Pressure transducer for use in a hydrogen-containing medium and method for making such a pressure transducer - Patents.com

Fine-grained austenitic iron-nickel-cobalt alloys with a hydrogen-resistant coating address thermal expansion and hydrogen embrittlement issues in pressure transducers, enhancing measurement accuracy and durability in hydrogen-containing environments.

JP7556089B2Active Publication Date: 2024-09-25KISTLER HLDG AG
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023061580
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-06-21
Filing Date
2023-04-05
Publication Date
2024-09-25
Estimated Expiration
2043-04-05

AI Technical Summary

Technical Problem

Pressure transducers used in hydrogen-containing environments face challenges due to high temperatures and hydrogen penetration, leading to thermal expansion issues and hydrogen embrittlement, which affect measurement accuracy and durability.

Method used

The use of fine-grained austenitic iron-nickel-cobalt alloys with a thermal expansion coefficient of 9.0×10^-6 K^-1 and a grain size below 20 μm for the diaphragm, combined with a hydrogen-resistant coating, to enhance resistance to hydrogen penetration and maintain mechanical integrity.

Benefits of technology

The solution provides improved measurement accuracy and durability by reducing thermal expansion effects and hydrogen embrittlement, ensuring precise pressure measurements even at high temperatures and in hydrogen-rich environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556089000001
    Figure 0007556089000001
  • Figure 0007556089000002
    Figure 0007556089000002
  • Figure 0007556089000003
    Figure 0007556089000003
Patent Text Reader

Abstract

To provide a pressure transducer for measuring pressure of liquid or gas medium containing hydrogen, and a manufacturing method for the same.SOLUTION: In a pressure transducer, a liquid or gas medium whose pressure is measured contains hydrogen, is disposed in a measuring chamber. The pressure transducer is in contact with and is disposed in the measuring chamber and is permanently exposed to a highest temperature 350°C during measurement. The pressure transducer has a diaphragm and a transducer element. The diaphragm protects the transducer element from direct contact with the medium. The pressure operates on the transducer element via the diaphragm. The transducer element generates measurement value under an influence of pressure. The diaphragm is made of a metallic material having 9.0×10-6K-1 or less of thermal expansion coefficient, and an average grain diameter of the metallic material is below 20 μm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pressure transducer for use in a hydrogen-containing medium and to a method for manufacturing a pressure transducer as defined in the preamble of the independent claim. [Background technology]

[0002] Pressure transducers are used to measure the pressure of a liquid or gaseous medium. The medium is placed in a measurement chamber. A pressure transducer is placed in contact with the measurement chamber to measure the pressure. The pressure transducer comprises parts such as a housing, a diaphragm, a transducer element, etc. The transducer element is placed inside the housing. The housing and the diaphragm seal the interior of the pressure transducer from the medium and thus protect the transducer element from the direct influence of the medium. The pressure of the medium acts on the transducer element via the diaphragm. Under the influence of the pressure, the transducer element generates a measurement value. The transducer element can be a piezoresistive transducer element with a silicon-based Wheatstone bridge, a piezoelectric transducer element made of piezoelectric material, a strain gauge with a Wheatstone bridge on a metal or plastic substrate, a strain gauge with a Wheatstone bridge on a metal or plastic substrate, etc.

[0003] During use, pressure transducers are often exposed to harsh measurement conditions, which are characterized by high temperatures, chemically aggressive substances such as hydrogen, etc. To ensure a long service life and perfect functionality even under harsh measurement conditions, the parts of the pressure transducer that are in direct contact with the medium (e.g. housing, diaphragm, etc.) are made of metallic materials with high mechanical resistance, e.g. iron alloys, nickel alloys, cobalt alloys, etc.

[0004] In internal combustion engines and turbines, for example, pressure transducers are permanently exposed to high temperatures of up to 350°C. At such high temperatures, differences between the thermal expansion coefficients of the pressure transducer components become detrimental. The different thermal expansion coefficients are manifested as a temperature effect on the zero value (TK0) and a temperature effect on the characteristic value (TKE). For TK0 there is a zero shift and for TKE there is a change in sensitivity. Both effects falsify the measurements.

