Cover window for flexible display device and flexible display device
A cover window for flexible display devices with a thin first coating layer and polysiloxane second layer addresses the challenge of balancing flexibility and hardness, ensuring durability through repeated bending and folding operations, suitable for flexible mobile devices.
Patent Information
- Application Number
- JP2023518342
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-08-18
- Filing Date
- 2021-08-23
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2041-08-23
AI Technical Summary
Existing cover windows for flexible display devices face challenges in achieving a balance between flexibility and high hardness, leading to issues such as cracking and peeling, especially with repeated bending and folding operations, and they are not suitable for replacing glass in terms of durability and aesthetics.
A cover window for flexible display devices is designed with a thin first coating layer of 200 μm or less on a light-transmitting substrate, paired with a second coating layer containing polysiloxane with two or more different structures, which enhances flexibility and hardness without adhesive layers, allowing for repeated bending and folding without significant damage.
The cover window exhibits high hardness and flexibility, minimizing damage from external impacts and maintaining structural integrity even after 200,000 folding cycles, making it suitable for bendable, flexible, or foldable mobile devices.
Smart Images

Figure 0007556187000006 
Figure 0007556187000005 
Figure 0007556187000004
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority based on Korean Patent Application No. 10-2020-0155895 filed on November 19, 2020, and Korean Patent Application No. 10-2021-0108808 filed on August 18, 2021, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference.
[0002] The present invention relates to a cover window for a flexible display device and a flexible display device. [Background technology]
[0003] Recently, with the development of mobile devices such as smartphones and tablet PCs, there is a demand for thinner and slimmer display substrates. Glass or tempered glass, which has excellent mechanical properties, is generally used for the display windows or front panels of such mobile devices. However, glass itself is a cause of the weight of the mobile device, and there is a problem of breakage due to external impact.
[0004] For this reason, plastic resins have been researched as a material that can replace glass. Plastic resin films are lightweight and less likely to break, which fits the trend toward lighter mobile devices. In particular, in order to achieve a film with high hardness and abrasion resistance, a film in which a hard coat layer made of a plastic resin is coated on a supporting substrate has been proposed.
[0005] One method for improving the surface hardness of the hard coat layer is to increase its thickness. In order to ensure a surface hardness sufficient to replace glass, it is necessary to achieve a certain thickness of the hard coat layer. However, as the thickness of the hard coat layer increases, the surface hardness increases, but wrinkles and curls increase due to the cure shrinkage of the hard coat layer, and cracks and peeling of the hard coat layer occur easily, making this method difficult to apply in practice.
[0006] Meanwhile, displays that are partially bent or bend flexibly for aesthetic and functional reasons have been attracting attention recently, and this trend is particularly noticeable in mobile devices such as smartphones and tablet PCs. However, glass is not suitable for use as a cover plate to protect such flexible displays, so a plastic resin or other alternative is necessary. However, this poses the difficulty of manufacturing a film that has sufficient flexibility while exhibiting high hardness at the same level as glass. Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention provides a cover window for a display device that is easily applicable to bendable, flexible, rollable, or foldable mobile devices or display devices, etc., with little damage to the film even when subjected to repeated bending or folding operations.
[0008] The present invention also provides a flexible display device including the cover window. [Means for solving the problem]
[0009] The present specification provides a cover window for a flexible display device, comprising: a light-transmitting substrate; a first coating layer formed on one side of the light-transmitting substrate and having a thickness of 200 μm or less; and a second coating layer formed on another side of the light-transmitting substrate opposite the first coating layer, the second coating layer comprising polysiloxane having two or more repeat units having different structures.
[0010] The present disclosure also provides a flexible display device including a cover window of the flexible display device.
[0011] Hereinafter, a cover window of a flexible display device and a flexible display device according to specific embodiments of the present invention will be described in more detail.
[0012] In this specification, "flexible" refers to a state in which the material has flexibility to the extent that no cracks of 3 mm or more in length occur when wound around a cylindrical mandrel with a diameter of 3 mm. For example, after placing the cover window of the flexible display device horizontally with the bottom, the interval between the folded parts in the middle of the first coating layer is mm, and both sides of the first coating layer are folded and unfolded 90 degrees to the bottom surface 200,000 times at 25°C at a speed of 1 time per second, and no cracks of 1 cm or more or 1 mm or more are generated, and the state where substantially no cracks are generated. Thus, the flexible display device of the present invention may refer to a bendable, flexible, rollable, or foldable display device.
[0013] However, this is presented as one example of the invention, and does not limit the scope of the invention. It will be obvious to those skilled in the art that various modifications to the embodiments are possible within the scope of the invention.
[0014] Unless otherwise expressly stated herein, the terminology used is for the purpose of referring to particular embodiments only and is not intended to be limiting of the invention.
[0015] As used herein, the singular forms "a," "an," and "the" include the plural forms unless the context clearly dictates to the contrary.
[0016] As used herein, the meaning of "comprising" is to embody certain features, regions, integers, steps, operations, elements, components and / or components, and does not exclude the presence or addition of other certain features, regions, integers, steps, operations, elements, components and / or groups.
[0017] In this specification, the term "(meth)acrylate" is intended to include both methacrylate and acrylate.
[0018] In the present specification, the weight average molecular weight means the weight average molecular weight in terms of polystyrene measured by the GPC method. In the process of measuring the weight average molecular weight in terms of polystyrene measured by the GPC method, a commonly known analyzer, a detector such as a refractive index detector, and an analytical column can be used, and commonly applied temperature conditions, solvents, and flow rates can be applied. Specific examples of the measurement conditions include a Waters 2695 instrument, an evaluation temperature of 40°C, THF solvent, and a flow rate of 1 mL / min.
[0019] According to one embodiment of the invention, there is provided a cover window for a flexible display device, comprising: a light-transmitting substrate; a first coating layer formed on one surface of the light-transmitting substrate and having a thickness of 200 μm or less; and a second coating layer formed on another surface of the light-transmitting substrate opposite to the first coating layer, the second coating layer comprising polysiloxane having two or more repeat units having different structures.
[0020] The present inventors have conducted research into a cover window applicable to a flexible display device having a thinner thickness, and have confirmed that a cover window for a flexible display device having a laminated structure including a second coating layer including polysiloxane including two or more repeating units having different structures on another surface of a light-transmitting substrate having a first coating layer having a thickness of 200 μm or less can simultaneously achieve a balance of physical properties of flexibility and high hardness while ensuring element stability with excellent impact resistance and pressure resistance, thereby completing the invention.
[0021] More specifically, the cover window of the flexible display device does not generate cracks of 3 mm or more in length when wound around a cylindrical mandrel with a diameter of 3 mm, and the film is substantially undamaged even when repeatedly bent or folded. Therefore, the cover window of the flexible display device can be easily applied to bendable, flexible, rollable, or foldable mobile devices or display devices using the same.
[0022] The cover window of the flexible display device may have physical properties that can replace tempered glass, etc., and therefore may not be broken by pressure or force applied from the outside, and may have properties that allow it to be sufficiently bent and folded.
[0023] As described above, the physical properties such as bending durability and surface hardness of the cover window of the flexible display device are achieved by forming a first coating layer having a thickness of 200 μm or less on one side of the light-transmitting substrate; and a second coating layer which is formed on the other side of the light-transmitting substrate opposite the first coating layer and contains polysiloxane containing two or more repeating units having different structures.
