Electronic component and manufacturing method thereof
By employing sintered magnetic ribbons and nonmagnetic layers in a laminate structure, the distortion-induced reduction in magnetic characteristics of electronic components is mitigated, resulting in improved magnetic properties and inductance.
Patent Information
- Application Number
- JP2023502197
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-02-26
- Filing Date
- 2022-01-27
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2042-01-27
AI Technical Summary
The distortion of magnetic materials due to stress in electronic components formed by build-up or mold methods reduces their magnetic characteristics and limits the freedom in material selection.
The use of sintered magnetic ribbons arranged perpendicularly to the element body with nonmagnetic layers and grooved magnetic layers filled with nonmagnetic material, forming a laminate structure to alleviate distortion during sintering.
Improves the magnetic characteristics of electronic components by reducing distortion and enhancing magnetic permeability, inductance, and DC superposition characteristics.
Smart Images

Figure 0007556450000012 
Figure 0007556450000017 
Figure 0007556450000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to electronic components and methods for manufacturing electronic components. [Background technology]
[0002] The inductor component, which is an electronic component described in Patent Document 1, includes an element body and wiring extending inside the element body. The element body is made of inorganic filler and resin. For example, in the case of a magnetic composite body, the inorganic filler is made of a magnetic material. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-192920 A Summary of the Invention [Problem to be solved by the invention]
[0004] In the electronic component described in Patent Document 1, various properties of the electronic component are improved by increasing the filling rate of the inorganic filler in the element body. However, when the composite body is formed by a build-up method like the electronic component described in Patent Document 1, or when the composite body is formed by a molding method like a general composite body, stress is applied to the composite body by press processing, etc. The distortion of the magnetic material caused by this stress prevents the magnetic material from fully exhibiting its properties, reducing the freedom of selection of the magnetic material. [Means for solving the problem]
[0005] In order to solve the above problems, one aspect of the present disclosure is an electronic component comprising: a base body having a plurality of flat magnetic ribbons made of a sintered magnetic material, in which the magnetic ribbons are stacked in a stacking direction that is perpendicular to a main surface of the magnetic ribbons; and wiring extending along the main surface inside the base body.
[0006] In order to solve the above problems, one aspect of the present disclosure is a method for manufacturing an electronic component, comprising: forming a nonmagnetic layer using a nonmagnetic paste containing a nonmagnetic material; forming a magnetic layer on the nonmagnetic layer using a magnetic paste containing a magnetic material; dividing the magnetic layer with grooves; filling the grooves with a nonmagnetic paste containing a nonmagnetic material to form split magnetic layers; disposing the split magnetic layers above a wiring pattern formed using a conductive paste containing a conductive material to form a laminate; and firing the laminate to convert the wiring pattern into wiring of a sintered body, the nonmagnetic layer into an interlayer nonmagnetic portion of the sintered body, and the magnetic layer into a magnetic ribbon of the sintered body.
[0007] According to the electronic component, the base body has a magnetic ribbon made of a sintered magnetic material. By using a sintered body as the magnetic ribbon, it is possible to reduce distortion of the magnetic ribbon during the sintering process. As a result, it is possible to improve the characteristics of the electronic component.
