Barium titanate particles, their manufacturing method, and dispersion of barium titanate particles
By controlling the atomic ratio and crystallite size of barium titanate particles and using specific organic solvents, the sintering retardation effect is enhanced, addressing the issue of crack formation in MLCCs and ensuring uniform paste application.
Patent Information
- Application Number
- JP2021551421
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-30
- Filing Date
- 2020-09-30
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2040-09-30
AI Technical Summary
Barium titanate particles with a perovskite structure have a high dielectric constant but face issues with increased particle size and crystallite size during firing, leading to low density filling around Ni particles, which increases the likelihood of cracks in multilayer ceramic capacitors (MLCCs) due to differing sintering temperatures.
Control the atomic ratio of Ba/Ti to 0.9 to 1.1, maintain crystallite diameter between 5 to 25 nm, and ensure a c/a axial ratio of 1.005 or less, producing barium titanate particles with high crystallinity and small particle size, and use specific organic solvents and additives to enhance sintering retardation effects.
The solution results in high-density filling of barium titanate particles around Ni particles, reducing the likelihood of cracks and enhancing the sintering retardation effect, ensuring uniform application and low viscosity of the paste for improved MLCC performance.
Smart Images

Figure 0007555945000003 
Figure 0007555945000001 
Figure 0007555945000002
Abstract
Description
[Technical field]
[0001] The present invention relates to barium titanate particles having a perovskite structure. [Background technology]
[0002] Barium titanate particles are used in dielectric materials for electronic components and optical materials with high refractive index and excellent transparency. Barium titanate particles have a high dielectric constant and are therefore used in multilayer ceramic capacitors (MLCCs). MLCCs have a structure in which electrode layers and dielectric layers are alternately stacked. The electrode layers contain Ni particles of 80 to 300 nm and barium titanate particles as a co-material. In the electrode layers, the barium titanate particles are packed around the Ni particles. This increases the temperature at which the Ni particles sinter together. In other words, the sintering retardation effect of the Ni particles is obtained. This makes the temperature at which the Ni particles sinter together closer to the temperature at which the dielectric layer sinters. This reduces the difference in shrinkage rate between the electrode layers and the dielectric layers during firing, resulting in an MLCC with fewer cracks (see, for example, Patent Document 1).
[0003] On the other hand, in order to improve the dielectric constant of barium titanate particles, it is known to make the barium titanate particles have a perovskite structure and further make the axial length of the c-axis of the crystal lattice longer than the axial length of the a-axis, that is, to make the barium titanate particles have a tetragonal system (see, for example, Patent Document 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2005-63707 A [Patent Document 2] JP 2004-300027 A Summary of the Invention [Problem to be solved by the invention]
[0005] In the barium titanate particles of Patent Document 2, the c-axis length of the perovskite structure is longer than the a-axis length, so the dielectric constant is high. However, since the barium titanate particles are sintered after being powdered, the particle size and crystallite size tend to become large. Therefore, the density of the barium titanate particles packed around the Ni particles tends to be low, making it difficult to obtain a sintering retardation effect. The greater the difference between the temperature at which the dielectric layer is sintered and the temperature at which the Ni particles are sintered, the more likely cracks are to occur in the MLCC. An object of the present invention is to provide barium titanate particles having a high sintering retardation effect and a method for producing the same. [Means for solving the problem]
[0006] Therefore, in the present invention, in the barium titanate particles having a perovskite structure, the atomic ratio of barium to titanium, Ba / Ti, is set to 0.9 to 1.1, and the crystallite size is set to 5 to 25 nm. The atomic ratio of barium to titanium, Ba / Ti, may be 0.95 to 1.05. Furthermore, the ratio c / a of the length of the c-axis to the length of the a-axis of the crystal lattice in the perovskite structure is preferably 1.005 or less. In such a dispersion of barium titanate particles containing barium titanate particles and an organic solvent, the water content is preferably less than 3% by weight. In addition, a method for producing barium titanate particles includes the steps of mixing barium hydroxide and an alkyl cellosolve, adding titanium alkoxide so that the atomic ratio of barium to titanium, Ba / Ti, is in the range of 0.9 to 1.1, adding water, and heating. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a structural diagram of a cyclic hydrocarbon group (R6). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The barium titanate particles having a perovskite structure according to the present invention have an atomic ratio of barium to titanium, Ba / Ti, in the range of 0.9 to 1.1. This makes it difficult for impurities such as crystals other than the perovskite structure to be generated. The crystallite diameter of the barium titanate particles is 5 to 25 nm. This increases the crystallinity of the barium titanate particles and reduces the particle diameter. Since such barium titanate particles enter the gaps between the Ni particles in the electrode layer, the barium titanate particles are present around the Ni particles at a high density. This increases the sintering retardation effect of Ni. If the crystallite diameter is larger than 25 nm, the viscosity of the dispersion of the barium titanate particles described below increases. When the crystallite diameter is 5 to 25 nm, the particle diameter measured by a transmission electron microscope is also 5 to 25 nm. The atomic ratio of barium to titanium, Ba / Ti, may be 0.95 to 1.05. Furthermore, the ratio of the lengths of the c-axis and a-axis of the crystal lattice in the perovskite structure (axial ratio c / a) is preferably 1.005 or less. This makes the barium titanate particles closer to cubic crystals. This increases the sintering retardation effect of Ni.