[0005] Typically, piezoresistive transducer elements have a resistance of 2.0×10 at temperatures up to 350°C. -6 K -1 and the piezoelectric transducer element exhibits a thermal expansion coefficient of 7.5×10 at temperatures up to 350°C. -6 K -1 has a thermal expansion coefficient of

[0006] To most accurately measure pressure at temperatures up to 350°C, the components of the pressure transducer that are in direct contact with the medium and are made from metallic materials must have a thermal expansion coefficient of 9.0 x 10 at temperatures up to 350°C. -6 K -1 It must have a low coefficient of thermal expansion of:

[0007] Known metallic materials with such low coefficients of thermal expansion are 5.2 × 10 in the temperature range of 20 to 400 °C. -6 K -1 and an iron-nickel-cobalt alloy with material number 1.3981, which has an average thermal expansion coefficient of 7.7 × 10 in the temperature range from 20 to 450 °C. -6 K -1 It is an iron-nickel-cobalt alloy having UNS number N19909, having an average coefficient of thermal expansion of

[0008] Both the iron-nickel-cobalt alloy with material number 1.3981 and the iron-nickel-cobalt alloy with UNS number N19909 are characterized by a high nickel content. Both alloys therefore have a predominantly austenitic structure with a face-centered cubic crystal structure. The austenitic structure is produced by hot forming at high temperatures of about 1100 °C, and the manufacturing process results in an average grain size significantly exceeding 20 μm.

[0009] For high sensitivity in measuring pressure, the diaphragm is as thin as possible. Therefore, the diaphragm offers little resistance to the introduction of forces and deforms very easily. Often the thickness of the diaphragm ranges from 40 to 150 μm.

[0010] The austenitic structure of the iron-nickel-cobalt alloy with material number 1.3981 and the iron-nickel-cobalt alloy with UNS number N19909 is not suitable for the manufacture of diaphragms, since the average grain size significantly exceeds 20 μm. This is because the material properties are anisotropic, with material properties that are direction-dependent, which complicates the structural mechanical design of the diaphragm by simulating the forces and moments acting during use. Such direction-dependent material properties can only be determined with great effort, and simulation is useless if the effort of determination is to be avoided. To obtain a sufficiently high strength, the thickness of the diaphragm should be at least 8 times the average grain size.

[0011] The diaphragm is in direct contact with the medium. If the medium contains hydrogen, hydrogen can permeate the diaphragm. A hydrogen-containing medium has at least 1% hydrogen by volume. In particular, for average grain sizes significantly greater than 20 μm for the austenitic structure of iron-nickel-cobalt alloys with material number 1.3981 and iron-nickel-cobalt alloys with UNS number N19909, hydrogen can permeate relatively easily along grain boundaries into the interior of the pressure transducer and accumulate therein. The permeated hydrogen can change the internal pressure of the pressure transducer, which can chemically react with the transducer element, thus adversely affecting the functionality of the pressure transducer.

[0012] Therefore, it is desirable for the metallic material of the diaphragm to have improved resistance to hydrogen permeation and accumulation within the pressure transducer. Summary of the Invention [Problem to be solved by the invention]

[0013] A first object of the present invention is a pressure transducer for measuring the pressure of a liquid or gaseous medium, the pressure transducer comprising a diaphragm of metallic material, the metallic material having a melting point of 9.0×10 at a temperature of up to 350° C. -6 K -1 The present invention provides a pressure transducer having a thermal expansion coefficient of 1000 .mu.m or less, the medium containing hydrogen, and the material having improved resistance to hydrogen.

[0014] And, a second object of the present invention is to demonstrate a low cost method for manufacturing such a pressure transducer. [Means for solving the problem]

[0015] The first object is solved by the features of the first independent claim.

[0016] The present invention relates to a pressure transducer for measuring the pressure of a liquid or gaseous medium, the medium containing hydrogen and being placed in a measurement chamber, the pressure transducer being placed in the measurement chamber and being permanently exposed to temperatures up to 350° C. during measurements, the pressure transducer comprising a diaphragm and a transducer element, the diaphragm protecting the transducer element from direct contact with the medium, pressure acting on the transducer element through the diaphragm, the transducer element producing a measurement value under the influence of the pressure, the diaphragm being 9.0×10 -6 K -1 The present invention relates to a pressure transducer made of a metal material having a thermal expansion coefficient of 0.1 to 1.0 μm, and an average grain size of the metal material is less than 20 μm.