[0008] Note that "along" also includes cases where there is no direct contact and the object is at a distance. For example, "along the first axis" includes not only something that is in direct contact with the first axis and runs along the first axis, but also something that is not in direct contact with the first axis and runs along the first axis at a distance. Also, "along" only needs to be in a substantially parallel relationship, and includes something that is slightly tilted due to manufacturing errors, etc. Effect of the Invention
[0009] In electronic components in which a plurality of magnetic ribbons are laminated, the characteristics can be improved. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is an exploded perspective view of the inductor component according to the first embodiment. [Diagram 2] FIG. 2 is a plan view of a first portion of the inductor component. [Diagram 3] 3 is a cross-sectional view of the inductor component taken along line 3-3 in FIG. 2. [Figure 4] FIG. 2 is an enlarged cross-sectional view of the magnetic ribbon in Example 1. [Diagram 5]FIG. 6 is an enlarged cross-sectional view of a magnetic ribbon in Example 2. [Figure 6] 13 is a graph showing inductance versus current for an inductor component of a comparative example and an inductor component of an embodiment. [Figure 7] 11 is a table showing parameters of an inductor component of a comparative example and an inductor component of an embodiment; [Figure 8] FIG. 11 is a cross-sectional view of an inductor component according to a second embodiment. [Figure 9] 5A to 5C are explanatory diagrams of a manufacturing method of an inductor component. [Figure 10] 5A to 5C are explanatory diagrams of a manufacturing method of an inductor component. [Figure 11] 5A to 5C are explanatory diagrams of a manufacturing method of an inductor component. [Figure 12] 5A to 5C are explanatory diagrams of a manufacturing method of an inductor component. [Figure 13] 5A to 5C are explanatory diagrams of a manufacturing method of an inductor component. [Figure 14] 5A to 5C are explanatory diagrams of a manufacturing method of an inductor component. [Figure 15] 5A to 5C are explanatory diagrams of a manufacturing method of an inductor component. [Figure 16] 5A to 5C are explanatory diagrams of a manufacturing method of an inductor component. [Figure 17] 5A to 5C are explanatory diagrams of a manufacturing method of an inductor component. [Figure 18] 5A to 5C are explanatory diagrams of a manufacturing method of an inductor component. [Figure 19] FIG. 11 is a cross-sectional view of an inductor component according to a modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] First Embodiment Hereinafter, a first embodiment of an inductor component will be described as an example of an electronic component. In addition, the drawings may show components enlarged to facilitate understanding. The dimensional ratios of the components may differ from the actual ones or from those in other drawings. In addition, although hatching is applied in the cross-sectional views, the hatching of some components may be omitted to facilitate understanding. Furthermore, reference symbols may be applied to only some of the multiple components.
[0012] (Overall composition) 1, the inductor component 10 includes an element body 20 and an inductor wiring 30. The element body 20 has a plurality of magnetic ribbons 40, a plurality of interlayer nonmagnetic portions 50, a plurality of nonmagnetic portions 60, and a plurality of nonmagnetic films 70.
[0013] The magnetic ribbon 40 is flat. The magnetic ribbons 40 are stacked in a stacking direction that is a direction perpendicular to the main surface MF of the magnetic ribbon 40. The flat shape means a thin shape having a main surface MF, but is not limited to a thin rectangular parallelepiped, and may have curved edges or corners, minute irregularities on the main surface MF, or holes inside.
[0014] The inductor wiring 30 extends linearly along the main surface MF inside the element body 20. The axis along which the inductor wiring 30 extends is defined as a central axis CA. In this embodiment, the extension direction of the central axis CA coincides with the extension direction of one of the sides of the rectangular main surface MF.
[0015] As shown in FIG. 3, in a cross-sectional view perpendicular to the central axis CA, an axis along the main surface MF is defined as a first axis X, and an axis perpendicular to the main surface MF is defined as a second axis Z. One of the directions along the first axis X is defined as a first positive direction X1, and the other of the directions along the first axis X is defined as a first negative direction X2. One of the directions along the central axis CA is defined as a positive direction Y1, and the other of the directions along the central axis CA is defined as a negative direction Y2. One of the directions along the second axis Z is defined as a second positive direction Z1, and the other of the directions along the second axis Z is defined as a second negative direction Z2. In this embodiment, the stacking direction coincides with the direction along the second axis Z.
[0016] 1, the inductor component 10 is composed of a first portion P1, a second portion P2, and a third portion P3, which are laminated in this order along the second axis Z. Of the three portions P1 to P3, the first portion P1 is located at the end in the second negative direction Z2 along the second axis Z.
[0017] 2, the first portion P1 has a square shape when viewed from the direction along the second axis Z. The first portion P1 has a plurality of magnetic ribbons 40, a plurality of interlayer nonmagnetic portions 50, a plurality of nonmagnetic portions 60, and a plurality of nonmagnetic films 70.
[0018] As shown in Fig. 3, in a cross-sectional view perpendicular to the central axis CA, each magnetic ribbon 40 in the first portion P1 is stacked in a direction along the second axis Z. As shown in Fig. 2, each magnetic ribbon 40 in the first portion P1 has a square shape when viewed from the direction along the second axis Z. When viewed from the direction along the second axis Z, each side of each magnetic ribbon 40 is parallel to the first axis X or the central axis CA. The dimensions of the multiple magnetic ribbons 40 in the direction along the second axis Z are all the same.