[0009] The crystal structure and crystallite size can be measured using an X-ray diffraction measurement device, Rigaku's RINT-Ultima. The crystal structure can be identified using analysis software, PDXL. The crystallite size can be calculated from the half-width β (rad) by measuring the half-width at Miller indices (110) near 2θ=31.5° using the Scherrer formula, D=Kλ / βcosθ. Here, D is the crystallite size (Å), K is the Scherrer constant, λ is the X-ray wavelength (1.7889 Å), and θ is the reflection angle. From the results of X-ray diffraction measurement using PDXL, the lengths of the a-axis and c-axis of the perovskite structure can be determined. The axial ratio c / a is preferably 1.003 or less, and more preferably 1.001 or less. The smaller the axial ratio c / a, the greater the sintering retardation effect of Ni.
[0010] It is preferable that the barium titanate particles contain at least one element (hereinafter referred to as an additive element) selected from Groups 2, 3, lanthanoids, actinoids, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, and 14. This enhances the sintering retardation effect. It is more preferable that the additive element is contained in an amount of 0.1 to 10 mol% when the composition formula of barium titanate, BaTiO3, is 100 mol%. This makes it easier to obtain the sintering retardation effect of Ni. Also, even if the additive element is contained in this range, no peaks other than those of the perovskite structure are observed.
[0011] A paste for printing an electrode layer can be prepared using a dispersion of barium titanate particles. The dispersion of barium titanate particles contains barium titanate particles and an organic solvent. The water content of the dispersion is preferably less than 3% by weight. If the water content is low, the viscosity of the paste is unlikely to increase even if a binder such as ethyl cellulose is added to the dispersion. If the viscosity of the paste is high, it is difficult to apply the paste evenly, and cracks are likely to occur in the electrode layer during firing. In addition, if the water content of the dispersion is 3% by weight or less, the dispersion is unlikely to aggregate.
[0012] The amount of water adsorbed to the solid content of the dispersion (adsorbed water amount) is preferably 5 parts by mass or more per 100 parts by mass of the solid content. If the amount of adsorbed water is within this range, the barium titanate particles in the dispersion have many hydroxyl groups on the surface. The solid content is obtained by drying the dispersion at 200°C for 3 hours. The amount of adsorbed water is the amount of water adsorbed to the solid content when the solid content is exposed to conditions of 25°C and 90 RH% for 1 hour.
[0013] It is preferable that the barium titanate particles are not surface-treated. This tends to reduce the viscosity of the paste. In particular, when the water content of the dispersion is 3% or less, the viscosity of the paste tends to be further reduced. If the barium titanate particles are surface-treated with an organic acid surface treatment agent such as linoleic acid or oleic acid, the viscosity of the paste may increase. However, the barium titanate particles may be surface-treated with a surface treatment agent as long as the viscosity of the paste does not increase.
[0014] The organic solvent preferably has an OH group. In other words, it is preferable that the organic solvent has high hydrophilicity. This makes it easier to reduce the viscosity of the dispersion or paste. When the organic solvent has an OH group, if the amount of adsorbed water is 5 parts by mass or more per 100 parts by mass of solid content, the viscosity of the dispersion is easier to reduce.