[0017] Grain refinement usually leads to mechanical strengthening of metallic materials. During mechanical strengthening, plastic deformation with dislocations occurs in the crystal lattice. These dislocations facilitate the penetration of hydrogen into metallic materials, resulting in an increase in the hydrogen corrosion rate. Hydrogen corrosion leads to hydrogen embrittlement, which can lead to brittle fracture when metallic materials are subjected to load. For this reason, grain refinement is not usually used for components that are subject to high mechanical loads, such as the diaphragms of pressure transducers. Nevertheless, the inventors have reported that the 9.0×10 -6 K -1 Grain refinement has been performed on metallic materials with thermal expansion coefficients below 9.0×10 to achieve average grain sizes significantly below 20 μm. Grain refinement is the result of temperature-controlled hot forming and cooling of the metallic materials. The grain-refined metallic materials have a thermal expansion coefficient below 9.0×10 -6 K -1 Not only does it meet the thermal expansion coefficient requirements below, but it also meets the grain fineness requirements for sufficient mechanical strength for thin diaphragms with a diaphragm thickness of 150 μm or less.

[0018] Advantageous embodiments of the invention are set forth in the dependent claims.

[0019] The metallic materials of dependent claims 2-4 are the austenitic structure of the iron-nickel-cobalt alloy material number 1.3981 or the iron-nickel-cobalt alloy UNS number N19909. The non-fine-grained austenitic structure of the iron-nickel-cobalt alloy material number 1.3981 or the iron-nickel-cobalt alloy UNS number N19909 has a low carbon content and a low hydrogen corrosion rate. Unfortunately, in metallic materials with such low carbon content, grain refinement is often accompanied by an increase in the hydrogen corrosion rate. Hydrogen corrosion leads to hydrogen embrittlement, which can lead to brittle fracture when the austenitic structure is stressed. However, surprisingly, this did not happen. The fine-grained austenitic structure of these two alloys also shows a low hydrogen corrosion rate.

[0020] In addition, the fine-grained austenitic diaphragms of iron-nickel-cobalt alloy material number 1.3981 or iron-nickel-cobalt alloy UNS number N19909 contain significantly more grain boundaries through their thickness than the non-fine-grained austenitic diaphragms of these two alloys. The number of grain boundaries is approximately twice as many. Doubling the number of grain boundaries makes it more difficult for hydrogen to penetrate the diaphragm along the grain boundaries and therefore more difficult for hydrogen to penetrate to and accumulate in the pressure transducer.

[0021] The second object is solved by the features of the second independent claim.

[0022] The invention also relates to a method for manufacturing a pressure transducer for measuring the pressure of a liquid or gaseous medium, the medium containing hydrogen and being placed in a measurement chamber, the pressure transducer comprising a diaphragm and a transducer element, the pressure transducer being designed to permanently measure pressure at temperatures up to 350° C. with the pressure transducer placed in the measurement chamber, the transducer element producing a measurement under the influence of pressure, the diaphragm protecting the transducer element from direct contact with the medium and allowing the pressure to act on the transducer element via the diaphragm, the manufacturing method comprising: -6 K -1 providing a metallic material having a thermal expansion coefficient of less than 100 μm; and refining the grains of the metallic material, such that after grain refining, the metallic material has an average grain size of less than 20 μm; and producing a diaphragm from the fine-grained metallic material.

[0023] Thus, the pressure transducer is manufactured with a diaphragm of fine-grained metallic material. Due to grain refinement, the average grain size of the metallic material is reduced by about half. In comparison with non-fine-grained metallic materials, fine-grained metallic materials are much easier to machine. When the diaphragm is machined with a tool, the tool wears correspondingly less and can be used for a longer period of time.

[0024] Compared to the manufacture of pressure transducers using non-fine grained metallic materials to manufacture the diaphragm, the process of the present invention involves an additional step involving grain refinement of the metallic material, but the machining of the diaphragm is greatly simplified by using fine grained metallic materials, and when considering overall labor and cost, the process of the present invention is significantly more economical in comparison.

[0025] In the following, the invention will be explained in more detail, by way of example, with reference to the figures. [Brief description of the drawings]

[0026] [Figure 1] 1 shows a schematic cross-section of a portion of a first embodiment of a pressure transducer 1 having a front seal across one face of a diaphragm 12 . [Diagram 2] 1 shows a schematic cross-section of a portion of a second embodiment of a pressure transducer 1 having a front seal over one face of the diaphragm 12 and a coating 18 on the diaphragm 12 . [Diagram 3] 1 shows a schematic cross-section of a portion of a third embodiment of a pressure transducer 1 having a shoulder seal across one face of the housing 11. [Figure 4] 1 shows a schematic cross-section of a portion of a fourth embodiment of a pressure transducer 1 having a shoulder seal over one face of the housing 11 and a coating 18 on the housing 11 and diaphragm 12. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] In the drawings, the same reference numerals indicate the same items.