[0019] Two magnetic ribbons 40 are arranged at the same position along the second axis Z, with a gap between them, in a direction along a first reference axis perpendicular to the second axis Z. Two magnetic ribbons 40 are arranged at the same position along the second axis Z, with a gap between them, in a direction along a second reference axis perpendicular to the second axis Z and the first reference axis. In this embodiment, the first reference axis coincides with the central axis CA, and the second reference axis coincides with the first axis X.
[0020] The magnetic ribbon 40 is a flat plate made of a sintered magnetic material. The magnetic ribbon 40 contains at least one of Fe, Ni, an alloy containing Fe and Si, an alloy containing Fe and Ni, and an alloy containing Fe and Co. In this embodiment, the magnetic ribbon 40 is a metal magnetic material containing an alloy containing Fe and Ni. Fe is metallic iron, and Ni is metallic nickel.
[0021] As shown in FIG. 3, the interlayer nonmagnetic portion 50 is located between the magnetic ribbons 40 adjacent to each other in the direction along the second axis Z. The magnetic ribbons 40 and the interlayer nonmagnetic portions 50 are alternately stacked, and in this embodiment, the interlayer nonmagnetic portions 50 fill all the spaces between the magnetic ribbons 40 adjacent to each other in the direction along the second axis Z. The interlayer nonmagnetic portions 50 are made of a sintered nonmagnetic material. The nonmagnetic material is, for example, alumina, silica, crystallized glass, or amorphous glass. In FIG. 3, the interlayer nonmagnetic portions 50 are illustrated by lines.
[0022] The interlayer nonmagnetic parts 50 all have the same dimension along the second axis Z. Moreover, the dimension of each interlayer nonmagnetic part 50 along the second axis Z is smaller than the dimension of each magnetic ribbon 40 along the second axis Z.
[0023] As shown in FIG. 2, the nonmagnetic portion 60 is located between the magnetic ribbons 40 arranged at the same position along the second axis Z. The nonmagnetic portion 60 fills all the spaces between the magnetic ribbons 40 arranged at the same position along the second axis Z. As described above, at the same position along the second axis Z, there are four magnetic ribbons 40 in total, two in the direction along the central axis CA and two in the direction along the first axis X, so there are four nonmagnetic portions 60. The nonmagnetic portion 60 is made of a nonmagnetic material. In this embodiment, the material of the nonmagnetic portion 60 is the same as that of the interlayer nonmagnetic portion 50. That is, the nonmagnetic portion 60 is made of a nonmagnetic material of a sintered body.
[0024] The nonmagnetic film 70 is located at an end of the first portion P1 in the first positive direction X1 along the first axis X and at an end of the first negative direction X2 opposite to the first positive direction X1. The nonmagnetic film 70 covers the entire area of both end faces of the magnetic ribbon 40 in the direction along the first axis X. The nonmagnetic film 70 also covers the entire area of both end faces of the interlayer nonmagnetic portion 50 in the direction along the first axis X. Furthermore, the nonmagnetic film 70 covers the entire area of both end faces of the nonmagnetic portion 60 in the direction along the first axis X. Therefore, all end faces of the first portion P1 in the first positive direction X1 along the first axis X are composed of the nonmagnetic film 70. Similarly, all end faces of the first portion P1 in the first negative direction X2 along the first axis X are composed of the nonmagnetic film 70. The nonmagnetic film 70 is made of a nonmagnetic material. In this embodiment, the material of the nonmagnetic film 70 is the same as that of the interlayer nonmagnetic portion 50 .
[0025] 1, when viewed from the first portion P1, the second portion P2 is located in a second positive direction Z1 along the second axis Z. When viewed from the direction along the second axis Z, the second portion P2 has the same square shape as the first portion P1.
[0026] The second portion P2 is composed of an inductor wiring 30, a plurality of magnetic ribbons 40, a plurality of interlayer nonmagnetic portions 50, a plurality of nonmagnetic portions 60, and a plurality of nonmagnetic films . The inductor wiring 30 has a rectangular shape when viewed along the second axis Z, and extends linearly along the central axis CA. An end face of the inductor wiring 30 in the positive direction Y1 along the central axis CA forms part of the outer surface of the second portion P2, and is exposed from the element body 20. Similarly, an end face of the inductor wiring 30 in the negative direction Y2, which is the opposite direction to the positive direction Y1 along the central axis CA, forms part of the outer surface of the second portion P2, and is exposed from the element body 20.