[0015] The organic solvent preferably has at least one of an ester bond, an ether bond, and a ketone group in addition to an OH group. This increases the hydrophilicity of the organic solvent. In particular, the presence of an ether bond provides high hydrophilicity.
[0016] Alternatively, the organic solvent preferably has a hydrophobic structure together with the OH group. Here, the hydrophobic structure refers to a cyclic structure or a chain structure in which two or more carbon atoms from the terminal are continuously bonded to each other by carbon-carbon bonds. Examples of the cyclic structure include a cyclic hydrocarbon group (R6) which is a monovalent substituent obtained by removing a hydrogen atom from any carbon atom of a cycloalkane, cycloalkene (cycloolefin), aromatic ring, etc. R6 may be any of a three-membered ring, a four-membered ring, a five-membered ring, a six-membered ring, and a seven-membered ring. The structure of the six-membered ring R6 is illustrated in FIG. 1. In FIG. 1, (a) is a six-membered aromatic ring, (b) is a six-membered cycloalkene, and (c) is a six-membered cycloalkane. In the structure of R6, some of the carbon atoms may be replaced by heteroatoms such as oxygen, nitrogen, and sulfur atoms. In this case, the number of hydrogen atoms bonded to the heteroatom may increase or decrease depending on the number of bonds to which the heteroatom can be bonded. In the structure of R6, R1 to R5 can be selected from hydrophilic groups such as hydrogen, OH, and carboxy groups, and hydrophobic groups such as methyl, ethyl, isopropyl, and t-butyl groups. R1 to R5 may be the same or different. R1 to R5 are preferably four hydrogen groups and one methyl group. This increases the compatibility of the organic solvent with the binder. The organic solvent having a cyclic structure can be represented by R6-R7 (wherein R7 has a structure containing elements such as carbon, hydrogen, nitrogen, and oxygen). It is preferable that the OH group is included in R7. This increases the compatibility of the organic solvent with the binder and the barium titanate particles.
[0017] Examples of the chain structure include a linear structure such as an alkyl group, and a branched structure such as an isopropyl group or a tert-butyl group. The organic solvent having a chain structure can be expressed by the rational formula R3-CR4R5-CH3. In this rational formula, the methyl group (-CH3) is the end. The carbon atom bonded to the methyl group at the end is the second carbon atom from the end. That is, the carbon atom of the methyl group and the carbon atom bonded to the methyl group are continuously carbon-carbon bonded from the end. Here, R3, R4, and R5 have a structure containing elements such as carbon, hydrogen, nitrogen, and oxygen. R3, R4, and R5 may be bonded to form a cyclic structure. When the organic solvent has a hydrophobic structure, it is considered that the compatibility between the organic solvent and the binder is increased. When the organic solvent has a hydrophobic structure and an OH group, the organic solvent increases the compatibility between the binder and the barium titanate particles. Therefore, the paste is less likely to aggregate. It is preferable that the number of carbon atoms continuously bonded to the end of the chain structure is 5 or less. This increases the hydrophilicity of the organic solvent. The number of carbon atoms in the carbon-carbon bond is more preferably 4 or less. When the organic solvent has an ether bond, it is preferable that an alkyl group is bonded to the oxygen atom of the ether bond. The number of carbon atoms in this alkyl group is preferably 3 to 5.
[0018] The solubility parameter (SP value) of the organic solvent is preferably 8.5 or more. When the SP value is 8.5 or more, the hydrophilicity of the organic solvent increases.
[0019] The boiling point of the organic solvent under atmospheric pressure is preferably 300°C or less. This makes the carbon chain of the organic solvent shorter than that of an organic solvent with a boiling point higher than 300°C. Therefore, the viscosity of the dispersion liquid is reduced. In addition, the viscosity of the printing paste is also reduced, so that the printing paste is easily applied uniformly during printing. The boiling point of the organic solvent under atmospheric pressure is preferably 200 to 300°C. This makes it easier to dry the paste uniformly with the Ni particles and barium titanate particles dispersed when applying and drying the paste. Therefore, the sintering retardation effect of the Ni particles is enhanced. In addition, cracks are less likely to occur in the MLCC. If an organic solvent with a boiling point of 200 to 300°C has an OH group, the dispersion liquid and the Ni particles can be easily mixed. Therefore, the paste is less likely to aggregate. If the paste is less likely to aggregate, the paste is easily dried uniformly, so that the printability is improved. From the viewpoint of boiling point and hydrophobic structure, the organic solvent is preferably butyl carbitol. The viscosity of the organic solvent is preferably 100 mPa·s or less at atmospheric pressure and 25° C. This reduces the viscosity of the dispersion liquid, and also reduces the viscosity of the printing paste.
