Optimizing the composition of electromagnetic soft iron with controlled elements like C, Si, Mn, P, S, Al, and B, particularly through BN formation, addresses the challenge of achieving both high magnetic properties and machinability, resulting in improved machining performance and magnetic characteristics.

JP7556024B2Active Publication Date: 2024-09-25JFE STEEL CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022518877
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-29
Filing Date
2021-10-22
Publication Date
2024-09-25
Estimated Expiration
2041-10-22

AI Technical Summary

Technical Problem

Existing electromagnetic soft iron materials face a technical limit in achieving both high magnetic properties and machinability due to the adverse effects of MnS and FeS precipitates, which improve machinability but deteriorate magnetic properties.

Method used

The composition of electromagnetic soft iron is optimized with specific ranges of C, Si, Mn, P, S, Al, N, B, and other elements to enhance machinability without compromising magnetic properties, utilizing BN formation for improved machinability.

Benefits of technology

The solution provides electromagnetic soft iron with stable and enhanced magnetic properties and machinability, as demonstrated by improved magnetic flux density, coercive force, and reduced tool wear during machining.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556024000001
    Figure 0007556024000001
  • Figure 0007556024000002
    Figure 0007556024000002
Patent Text Reader

Abstract

The present invention provides technology that achieves high levels of both magnetic properties and machinability, which couldn't be achieved with just conventional machinability-improving technology utilizing MnS. This soft magnetic iron has a component composition containing, in mass%, less than 0.02% C, less than 0.05% Si, more than 0.03% to 0.50% Mn, 0.002% to less than 0.006% P, 0.013% to 0.050% S, 0.010% or less Al, 0.0010% to 0.0100% N, and 0.0003% to 0.0065% B, with the remainder comprising iron and unavoidable impurities.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electromagnetic soft iron having excellent machinability and magnetic properties. [Background technology]

[0002] In recent years, there has been a worldwide demand for resource and energy conservation in order to protect the global environment, and in the field of electrical equipment, there has been active promotion of high efficiency and miniaturization for the purpose of energy conservation. Against this background, there is a demand for power saving and improved response speed to external magnetic fields in electrical components used in automobiles, etc.

[0003] Pure iron-based electromagnetic soft iron is usually used as a material that easily responds to external magnetic fields. This electromagnetic soft iron is made of steel with a C content of approximately 0.01% by mass or less, and is generally manufactured into electrical components by forging and cutting the steel bar obtained by hot rolling and wire drawing.

[0004] Here, in the processing of parts, it is known that the soft ferrite single phase structure of electromagnetic soft iron has very poor machinability, so in addition to magnetic properties, it is becoming important for electromagnetic soft iron to have excellent machining performance.

[0005] For example, Patent Document 1 discloses a technique for producing a soft magnetic steel material having excellent magnetic properties and machinability by controlling the size and number of MnS particles dispersed in steel.

[0006] Patent Document 2 discloses a technique for controlling the size and density of FeS precipitates to produce a soft magnetic steel material having excellent cold forgeability, machinability and magnetic properties. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2007-51343 A [Patent Document 2] JP 2007-46125 A Summary of the Invention [Problem to be solved by the invention]

[0008] The techniques described in Patent Documents 1 and 2 are techniques for improving machinability by the sole effect of MnS or FeS. However, an increase in the amount of these precipitates (MnS, FeS) may lead to a deterioration of magnetic properties. Therefore, there is a technical limit to achieving both magnetic properties and machinability at a higher level.

[0009] The present invention has been made in consideration of the above circumstances, and aims to provide a technology for achieving both high levels of magnetic properties and machinability, which could not be realized by conventional machinability improvement technology using MnS or the like. [Means for solving the problem]

[0010] In order to solve the above problems, the inventors conducted extensive research and discovered that by utilizing BN, it is possible to improve machinability without deteriorating magnetic properties.