[0027] When viewed from the second axis Z, the end face in the positive direction Y1 and the end face in the negative direction Y2 of the inductor wiring 30 are parallel to the first axis X. Furthermore, the central axis CA of the inductor wiring 30 is located at the center of the second portion P2 in the direction along the first axis X. Therefore, the central axis CA, which is the axis along which the inductor wiring 30 extends, passes through the center of the second portion P2 in the direction along the first axis X. The dimension of the inductor wiring 30 in the direction along the first axis X is half the dimension of the second portion P2 in the direction along the first axis X.
[0028] The inductor wiring 30 is made of a conductive material. The conductive material is, for example, Cu, Ag, Au, Al, or an alloy containing these elements. In this embodiment, the inductor wiring 30 is made of Cu.
[0029] As shown in FIG. 3, in a cross section perpendicular to the central axis CA, the inductor wiring 30 has a rectangular shape. Here, in a cross section perpendicular to the central axis CA, a virtual rectangle VR is drawn that circumscribes the inductor wiring 30 and has a first side along the first axis X and a second side along the second axis Z, and has a minimum area. In this embodiment, in a cross section perpendicular to the central axis CA, the inductor wiring 30 is rectangular. In addition, in a cross section perpendicular to the central axis CA, the long side of the outer shape of the inductor wiring 30 is aligned with the first axis X. Furthermore, in a cross section perpendicular to the central axis CA, the short side of the outer shape of the inductor wiring 30 is aligned with the second axis Z. Therefore, the virtual rectangle VR coincides with the outer shape of the inductor wiring 30. In addition, the first side of the virtual rectangle VR is longer than the second side of the virtual rectangle VR.
[0030] In the second portion P2, the portion that is not the inductor wiring 30 is composed of a plurality of magnetic ribbons 40, a plurality of interlayer nonmagnetic portions 50, a plurality of nonmagnetic portions 60, and a plurality of nonmagnetic films 70, similar to the first portion P1.
[0031] As shown in Fig. 3, in a cross-sectional view perpendicular to the central axis CA, each magnetic ribbon 40 in the second portion P2 is stacked in a direction along the second axis Z. As shown in Fig. 2, each magnetic ribbon 40 in the second portion P2 has a rectangular shape when viewed from the direction along the second axis Z. When viewed from the direction along the second axis Z, the long side of each magnetic ribbon 40 is parallel to the central axis CA. The dimensions of the multiple magnetic ribbons 40 in the direction along the second axis Z are all the same.
[0032] 1, in the second portion P2, the magnetic ribbons 40 are located on both sides of the first positive direction X1 and the first negative direction X2 along the first axis X when viewed from the inductor wiring 30. That is, in the second portion P2, two magnetic ribbons 40 are lined up in a direction along the first axis X with the inductor wiring 30 therebetween. Also, two magnetic ribbons 40 are lined up at an interval in a direction along the central axis CA at the same position along the second axis Z.
[0033] Similar to the above-described first portion P1, the interlayer nonmagnetic portions 50 of the second portion P2 are located between adjacent magnetic ribbons 40 in the direction along the second axis Z. That is, as shown in Fig. 3, the magnetic ribbons 40 and the interlayer nonmagnetic portions 50 are alternately stacked in the direction along the second axis Z, similar to the first portion P1.
[0034] The nonmagnetic portion 60 of the second portion P2 is located between the magnetic ribbons 40 that are aligned at the same position along the second axis Z. The nonmagnetic portion 60 fills all the spaces between the magnetic ribbons 40 that are aligned at the same position along the second axis Z. The position of the nonmagnetic portion 60 of the second portion P2 overlaps with a part of the nonmagnetic portion 60 of the first portion P1 when viewed from the direction along the second axis Z. The nonmagnetic portion 60 of the second portion P2 is continuous with the nonmagnetic portion 60 of the first portion P1. Note that, in the second portion P2, the nonmagnetic portion 60 does not exist between the inductor wiring 30 and the magnetic ribbon 40.
[0035] In the second portion P2, the nonmagnetic film 70 is located at an end in a first positive direction X1 along the first axis X and at an end in a first negative direction X2 that is the opposite direction to the first positive direction X1. The nonmagnetic film 70 in the second portion P2 is continuous with the nonmagnetic film 70 in the first portion P1.
