing the photopolymerization initiator, polymerization proceeds reliably, and an intermediate layer having the above-mentioned characteristics can be easily obtained.

[0064] Examples of the photopolymerization initiator include photopolymerization initiators such as benzoin compounds, acetophenone compounds, acylphosphine oxide compounds, titanocene compounds, thioxanthone compounds, and peroxide compounds, and photosensitizers such as amines and quinones.Specific examples include 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and 2,2-dimethoxy-1,2-diphenylethan-1-one.These photopolymerization initiators may be used alone or in combination of two or more.

[0065] The amount of the photopolymerization initiator is preferably 0.05 to 15 parts by mass, and more preferably 0.5 to 10 parts by mass, per 100 parts by mass of the total of the urethane (meth)acrylate and the polymerizable monomer.

[0066] 3.3.4 Chain Transfer Agents The intermediate layer composition preferably contains a chain transfer agent. The chain transfer agent can cause a chain transfer reaction and adjust the progress of the curing reaction of the intermediate layer composition. By containing the chain transfer agent, it becomes possible for components with short molecular chains to remain relatively even after curing, so that the cured polymer has a structure with relatively high flexibility. As a result, the residual stress applied to the intermediate layer can be sufficiently relaxed, and it becomes easy to set the residual stress of the intermediate layer within the above range.

[0067] Examples of the chain transfer agent include thiol group-containing compounds. Examples of the thiol group-containing compounds include nonyl mercaptan, 1-dodecanethiol, 1,2-ethanedithiol, 1,3-propanedithiol, triazine thiol, triazine dithiol, triazine trithiol, 1,2,3-propane trithiol, tetraethylene glycol-bis(3-mercaptopropionate), trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetraki ... Examples of the chain transfer agent include thritol tetrakis thioglucolate, dipentaerythritol hexakis (3-mercaptopropionate), tris [(3-mercaptopropionyloxy)-ethyl]-isocyanurate, 1,4-bis (3-mercaptobutyryloxy) butane, pentaerythritol tetrakis (3-mercaptobutyrate), and 1,3,5-tris (3-mercaptobutyloxyethyl)-1,3,5-triazine-2,4,6- (1H,3H,5H)-trione. The chain transfer agent may be used alone or in combination of two or more.

[0068] The amount of the chain transfer agent is preferably 0.1 to 10 parts by mass, and more preferably 0.3 to 5 parts by mass, per 100 parts by mass of the total of the urethane (meth)acrylate and the polymerizable monomer.

[0069] (4. Adhesive Layer) The adhesive layer is attached to the circuit surface of the semiconductor wafer, and protects the circuit surface and supports the semiconductor wafer until it is peeled off from the circuit surface. The adhesive layer may be composed of one layer (single layer), or may be composed of two or more layers. When the adhesive layer has multiple layers, these multiple layers may be the same or different from each other, and the combination of layers constituting these multiple layers is not particularly limited.

[0070] The thickness of the adhesive layer is not particularly limited, but is preferably 1 μm or more and 50 μm or less, more preferably 2 μm or more and 30 μm or less. The thickness of the adhesive layer means the thickness of the entire adhesive layer. For example, the thickness of an adhesive layer composed of multiple layers means the total thickness of all layers constituting the adhesive layer.

[0071] The composition of the adhesive layer is not limited as long as it has enough adhesiveness to protect the circuit surface of the semiconductor wafer. In this embodiment, the adhesive layer is preferably composed of, for example, an acrylic adhesive, a urethane adhesive, a rubber adhesive, a silicone adhesive, or the like.

[0072] In addition, the adhesive layer is preferably formed from an energy ray curable adhesive. By forming the adhesive layer of the semiconductor processing protective sheet from an energy ray curable adhesive, when the sheet is attached to the semiconductor wafer, the sheet adheres to the semiconductor wafer with high adhesive strength, and when the sheet is peeled off from the semiconductor wafer, the adhesive strength can be reduced by irradiating the sheet with energy rays. Therefore, while appropriately protecting the circuits of the semiconductor wafer, the circuit on the surface of the semiconductor wafer is prevented from being destroyed and the adhesive is prevented from being transferred onto the semiconductor wafer when the semiconductor processing protective sheet is peeled off.