[0028] The pressure transducer 1, which is shown diagrammatically in the four embodiments according to Fig. 1 to Fig. 4, is arranged in a measurement chamber 20. The measurement chamber 20 can be a combustion chamber of an internal combustion engine, a turbine, etc. A liquid or gaseous medium 2 is arranged in the measurement chamber 20. The medium 2 exhibits a pressure P2 of up to 1000 bar. The medium 2 has a temperature T2 of up to 1000 °C. The medium 2 contains hydrogen. By hydrogen-containing medium 2 is meant a medium 2 which contains at least 1% by volume of hydrogen. The hydrogen can be present in molecular and / or atomic form. The measurement chamber 20 comprises a measurement chamber wall 21. The measurement chamber wall 21 keeps the medium 2 from escaping into an environment 40. The environment 40 is for example a machine room, a test bench, etc. The environment 40 is substantially subjected to a pressure P of 1 bar. 40 and temperature T below 80°C 40 The adjective "substantially" has the meaning of "±25%."

[0029] The pressure transducer 1 is arranged in the environment 40. The pressure transducer 1 is arranged in contact with the measurement chamber 20 through a wall opening 22 in the measurement chamber wall 21. The pressure transducer 1 comprises a housing 11 and a diaphragm 12. The housing 11 and the diaphragm 12 are made of a metallic material 30, for example an iron alloy, a nickel alloy, a cobalt alloy, etc. The metallic material 30 is mechanically resistant. In the following, the housing 11 and the diaphragm 12 are also referred to as the metallic parts 11, 12 of the pressure transducer. The housing 11 is hollow cylindrical and has an interior 111. With respect to the longitudinal axis 10, the housing 11 has a surface facing the interior 111. The diaphragm 12 is disc-shaped.

[0030] In the region of the wall opening 22, the pressure transducer 1 is in contact with the medium 2 via the diaphragm 2. With respect to the longitudinal axis 10 of the pressure transducer 1, the diaphragm 12 has a radially outer region and a radially inner region. Along the longitudinal axis 10, the diaphragm 12 has a face facing the medium 2 and a face facing the interior 111. The housing 11 and the diaphragm 12 are connected to each other via a material closure 121. The material closure 121 is advantageously an annular welded joint. Preferably, the material closure 121 is made in the radially outer region of the diaphragm 12 with the housing 11. The housing 11 and the diaphragm 12 close the interior 111 of the housing 11 in a sealed manner against the wall opening 22 via the material closure 121. The term "sealed" is used in the sense of 10 with respect to helium. -6 mbar x 1s -1 In the radially inner region, the diaphragm 12 has a diaphragm thickness 122 of 150 μm or less.

[0031] In the first and second embodiments of the pressure transducer 1 according to Fig. 1 and Fig. 2, the pressure transducer 1 is in contact with the medium 2 in the area of ​​the wall opening 22 only via the diaphragm 12. The wall opening 22 is closed from the environment 40 by a sealing surface 23 in the form of a front seal. For the front seal, a sealing element 24 is used. The sealing element 24 is arranged between the measurement chamber wall 21 and the diaphragm 12. The sealing element 24 directly adjoins the radially outer area of ​​the diaphragm 12. The sealing surface 23 seals the wall opening 22 from the environment 40.

[0032] In the third and fourth embodiments of the pressure transducer 1 according to figures 3 and 4, the pressure transducer 1 is in contact with the medium 2 via the housing 1 and the diaphragm 12 in the region of the wall opening 22. The wall opening 22 is closed from the environment 40 by a sealing surface 23 in the form of a shoulder seal. A sealing element 24 is used for the shoulder seal. The sealing element 24 is arranged between the measurement chamber wall 21 and the housing 11. The sealing surface 23 closes the wall opening 22 hermetically against the environment 40.

[0033] Preferably, the sealing element 24 is annular and made of a soft metal, such as, for example, copper, aluminum, or an elastomer, such as, for example, fluororubber, ethylene propylene diene rubber.

[0034] During operation, the pressure transducer 1 is permanently exposed to a temperature T1 of up to 350° C. The pressure P2 and the temperature T2 of the medium 2 act directly on the radially inner area of ​​the diaphragm 12. The transducer element 13 is arranged in the interior 111 of the housing 11. The diaphragm 2 and the transducer element 13 in particular are therefore permanently exposed to a temperature T1 of up to 350° C. during operation.

[0035] In the two embodiments according to Fig. 1 and Fig. 2, the transducer element 13 is preloaded between a preload base 16 and a preload sleeve 17. The preload base 16 and the preload sleeve 17 are made of a metallic material 30, for example an iron alloy, a nickel alloy, a cobalt alloy, etc. The metallic material 30 is mechanically resistant. The preload base 16 and the preload sleeve 17 are also referred to below as the metallic parts 16, 17 of the pressure transducer 1. The preload sleeve 17 has a preload sleeve thickness 172 of 150 μm or less. The preloaded transducer element 13 is placed against the face of the diaphragm 12 that faces the interior 111 immediately behind the diaphragm 12.