[0024] Specifically, the cover window of the flexible display device according to the embodiment has a laminated structure including: a first coating layer formed on one side of the light-transmitting substrate and having a thickness of 200 μm or less; and a second coating layer formed on the other side of the light-transmitting substrate opposite the first coating layer and including polysiloxane having two or more repeating units having different structures; and thus does not need to include an adhesive layer.
[0025] In the case of cover windows of conventional flexible display devices, in order to ensure impact resistance when applied to a display device or to improve surface hardness and pressure characteristics when installed in a display device, an adhesive layer of a certain thickness was formed, or an adhesive layer such as an adhesive or adhesive film was formed together with a hard coat layer.
[0026] Unlike the cover window of a conventional flexible display device, the cover window of the flexible display device of the present embodiment does not include an adhesive layer, thereby enabling a thinner flexible display device to be realized. Even if a thin first coating layer having a thickness of 200 μm or less is included, excellent compression characteristics can be achieved, and damage due to external impact can be minimized.
[0027] Specifically, the cover window of the flexible display device of the embodiment may include a first coating layer having a thickness of 200 μm or less, 10 μm to 200 μm, 10 μm to 100 μm, or 10 μm to 60 μm.
[0028] As described above, the cover window of the flexible display device according to the embodiment has a laminated structure including a first coating layer formed on one side of the light-transmitting substrate and having a thickness of 200 μm or less; and a second coating layer formed on another side of the light-transmitting substrate opposite the first coating layer and including polysiloxane having two or more repeating units having different structures. This makes it possible to achieve excellent compression characteristics even with a thin first coating layer having a thickness of 200 μm or less, and minimize damage due to external impact.
[0029] Meanwhile, when the cover window of the flexible display device according to the embodiment is folded and unfolded 200,000 times at a speed of once per second at room temperature at an angle of 90° so that the first coating layer faces the first coating layer with an interval of 8 mm in between, no cracks of 1 mm or more are generated, and the film is hardly damaged even by repeated bending and folding operations, and the cover window of the flexible display device according to the embodiment can be easily applied to the cover window of a bendable, flexible, rollable, or foldable mobile device or display device.
[0030] FIG. 1 is a diagram showing a schematic diagram of a method for evaluating dynamic bending properties.
[0031] Referring to FIG. 1, the bending durability can be measured by placing the cover window of the flexible display device horizontally with the bottom, folding the first coating layer at the center of the first coating layer at an interval of mm, and folding and unfolding both sides of the first coating layer at 90 degrees with respect to the bottom 200,000 times at a speed of once per second at 25° C. In order to keep the interval of the folded parts constant, for example, the first coating layer can be placed against a rod with a diameter of (R) mm, the remaining part of the first coating layer can be fixed, and both sides of the first coating layer can be folded and unfolded repeatedly around the rod. The folded part is not particularly limited as long as it is within the first coating layer, and for the convenience of measurement, the center part of the first coating layer is folded so that both sides of the remaining first coating layer excluding the folded part are symmetrical.
[0032] In the dynamic bending characteristic evaluation, the cover window of the flexible display device did not have any cracks of 1 cm or more or 1 mm or more even after 200,000 bendings, and thus was substantially free of cracks. Therefore, the possibility of cracks occurring even in actual use conditions such as repeated folding, rolling, and bending is very low, and the flexible display device can be suitably used for the cover window of the flexible display device.
[0033] Meanwhile, the cover window of the flexible display device according to the embodiment may include a functional layer having a thickness of 10 μm to 300 μm formed on one surface of the second coating layer formed on the other surface of the light-transmitting substrate to face the first coating layer.
[0034] In the cover window of the flexible display device according to the embodiment, the type of the functional layer is not limited to a specific type, and various functional layers applicable to the flexible display device may be applied. Specifically, the functional layer may be any one of a black matrix film, a polarizing film, an ultraviolet blocking film, a release film, and a conductive film.
[0035] In the cover window of the flexible display device according to the embodiment, the functional layer may have a thickness of 10 μm to 300 μm, 10 μm to 100 μm, or 3 μm to 30 μm.
[0036] If the thickness of the functional layer exceeds 300 μm, the flexibility decreases and it may be difficult to form a flexible film.
[0037] The cover window of the flexible display device of the embodiment may have a maximum hardness of 2B or more, 2B to 5H, B to 5H, or B to HB, measured using a pencil hardness tester according to measurement standard JIS K5400 on the surface of the first coating layer immediately after a functional layer of 10 μm to 300 μm is formed on one side of the second coating layer formed on the other side of the light-transmitting substrate so as to face the first coating layer.
[0038] In the cover window of the flexible display device according to the embodiment, immediately after a functional layer having a thickness of 10 μm to 300 μm is formed on one side of the second coating layer formed on the other side of the light-transmitting substrate so as to face the first coating layer, the surface of the first coating layer is measured using a pencil hardness tester and has a maximum hardness of 2B or more at which no pressure is generated along the path of a pencil according to the measurement standard JIS K5400. This provides excellent pressure resistance, and the film is hardly damaged even when repeatedly bent or folded, thereby providing element stability. Therefore, the cover window of the flexible display device and the bendable, flexible, rollable, or foldable mobile device or display device using the same can be easily applied.
[0039] Specifically, in the cover window of the flexible display device, the second coating layer may include a polysiloxane including two or more repeating units having different structures, more specifically, the second coating layer may include a polysiloxane including two or more types of repeating units substituted with a crosslinkable functional group.
[0040] The second coating layer includes polysiloxane including two or more repeating units substituted with a crosslinkable functional group, and the cage-type polysiloxane repeating unit can increase the curing density to achieve high hardness, and the ladder-type polysiloxane repeating unit can improve the flexibility of the cured film due to its flexible molecular structure. As a result, the cover window of the flexible display device according to the embodiment can exhibit a balance of physical properties of high flexibility and high hardness.
[0041] The polysiloxane may have a variety of structures, for example, a cage-type polysiloxane repeating unit, a ladder-type polysiloxane repeating unit, or a random-type polysiloxane repeating unit.
[0042] The cover window of the flexible display device according to the embodiment includes a polysiloxane including two or more repeat units having different structures, and thus may include a cage-type polysiloxane repeat unit and a ladder-type polysiloxane repeat unit, a cage-type polysiloxane repeat unit and a random-type polysiloxane repeat unit, a ladder-type polysiloxane repeat unit and a random-type polysiloxane repeat unit, or all of a cage-type polysiloxane repeat unit, a ladder-type polysiloxane repeat unit, and a random-type polysiloxane repeat unit.
[0043] More specifically, the polysiloxane containing two or more repeating units having different structures can contain a cage-type polysiloxane repeating unit substituted with a crosslinkable functional group and a ladder-type polysiloxane repeating unit substituted with a crosslinkable functional group.
[0044] In the cover window of the flexible display device of the embodiment, the second coating layer includes both the cage-type polysiloxane repeating unit and the ladder-type polysiloxane repeating unit. Compared with a case where only one type of polysiloxane repeating unit, either the cage-type polysiloxane repeating unit or the ladder-type polysiloxane repeating unit, the cage type having a relatively small molecular weight increases the curing density and increases the hardness, and the linear ladder-type polysiloxane is widely distributed during the formation of the cured network, thereby increasing the flexibility and toughness. As a result, the cover window of the flexible display device of the embodiment can exhibit a balance of physical properties of high flexibility and high hardness.