[0073] In this embodiment, the energy ray curable adhesive is preferably composed of an adhesive composition containing an acrylic adhesive. As the acrylic adhesive, it is preferable to use an acrylic polymer.

[0074] The acrylic polymer may be any known acrylic polymer, but in this embodiment, a functional group-containing acrylic polymer is preferred. The functional group-containing acrylic polymer may be a homopolymer formed from one type of acrylic monomer, a copolymer formed from multiple types of acrylic monomers, or a copolymer formed from one or multiple types of acrylic monomers and a monomer other than the acrylic monomer.

[0075] In this embodiment, the functional group-containing acrylic polymer is preferably an acrylic copolymer obtained by copolymerizing an alkyl (meth)acrylate with a functional group-containing monomer.

[0076] Examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, and n-octyl (meth)acrylate.

[0077] The functional group-containing monomer is a monomer containing a reactive functional group. The reactive functional group is a functional group capable of reacting with other compounds such as a crosslinking agent described later. Examples of the functional group in the functional group-containing monomer include a hydroxyl group, a carboxyl group, and an epoxy group, and a hydroxyl group is preferred.

[0078] Examples of hydroxyl group-containing monomers include hydroxyalkyl (meth)acrylates such as hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; and non-(meth)acrylic unsaturated alcohols (unsaturated alcohols not having a (meth)acryloyl skeleton) such as vinyl alcohol and allyl alcohol.

[0079] The pressure-sensitive adhesive composition preferably further contains an energy ray-curable compound having an energy ray-curable group. The energy ray-curable compound having an energy ray-curable group is preferably a compound having one or more groups selected from an isocyanate group, an epoxy group, and a carboxy group, and more preferably a compound having an isocyanate group.

[0080] Examples of compounds having an isocyanate group include 2-methacryloyloxyethyl isocyanate, meta-isopropenyl-α,α-dimethylbenzyl isocyanate, methacryloyl isocyanate, allyl isocyanate, 1,1-(bisacryloyloxymethyl)ethyl isocyanate; acryloyl monoisocyanate compounds obtained by reacting a diisocyanate compound or a polyisocyanate compound with hydroxyethyl (meth)acrylate; and acryloyl monoisocyanate compounds obtained by reacting a diisocyanate compound or a polyisocyanate compound with a polyol compound and hydroxyethyl (meth)acrylate. The isocyanate group undergoes an addition reaction with the hydroxyl group of the functional group-containing acrylic polymer.

[0081] The pressure-sensitive adhesive composition preferably further contains a crosslinking agent, which reacts with functional groups, for example, to crosslink resins contained in the functional-group-containing acrylic polymer.

[0082] Examples of the crosslinking agent include isocyanate-based crosslinking agents (crosslinking agents having an isocyanate group) such as tolylene diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, and adducts of these diisocyanates; epoxy-based crosslinking agents (crosslinking agents having a glycidyl group) such as ethylene glycol glycidyl ether; aziridine-based crosslinking agents (crosslinking agents having an aziridinyl group) such as hexa[1-(2-methyl)-aziridinyl]triphosphatriazine; metal chelate-based crosslinking agents (crosslinking agents having a metal chelate structure) such as aluminum chelate; and isocyanurate-based crosslinking agents (crosslinking agents having an isocyanuric acid skeleton).

[0083] The crosslinking agent is preferably an isocyanate-based crosslinking agent from the viewpoints of improving the cohesive strength of the pressure-sensitive adhesive and thereby improving the adhesive strength of the pressure-sensitive adhesive layer, and of easy availability.

[0084] The pressure-sensitive adhesive composition may further contain a photopolymerization initiator. When the pressure-sensitive adhesive composition contains a photopolymerization initiator, the curing reaction proceeds sufficiently even when irradiated with relatively low-energy energy rays such as ultraviolet rays.