[0036] The third portion P3 is located in the second positive direction Z1 of the second portion P2. When viewed from the second axis Z, the third portion P3 has the same square shape as the first portion P1. The third portion P3 is composed of a plurality of magnetic ribbons 40, a plurality of interlayer nonmagnetic portions 50, a plurality of nonmagnetic portions 60, and a plurality of nonmagnetic films 70. In this embodiment, the third portion P3 has a structure symmetrical to the first portion P1 with respect to the second portion P2, and therefore a detailed description thereof will be omitted. In this way, the element body 20 includes a plurality of magnetic ribbons 40, a plurality of interlayer nonmagnetic portions 50, a plurality of nonmagnetic portions 60, and a plurality of nonmagnetic films 70.
[0037] (Regarding the first magnetic ribbon) As shown in FIG. 3, among the multiple magnetic ribbons 40, the magnetic ribbon 40 closest to the inductor wiring 30 in the stacking direction, i.e., the direction along the second axis Z, is defined as the first magnetic ribbon 41. In this embodiment, the first magnetic ribbon 41 is the magnetic ribbon 40 located closest to the second negative direction Z2 among the magnetic ribbons 40 in the first portion P1, and the magnetic ribbon 40 located closest to the second positive direction Z1 among the magnetic ribbons 40 in the third portion P3. That is, the first magnetic ribbon 41, which is the magnetic ribbon 40 closest to the inductor wiring 30, is not arranged in the same layer as the inductor wiring 30. Therefore, the magnetic ribbon 40 located in the second portion P2 is not the first magnetic ribbon 41.
[0038] The multiple magnetic ribbons 40 are arranged at the same position as the first magnetic ribbon 41 in the stacking direction, i.e., the direction along the second axis Z, with two arranged in the direction along the first reference axis, i.e., the central axis CA, and two arranged in the direction along the second reference axis, i.e., the first axis X.
[0039] Furthermore, at the positions of the magnetic ribbons 40 stacked in the first positive direction X1 of the first magnetic ribbon 41 in the first portion P1, the magnetic ribbons 40 are lined up in pairs in the direction along the central axis CA and in pairs in the direction along the first axis X. In this way, at each position in the direction along the second axis Z, the magnetic ribbons 40 in the first portion P1 are lined up in pairs in the direction along the central axis CA and in pairs in the direction along the first axis X.
[0040] Similarly, the multiple magnetic ribbons 40 in the third portion P3 are lined up in pairs in the direction along the central axis CA and in pairs in the direction along the first axis X at each position in the direction along the second axis Z. In this manner, the multiple magnetic ribbons 40 in the element body 20 are regularly arranged in the direction along the central axis CA, the direction along the first axis X, and the direction along the second axis Z.
[0041] (About the second magnetic ribbon) 3, in a cross-sectional view perpendicular to the central axis CA, an end of the inductor wiring 30 in the first positive direction X1 is defined as a first wiring end IP1. Also, in a cross-sectional view perpendicular to the central axis CA, an end of the inductor wiring 30 in the first negative direction X2 is defined as a second wiring end IP2.
[0042] Among the magnetic ribbons 40 stacked on the inductor wiring 30 in the direction along the second axis Z, the magnetic ribbon 40 having the shortest distance from the first wiring end IP1 along the second axis Z is defined as the second magnetic ribbon 41A. Note that the magnetic ribbon 40 that at least partially overlaps with the inductor wiring 30 when viewed from the direction along the second axis Z is the magnetic ribbon 40 stacked on the inductor wiring 30 in the direction along the second axis Z. Therefore, in this embodiment, the magnetic ribbon 40 in the first portion P1 and the magnetic ribbon 40 in the third portion P3 are the magnetic ribbons 40 stacked on the inductor wiring 30 in the direction along the second axis Z. On the other hand, the magnetic ribbon 40 in the second portion P2 is not stacked on the inductor wiring 30 in the direction along the second axis Z. Also, in this embodiment, the second magnetic ribbon 41A is the magnetic ribbon 40 stacked on the first magnetic ribbon 41 in the direction along the second axis Z at the first wiring end IP1. Therefore, the second magnetic ribbon 41A is the magnetic ribbon 40 in the first portion P1 that is located furthest in the second negative direction Z2, and the magnetic ribbon 40 in the third portion P3 that is located furthest in the second positive direction Z1.