[0045] In addition, the molar ratio of the cage-type polysilsesquioxane repeating unit to the ladder-type polysilsesquioxane repeating unit may be 1.2 to 2.5, 1.2 to 2.0, 1.2 to 1.8, or 1.4 to 1.8. The molar ratio of 1.2 to 2.5 allows the cage and ladder types to be well balanced in the composition, and the cover window can exhibit a balance of high flexibility and high hardness properties. Specifically, the cage-type polysilsesquioxane structure increases the curing density to achieve high hardness, and the ladder-type polysilsesquioxane structure improves the flexibility of the cured film due to its flexible molecular structure, so that the cage-type polysilsesquioxane repeating unit and the ladder-type polysilsesquioxane repeating unit are contained in the specific ratio, thereby simultaneously achieving high flexibility and high hardness properties.
[0046] In the FT-IR (Fourier Transform-Infra Red) spectrum measured by the attenuated total reflection (ATR) method for the polysiloxane containing two or more repeating units having different structures, -1 ~1070cm -1At least one peak in the region of 1075 cm -1 ~1130cm -1 The spectrum may have at least one peak in the region of
[0047] For example, in the FT-IR spectrum, -1 ~1070cm -1 , 1030cm -1 ~1065cm -1 or 1040cm -1 ~1060cm -1 At least one peak can be shown in the region of 1075 cm -1 ~1130cm -1 , 1080cm -1 ~1110cm -1 or 1090cm -1 ~1100cm -1 At least one peak can be shown in the region of
[0048] By having peaks in two or more different regions in the FT-IR spectrum by the ATR method, the polysiloxane contained in the second coating layer of the cover window of the flexible display device may contain two or more repeating units having different structures.
[0049] Specifically, the 1010 cm -1 ~1070cm -1 The region may show two or more peaks or only one peak, and the 1010 cm -1 ~1070cm -1 The peak appearing in the region of 1075 cm may be a peak related to the ladder-type polysiloxane. -1 ~1130cm -1 The region may show two or more peaks or only one peak, and the 1075 cm -1 ~1130cm -1 The peak appearing in the region may be a peak related to the cage-type polysiloxane.
[0050] Furthermore, the 1010 cm -1 ~1070cm -1 The intensity (I1) of the peak having the greatest intensity among at least one peak appearing in the 1075 cm -1 ~1130cm -1 The peak intensity ratio (I2 / I1) of the intensity (I2) of the peak with the greatest intensity among at least one peak appearing in this region may be 1.2 or more and 2.5 or less, 1.2 or more and 2.0 or less, 1.2 or more and 1.8 or less, or 1.4 or more and 1.8 or less.
[0051] The intensity of the peak (I1) is the 10 -1 ~1070cm -1 When two or more peaks appear in the region, it means the intensity of the peak with the greatest intensity, and when one peak appears, it means the intensity of that peak. In addition, the intensity of the peak (I2) is the intensity of the peak at 1075 cm -1 ~1130cm -1 When two or more peaks appear in the region, it means the intensity of the peak with the greatest intensity, and when one peak appears, it means the intensity of that peak.
[0052] The peak intensity ratio (I2 / I1) can be measured by an FT-IR spectrum using an ATR method, using polysiloxane in an uncured state before undergoing a curing step or in a solid phase after curing as a sample.
[0053] When the peak intensity ratio (I2 / I1) is 1.2 to 2.5, a composition can be formed with a good balance of cage and ladder types, and the cover window can exhibit a balance of physical properties of high flexibility and high hardness. When the peak intensity ratio (I2 / I1) is less than 1.2 or exceeds 2.5, the flexibility is poor and the hardness is also reduced, and physical properties sufficient for use in a cover window of a flexible display device may not be achieved.
[0054] Meanwhile, the crosslinkable functional group may include any one selected from the group consisting of an alicyclic epoxy group and a functional group represented by the following Chemical Formula 1: [Chemical formula 1] [ka] In the above formula 1, R a represents a substituted or unsubstituted alkylene group having 1 to 6 carbon atoms, a substituted or unsubstituted alkenylene group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynylene group having 2 to 20 carbon atoms, -R b -CH=CH-COO-R c -, -R d -OCO-CH=CH-R e -, -R f OR g -, -R h COOR i -, or -R j OCOR k - and R b ~R k are each independently a single bond, or a substituted or unsubstituted alkylene group having 1 to 6 carbon atoms.
[0055] The functional group represented by Chemical Formula 1 contains an epoxy group, which not only improves the hardness and scratch resistance of the cover window of a flexible display device, but also causes little damage to the film even when repeatedly bent or folded, making it easily applicable to bendable, flexible, rollable, or foldable mobile devices or display devices.
[0056] For example, the functional group represented by the formula 1 is R a is methylene, ethylene, propylene, arylene, -R b -CH=CH-COO-R c -, -R d -OCO-CH=CH-R e -, -R f OR g -, -R h COOR i -, or -R j OCOR k For example, in the above formula 1, R b ~R kmay be a single bond, methylene, ethylene, propylene or butylene. For example, R a is methylene, ethylene, or -R f OR g In this case, R f and R g may be a direct bond, methylene or propylene. For example, the functional group represented by Chemical Formula 1 may be, but is not limited to, a glycidoxy group, a glycidoxyethyl group, a glycidoxypropyl group, a glycidoxybutyl group, etc.
[0057] The alicyclic epoxy group is not limited thereto, but may be, for example, an epoxycyclohexyl group, an epoxycyclopentyl group, or the like.
[0058] In other words, the polysiloxane repeating unit substituted with the crosslinkable functional group has a T3 unit represented by (R 1 SiO 3 / 2 ) silsesquioxane units.
[0059] The above (R 1 SiO 3 / 2 In the silsesquioxane structural unit of 1 may be a crosslinkable functional group. 1 may be any one selected from the group consisting of an alicyclic epoxy group and a functional group represented by the following Chemical Formula 1: [Chemical formula 1] [ka] In the above formula 1, R a represents a substituted or unsubstituted alkylene group having 1 to 6 carbon atoms, a substituted or unsubstituted alkenylene group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynylene group having 2 to 20 carbon atoms, -R b -CH=CH-COO-R c -, -R d -OCO-CH=CH-R e -, -R f ORg -, -R h COOR i -, or -R j O.C.O.R. k - and R b ~R k may each independently be a single bond, or a substituted or unsubstituted alkylene group having 1 to 6 carbon atoms.
[0060] More specifically, in the above formula 1, R a is methylene, ethylene, propylene, arylene, -R b -CH=CH-COO-R c -, -R d -OCO-CH=CH-R e -, -R f OR g -, -R h COOR i -, or -R j O.C.O.R. k In this case, the R b ~R k may each independently be a single bond or a substituted or unsubstituted alkylene group having 1 to 6 carbon atoms, more specifically, may be a single bond or a linear alkylene group having 1 to 6 carbon atoms such as methylene, ethylene, propylene, butylene, etc. Even more specifically, the R a is methylene, ethylene, or -R f OR g In this case, R f and R g may be a direct bond or a linear alkylene group having 1 to 6 carbon atoms such as methylene, propylene, and the like.
[0061] When considering the surface hardness and curability improvement effect of the cured product, 1 may be a glycidyl group or a glycidoxypropyl group.