[0085] Examples of the photopolymerization initiator include photoinitiators such as benzoin compounds, acetophenone compounds, acylphosphine oxide compounds, titanocene compounds, thioxanthone compounds, and peroxide compounds, and photosensitizers such as amines and quinones.Specific examples include α-hydroxycyclohexyl phenyl ketone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzyl diphenyl sulfide, benzyl dimethyl ketal, tetramethylthiuram monosulfide, azobisisobutyronitrile, dibenzyl, diacetyl, β-chloroanthraquinone, and 2,4,6-trimethylbenzoyldiphenylphosphine oxide.

[0086] (5. Manufacturing method of protective sheet for semiconductor processing) The method for producing the semiconductor processing protection sheet according to this embodiment is not particularly limited as long as it is a method capable of laminating an intermediate layer and a pressure-sensitive adhesive layer on one side of a substrate, and any known method may be used.

[0087] First, as a composition for forming an intermediate layer, for example, a composition for intermediate layer containing the above-mentioned components, or a composition obtained by diluting the composition for intermediate layer with a solvent, etc. is prepared. Similarly, as a pressure-sensitive adhesive composition for forming a pressure-sensitive adhesive layer, for example, a pressure-sensitive adhesive composition containing the above-mentioned components, or a composition obtained by diluting the pressure-sensitive adhesive composition with a solvent, etc. is prepared.

[0088] Examples of the solvent include organic solvents such as methyl ethyl ketone, acetone, ethyl acetate, tetrahydrofuran, dioxane, cyclohexane, n-hexane, toluene, xylene, n-propanol, and isopropanol.

[0089] Then, the intermediate layer composition or the like is applied onto the substrate by a known method such as spin coating, spray coating, bar coating, knife coating, roll coating, blade coating, die coating, or gravure coating to form a coating film, and the coating film is cured to form an intermediate layer on the substrate. In this embodiment, the coating film is preferably cured by irradiation with energy rays. Examples of the energy rays include ultraviolet rays and electron beams, and ultraviolet rays are preferred.

[0090] Furthermore, in this embodiment, it is preferable to cure the coating film by irradiating the energy rays multiple times, which makes it possible to control the degree of cure of the intermediate layer and to easily set the residual stress of the intermediate layer within the above range.

[0091] Specifically, it is preferable to irradiate the coating film with energy rays multiple times while keeping the coating film isolated from oxygen.

[0092] In addition, when the energy rays are ultraviolet rays, the conditions for the first ultraviolet irradiation are preferably an ultraviolet ray illuminance of 30 to 500 mW / cm2 , more preferably 50 to 340 mW / cm 2 The amount of ultraviolet light irradiation is preferably 100 to 2500 mJ / cm 2 , more preferably 150 to 2000 mJ / cm 2 It is.

[0093] The second UV irradiation is preferably performed under conditions in which the illuminance and dose are greater than those of the first irradiation.

[0094] An adhesive composition or the like is applied to the intermediate layer thus cured and formed by a known method, and then heated and dried to produce a protective sheet for semiconductor processing in which an intermediate layer and an adhesive layer are formed in that order on the substrate.

[0095] Alternatively, the protective sheet for semiconductor processing may be produced as follows: That is, the intermediate layer composition or the like is applied to the release-treated surface of one release sheet to form a coating film, which is then cured as described above to form an intermediate layer on the release sheet.

[0096] The release-treated surface of the other release sheet is coated with an adhesive composition or the like, and heated and dried to form an adhesive layer on the release sheet. After that, the intermediate layer on one release sheet is bonded to the substrate, and the release sheet is removed. Then, the intermediate layer and the adhesive layer on the other release sheet are bonded to produce a semiconductor processing protective sheet in which the intermediate layer, adhesive layer, and release sheet are provided in this order on the substrate. The release sheet may be appropriately peeled off and removed before using the semiconductor processing protective sheet.

[0097] (6. Manufacturing method of semiconductor device) A method for manufacturing a semiconductor device using the semiconductor processing protective sheet of this embodiment is not particularly limited, as long as it includes a step of attaching the semiconductor processing protective sheet of this embodiment to a semiconductor wafer in which residual stress has occurred, and a step of reducing the rigidity of the semiconductor wafer to which the semiconductor processing protective sheet is attached.