[0020] Next, a method for producing barium titanate particles and a dispersion thereof will be described.
[0021] First, barium hydroxide is mixed with alkyl cellosolve as a solvent to prepare mixed solution A (first step). By using barium hydroxide, counter ions do not diffuse into the dielectric layer when the electrode layer is fired. Therefore, the performance of the MLCC is likely to be improved. Since the solvent is alkyl cellosolve, the viscosity of the dispersion is reduced. In addition, the viscosity of the paste is unlikely to increase. The water content of mixed solution A is preferably 5% by mass or less. This makes it difficult for titanium alkoxide to hydrolyze when it is added, as described later. Therefore, the particle size is likely to be small. Before the second step described later, mixed solution A may be decompressed or heated to reduce the water content of mixed solution A to 5% by mass or less.
[0022] Next, titanium alkoxide is added to the mixed solution A to prepare mixed solution B (second step). In mixed solution B, the atomic ratio of barium to titanium, Ba / Ti, is preferably 0.95 to 1.05. In this range, crystals other than the perovskite structure are less likely to be generated. The atomic ratio of barium to titanium may be 0.9 to 1.1. The titanium alkoxide is preferably added under a nitrogen atmosphere. This reduces the reaction rate of the titanium alkoxide. Therefore, barium titanate particles with small particle size and crystallite size are easily obtained.
[0023] The structure of titanium alkoxide is preferably "Ti(OR)4". Here, R is a hydrocarbon group having 1 to 4 carbon atoms, or a substituted hydrocarbon group in which one or more hydrogen atoms of the hydrocarbon group are substituted with halogen atoms. R may be the same or different. With such a structure, the crystallinity of barium titanate particles tends to be high. Specific examples include titanium tetramethoxide, titanium tetraethoxide, titanium tetra n-propoxide, titanium tetraisopropoxide, titanium tetra n-butoxide, and titanium tetraisobutoxide.
[0024] Next, water is added to the mixed solution B to prepare the mixed solution C (third step). The amount of water added is preferably equal to or greater than the molar equivalent of the titanium alkoxide. This reduces the amount of titanium alkoxide remaining in the mixed solution C without being hydrolyzed. This increases the crystallinity of the barium titanate particles.
[0025] Next, the mixed liquid C is heated (fourth step). It is preferable to heat at 40°C or higher for 2 to 200 hours. This step promotes aging, and barium titanate particles are generated in the aged product. If the heating temperature is 40°C or higher, the particle size distribution tends to become uniform, although this varies depending on the gel concentration. Furthermore, the crystallinity is improved. Moreover, a heating temperature of 120°C or lower is easy to handle industrially. If the heating time is 2 hours or more, the particle size distribution tends to become uniform. Furthermore, the crystallinity is easily improved. If the heating time is 200 hours or less, the particle size and crystallite size tend to become small. A heating time of 5 hours to 100 hours is more preferable.
[0026] The aged product obtained in the fourth step is ultrafiltered or distilled (fifth step). When ultrafiltered or distilled, the water content of the dispersion is adjusted to less than 3% by weight. An organic solvent may be added before ultrafiltered or distilled. When the boiling point of the organic solvent is lower than that of the alkyl cellosolve, ultrafiltered is preferred. When the boiling point is higher than that of the alkyl cellosolve, distillation is preferred. The organic solvent preferably has the characteristics of the organic solvent described in the above description of the dispersion.
[0027] The dispersion prepared by such a manufacturing method has a low water content. Therefore, the viscosity of the paste is less likely to increase. In addition, the particle size and crystallite size of the barium titanate particles in the dispersion are small, and the crystallinity is high. Furthermore, since the crystal system of the barium titanate particles is close to a cubic system, when used in an electrode layer, the sintering retardation effect of Ni is enhanced.