[0062] In addition, the R aWhen substituted, specifically, it may be substituted with one or more substituents selected from the group consisting of an alkyl group having 1 to 12 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, a hydroxy group, an alkoxy group having 1 to 12 carbon atoms, an amino group, an acryl group (or an acryloyl group), a methacryl group (or a methacryloyl group), an acrylate group (or an acryloyloxy group), a methacrylate group (or a methacryloyloxy group), a halogen group, a mercapto group, an ether group, an ester group, an acetyl group, a formyl group, a carboxyl group, a nitro group, a sulfonyl group, a urethane group, an epoxy group, an oxetanyl group, and a phenyl group, or more specifically, it may be substituted with one or more substituents selected from the group consisting of an alkyl group having 1 to 6 carbon atoms such as methyl, ethyl, etc.; an acryl group; a methacryl group; an acrylate group; a methacrylate group; a vinyl group; an allyl group; an epoxy group; and an oxetanyl group.
[0063] The polysiloxane may be the above-mentioned (R 1 SiO 3 / 2 ) silsesquioxane unit and (R 2 SiO 3 / 2 The silsesquioxane unit (R 2 SiO 3 / 2 The silsesquioxane unit of the polysiloxane can increase the curing density of the polysiloxane and improve the surface hardness properties of the coating layer.
[0064] The above (R 2 SiO 3 / 2 In the silsesquioxane structural unit of 2 Specifically, may be selected from the group consisting of a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 12 carbon atoms, a substituted or unsubstituted aryl group having 6 to 12 carbon atoms, a substituted or unsubstituted arylalkyl group having 7 to 12 carbon atoms, a substituted or unsubstituted alkylaryl group having 7 to 12 carbon atoms, an epoxy group, an oxetanyl group, an acrylate group, a methacrylate group, and a hydrogen atom.
[0065] In addition, the R 2 may be substituted with one or more substituents selected from the group consisting of an alkyl group having 1 to 12 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, a hydroxy group, an alkoxy group having 1 to 12 carbon atoms, an amino group, an acryl group, a methacryl group, an acrylate group, a methacrylate group, a halogen group, a mercapto group, an ether group, an ester group, an acetyl group, a formyl group, a carboxyl group, a nitro group, a sulfonyl group, a urethane group, an epoxy group, an oxetanyl group, and a phenyl group, or more specifically, may be substituted with one or more substituents selected from the group consisting of an acryl group, a methacryl group, an acrylate group, a methacrylate group, a vinyl group, an allyl group, an epoxy group, and an oxetanyl group.
[0066] Among these, the above-mentioned R 2 More specifically, R may be an alkyl group having 1 to 6 carbon atoms or a phenyl group having 6 carbon atoms, which may be substituted or unsubstituted with one or more substituents selected from the group consisting of an acrylic group, a methacrylic group, an acrylate group, a methacrylate group, a vinyl group, an allyl group, an epoxy group, and an oxetanyl group; an epoxy group; or an oxetanyl group. 2 may be an unsubstituted phenyl group or an epoxy group.
[0067] Meanwhile, in the present invention, the "epoxy group" refers to a functional group containing an oxirane ring, and unless otherwise specified, includes an unsubstituted epoxy group containing only an oxirane ring, an alicyclic epoxy group having 6 to 20 carbon atoms or 6 to 12 carbon atoms (e.g., epoxycyclohexyl, epoxycyclopentyl, etc.); and an aliphatic epoxy group having 3 to 20 carbon atoms or 3 to 12 carbon atoms (e.g., glycidyl group, etc.).
[0068] In the present invention, the term "oxetanyl group" refers to a functional group containing an oxetane ring, and unless otherwise specified, includes an unsubstituted oxetanyl group containing only an oxetane ring, an alicyclic oxetanyl group having 6 to 20 carbon atoms or 6 to 12 carbon atoms, and an aliphatic oxetanyl group having 3 to 20 carbon atoms or 3 to 12 carbon atoms.
[0069] The polysiloxane may also contain a structural unit of (OR). By containing the structural unit, it is possible to improve flexibility while maintaining excellent hardness properties. Specifically, R may be a hydrogen atom or an alkyl group having 1 to 12 carbon atoms, or more specifically, R may be a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, such as a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, or an isobutyl group.
[0070] Polysiloxanes containing the above-mentioned structural units can be produced by hydrolysis and condensation reactions of siloxane monomers of each structural unit, specifically, an alkoxysilane having an epoxyalkyl group alone, or between an alkoxysilane having an epoxyalkyl group and a different kind of alkoxysilane, and in this case, the molar ratio of each structural unit can be controlled by controlling the content ratio of the alkoxysilanes.
[0071] Meanwhile, in the cover window of the flexible display device according to the embodiment, the second coating layer may include an elastic polymer.
[0072] The inclusion of the elastic polymer in the second coating layer can impart stress resistance properties due to high toughness to the second coating layer, minimizing shrinkage during curing, thereby improving warpage properties and simultaneously improving flexibility such as bendability.
[0073] The elastic polymer may be an alkanediol having 1 to 20 carbon atoms, a polyolefin polyol, a polyester polyol, a polycaprolactone polyol, a polyether polyol, or a polycarbonate polyol, and any one or a mixture of two or more of these may be used. Compared to ordinary elastic polymers such as rubber, these elastic polymers can be crosslinked by UV irradiation, and can achieve high hardness and flexibility without reducing other physical properties. Among these, the elastic polymer may be polycaprolactone diol or polycarbonate diol, and in particular, the polycaprolactone diol is more preferable because it has an ester group and an ether group in the repeating unit, and is therefore more effective in terms of flexibility, hardness, and impact resistance when used in combination with two or more polysiloxanes substituted with the crosslinkable functional group.
[0074] The elastic polymer may have a number average molecular weight (Mn) of 500 to 10,000 Da, more specifically, 1,000 to 5,000 Da. When the number average molecular weight satisfies the condition, compatibility with other components increases, the surface hardness of the cured product increases, and the heat resistance and abrasion resistance of the cured product can be further improved.
[0075] In the cover window of the flexible display device according to the embodiment, the second coating layer may include 10 to 80 parts by weight, 10 to 75 parts by weight, 10 to 50 parts by weight, or 15 to 50 parts by weight of the elastic polymer, relative to 100 parts by weight of the polysiloxane including two or more repeating units having different structures.
[0076] The second coating layer includes 10 parts by weight to 80 parts by weight of the elastic polymer relative to 100 parts by weight of the polysiloxane including two or more repeating units having different structures, so that the cover window of the flexible display device according to the embodiment can achieve excellent optical properties and a balance of physical properties including flexibility and high hardness.
[0077] If the elastic polymer is contained in an amount of less than 10 parts by weight per 100 parts by weight of the polysiloxane containing two or more repeating units having different structures, a strong cured film cannot be formed, and technical problems may arise in that durability against repeated bending and folding operations is not sufficiently achieved.
[0078] If the elastomeric polymer is contained in an amount of more than 80 parts by weight per 100 parts by weight of the polysiloxane containing two or more repeating units having different structures, problems may occur in that the flexibility is reduced during curing, and partial uncuring occurs, resulting in reduced hardness.
[0079] Meanwhile, the first coating layer may include a (meth)acrylate resin or an epoxy resin.
[0080] Specifically, the epoxy resin may include a polysiloxane including two or more repeating units substituted with a crosslinkable functional group. The content relating to the polysiloxane including two or more repeating units substituted with a crosslinkable functional group includes all of the above.