[0098] A preferred process for attaching the protective sheet for semiconductor processing according to this embodiment to a semiconductor wafer is, for example, a process for attaching the protective sheet for semiconductor processing according to this embodiment to the surface of the semiconductor wafer on which circuits are formed.

[0099] An example of a process for reducing the rigidity of a semiconductor wafer is a process for grinding the semiconductor wafer to reduce its thickness.

[0100] As an example of a method for manufacturing a semiconductor device using the protective sheet for semiconductor processing according to this embodiment, a method for manufacturing a semiconductor device from a semiconductor wafer in which residual stress has occurred will be described below with reference to FIGS. 2 to 4.

[0101] First, a semiconductor wafer is prepared. Any known semiconductor wafer may be used. The thickness of the semiconductor wafer before grinding is usually about 500 to 1000 μm. The thickness of the semiconductor wafer after grinding is preferably 100 to 300 μm.

[0102] In this embodiment, the semiconductor wafer in which residual stress occurs is a semiconductor wafer in which the above-mentioned circuit protection layer is formed. The circuit protection layer is usually formed by applying a composition constituting the circuit protection layer and thermally curing it. During thermal curing, the composition shrinks, so a force that tries to bend the semiconductor wafer, i.e., residual stress, acts on the circuit surface side. Therefore, as shown in FIG. 2, in the semiconductor wafer after the circuit protection layer is formed, residual stress RS1 occurs in the circuit protection layer 51. Note that convex electrodes such as bumps and pillar electrodes may be formed on the circuit surface to which the semiconductor processing protection sheet according to this embodiment is attached.

[0103] Next, before grinding the back surface of the semiconductor wafer, as shown in Fig. 2, a protective sheet for semiconductor processing 1 is attached to the circuit side surface of the semiconductor wafer 50 on which the circuit protection layer 51 is formed, i.e., the surface 51a of the circuit protection layer 51, to protect the circuit surface from adverse effects caused by grinding. At this time, the protective sheet for semiconductor processing 1 is attached to the circuit surface while being pulled. Therefore, after attachment, a residual stress RS2 acting in the direction of shrinkage of the substrate is generated in the protective sheet for semiconductor processing 1, particularly in the substrate with high rigidity.

[0104] As shown in Fig. 4, the residual stress RS2 causes the substrate 10 to shrink, and the residual stress generated in the substrate 10 is eliminated, but the deformation of the substrate 10 generates residual stress RS2 in the intermediate layer 20 formed on the substrate. However, in this embodiment, since the intermediate layer has the above-mentioned characteristics, most of the residual stress is alleviated in the intermediate layer and becomes equal to or less than the above-mentioned value. Furthermore, when a convex electrode is formed on the circuit surface, the intermediate layer can protect the convex electrode by fully conforming to the step of the circuit surface while alleviating the residual stress.

[0105] Thereafter, the back surface of the semiconductor wafer to which the protective sheet for semiconductor processing 1 is attached is ground. When the semiconductor wafer becomes thinner and the rigidity of the semiconductor wafer decreases, warping occurs due to the residual stress of the semiconductor wafer. When the rigidity of the substrate is low, as shown in FIG. 3C, the warping can be reduced to a level that does not affect the handling of the semiconductor wafer. When the rigidity of the substrate is high, as shown in FIG. 3D, even a part of the warping caused by the residual stress generated in the semiconductor wafer can be suppressed. This makes it easier to transport the semiconductor wafer to the next process, and prevents damage to the semiconductor wafer.

[0106] After the backside grinding, the semiconductor wafer is diced into individual semiconductor chips by a known method. The resulting semiconductor chips are mounted on a substrate by a prescribed method to obtain a semiconductor device.

[0107] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and may be modified in various aspects within the scope of the present invention. EXAMPLES

[0108] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.

[0109] The measurement and evaluation methods in the present examples are as follows.