[0028] In addition, it is preferable to add a metal salt containing at least one selected from group 2, group 3, lanthanoid, actinoid, group 4, group 5, group 6, group 7, group 8, group 9, group 10, group 11, group 12, group 13, and group 14 before the fourth step. By adding such a metal salt, the sintering retardation effect is increased. In addition, the metal salt makes it difficult for crystals other than the perovskite structure to be generated. Furthermore, by adding the metal salt before the fourth step, the metal salt is dispersed in the barium titanate gel. Therefore, the sintering retardation effect is likely to be increased.
[0029] Examples of the present invention will be specifically described below. Preparation conditions for each of the examples and comparative examples are shown in Table 1.
[0030] [Example 1] <Preparation of Dispersion> 50 g of barium hydroxide octahydrate (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) and 315 g of 2-methoxyethanol (methyl cellosolve) were placed in a beaker and dissolved at 30°C for 20 minutes. The Ba concentration of this solution was 6.0% by weight, and the water content was 6.2% by weight. 3The mixture was placed in a round-bottom flask and distilled using a rotary evaporator to obtain mixed solution A. The distillation conditions were a temperature of 70°C, a reduced pressure of 0.015 MPa, and a duration of 1 hour. The Ba concentration of mixed solution A was 16.0% by weight, and the water content was 0.5% by weight.
[0031] In a glove box under a nitrogen gas atmosphere, 170 g of mixed solution A was mixed with 56.18 g of tetraisopropoxytitanium (manufactured by Matsumoto Fine Chemical Co., Ltd.: Orgatix (registered trademark) TA-10, Ti concentration 16.88 wt %) to prepare mixed solution B.
[0032] Further, a mixture of 57.1 g of water and 171.2 g of methanol was added over 1 minute. During the addition, the mixture was stirred while maintaining the temperature at 25° C. The temperature of the resulting hydrate gel was raised to 80° C. and aged for 96 hours. The aged product was ultrafiltered to obtain a dispersion containing 40% by mass of barium titanate.
[0033] The dispersions were measured as follows. The measurement results for each of the Examples and Comparative Examples are shown in Table 2.
[0034] <Moisture content measurement> The measurements were performed using a benchtop coulometric moisture meter, Model CA-200 (Mitsubishi Chemical Analytech Co., Ltd.).
[0035] <Measurement of adsorbed water content> 30 g of the dispersion was dried at 200°C for 3 hours and cooled in a desiccator to obtain a dry powder. The dry powder was left to stand for 1 hour in a thermohygrostat (Espec PL-3J) adjusted to 25°C and 90 RH%. The amount of adsorbed water was calculated from the change in weight before and after.
[0036] <X-ray diffraction measurement> The dispersion liquid was dried at 400°C to obtain a powder of barium titanate particles. X-ray diffraction measurement was performed on this powder using Rigaku's RINT-Ultima. X-ray diffraction measurement was also performed in the examples and comparative examples described below. In the X-ray diffraction measurement, no X-ray diffraction peaks other than those of the perovskite structure were observed except for Comparative Example 1.
[0037] <Viscosity measurement> A binder liquid was prepared by dispersing 3 g of ethyl cellulose powder in 74 g of terpineol (manufactured by Yasuhara Chemical Co., Ltd.). 4.5 g of this binder liquid was mixed with 3 g of the dispersion liquid to obtain a paste for viscosity measurement. Using a rheometer RS3000 (HAAKE Co., Ltd.), dγ / dt = 0.1 to 1000 s -1 Dynamic viscosity measurement was performed in the range of dr / dt=40s -1 The value at this point was taken as the viscosity.
[0038] <Evaluation of printability> The paste for viscosity measurement was applied to a glass plate and dried at 200° C. The printability was evaluated by visually checking for agglomerates and smoothness in the dried film. ◎: No agglomerates, excellent smoothness ○: Almost no agglomerates, excellent smoothness △: Almost no agglomerates, slight problem with smoothness ×: Many aggregates are observed or the surface is not smooth.