[0043] As shown in FIG. 3, in one magnetic ribbon 40, the end in the first positive direction X1 is the first end MP1, and the end in the first negative direction X2 is the second end MP2. In this case, the range in one magnetic ribbon 40 excluding both ends in the direction along the first axis X is the first range AR1. In other words, in one magnetic ribbon 40, the coordinate indicating the position of the second end MP2 in the direction along the first axis X is set to 0. In one magnetic ribbon 40, the coordinate indicating the position of the first end MP1 in the first positive direction X1 along the first axis X in the direction along the first axis X is set to 1. In this case, the range in which the coordinate indicating the position in the direction along the first axis X is greater than 0 and less than 1 is the first range AR1. Then, as shown in FIG. 3, a first virtual straight line VL1 is drawn in the direction along the second axis Z while passing through the first wiring end IP1. In this case, the first virtual straight line VL1 passes through the first range AR1 of the second magnetic ribbon 41A.
[0044] In the present embodiment, in the first portion P1, a plurality of magnetic ribbons 40 are continuously stacked in the second positive direction Z1 with respect to the inductor wiring 30. In a cross-sectional view perpendicular to the central axis CA, the first virtual straight line VL1 passes through a first range AR1 of two or more magnetic ribbons 40 continuously stacked including the second magnetic ribbon 41A among the plurality of magnetic ribbons 40 continuously stacked in the second positive direction Z1 from the second magnetic ribbon 41A. Specifically, the first virtual straight line VL1 passes through the first range AR1 of all magnetic ribbons 40 continuously stacked on the second magnetic ribbon 41A among the magnetic ribbons 40 included in the first portion P1.
[0045] Furthermore, in the third portion P3, a plurality of magnetic ribbons 40 are continuously stacked in the second negative direction Z2 with respect to the inductor wiring 30. In a cross-sectional view perpendicular to the central axis CA, the first virtual straight line VL1 passes through a first range AR1 of two or more magnetic ribbons 40 continuously stacked including the second magnetic ribbon 41A among the plurality of magnetic ribbons 40 continuously stacked in the second negative direction Z2 from the second magnetic ribbon 41A. Specifically, the first virtual straight line VL1 passes through the first range AR1 of all magnetic ribbons 40 continuously stacked on the second magnetic ribbon 41A among the magnetic ribbons 40 included in the third portion P3.
[0046] The magnetic ribbon 40 is a sintered body. In this embodiment, as described above, the magnetic material contains Fe and Ni. Specifically, for example, in Example 1 shown in FIG. 4, the magnetic ribbon 40 has a plurality of metal magnetic bodies 45. Specifically, in Example 1, the metal magnetic bodies 45 are metal magnetic particles of an alloy containing Fe and Ni. An insulating material 46, which is an oxide containing O, exists at the grain boundaries between the metal magnetic bodies 45. Note that, as in Example 2 shown in FIG. 5, in the magnetic ribbon 40, the alloy containing Fe and Ni may be completely dissolved and integrated. In this case, the metal magnetic body 45 of the alloy containing Fe and Ni does not have a structure in which a plurality of metal magnetic particles are bonded with a clear interface as in FIG. 4.
[0047] A second virtual straight line VL2 is drawn passing through the second end MP2 in the first negative direction X2, which is the opposite direction to the first positive direction X1 along the first axis X of the second magnetic ribbon 41A, and extending along the second axis Z. At this time, the second virtual straight line VL2 passes through the inductor wiring 30. In this embodiment, the second virtual straight line VL2 is located approximately in the center of the inductor wiring 30 in the direction along the first axis X.
[0048] In this embodiment, the inductor component 10 has a structure that is symmetrical with respect to the second axis Z that passes through the center in the direction along the first axis X. Here, a third virtual straight line VL3 is drawn in the direction along the second axis Z while passing through the second wiring end IP2 of the inductor wiring 30. In addition, among the magnetic ribbons 40 stacked in the direction along the second axis Z with respect to the inductor wiring 30, the magnetic ribbon 40 that has the shortest distance along the second axis Z from the second wiring end IP2 is defined as the third magnetic ribbon 41B. In this case, the third virtual straight line VL3 passes through the first range AR1 of the third magnetic ribbon 41B in a cross-sectional view perpendicular to the central axis CA. More specifically, the third virtual straight line VL3 passes through the center of the third magnetic ribbon 41B in the direction along the first axis X.