[0110] (residual stress in the middle layer) The intermediate layer composition described below was applied by knife coating onto a PET-based release film (manufactured by Lintec Corporation, SP-PET382150, thickness 38 μm) to a thickness of 400 μm to form an intermediate layer composition layer. Next, the intermediate layer composition layer thus formed was laminated with a PET-based release film (manufactured by Lintec Corporation, SP-PET381130, thickness 38 μm) to insulate the intermediate layer composition layer from oxygen. Next, a high-pressure mercury lamp was used to illuminate the intermediate layer composition layer at an illumination intensity of 80 mW / cm. 2 , irradiation amount 200mJ / cm 2 After ultraviolet irradiation under the conditions of 330 mW / cm illuminance using a metal halide lamp, 2 , irradiation amount 1260mJ / cm 2 The intermediate layer composition layer was cured by irradiating ultraviolet rays under the conditions of 100° C. to obtain an intermediate layer having a thickness of 400 μm. The intermediate layers were laminated to prepare a measurement sample having a thickness of about 0.8 mm. Residual stress measurement was performed using a rheometer MCR302 manufactured by Anton Paar. The measurement conditions are as follows. The sample was sandwiched from above and below by parallel plates, and shear stress was applied to the sample under the conditions of a measurement temperature of 65° C., a gap of 1 mm, and a strain of 100%, and the sample was maintained for a predetermined time. The shear stress value of the intermediate layer after a relaxation time of 300 seconds was taken as the residual stress value.

[0111] (loss tangent of middle layer) A sample for measuring loss tangent was prepared in the same manner as the sample for measuring residual stress. The loss tangent (tan δ) was measured using an Anton Paar rheometer MCR302. The measurement conditions were as follows. The sample was sandwiched from above and below by parallel plates, and shear stress was applied to the sample under the following conditions: measurement temperature 0-100°C, gap 1mm, strain 0.05-0.5%, and angular frequency 1Hz, and the loss tangent (tan δ) at 65°C was calculated from these values.

[0112] (Wafer warpage evaluation) Two sheets of LC2850 (25 μm thick) manufactured by Lintec Corporation were attached to a 12-inch silicon wafer as a pseudo-circuit protection layer, and the wafer was heated at 180°C for three hours and then slowly cooled to room temperature. This silicon wafer was used as a silicon wafer with a pseudo-circuit protection layer formed thereon. A general-purpose backgrind tape was attached to the protection layer side of this silicon wafer with the circuit protection layer formed thereon, and the wafer was ground until the thickness reached 250 μm. When the tape was peeled off after grinding, it was confirmed that the wafer had warped by approximately 9.0 mm.

[0113] The protective sheet for semiconductor processing prepared in the examples and comparative examples was attached to the surface of the pseudo-circuit protective layer of the silicon wafer on which the pseudo-circuit protective layer was formed at 65° C., and the surface opposite to the surface to which the protective sheet for semiconductor processing was attached was ground until the thickness became 250 μm. In other words, the thickness of the silicon wafer after grinding was 200 μm.

[0114] The silicon wafer was placed on a flat plate with the semiconductor processing protection sheet attached side (pseudo circuit protection layer side) facing up, and the maximum distance between the back surface of the silicon wafer and the flat plate was measured to evaluate the warpage of the silicon wafer. In this example, the difference from the warpage (9.0 mm) after peeling off the back grind tape was calculated, and samples with a warpage difference of 5.0 mm or less were judged to be good, and samples with a warpage of more than 5.0 mm were judged to be bad.

[0115] Example 1 A composition for an intermediate layer was obtained by blending 65 parts by weight of a urethane acrylate oligomer (CN9021 NS, manufactured by Arkema Co., Ltd.), 25 parts by weight of isobornyl acrylate, and 10 parts by weight of dodecyl acrylate, totaling 100 parts by weight, with 3.4 parts by weight of a photopolymerization initiator (Irgacure 1173, manufactured by BASF Co., Ltd.) and 1.0 part by weight of a chain transfer agent (Karenz MT PE1, manufactured by Showa Denko K.K.).