[0011] The present invention was completed as a result of further investigation based on the above-mentioned novel findings, and the gist of the present invention is as follows. 1. In mass percent, C: less than 0.02%, Si: less than 0.05% Mn: more than 0.03% and less than 0.50%, P: 0.002% or more and less than 0.006% S: 0.013% or more and 0.050% or less, Al: 0.010% or less, N: 0.0010% to 0.0100% and B: 0.0003% or more and 0.0065% or less and the remainder being iron and unavoidable impurities.

[0012] 2. The composition further comprises: In mass%, Cu: 0.20% or less, Ni: 0.30% or less, Cr: 0.30% or less, Mo: 0.10% or less V: 0.02% or less, Nb: less than 0.015% and Ti: less than 0.010% 2. The electromagnetic soft iron according to claim 1, comprising one or more selected from the following:

[0013] 3. The composition further includes, in mass%, Pb: 0.30% or less, Bi: 0.30% or less, Te: 0.30% or less, Se: 0.30% or less Ca: 0.0100% or less, Mg: less than 0.0050% Zr: 0.200% or less and REM: 0.0100% or less 3. The electromagnetic soft iron according to 1 or 2 above, comprising one or more selected from the following: Effect of the Invention

[0014] According to the present invention, it is possible to stably provide pure iron-based electromagnetic soft iron having excellent magnetic properties and machinability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, a pure iron-based electromagnetic soft iron according to an embodiment of the present invention will be described. First, the reasons for limiting each component in the composition of the pure iron-based electromagnetic soft iron will be described. In this specification, "%" representing the content of each component element means "mass %" unless otherwise specified.

[0016] C: Less than 0.02% If the C content is 0.02% or more, the iron loss is significantly deteriorated due to magnetic aging, so it is limited to less than 0.02%. Note that even if the C content is less than 0.001%, the effect on magnetic properties is saturated, while reducing the C content to less than 0.001% increases the refining cost, so the C content is preferably 0.001% or more. It is preferably 0.001% or more and 0.015% or less, more preferably 0.001% or more and 0.010% or less.

[0017] Silicon: Less than 0.05% Silicon is an effective deoxidizing element. If the silicon content is 0.05% or more, it hardens ferrite and reduces cold workability. For this reason, silicon may be contained, but the silicon content is less than 0.05%. It is preferably 0.03% or less. Of course, silicon may be 0%.

[0018] Mn: More than 0.03% and less than 0.50% Mn is an element that is effective in improving strength through solid solution strengthening, and is also effective in improving machinability by dispersing MnS bonded with S in the steel. To achieve this, the content is set to more than 0.03%. On the other hand, excessive addition of Mn deteriorates the magnetic properties, so the content is set to 0.50% or less. The content is preferably more than 0.03% and 0.40% or less. More preferably, the content is more than 0.03% and 0.35% or less.

[0019] P: 0.002% or more and less than 0.006% Even a relatively small amount of P can provide significant solid solution strengthening. To achieve this, the P content must be 0.002% or more. However, excessive addition of P impairs cold workability, so the P content must be less than 0.006%.

[0020] S: 0.013% or more and 0.050% or less S forms MnS in steel and contributes to improving machinability. To achieve this effect, the addition of 0.013% or more is necessary. On the other hand, the addition of more than 0.050% deteriorates cold workability. Therefore, the S content is set to 0.013% or more and 0.050% or less. Preferably, the S content is 0.013% or more and 0.045% or less, and more preferably, the S content is 0.013% or more and 0.040% or less.

[0021] Al: 0.010% or less Al combines with N in the steel to form fine AlN. This fine AlN inhibits the growth of crystal grains and deteriorates the magnetic properties, so the content must be 0.010% or less. Of course, Al may be 0%.

[0022] N: 0.0010% or more and 0.0100% or less N combines with B to form BN, which contributes to machinability. To achieve this effect, an addition of 0.0010% or more is necessary. On the other hand, an addition of more than 0.0100% deteriorates cold workability and magnetic properties, so the upper limit is set at 0.0100%. The preferred range is 0.0015% to 0.0090%.