[0036] Towards the medium 2, the diaphragm 12 has a surface of constant size in its radially inner area. A pressure P2 of the medium 2 is introduced via the surface as a force on the transducer element 13. This causes the diaphragm 12 to deform. The transducer element 13 generates a measurement value M under the influence of the pressure P2. The measurement value M is dissipated into the environment via at least one measurement lead 14.

[0037] The pressure transducer 1 is either a piezoresistive pressure transducer or a piezoelectric pressure transducer. In the first and second embodiments of the pressure transducer 1 according to Fig. 1 and Fig. 2, the pressure transducer 1 is a piezoelectric pressure transducer. The piezoelectric pressure transducer has a piezoelectric transducer element 13 as a transducer element. The piezoelectric transducer element is made of a piezoelectric material and the measured value M is an electric charge.

[0038] In the third and fourth embodiments of the pressure transducer 1 according to figures 3 and 4, the pressure transducer 1 is a piezoresistive pressure transducer or a transducer of elastic deformation. The piezoresistive pressure transducer comprises a piezoresistive transducer element 13 as transducer element. The piezoresistive transducer element consists of a silicon-based Wheatstone bridge, the measured value M being a voltage. The transducer of elastic deformation comprises a strain gauge with a Wheatstone bridge on a metal or plastic substrate as transducer element 13, the measured value M being a voltage.

[0039] Preferably, the metallic material 30 is of an austenitic structure containing at least 20% nickel by weight with the average grain size 31 of the material 30 being smaller than 20 μm. Nickel is crucial for the low thermal expansion coefficient of the metallic material 30. Compared to an austenitic structure containing less than 20% nickel by weight, an austenitic metallic material 30 containing at least 20% nickel by weight has a thermal expansion coefficient of 9.0×10 -6 K -1 A low thermal expansion coefficient α 30 has.

[0040] Preferably, the metallic material 30 is an iron-nickel-cobalt alloy with material number 1.3981, having an average grain size 31 of less than 20 μm and a melting point of 5.2×10 in the temperature range of 20 to 400° C. -6 K -1 The average thermal expansion coefficient α 30 This means that at temperatures T1 of the pressure transducer 1 up to 350 °C, the thermal expansion coefficient α of the iron-nickel-cobalt alloy with material number 1.3981 is 30 However, the piezoresistive transducer element has a capacitance of 2.0×10 -6 K -1 Very small thermal expansion coefficient α 13 7.5 × 10 of the piezoelectric transducer element. -6 K -1 Thermal expansion coefficient α 13 The iron-nickel-cobalt alloy with material number 1.3981 can therefore be used both for pressure transducers 1 with piezoresistive transducer elements and for pressure transducers 1 with piezoelectric transducer elements without adverse differences between the thermal expansion of the at least one metal part 11, 12, 16, 17 and the thermal expansion of the transducer element 13, even at the high temperature T1 of the pressure transducer 1 of 350° C.

[0041] Preferably, the metallic material 30 is an iron-nickel-cobalt alloy having UNS number N19909, the average grain size 31 of the material 30 being less than 20 μm, and the average thermal expansion coefficient in the temperature range of 20 to 450° C. being less than 7.7×10 -6 K -1 This is the thermal expansion coefficient α of the iron-nickel-cobalt alloy with UNS number N19909 at the temperature T1 of the pressure transducer 1 up to 350 °C. 30 But 7.5×10 -6 K -1 The thermal expansion coefficient α of the piezoelectric transducer element 13In this way, even if the pressure transducer 1 is at a high temperature T1 of 350° C., there is no difference between the thermal expansion of the at least one metal part 11, 12, 16, 17 and the thermal expansion of the piezoelectric transducer element.

[0042] Preferably, the metallic material 30 has an average grain size 31 of the material 30 of less than 20 μm and a yield strength R P0.2 It is an iron-nickel-cobalt alloy with UNS number N19909, whose strength is 1000 MPa or more. P0.2 The yield strength is measured at a temperature of 20°C according to EN ISO 6892-1. The at least one metal part 11, 12, 16, 17 therefore does not deform plastically but only elastically, even under high pressures P2 of the medium 2 of up to 1000 bar. By avoiding plastic deformation, there is no possibility of the position of the diaphragm 12 relative to the transducer element 13 changing, which could lead to an incorrect measurement of the pressure P2.