[0039] <Preparation of electrode paste> 50 g of the dispersion (the amount of barium titanate in the dispersion is 10 g), 40 g of Ni nanoparticles (NFP301SD manufactured by JFE Mineral Co., Ltd.) having a particle size of 200 nm, and 10 g of ethyl cellulose powder were mixed and primarily dispersed using Thinky Corporation's Awatori Rentaro (registered trademark) AR-250. Further, secondary dispersion was performed using a three-roll mill (HHC type manufactured by Inoue Seisakusho Co., Ltd.) to prepare an electrode paste. The concentration of the electrode paste was 60% by weight. In the examples and comparative examples described later, electrode pastes were similarly prepared and measured and evaluated.
[0040] <Preparation of Dielectric Layer Paste> 90g of barium titanate (Sakai Chemical Industry Co., Ltd.: BT-01, average particle size = 300nm) and 10g of ethyl cellulose powder were added to 56.5g of terpineol solvent, and the mixture was primarily dispersed using a foaming mixer. A paste for the dielectric layer was then prepared by secondary dispersion using a three-roll mill.
[0041] <Preparation of Multilayer Ceramic Capacitors (MLCC)> The electrode paste was screen printed on a barium titanate ceramic sheet (thickness = 4.0 μm). This was dried at 600 °C for 1 hour. The dielectric layer paste was screen printed on top of this. This was dried at 600 °C for 1 hour. These steps were repeated to stack a total of 20 layers. This stack was reduced at 1200 °C for 2 hours in a nitrogen gas atmosphere containing 3% H2. It was then heated at 1000 °C for 3 hours in a nitrogen gas atmosphere.
[0042] Number of cracks The MLCC was cut vertically into 100 μm squares, and cross-sectional photographs were taken at 100,000 magnifications using a scanning electron microscope (SEM). Cracks present in each layer of the 100 μm square MLCC were confirmed and counted in the cross-sectional photographs.
[0043] <Evaluation of aggregation> The electrode paste was dropped onto a glass plate and the presence or absence of aggregates was visually determined.
[0044] In the following examples and comparative examples, samples were prepared, measured, and evaluated in the same manner as in Example 1.
[0045] [Example 2] A dispersion was obtained in the same manner as in Example 1, except that the mixture in Example 1 was changed to a mixture of 71.3 g of water and 214.0 g of methanol.
[0046] [Example 3] A dispersion was obtained in the same manner as in Example 1, except that the mixture in Example 1 was changed to a mixture of 2.46 g of nickel acetate tetrahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 57.1 g of water, and 171.3 g of methanol.
[0047] [Example 4] A dispersion was obtained in the same manner as in Example 1, except that the mixture in Example 1 was changed to a mixture of 0.85 g of magnesium acetate tetrahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 57.1 g of water, and 171.3 g of methanol.
[0048] [Example 5] When the barium hydroxide octahydrate of Example 1 was dissolved in 2-methoxyethanol, 1.79 g of tin methoxide (manufactured by Alfa Aesar) was added. Otherwise, a dispersion was prepared in the same manner as in Example 1.
[0049] [Example 6] A dispersion was obtained in the same manner as in Example 1, except that 2.02 g of calcium methoxide (manufactured by Strem Chemicals) was added when dissolving the barium hydroxide octahydrate in 2-methoxyethanol in Example 1. 178 g of this solution was used.
[0050] [Example 7] A dispersion was obtained in the same manner as in Example 1 except that 0.67 g of tantalum methoxide (manufactured by Strem Chemicals) was added when dissolving the barium hydroxide octahydrate of Example 1 in 2-methoxyethanol.
[0051] [Example 8] A dispersion was obtained in the same manner as in Example 1, except that the mixture in Example 1 was changed to a mixture of 0.92 g of nickel hydroxide hydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 57.1 g of water, and 171.2 g of methanol.
[0052] [Example 9] When the barium hydroxide octahydrate of Example 1 was dissolved in 2-methoxyethanol, 0.67 g of dysprosium isopropoxide (manufactured by Fuji Film Wako Chemicals Co., Ltd.) was added. Otherwise, a dispersion was obtained in the same manner as in Example 1.