[0023] B: 0.0003% or more and 0.0065% or less B combines with N in steel to form BN. BN has the effect of improving machinability. To obtain this effect, it is necessary to add 0.0003% or more. On the other hand, addition of more than 0.0065% leads to deterioration of magnetic properties and castability, so the upper limit is set to 0.0065%. The content is preferably 0.0005% or more and 0.0060% or less, and more preferably 0.0010% or more and 0.0055% or less.

[0024] The basic components of the present invention have been described above. The balance other than the above components is Fe and unavoidable impurities. Furthermore, if necessary, any one or more of the elements described below may be appropriately contained. Cu:0.20% or less Ni: 0.30% or less Cr:0.30% or less Mo: 0.10% or less V:0.02% or less Nb: Less than 0.015% Ti: less than 0.010% Cu, Ni and Cr contribute to increasing strength mainly through solid solution strengthening, and to realize this effect, it is preferable to add 0.01% or more of each. However, since excessive addition deteriorates the magnetic properties, it is preferable to set the upper limits to 0.20%, 0.30% and 0.30%, respectively.

[0025] In addition, Mo, V, Nb and Ti contribute to increasing strength mainly through precipitation strengthening, and in order to realize this effect, it is preferable to add 0.001%, 0.0001%, 0.0001% and 0.0001% or more, respectively. However, since excessive addition deteriorates the magnetic properties, it is preferable to add 0.10% or less, 0.02% or less, less than 0.015% and less than 0.010%, respectively.

[0026] Furthermore, the present invention may contain one or more of the following elements. Pb: 0.30% or less Bi:0.30% or less Te: 0.30% or less Se: 0.30% or less, Ca:0.0100% or less Mg: Less than 0.0050% Zr: 0.200% or less REM: 0.0100% or less Pb, Bi, Te, Se, Ca, Mg, Zr and REM are elements that contribute to improving machinability. To achieve their respective effects, it is preferable to add 0.001% or more of Pb, 0.001% or more of Bi, 0.001% or more of Te, 0.001% or more of Se, 0.001% or more of Ca, 0.0001% or more of Mg, 0.0001% or more of Zr and 0.0001% or more of REM. However, excessive addition of these elements causes deterioration of magnetic properties, so it is preferable to add 0.30% or less of Pb, 0.30% or less of Bi, 0.30% or less of Te, 0.30% or less of Se, 0.0100% or less of Ca, less than 0.0050% of Mg, 0.200% or less of Zr and 0.0100% or less of REM.

[0027] In the composition of the present invention, the components other than those mentioned above are Fe and unavoidable impurities.

[0028] A preferred method for producing the pure iron-based electromagnetic soft iron according to the present invention will be described. Molten steel having the above-mentioned composition is melted by a conventional melting method such as a converter or an electric furnace, and is made into a steel material by a conventional continuous casting or blooming method. Next, the steel material is heated as necessary, and is made into electromagnetic soft iron by hot rolling such as steel billet rolling and bar and wire rolling. The above heating and rolling conditions are not particularly limited, but may be appropriately determined according to the required material, and for example, the structure may be controlled so as to be advantageous for forging and machining for subsequent part forming. Since the electromagnetic soft iron of the present invention has excellent machinability, the shape of the electromagnetic soft iron is preferably any of the shapes of a bar, rod, or wire, which are mainly used in applications where cutting is performed.

[0029] The content of each element can be determined by spark discharge optical emission spectrometry, fluorescent X-ray analysis, ICP optical emission spectrometry, ICP mass spectrometry, combustion method, or the like. Other manufacturing conditions may be the same as those for general steel manufacturing methods. EXAMPLES

[0030] Next, examples of the present invention will be described, but the present invention is not limited to the following examples. Steel containing the chemical composition shown in Table 1 was melted, hot forged at about 1200°C, and then annealed at 950°C to produce steel bars with a diameter of 25 mm. The magnetic properties, cold workability, and machinability of the resulting steel bars were evaluated according to the methods described below. The evaluation results are shown in Table 2.