[0081] On the other hand, the hard coat layer contains an epoxy resin, so that a strong cured film can be formed and durability against repeated bending and folding operations can be ensured. If the hard coat layer does not contain an epoxy resin, a technical problem may occur in that durability against repeated bending and folding operations is reduced.
[0082] The type of the epoxy resin is not particularly limited, but may include a bisphenol-based epoxy resin.
[0083] For example, the epoxy resin may include one or more selected from the group consisting of bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol A type novolac epoxy resin, and hydrogenated bisphenol A type epoxy resin. The epoxy resin includes a bisphenol-based epoxy resin, which is relatively straighter and harder than a silsesquioxane molecular structure, and therefore the molecular chain of the cured film also has excellent rigidity, a high Tg, and a low CTE value, and can achieve excellent durability against repeated bending and folding at high and low temperatures compared to the case where a linear epoxy resin such as a polyethylene glycol-based epoxy resin is included.
[0084] More specifically, the epoxy resin may have an epoxy equivalent of 120 g / eq or more and 600 g / eq or less, 120 g / eq or more and 550 g / eq or less, 150 g / eq or more and 550 g / eq or less, or 155 g / eq or more and 500 g / eq or less.
[0085] If the epoxy equivalent of the epoxy resin is less than 120 g / eq, there will be an excess of curable epoxy reactive groups, which may result in some parts remaining uncured during the curing reaction or the cured film becoming brittle, resulting in poor durability against repeated bending or folding at low temperatures. If the epoxy equivalent exceeds 600 g / eq, a technical problem may occur in which the optical properties of the hard coat layer are reduced.
[0086] The equivalent weight of such functional groups is the molecular weight of the epoxy resin divided by the number of epoxy functional groups, and can be analyzed by H-NMR or chemical titration.
[0087] The (meth)acrylate resin may contain a (co)polymer of one or more compounds selected from the group consisting of monofunctional or polyfunctional acrylate monomers and polyfunctional urethane acrylate oligomers.
[0088] Examples of the monofunctional or polyfunctional acrylate monomer include 2-ethylhexyl acrylate, octadecyl acrylate, isodecyl acrylate, 2-phenoxyethyl acrylate, lauryl acrylate, stearyl acrylate, behenyl acrylate, tridecyl methacrylate, nonylphenol ethoxylate monoacrylate, β-carboxyethyl acrylate, isobornyl acrylate, tetrahydrofurfuryl acrylate, tetrahydrofurfuryl methacrylate, 4-butylcyclohexyl acrylate, dicyclopentenyl acrylate, dicyclopentenyloxyethyl acrylate, ethoxyethoxyethyl acrylate, ethoxylated monoacrylate, 1,6-hexanediol diacrylate, triphenyl glycol diacrylate, butanediol diacrylate, 1,3-butylene glycol dimethacrylate, 1,6-Hexanediol dimethacrylate, neopentyl glycol diacrylate, ethylene glycol dimethacrylate, diethylene glycol diacrylate, diethylene glycol dimethacrylate, tetraethylene glycol diacrylate, tetraethylene glycol dimethacrylate, triethylene glycol diacrylate, triethylene glycol dimethacrylate, polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, dipropylene glycol diacrylate, ethoxylated neopentyl glycol diacrylate, trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, pentaerythritol triacrylate Examples of the acrylate monomer include pentaerythritol trimethacrylate, pentaerythritol tetramethacrylate, pentaerythritol tetraacrylate, ethoxylated triacrylate, tris(2-hydroxyethyl)isocyanurate triacrylate, dipentaerythritol pentaacrylate, ditrimethylolpropane tetraacrylate, and alkoxylated tetraacrylate. Preferred examples include acrylate monomers such as pentaerythritol triacrylate, pentaerythritol trimethacrylate, pentaerythritol tetramethacrylate, and pentaerythritol tetraacrylate. Any one or a mixture of two or more of these can be used.
[0089] In addition, when the multifunctional urethane acrylate oligomer is used in combination with the above-mentioned polysiloxane, the surface hardness improving effect may be significant. The urethane acrylate oligomer may have 6 to 9 functional groups. If the number of functional groups is less than 6, the hardness improving effect is slight, and if the number of functional groups is more than 9, the hardness is excellent but the viscosity may increase. Furthermore, the multifunctional urethane acrylate oligomer may be any one used in the relevant field without limitation, and preferably, it is prepared by reacting a compound having one or more isocyanate groups in the molecule with a (meth)acrylate compound having one or more hydroxyl groups in the molecule.
[0090] Additionally, in the cover window of the flexible display device according to an embodiment of the present invention, the first coating layer may also include an elastic polymer. When the first coating layer further includes an elastic polymer, shrinkage during hardening of the first coating layer may be minimized, and warpage characteristics and bending properties may be further improved.
[0091] In addition, when the first coating layer further includes an elastic polymer, the content of the elastic polymer included in the first coating layer and the second coating layer may be the same or different. Considering the excellent surface hardness characteristics, warpage characteristics, and flexibility improvement effects due to minimization of shrinkage in the lower coating layer in contact with the light-transmitting substrate, the cover window of the flexible display device according to an embodiment of the present invention may include a higher content of the elastic polymer in the second coating layer than in the first coating layer.
[0092] Meanwhile, in order to realize the above-mentioned characteristics, it is preferable that the cover window of the flexible display device includes a light-transmitting substrate that has excellent optical characteristics, satisfies a balance of physical properties such as flexibility and high hardness, and can prevent damage to the internal structure even when repeatedly bent or folded.
[0093] The type of the light-transmitting substrate is not particularly limited as long as it satisfies the above-mentioned characteristics, but for example, a glass substrate may be used, or the substrate may contain one or more resins selected from the group consisting of polyester-based resins, cellulose-based resins, polycarbonate-based resins, acrylic-based resins, styrene-based resins, polyolefin-based resins, polyimide-based resins, polyamideimide-based resins, polyethersulfone-based resins, and sulfone-based resins.
[0094] The light-transmitting substrate may have an elastic modulus of about 4 GPa or more, or about 5 GPa or more, or about 5.5 GPa, or about 6 GPa or more, or a modulus of elasticity of 4 GPa to 9 GPa.
[0095] If the elastic modulus of the light-transmitting substrate is less than 4 GPa, the cover window of the flexible display device may not achieve sufficient hardness, and if the elastic modulus of the light-transmitting substrate is more than 9 GPa, the cover window of the flexible display device may not have sufficient flexibility and elasticity.
[0096] As described above, it is usually possible to ensure flexibility in a thin film or optical laminate, but it is not easy to ensure durability against repeated bending and folding operations while ensuring high surface hardness.
[0097] In contrast, the cover window of the flexible display device of the above embodiment includes a first coating layer and a second coating layer that have high hardness together with the light-transmitting substrate having the above-mentioned characteristics, while ensuring durability against repeated bending and folding operations, and can have the above-mentioned characteristics.
[0098] Meanwhile, the cover window of the flexible display device satisfies a balance of physical properties, such as flexibility and high hardness, even in a thin thickness range, compared to cover windows of other previously known flexible display devices, and can prevent damage to the internal structure even when repeatedly bent or folded. The cover window of the flexible display device can have optical properties such as high transparency as well as high mechanical properties and heat resistance.
[0099] More specifically, the light-transmitting substrate may have a thickness of 5 μm to 100 μm, or 10 μm to 80 μm, or 20 μm to 60 μm. If the substrate is less than 5 μm thick, it may be prone to breakage or curling during the coating layer formation process, and it may be difficult to achieve high hardness. On the other hand, if the thickness exceeds 100 μm, it may be difficult to form a flexible film due to reduced flexibility.