[0043] The metallic components 11, 12, 16, and 17 may be made of a metallic material 30, such as an iron-nickel-cobalt alloy having an austenitic structure containing at least 20% nickel by weight, material number 1.3981, or an iron-nickel-cobalt alloy having UNS number N19909.

[0044] In the first and second embodiments of the pressure transducer 1 according to Figures 1 and 2, the pressure transducer 1 is in contact with the medium 2 in the area of ​​the wall opening 22 only via the diaphragm 12, so that hydrogen of the medium 2 has difficulty penetrating into the interior of the pressure transducer 1 and can accumulate there, at least the metallic material 30 of the diaphragm 12 consists of an iron-nickel-cobalt alloy with an austenitic structure containing at least 20% by weight of nickel, material number 1.3981, or an iron-nickel-cobalt alloy with UNS number N19909.

[0045] In the third and fourth embodiments of the pressure transducer 1 according to Figures 3 and 4, the pressure transducer 1 is in contact with the medium 2 in the area of ​​the wall opening 22 via the housing 1 and the diaphragm 12, and in order to make it more difficult for the hydrogen of the medium 2 to penetrate into the interior of the pressure transducer 1 and accumulate there, at least the metallic material 30 of the housing 11 and the diaphragm 12 is made from an austenitic structure containing at least 20% by weight of nickel, an iron-nickel-cobalt alloy with material number 1.3981, or an iron-nickel-cobalt alloy with UNS number N19909.

[0046] In the second and fourth embodiments of the pressure transducer 1 according to figures 2 and 4, the diaphragm 12 has a coating 18. The coating 18 reduces the permeability of the diaphragm 12 to the hydrogen of the medium 2. Preferably, the coating 18 is applied to the face of the diaphragm 12 facing the medium 2. The coating 18 therefore prevents direct contact between the diaphragm 12 and the medium 2. Thus, hydrogen cannot even reach the diaphragm 12.

[0047] The coating 18 is significantly thinner than the diaphragm thickness 122. Preferably, the thickness of the coating 18 is at most 10% of the diaphragm thickness 122. Preferably, the thickness of the coating 18 is in the range of 1 μm to 5 μm. Thus, the thermal expansion coefficient α of the pressure transducer 1 is 30 and yield strength R P0.2 is primarily determined by the metallic material 30 of the at least one metallic component 11 , 12 , 16 , 17 .

[0048] Coating 18 includes oxides, carbides, nitrides, etc. For example, coating 18 can include aluminum oxide, aluminum carbide, aluminum nitride, chromium oxide, chromium nitride, erbium oxide, silicon oxide, silicon carbide, silicon nitride, titanium oxide, titanium carbide, titanium nitride, zirconium oxide, rare earth carbides, rare earth nitrides, rare earth oxides, etc.

[0049] Preferably, the coating 18 comprises aluminum oxide. Aluminum oxide is known in the industry as a chemically inert material. Moreover, aluminum oxide is relatively inexpensive compared to rare earths or zirconium. In contrast to gold, which is also almost chemically inert and has a Vickers hardness of less than 100 HV10, aluminum oxide has a Vickers hardness of more than 1500 HV10 and therefore, as coating 18 of material 30, shows increased mechanical resistance compared to gold coatings. By Vickers hardness is meant the Vickers hardness at a test load of 10 kilopounds, the so-called HV10. Tests of Vickers hardness are described in the standards DIN EN ISO 6507-1:2018 to DIN EN ISO 6507-4:2018.

[0050] Preferably, the coating 18 is made of titanium carbide, which is widely used in the industrial field and is known as a good and almost chemically inert material. Titanium carbide has a Vickers hardness of more than 2500 HV10 and therefore, by way of comparison, as the coating 18 of the metallic material 30, it exhibits a higher mechanical resistance than a gold coating.

[0051] Preferably, the diaphragm 12 has an adhesion promoter layer 19. The adhesion promoter layer 19 is provided between the metallic material 30 and the coating 18. As a result, the temperature-induced mechanical stress is divided into a first boundary layer between the metallic material 30 and the adhesion promoter layer 19 and a further boundary layer between the adhesion promoter layer 19 and the coating 18. Thus, the temperature-induced mechanical stress is reduced and delamination and cracking of the coating 18 of the metallic material 30 is prevented. The adhesion promoter layer 19 is a metal having a high affinity for oxygen, such as, for example, a refractory metal, aluminum, a rare earth metal, etc. Refractory metals include titanium, vanadium, chromium, zirconium, niobium, hafnium, tantalum, molybdenum, tungsten, etc.