[0031] [Table 1]

[0032] [Table 2]

[0033] [Magnetic properties] The magnetic properties were measured in accordance with JIS C2504. That is, a ring-shaped test piece was taken from the above steel bar (material) and subjected to magnetic annealing at 750°C for 2 hours. Then, an excitation winding (220 turns of primary winding) and a detection winding (100 turns of secondary winding) were wound around the ring test piece and used for testing. The magnetic flux density was obtained by measuring the BH curve using a DC magnetization measuring device. Specifically, the magnetic flux density was obtained at 100 and 300 A / m during the magnetization process with a maximum magnetic field of 10,000 A / m. If the magnetic flux density is 1.20 T and 1.50 T or more, respectively, it can be said that the magnetic properties are excellent.

[0034] The coercive force was measured using a ring-shaped test piece with the same winding as above, using a DC magnetic property tester at a reversal magnetization force of ±400 A / m. If the coercive force is 60 A / m or less, it can be said that the magnetic properties are excellent.

[0035] [Cold workability] Cold workability was evaluated by the critical upsetting ratio. That is, the critical upsetting ratio was measured by taking a test piece from the circumferential surface of the steel bar at a depth position of 1 / 2 the diameter, with a diameter of 15 mm, a height of 22.5 mm, and a notch on the side with a depth of 0.8 mm and a notch bottom R of 0.15, and compressing the test piece. Sequential compression was performed until a crack with a width of 0.5 mm or more appeared at the notch bottom of the test piece. The upsetting ratio at this time was taken as the critical upsetting ratio. If the limiting upset ratio is 55% or more, it can be said that the cold workability is excellent.

[0036] [Machinability] Machinability was evaluated by measuring the amount of flank wear of the tool. Specifically, using an NC lathe, a steel bar with a diameter of 25 mm was cut with a coated tool made of carbide substrate at a cutting depth of 0.2 mm, a feed rate of 0.15 mm / rev, a peripheral speed of 300 m / min, and a cutting length of 1000 m in a wet manner. The amount of flank wear of the tool was then measured. If the amount of flank wear is 35 μm or less, it can be said that the tool has excellent machinability.

Claims

1. In mass percent, C: less than 0.02%; Si: less than 0.05% Mn: more than 0.03% and less than 0.50%, P: 0.003% or more and less than 0.006%; S: 0.013% or more and 0.050% or less, Al: 0.010% or less, N: 0.0010% or more and 0.0100% or less; B: 0.0003% or more and 0.0065% or less and the remainder being iron and unavoidable impurities.

2. The composition further comprises: In mass percent, Cu: 0.20% or less, Ni: 0.30% or less, Cr: 0.30% or less, Mo: 0.10% or less, V: 0.02% or less, Nb: less than 0.015% and Ti: less than 0.010% The electromagnetic soft iron according to claim 1, comprising one or more selected from the following:

3. The composition further includes, in mass%, Pb: 0.30% or less, Bi: 0.30% or less, Te: 0.30% or less, Se: 0.30% or less Ca: 0.0100% or less, Mg: less than 0.0050% Zr: 0.200% or less; REM: 0.0100% or less The electromagnetic soft iron according to claim 1 or 2, comprising one or more selected from the following:

Citation Information

Patent Citations

  • Bn-base free cutting steel excellent in soft magnetism

    JP2001303209A

  • Soft magnetic low carbon steel having excellent machinability and magnetic property, production method therefor and method for producing soft magnetic low carbon steel parts obtained by using the same steel

    JP2003055745A

  • Soft magnetic steel material superior in cold forgeability, machinability and magnetic property, and soft magnetic steel parts superior in magnetic property

    JP2007046125A

  • Soft magnetic steel having excellent magnetic property in high magnetic field and excellent machinability, and soft magnetic steel component having excellent magnetic property in high magnetic field

    JP2007051343A

  • Soft magnetic steel material and manufacturing method therefor, and soft magnetic part obtained from soft magnetic steel material

    JP2015127454A