[0100] The first coating layer may have a thickness of 200 μm or less, 10 μm to 200 μm, 10 μm to 100 μm, or 10 μm to 60 μm. If the thickness of the first coating layer is too large, the flexibility of the cover window of the flexible display device and durability against repeated bending and folding operations may be reduced.
[0101] The second coating layer may have a thickness of 5 μm to 200 μm, or 5 μm to 100 μm, or 10 μm to 80 μm, or 20 μm to 80 μm. If the thickness of the second coating layer is less than 5 μm, breakage or curling may occur during the coating layer formation process, and it may be difficult to achieve high hardness. On the other hand, if the thickness exceeds 100 μm, flexibility may decrease, making it difficult to form a flexible film.
[0102] In addition, the cover window of the flexible display device according to the embodiment may have a thickness of 80 μm to 350 μm, 80 μm to 300 μm, 80 μm to 250 μm, or 80 μm to 210 μm. That is, the thickness of the laminate including the second coating layer, the light-transmitting substrate, and the first coating layer may be 80 μm to 350 μm, 80 μm to 300 μm, 80 μm to 250 μm, or 80 μm to 210 μm. If the thickness of the cover window of the flexible display device is less than 80 μm, breakage or curling may occur during the coating layer formation process, and it may be difficult to achieve high hardness. On the other hand, if the thickness exceeds 350 μm, flexibility may decrease and it may be difficult to form a flexible film.
[0103] Furthermore, the cover window of the flexible display device may have a ratio of the thickness of the first coating layer to the thickness of the light-transmitting substrate of 0.1 to 2.0.
[0104] Specifically, the cover window of the flexible display device may have a ratio of the thickness of the first coating layer to the thickness of the light-transmitting substrate of 0.1 or more, 0.2 or more, 2.0 or less, 1.5 or less, 1.0 or less, or 0.5 or less, or 0.1 to 2.0, 0.1 to 1.5, 0.1 to 1.0, 0.2 to 1.0, or 0.2 to 0.5. The cover window of the flexible display device may have a ratio of the thickness of the first coating layer to the thickness of the light-transmitting substrate of 0.1 to 2.0, thereby suppressing the occurrence of breakage or curl during the coating layer formation process, achieving high hardness and at the same time achieving sufficient flexibility, thereby achieving a balance of physical properties of flexibility and high hardness at the same time.
[0105] In addition, the cover window of the flexible display device may have a ratio of a thickness of the second coating layer to a thickness of the first coating layer of 1.0 to 10.0.
[0106] Specifically, the cover window of the flexible display device may have a ratio of the thickness of the second coating layer to the thickness of the first coating layer of 1.0 or more, 2.0 or more, 4.0 or more, 10.0 or less, 8.0 or less, or 6.0 or less, or 2.0 to 10.0, 2.0 to 8.0, 4.0 to 8.0, or 4.0 to 6.0. The cover window of the flexible display device may have a ratio of the thickness of the second coating layer to the thickness of the first coating layer of 1.0 to 10.0, thereby suppressing the occurrence of breakage or curling during a coating layer formation process, achieving high hardness and at the same time achieving sufficient flexibility, thereby achieving a balance of physical properties of flexibility and high hardness at the same time.
[0107] Meanwhile, the cover window of the flexible display device may be provided by applying a coating composition for forming the first coating layer to one side of the light-transmitting substrate, photo-curing the coating composition, and then applying a coating composition for forming the second coating layer to another side of the light-transmitting substrate, and photo-curing the coating composition.
[0108] The method of applying the coating composition is not particularly limited as long as it can be used in the technical field to which the present technology belongs, and for example, a bar coating method, a knife coating method, a roll coating method, a blade coating method, a die coating method, a microgravure coating method, a comma coating method, a slot die coating method, a lip coating method, a solution casting method, etc. may be used.
[0109] The upper surface of the first coating layer or between the light-transmitting substrate or polymer substrate and the first coating layer may further include one or more layers, films, or the like, such as a plastic resin film, a release film, a conductive film, a conductive layer, a liquid crystal layer, a coating layer, a cured resin layer, a non-conductive film, a metal mesh layer, or a patterned metal layer.
[0110] For example, after forming an antistatic layer having conductivity on the substrate, a coating layer can be formed on the antistatic layer to provide an antistatic function, or a low refractive index layer can be introduced on the coating layer to provide a low reflection function.
[0111] The layer, film, or the like may be in any form such as a single layer, a double layer, or a laminated type. The layer, film, or the like may be laminated on the coating layer by laminating a freestanding film with an adhesive or a pressure-sensitive adhesive film, or by coating, deposition, sputtering, or the like, but the present invention is not limited thereto.
[0112] Meanwhile, the first coating layer and the second coating layer may additionally contain components commonly used in the technical field to which the present invention belongs, such as a photoinitiator, an organic solvent, a surfactant, a UV absorber, a UV stabilizer, an anti-yellowing agent, a leveling agent, an antifouling agent, a dye for improving color value, etc. Also, the content of the components is not particularly limited since it can be variously adjusted within a range that does not deteriorate the physical properties of the coating layer, but is, for example, about 0.01 to about 30 parts by weight per 100 parts by weight of the coating layer.
[0113] The surfactant may be a mono- or di-functional fluorine-based acrylate, a fluorine-based surfactant, or a silicone-based surfactant, and the surfactant is contained in the coating layer in a dispersed or crosslinked form.
[0114] The additive may include a UV absorber or a UV stabilizer. Examples of the UV absorber include a benzophenone-based compound, a benzotriazole-based compound, or a triazine-based compound, and examples of the UV stabilizer include tetramethyl piperidine.
[0115] The photoinitiator may include, but is not limited to, 1-hydroxy-cyclohexyl-phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2-hydroxy-1-[4-(2-hydroxyethoxy)phenyl]-2-methyl-1-propanone, methylbenzoyl formate, α,α-dimethoxy-α-phenylacetophenone, 2-benzoyl-2-(dimethylamino)-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone diphenyl(2,4,6-trimethylbenzoyl)-phosphine oxide, or bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide. Currently available commercial products include Irgacure 184, Irgacure 500, Irgacure 651, Irgacure 369, Irgacure 907, Darocur 1173, Darocur MBF, Irgacure 819, Darocur TPO, Irgacure 907, Esacure KIP 100F, etc. These photoinitiators can be used alone or in combination of two or more different types.
[0116] Examples of the organic solvent include alcohol-based solvents such as methanol, ethanol, isopropyl alcohol, and butanol; alkoxy alcohol-based solvents such as 2-methoxyethanol, 2-ethoxyethanol, and 1-methoxy-2-propanol; ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, methyl propyl ketone, and cyclohexanone; ether-based solvents such as propylene glycol monopropyl ether, propylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethyl glycol monoethyl ether, diethyl glycol monopropyl ether, diethyl glycol monobutyl ether, and diethylene glycol-2-ethylhexyl ether; and aromatic solvents such as benzene, toluene, and xylene, which may be used alone or in combination.
[0117] According to another embodiment of the present invention, there is provided a flexible display device including a cover window of the flexible display device according to the above embodiment.
[0118] The flexible display device includes curved, bendable, flexible, rollable, or foldable mobile communication terminals, touch panels of smartphones or tablet PCs, and various displays.