[0116] The obtained intermediate layer composition was applied by knife coating onto a substrate PET film (manufactured by Toray Industries, Inc., thickness 75 μm) to a thickness of 400 μm to form an intermediate layer composition layer. Next, an intermediate layer composition layer formed from a PET-based release film (manufactured by Lintec Corporation, SP-PET752150, thickness 75 μm) was laminated to insulate the intermediate layer composition layer from oxygen. Next, a high-pressure mercury lamp was used to illuminate the intermediate layer composition layer at an illumination intensity of 80 mW / cm. 2 , irradiation amount 200mJ / cm 2 After ultraviolet irradiation under the conditions of 330 mW / cm illuminance using a metal halide lamp, 2 , irradiation amount 1260mJ / cm 2 The intermediate layer composition layer was cured by irradiating ultraviolet light under the above conditions, thereby forming an intermediate layer having a thickness of 400 μm on the PET film substrate.

[0117] The tensile storage modulus of the substrate PET film is 4.0 × 10 9 N / m 2 Therefore, the product of the tensile storage modulus of the substrate and the thickness of the substrate (75 μm) was 3.0 × 10 5 (N / m).

[0118] Next, 1.1 parts by mass of trimethylolpropane adduct tolylene diisocyanate (Tosoh Corporation, Coronate L) as a crosslinking agent and 2.2 parts by mass of 2,2-dimethoxy-2-phenylacetophenone (BASF, Irgacure 651) as a photopolymerization initiator were added to 100 parts by mass of an acrylic copolymer (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., composition: 2EHA / EA / MMA / / HEA-MOI%=60 / 15 / 5 / 20 / / 60%, Mw=800,000), and toluene was further added to adjust the solids concentration to 30%, and the mixture was stirred for 30 minutes to prepare a pressure-sensitive adhesive composition.

[0119] Next, the prepared solution of the adhesive composition was applied to a PET-based release film (manufactured by Lintec Corporation, SP-PET382150, thickness 38 μm) and dried to form an adhesive layer with a thickness of 10 μm, thereby producing an adhesive sheet.

[0120] The release film on the substrate having the intermediate layer obtained above was removed, and the intermediate layer and the adhesive layer of the adhesive sheet were attached to each other to prepare a protective sheet for semiconductor processing.

[0121] Example 2 A semiconductor processing protective sheet was prepared in the same manner as in Example 1, except that a composition was used for the intermediate layer, which was a blend of 65 parts by mass of a urethane acrylate oligomer (CN9021 NS, manufactured by Arkema Co., Ltd.) and 35 parts by mass of isobornyl acrylate, totaling 100 parts by mass, with 3.4 parts by mass of a photopolymerization initiator (Irgacure 1173, manufactured by BASF Co., Ltd.) and 1.0 part by mass of a chain transfer agent (Kalends MT PE1, manufactured by Showa Denko K.K.).

[0122] Example 3 A semiconductor processing protective sheet was prepared in the same manner as in Example 1, except that a composition was used for the intermediate layer, which was a blend of 65 parts by mass of a urethane acrylate oligomer (CN9021 NS, manufactured by Arkema Co., Ltd.) and 35 parts by mass of isobornyl acrylate, totaling 100 parts by mass, with 3.4 parts by mass of a photopolymerization initiator (Irgacure 1173, manufactured by BASF Co., Ltd.) and 0.9 parts by mass of a chain transfer agent (Kalends MT PE1, manufactured by Showa Denko K.K.).

[0123] Example 4 A protective sheet for semiconductor processing was prepared in the same manner as in Example 1, except that a composition was used for the intermediate layer, which was a mixture of 65 parts by weight of a urethane acrylate oligomer (CN9021 NS, manufactured by Arkema Co., Ltd.), 25 parts by weight of isobornyl acrylate, and 10 parts by weight of dodecyl acrylate, totaling 100 parts by weight, and 3.4 parts by weight of a photopolymerization initiator (Irgacure 1173, manufactured by BASF Co., Ltd.).

[0124] (Examples 5 and 6) A protective sheet for semiconductor processing was produced in the same manner as in Example 4, except that the thickness of the substrate was set to the thickness shown in Table 1.