[0052] Preferably, the adhesion promoter layer 19 is composed of at least 90% by weight of zirconium or tungsten. Zirconium or tungsten can be easily applied as a coating.

[0053] Preferably, the coating 18 is composed of non-stoichiometric alumina (1-y)Al-yAlO x (0 < x ≦ 1.5 and 0 ≦ y ≦ 1). The coefficient of thermal expansion α of the non-stoichiometric aluminum oxide coating 18 18 is adjustable. Preferably, the coefficient of thermal expansion of the coating 18 is substantially the same as the coefficient of thermal expansion α of the metal material 30 30 . This prevents delamination and cracking of the coating 18 under thermal stress. In this case, an adhesion promoter layer is not necessary.

[0054] Preferably, the non-stoichiometric alumina (1-y)Al-yAlO x (where 0 < x ≦ 1.5 and 0 ≦ y ≦ 1) of the coating 18 shows a gradient within the coating 18. The ratio y gradually increases within the coating 18 as the distance from the metal material 30 increases, and the ratio x also gradually increases within the coating 18 as the distance from the metal material 30 increases.

[0055] Preferably, the non-stoichiometric alumina (1-y)Al-yAlO x (0 < x ≦ 1.5 and 0 ≦ y ≦ 1) of the coating 18 shows a gradient within the coating 18 where the ratio y becomes equal to 1 at a defined distance from the metal material 30, and the ratio x becomes equal to 1.5 at a defined distance from the metal material 30, and the non-stoichiometric alumina changes to stoichiometric Al2O3.

Explanation of Reference Numerals

[0056] 1 Pressure transducer 2 Medium 10 Longitudinal axis 11 Housing 12 Diaphragm 13 Transducer element 14 Measurement line 16 Preload base 17 Preload sleeve 18 Coating 19 Adhesion promoters 20 Measurement chamber 21 Measurement chamber wall 22 Wall opening 23 Sealing surface 24 Sealing elements 30 Metal materials 31 Average particle size 40 Environment 111 Inside 121 Material closure 122 Diaphragm Thickness 171 Material closure 172 Thickness of preload sleeve α 13 , α 18 , α 30 Thermal expansion coefficient M Measurement P2, P 40 pressure R P0.2 yield strength T1, T2, T 40 temperature

Claims

1. The pressure of the liquid or gas medium (2) (P 2 A pressure transducer (1) for measuring a pressure The medium (2) contains hydrogen and is placed in a measuring chamber (20); The pressure transducer (1) is placed in contact with a measurement chamber (20) and is exposed to temperatures of up to 350° C. (T 1 ) permanently exposed to The pressure transducer (1) has a diaphragm (12) and a transducer element (13), and the transducer element (13) has a 2.0×10 -6 K -1 ~7.5 x 10 -6 K -1 and having a thermal expansion coefficient of The diaphragm (12) protects the transducer elements (13) from direct contact with the medium (2); The pressure (P 2 ) acts on the transducer element (13) through the diaphragm (12), and the transducer element (13) detects the pressure (P 2 ) generating a measurement (M) under the influence of The diaphragm (12) is 9.0 x 10 -6 K -1 The following thermal expansion coefficients (α 30 The pressure transducer (1) is made of a metal material (30) having a A pressure transducer (1), characterized in that the metallic material (30) has an average grain size (31) of less than 20 μm.

2. 2. A pressure transducer (1) according to claim 1, characterized in that the metallic material (30) has an austenitic structure containing at least 20% by weight of nickel.

3. The metal material (30) is an iron-nickel-cobalt alloy with material number 1.3981, and has a melting point of 5.2×10 in the temperature range of 20 to 400° C. -6 K -1 The average thermal expansion coefficient (α 30 3. A pressure transducer (1) according to claim 1 or 2, characterized in that it comprises a pressure transducer (1) having a pressure sensor (1) and a pressure sensor (1) for detecting a pressure change in the pressure sensor.

4. The metallic material (30) is an iron-nickel-cobalt alloy with UNS number N19909, and has a melting point of 7.7×10 in the temperature range of 20 to 450° C. -6 K -1 The average thermal expansion coefficient (α 30 3. A pressure transducer (1) according to claim 1 or 2, characterized in that it comprises a pressure transducer (1) having a pressure sensor (1) and a pressure sensor (1) for detecting a pressure change in the pressure sensor.