[0119] An example of the flexible display device is a flexible light-emitting element display device.
[0120] For example, the OLED display may be disposed at an outer corner of the flexible display device in a direction in which light or a screen emerges, and may include a cathode for providing electrons, an electron transport layer, an emission layer, a hole transport layer, and an anode for providing holes, which are sequentially formed.
[0121] The OLED display may further include a hole injection layer (HIL) and an electron injection layer (EIL).
[0122] In order for the OLED display to function and operate as a flexible display, in addition to using the polymer film as a cover window, the cathode and anode electrodes and each component can be made of a material having a certain elasticity.
[0123] Another example of the flexible display device is a rollable display or a foldable display.
[0124] The rollable display device may have various structures depending on the application field and specific form, for example, it may have a structure including a cover plastic window, a touch panel, a polarizing plate, a barrier film, a light emitting element (such as an OLED element), a transparent substrate, etc. Effect of the Invention
[0125] According to the present invention, a cover window for a flexible display device and a flexible display device can be provided that exhibit high hardness while simultaneously achieving a satisfactory balance of physical properties of flexibility and high hardness, and that is hardly damaged even when repeatedly bent or folded, and can be easily applied to bendable, flexible, rollable, or foldable mobile devices or display devices.
[0126] The cover window of the flexible display device may have physical properties that can replace tempered glass, etc., and therefore may not be broken by pressure or force applied from the outside, and may have properties that allow it to be sufficiently bent and folded. The cover window of the flexible display device may exhibit flexibility, bendability, high hardness, scratch resistance, and high transparency, and may be less damaged even when repeatedly and continuously bent or folded for a long period of time. The cover window of the flexible display device may be usefully applied to bendable, flexible, rollable, or foldable mobile devices, display devices, front panels of various instrument panels, display units, etc. [Brief description of the drawings]
[0127] [Figure 1] FIG. 1 is a schematic diagram showing a method for evaluating dynamic bending properties. [Diagram 2] FIG. 2 is a diagram showing an FT-IR spectrum measured for the polysiloxane of Production Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0128] The present invention will be described in more detail with reference to the following examples, however, the following examples are merely illustrative of the present invention and are not intended to limit the scope of the present invention.
[0129] <Production Example>
[0130] Production Example 1: Production of composition for forming hard coat layer 60 wt% of urethane acrylate oligomer (UF-8001G, Kyoeisha), 37 wt% of methyl ethyl ketone, 2.5 wt% of photoinitiator (I-184, Ciba), and 0.5 wt% of leveling agent (BYK-3570, BYK Chemie) were mixed using a stirrer and filtered to produce a composition for forming a hard coat layer.
[0131] Production Example 2: Production of Polysiloxane A In a 1000 mL 3-neck flask, add the silane monomer 3-glycidoxypropyltrimethoxysilane (GPTMS, KBM-403 TM , Shinetsu), water and toluene were added and mixed with stirring (GPTMS:water=1 mol:3 mol).
[0132] Next, a basic catalyst (trimethylammonium hydroxide; TMAH) was added to the resulting mixed solution in an amount of 1 part by weight per 100 parts by weight of the silane monomer, and the mixture was allowed to react at 100°C for 2 hours to produce polysiloxane A having the following composition, which contains 100 mol% glycidoxypropyl modified silicone (hereinafter referred to as GP).
[0133] The FT-IR spectrum was measured by ATR method, and the transmittance intensity of the cage-type polysiloxane relative to the ladder-type polysiloxane in the prepared polysiloxane was measured to be 1.4. The FT-IR spectrum actually measured is shown in Figure 2 below.
[0134] Comparative Production Example: Production of Polysiloxane B In a 1000 mL 3-neck flask, add the silane monomer 3-glycidoxypropyltrimethoxysilane (GPTMS, KBM-403 TM , Shinetsu), water and toluene were added and mixed with stirring (GPTMS:water=1 mol:3 mol).
[0135] Next, a basic catalyst (trimethylammonium hydroxide; TMAH) was added to the resulting mixed solution in an amount of 1 part by weight per 100 parts by weight of the silane monomer, and the mixture was allowed to react at 100°C for 8 hours to produce polysiloxane B having the following composition, containing 100 mol% glycidoxypropyl modified silicone (hereinafter referred to as GP).
[0136] The FT-IR spectrum was measured by the ATR method, and the transmittance intensity of the cage-type polysiloxane relative to the ladder-type polysiloxane in the prepared polysiloxane was measured and found to be 1.1.
[0137] <Examples and Comparative Examples>
[0138] Example 1 The composition for forming a hard coat layer prepared in Preparation Example 1 was applied to one side of a 15 cm x 20 cm, 50 μm-thick polyimide film (elastic modulus value of 7.0 GPa measured according to ASTM D882), and ultraviolet light was irradiated using a lamp (irradiation dose: 1,000 mJ / cm 2 ) and photocured to form a first coating layer having a thickness of 10 μm.
[0139] A resin composition for forming a second coating layer was prepared by mixing 100 g of the polysiloxane A prepared in Preparation Example 2, 48 g of an elastomeric polymer (polycaprolactone diol, Mn=500 g Da), 3 g of an initiator I-250 (BASF), 0.6 g of a leveling agent F-477 (DIC), and 5 g of a solvent methyl ethyl ketone.
[0140] The resin composition for forming the second coating layer was applied to the other surface of the polyimide film, and ultraviolet light was irradiated using a lamp (irradiation dose: 1,000 mJ / cm 2 ) and photocured to form a second coating layer having a thickness of 40 μm.
[0141] Example 2 An optical laminate for a cover window of a flexible display device was produced in the same manner as in Example 1, except that a resin composition for forming a second coating layer using 16 g of an elastic polymer was used.
[0142] Example 3 An optical laminate for a cover window of a flexible display device was manufactured in the same manner as in Example 1, except that a 60 μm second coating layer was formed using a resin composition for forming a second coating layer using 16 g of an elastic polymer to manufacture an optical laminate with a total thickness of 120 μm.
[0143] Comparative Example 1 An optical laminate for a cover window of a flexible display device was manufactured in the same manner as in Example 1, except that, when manufacturing the resin composition for forming the second coating layer, polysiloxane B of the comparative manufacturing example was used instead of polysiloxane A manufactured in the manufacturing example.
[0144] Comparative Example 2 In the same manner as in Example 1, a first coating layer was formed on one surface of the polyimide.
[0145] An optical clear adhesive film (3M, thickness: 20 μm) and CPI (Kolon, thickness: 20 μm) were sequentially laminated on the other side of the polyimide at room temperature using a lamination device to prepare an optical laminate for a cover window of a flexible display device including a functional layer.
[0146] <Experimental Example> The physical properties of the optical laminates produced in the examples and comparative examples were measured by the following methods, and the results are shown in Table 1 below.
[0147] 1.Dent characteristics An optical clear adhesive film (3M, thickness: 20 μm) and CPI (Kolon, thickness: 20 μm) were sequentially laminated on the second coating layer at room temperature using a lamination device to prepare an optical laminate for a cover window of a flexible display device including a functional layer.
[0148] After the functional layer was bonded, a pencil was fixed at an angle of 45° with a load of 300 g on the surface of the first coating layer of the optical laminate using a pencil hardness tester, and then 20 mm at a time was scratched a total of five times for each pencil hardness, and whether or not it was scratched was judged with the naked eye. The maximum pencil hardness at which no surface damage (cracks of 1 mm or more) occurred more than three times was measured.