[0125] Example 7 The intermediate layer composition obtained in the same manner as in Example 1 was applied by knife coating onto a PET-based release film (manufactured by Lintec Corporation, SP-PET382150, thickness 38 μm) to a thickness of 400 μm to form an intermediate layer composition layer. Next, the intermediate layer composition layer thus formed was laminated with a PET-based release film (manufactured by Lintec Corporation, SP-PET381130, thickness 38 μm) to insulate the intermediate layer composition layer from oxygen. Next, a high-pressure mercury lamp was used to illuminate the intermediate layer composition layer at an illumination intensity of 80 mW / cm. 2 , irradiation amount 200mJ / cm 2 After ultraviolet irradiation under the conditions of 330 mW / cm illuminance using a metal halide lamp, 2 , irradiation amount 1260mJ / cm 2The intermediate layer composition layer was cured by irradiating ultraviolet light under the conditions of. Furthermore, a PET-based release film (manufactured by Lintec Corporation, SP-PET381130, thickness 38 μm) was peeled off from the intermediate layer, and the intermediate layer surface was bonded to a substrate PET film (manufactured by Toray Industries, Inc., thickness 2 μm) to obtain a configuration in which an intermediate layer having a thickness of 400 μm was laminated on a PET film. The subsequent operations were performed in the same manner as in Example 1 to produce a semiconductor processing protection sheet.

[0126] Example 8 A protective sheet for semiconductor processing was produced in the same manner as in Example 7, except that the intermediate layer composition obtained in the same manner as in Example 4 was used.

[0127] Comparative Example 1 A protective sheet for semiconductor processing was prepared in the same manner as in Example 1, except that a composition was used for the intermediate layer, which was a mixture of 65 parts by weight of a urethane acrylate oligomer (CN9021 NS, manufactured by Arkema Co., Ltd.), 25 parts by weight of isobornyl acrylate, and 10 parts by weight of dodecyl acrylate, totaling 100 parts by weight, and 3.4 parts by weight of a photopolymerization initiator (Irgacure 1173, manufactured by BASF Co., Ltd.).

[0128] (Comparative Examples 2 and 3) A protective sheet for semiconductor processing was produced in the same manner as in Comparative Example 1, except that the thickness of the substrate was set to the thickness shown in Table 1.

[0129] Comparative Example 4 A protective sheet for semiconductor processing was produced in the same manner as in Example 1, except that the thickness of the substrate was set to the thickness shown in Table 1.

[0130] The above measurements and evaluations were carried out on the obtained samples (Examples 1 to 8 and Comparative Examples 1 to 4). The results are shown in Table 1.

[0131] [Table 1]

[0132] From Table 1, it was confirmed that when the product of the tensile storage modulus of the substrate and the thickness of the substrate is within the above-mentioned range and the residual stress of the intermediate layer after being held at 65°C for 300 seconds is within the above-mentioned range, warping of the wafer caused by residual stress can be suppressed. [Explanation of symbols]

[0133] 1...Semiconductor processing protection sheet 10...Base material 20. Middle class 30...Adhesive layer 50...Semiconductor wafer 51...Circuit surface protection layer

Claims

1. A semiconductor processing protection sheet having a substrate, an intermediate layer and a pressure-sensitive adhesive layer on the substrate in this order, the intermediate layer composition for forming the intermediate layer contains urethane (meth)acrylate, The product of the tensile storage modulus of the substrate and the thickness of the substrate is 8.0×10 5 N / m or less, The residual stress of the intermediate layer after being held at 65° C. for 300 seconds is 10,000 Pa or less, A protective sheet for semiconductor processing, wherein the loss tangent of the intermediate layer at 65°C is 1.0 or more.

2. A step of attaching the protective sheet for semiconductor processing according to claim 1 to a semiconductor wafer having residual stress; and reducing the rigidity of the semiconductor wafer to which the protective sheet for semiconductor processing is attached.

Citation Information

Patent Citations

  • Gaibudenkyokugatagasuhodenpaneruno adoresuhoshiki

    JP1976017629A

  • Pressure sensitive adhesive sheet for processing, and method for producing the same

    JP2004107644A

  • Protecting method of semiconductor wafer and semiconductor wafer protective adhesive film

    JP2005244206A

  • Pressure-sensitive adhesive sheet and method of processing product using the pressure-sensitive adhesive sheet

    JP2007070432A

  • Adhesive tape for semiconductor wafer processing, and manufacturing method therefor

    JP2010287819A