[0053] [Example 10] A hydrolysis solution prepared by mixing 57.1 g of water and 171.3 g of methanol was added to the mixed solution B obtained in Example 1 over a period of 1 minute while maintaining the temperature at 25°C under stirring. This resulted in a hydrate gel. The temperature of this hydrate gel was raised to 80°C and aged for 96 hours. Ethanol was mixed with this aged product, and ultrafiltration was performed to obtain a dispersion containing 40% by mass of barium titanate.
[0054] [Example 11] Mixture B was prepared in the same manner as in Example 1, except that the weight of mixture A was changed to 178 g. A dispersion was obtained in the same manner as in Example 1, except that 70 g of butyl carbitol (manufactured by Kanto Chemical Co., Ltd.) was mixed with the aged product and solvent replacement was performed using a rotary evaporator instead of ultrafiltration. The solvent replacement was performed under the conditions of a temperature of 70°C, a reduced pressure of 0.015 MPa, and one hour.
[0055] [Example 12] A dispersion was obtained in the same manner as in Example 11, except that the weight of the mixed liquid A was changed to 170 g.
[0056] [Example 13] A dispersion was obtained in the same manner as in Example 12, except that the solution for hydrolysis was changed to a solution of 2.46 g of nickel acetate tetrahydrate (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.), 57.1 g of water, and 171.3 g of methanol.
[0057] [Example 14] A dispersion was obtained in the same manner as in Example 12, except that the weight of mixed solution A was changed to 168 g, and 70 g of terpineol and 3.5 g of linoleic acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were mixed with the aged product instead of butyl carbitol.
[0058] [Example 15] 3.5 g of linoleic acid was added to the aged product obtained in Example 11 and stirred at 50° C. for 15 hours. 70 g of butyl carbitol was added thereto and distilled with a rotary evaporator to obtain a dispersion. The distillation conditions were a temperature of 70° C., a reduced pressure of 0.015 MPa, and 1 hour.
[0059] [Example 16] 70 g of terpineol was added to the aged product obtained in Example 10. Using a rotary evaporator, distillation was carried out under the conditions of a temperature of 70° C., a reduced pressure of 0.015 MPa, and 1 hour.
[0060] [Example 17] 70 g of triethanolamine was added to the aged product obtained in Example 10. Distillation was carried out using a rotary evaporator under the conditions of a temperature of 70° C., a reduced pressure of 0.015 MPa, and 1 hour.
[0061] [Comparative Example 1] A dispersion was obtained in the same manner as in Example 1, except that the weight of the barium hydroxide solution was changed to 204 g.
[0062] [Comparative Example 2] Barium carbonate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and titanium oxide powder (manufactured by Ishihara Sangyo Kaisha, Ltd.) were weighed out so that the Ba / Ti molar ratio was 1.01, and mixed using a ball mill. The mixed powder was fired at 900°C in air, and the fired powder was further crushed using a mortar.
[0063] [Table 1]
[0064] [Table 2]
Claims
1. The present invention comprises barium titanate particles having a perovskite structure and an organic solvent having a boiling point of 200 to 300° C., the barium titanate particles have an atomic ratio of barium to titanium, Ba / Ti, of 0.9 to 1.1; The axial ratio c / a of the perovskite structure is 1.005 or less, The barium titanate particles have a crystallite size of 5 to 25 nm; The moisture content is less than 3% by weight, The organic solvent has an OH group, A dispersion of barium titanate particles, characterized in that when the solid content obtained by drying the dispersion at 200°C for 3 hours is exposed to conditions of 25°C and 90RH% for 1 hour, the amount of water adsorbed by the solid content is 5 parts by mass or more per 100 parts by mass of the solid content.
2. 2. The dispersion according to claim 1, wherein the organic solvent has a cyclic structure or a chain structure in which two or more carbon atoms from the terminal are successively carbon-carbon bonded.
3. 3. The dispersion according to claim 1, wherein the organic solvent has an ether bond.
Citation Information
Patent Citations
Barium titanate and its production method
JP2004300027A
Electrode paste, and manufacturing method of ceramic electronic component
JP2005063707A
Method for producing crystalline titanic acid salt, and crystalline titanic acid salt
JP2012240904A
Sol comprising titanic acid alkali earth metal particles, production method thereof and paste comprising the same
JP2018172242A
Method for producing composite oxide particle, composite oxide particle powder, dispersion liquid and dielectric for capacitor
JP2019026542A