[0149] The maximum pencil hardness at which no surface damage (cracks of 1 mm or more) occurs immediately after the functional layer is bonded is defined as the initial Dent value, and the maximum pencil hardness at which no surface damage (cracks of 1 mm or more) occurs after the functional layer is bonded and left at room temperature for 24 hours is defined as the later Dent value.
[0150] 2.Dynamic bending properties FIG. 1 is a diagram that illustrates a method for evaluating dynamic bending characteristics of an optical laminate according to an embodiment of the present invention.
[0151] Specifically, the optical laminate was cut and laser cut into a size of 80x140mm to minimize microcracks at the edges. The laser cut film was placed on a measuring device, with the first coating layer on the inside and the interval between the folded parts (inner curvature diameter) being 8mm, and both sides of the film were folded and unfolded at 90 degrees to the bottom at room temperature (the film was folded at a speed of 1 time per second at 25°C) 200,000 times at room temperature, and the room temperature dynamic bending properties were evaluated according to the following criteria.
[0152] Good: No cracks of 1mm or more Defective: Cracks of 1 mm or more
[0153] 3. Pressure resistance A Wacom pen was used to move back and forth in a circular motion 200 times with a load of 250 g against the surface of the first coating layer of the optical laminate, and then it was checked whether there was any pressure along the path of the pen. If no pressure was observed, it was judged as "good", and if pressure was observed, it was judged as "poor".
[0154] 4. Scratch resistance A load of 500 g was applied to steel wool (#0000) on the surface of the first coating layer of the optical laminate, and the surface was reciprocated 1000 times at a speed of 40 rpm to check for the occurrence of scratches using an optical microscope. If no scratches were observed using the optical microscope, the surface was judged as "good", and if scratches were observed, specifically, if one or more scratches of 1 mm or more were observed, the surface was judged as "poor".
[0155] [Table 1]
[0156] According to Table 1, it was confirmed that the cover windows of the flexible display devices of Examples 1 to 3 have excellent scratch resistance and good dynamic bending properties. In particular, as confirmed by the results of the Dent properties and pressure resistance experiments, it was confirmed that they have sufficient impact resistance and pressure resistance even when formed on a specified substrate.
[0157] In contrast, it was confirmed that the cover windows of Comparative Examples 1 and 2 were unable to have sufficient pressure resistance (dent characteristics) even though they ensured a certain level of scratch resistance.
Claims
1. Light-transmitting base material; a first coating layer formed on one surface of the light-transmitting substrate and having a thickness of 200 μm or less; and a second coating layer formed on another surface of the light-transmitting substrate so as to face the first coating layer, the second coating layer including a polysiloxane having two or more repeating units having different structures; the first coating layer comprises a (meth)acrylate resin or an epoxy resin; The (meth)acrylate resin comprises a (co)polymer of a multifunctional urethane acrylate oligomer, The second coating layer contains an elastic polymer in an amount of 10 parts by weight or more and 80 parts by weight or less based on 100 parts by weight of the polysiloxane containing two or more repeating units having different structures, In an FT-IR spectrum measured by an attenuated total reflectance (ATR) method for the polysiloxane containing two or more repeating units having different structures, the polysiloxane has at least one peak in the region of 1010 cm -1 to 1070 cm -1 and at least one peak in the region of 1075 cm -1 to 1130 cm -1 ; a peak intensity ratio (I 2 / I 1 ) of the intensity (I 2 ) of the peak having the greatest intensity among the at least one peak appearing in the 1075 cm -1 to 1130 cm -1 region to the intensity (I 1 ) of the peak having the greatest intensity among the at least one peak appearing in the 1010 cm -1 to 1070 cm -1 region is 1.2 or more and 2.5 or less; A cover window for a flexible display device.
2. When the first coating layer is folded and unfolded at an angle of 90° toward the inside of the first coating layer so that the first coating layer faces the first coating layer with a gap of 8 mm in between, and the folding and unfolding is repeated 200,000 times at room temperature at a speed of once per second, no cracks of 1 mm or more are generated. The cover window of the flexible display device according to claim 1 .
3. Immediately after a functional layer having a thickness of 10 μm to 300 μm is formed on one surface of the second coating layer formed on the other surface of the light-transmitting substrate so as to face the first coating layer, The surface of the first coating layer has a maximum hardness of 2B or more according to the measurement standard JIS K5400 using a pencil hardness tester, at which no pressure is generated along the path of a pencil. A cover window for a flexible display device according to claim 1 or 2.
4. The polysiloxane containing two or more repeating units having different structures is The crosslinkable functional group-substituted cage-type polysiloxane repeating unit and the crosslinkable functional group-substituted ladder-type polysiloxane repeating unit are included. A cover window for a flexible display device according to any one of claims 1 to 3.
5. The crosslinkable functional group includes any one selected from the group consisting of an alicyclic epoxy group and a functional group represented by the following Chemical Formula 1: The cover window of the flexible display device according to claim 4: [Chemical formula 1] [Case 1] In the above Chemical Formula 1, R a represents a substituted or unsubstituted alkylene group having 1 to 6 carbon atoms, a substituted or unsubstituted alkenylene group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynylene group having 2 to 20 carbon atoms, -R b -CH=CH-COO-R c -, -R d -OCO-CH=CH-R e -, -R f OR g -, -R h COOR i - or -R j O.C.O.R. k - and R b ~R kare each independently a single bond or a substituted or unsubstituted alkylene group having 1 to 6 carbon atoms.
6. a functional layer formed on one surface of the second coating layer formed on the other surface of the light-transmitting substrate so as to face the first coating layer; The functional layer is any one of a black matrix film, a polarizing film, an ultraviolet blocking film, a release film, and a conductive film. A cover window for a flexible display device according to any one of claims 1 to 5.
7. The thickness of the light-transmitting substrate is 5 μm to 100 μm, The first coating layer has a thickness of 5 μm to 200 μm. A cover window for a flexible display device according to any one of claims 1 to 6.
8. The second coating layer has a thickness of 5 μm to 200 μm. A cover window for a flexible display device according to any one of claims 1 to 7.
9. the ratio of the thickness of the first coating layer to the thickness of the light-transmitting substrate is 0.1 to 2.0; A cover window for a flexible display device according to any one of claims 1 to 8.
10. The ratio of the thickness of the second coating layer to the thickness of the first coating layer is 1.0 to 10.0; A cover window for a flexible display device according to any one of claims 1 to 9.
11. The light-transmitting substrate contains one or more resins selected from the group consisting of polyester-based resins, cellulose-based resins, polycarbonate-based resins, acrylic-based resins, styrene-based resins, polyolefin-based resins, polyimide-based resins, polyamideimide-based resins, polyethersulfone-based resins, and sulfone-based resins. A cover window for a flexible display device according to any one of claims 1 to 10.
12. The cover window of the flexible display device does not generate a crack having a length of 3 mm or more when wound around a cylindrical mandrel having a diameter of 3 mm. A cover window for a flexible display device according to any one of claims 1 to 11.
13. A flexible display device comprising a cover window of a flexible display device according to any one of claims 1 to 12.
Citation Information
Patent Citations
Composition for forming hard coat layer
JP2016188354A
Window film and flexible display device including the same
JP2017032993A
Composition for window film, window film formed therefrom, and flexible display device comprising same
WO2017217609A1