5. The metal material (30) is an iron-nickel-cobalt alloy with UNS number N19909, and has a yield strength (R) of 1000 MPa or more. P0.2 3. A pressure transducer (1) according to claim 1 or 2, characterized in that it comprises a pressure transducer (1) having a pressure sensor (1) and a pressure sensor (1) for detecting a pressure change in the pressure sensor.

6. The measuring chamber (20) comprises a measuring chamber wall (21), The pressure transducer (1) is arranged in a wall opening (22) in a measuring chamber wall (21), The medium (2) can be subjected to a pressure of up to 1000 bar (P 2 ) and The pressure transducer (1) detects the ambient pressure (P 40 ) is disposed in an environment (40) of approximately 1 bar; The pressure transducer (1) comprises a housing (11), The housing (11) and the diaphragm (12) are connected via a material closure (121), 3. The pressure transducer (1) according to claim 1 or 2, characterized in that the housing (11) and the diaphragm (12) seal in a sealed manner against the wall opening (22) via the material closing portion (121) an interior (111) of the housing (11), in which the transducer element (13) is arranged.

7. the pressure transducer (1) is in contact with the medium (2) in the area of ​​the wall opening (22) only via the diaphragm (12); 7. A pressure transducer (1) according to claim 6, characterized in that at least said diaphragm (12) is made of said metallic material (30).

8. a sealing surface (23) sealingly closes the wall opening (22) against said environment (40); 8. The pressure transducer (1) according to claim 7, characterized in that the sealing surface (23) is arranged between the measuring chamber wall (21) and the diaphragm (12).

9. the pressure transducer (1) is in contact with the medium (2) in the area of ​​the wall opening (22) via the housing (11) and the diaphragm (12); 7. A pressure transducer (1) according to claim 6, characterized in that both the housing (11) and the diaphragm (12) are made of the metallic material (30).

10. a sealing surface (23) sealing the wall opening (22) from the environment (40); 10. The pressure transducer (1) according to claim 9, characterized in that the sealing surface (23) is arranged between the measuring chamber wall (21) and the housing (11).

11. The diaphragm (12) has a diaphragm thickness (122) of 150 μm or less; 7. The pressure transducer (1) of claim 6, characterized in that the diaphragm thickness (122) is more than eight times the average grain size (31) of the metallic material (30) and a corresponding large number of grain boundaries along the diaphragm thickness (122) make it more difficult for hydrogen of the medium (2) to penetrate and accumulate in the interior (111) of the housing (11).

12. 7. The pressure transducer (1) according to claim 6, characterized in that the housing (11) and / or the diaphragm (12) have a coating (18) for reducing the permeability of the medium (2) to hydrogen, the coating (18) comprising aluminium oxide or titanium carbide.

13. 13. The pressure transducer (1) according to claim 12, characterized in that the diaphragm (12) has an adhesion promoter layer (19) applied between the metal material (30) of the diaphragm (12) and the coating (18).

14. The transducer element (13) is preloaded between a preload base (16) and a preload sleeve (17); 3. The pressure transducer (1) according to claim 1 or 2, characterized in that the preload base (16) and the preload sleeve (17) are made of a metallic material (30).

15. The pressure of the liquid or gas medium (2) (P 2 A method for manufacturing a pressure transducer (1) for measuring a pressure The medium (2) contains hydrogen and is placed in a measuring chamber (20); The pressure transducer (1) comprises a diaphragm (12) and a transducer element (13); The pressure transducer (1) measures the pressure (P 2 ) at a maximum temperature of 350°C (T 1 ), the diaphragm (12) protects the transducer element (13) from direct contact with the medium (2), and transmits the pressure (P 2 ) acts on the transducer element (13), and the pressure (P 2 ) and the transducer element (13) produces a measurement (M) under the influence of 2.0×10 -6 K -1 ~7.5 x 10 -6 K -1 and having a thermal expansion coefficient of The manufacturing method comprises: 9.0 x 10 -6 K -1 The following thermal expansion coefficients (α 30 The method includes providing a metal material (30) having a grain refinement step of refining the crystal grains of the metal material (30), the average grain size (31) of the metal material (30) being less than 20 μm after the grain refinement; manufacturing the diaphragm (12) from the finely divided metal material (30); A manufacturing method comprising the steps of:

Citation Information

Patent Citations

  • Capacity type sensor

    JP1980016228A

  • Pressure sensor and its manufacturing method

    JP2008070241A

  • Pressure sensor and manufacturing method thereof

    JP2013036935A

  • Differential pressure transmitter

    JP2013190325A

  • Physical quantity measurement device and method for manufacturing same, and physical quantity measurement element

    WO2018163632A1