[0049] In the present embodiment, in a cross-sectional view perpendicular to the central axis CA, the third virtual straight line VL3 passes through the first area AR1 of two or more magnetic ribbons 40 that are continuously stacked including the third magnetic ribbon 41B. Specifically, the third virtual straight line VL3 passes through the first area AR1 of all the magnetic ribbons 40 that are continuously stacked on the third magnetic ribbon 41B among the magnetic ribbons 40 included in the first portion P1.
[0050] Furthermore, the third virtual straight line VL3 passes through the first range AR1 of all the magnetic ribbons 40 that are continuously stacked on the third magnetic ribbon 41B among the magnetic ribbons 40 included in the third portion P3. More specifically, the third virtual straight line VL3 passes through the center of all the magnetic ribbons 40 that are continuously stacked on the third magnetic ribbon 41B. In this way, in a cross-sectional view perpendicular to the central axis CA, it is preferable that the third virtual straight line VL3 passes through the above-mentioned first range AR1 with respect to the third magnetic ribbon 41B.
[0051] (Simulation results) Next, a description will be given of the results of a simulation in which the characteristics obtained for the inductor component 10 are compared with those of an inductor component of a comparative example. Femtet (registered trademark) from Murata Software Co., Ltd. was used for the simulation.
[0052] First, the conditions of the simulation will be described. The software used is Femtet2019 from Murata Software. The solver is a static magnetic field analysis. The model is three-dimensional. The standard mesh size is 0.01 mm. The magnetic material is a metallic magnetic ribbon made of Fe and Ni elements. The magnetic material BH curve used satisfies B=Bs×tanh(μ0×μr×H / Bs). Note that the magnetic material BH curve uses a portion with a relative magnetic permeability μr of 1 or more so as not to fall below the magnetic permeability of a vacuum, and is further extrapolated to the magnetic permeability of a vacuum using the function of Femtet2019. The material of the inductor wiring 30 is copper.
[0053] Next, the conditions regarding the dimensions and position of the inductor component model used in the simulation will be described. The dimension of the inductor wiring 30 in the direction along the first axis X is 500 μm. The dimension of the inductor wiring 30 in the direction along the second axis Z is 100 μm. The dimension of the inductor wiring 30 in the direction along the central axis CA is 2400 μm.
[0054] The dimension of the magnetic ribbon 40 in the direction along the first axis X is 990 μm. The dimension of the magnetic ribbon 40 in the direction along the second axis Z is 20 μm. The dimension of the magnetic ribbon 40 in the direction along the central axis CA is 990 μm.
[0055] The dimension of the interlayer nonmagnetic portion 50 in the direction along the second axis Z is 2.0 μm. The dimension of the nonmagnetic portion 60 in the direction along the first axis X is 20 μm. The dimension of the nonmagnetic portion 60 in the direction along the central axis CA is 20 μm. The number of magnetic ribbons 40 stacked in the direction along the second axis Z is 41. The number of magnetic ribbons 40 lined up in the direction along the first axis X is 2. The number of magnetic ribbons 40 lined up in the direction along the central axis CA is 2.
[0056] The dimension of the inductor component 10 in the direction along the second axis Z is 902 μm. In the simulation, the element body 20 has a film of the same nonmagnetic material as the nonmagnetic film 70 at both ends in the direction along the central axis CA. The dimension of the film in the direction along the central axis CA is 10 μm. Therefore, the dimension of the inductor component 10 in the direction along the first axis X is 2020 μm. The dimension of the element body 20 in the direction along the central axis CA is 2020 μm. That is, in this simulation, the dimension of the inductor wiring 30 in the direction along the central axis CA is 380 μm larger than the dimension of the element body 20 in the direction along the central axis CA. Therefore, the simulation is performed in a state in which the inductor wiring 30 protrudes by 190 μm from the end face of the element body 20 in the positive direction Y1 and the inductor wiring 30 protrudes by 190 μm from the end face of the element body 20 in the negative direction Y2.
[0057] The dimension of the inductor wiring 30 in the direction along the second axis Z is 100 μm. The position of the inductor wiring 30 was arranged so that the center of gravity of the inductor wiring 30 coincided with the center of gravity of the element body 20. The relative permeability μr of the nonmagnetic material of the interlayer nonmagnetic portion 50, the nonmagnetic portion 60 and the nonmagnetic film 70 was set to 1.
[0058] In the simulation, in the magnetic ribbon 40 in Example 1, the metal magnetic bodies 45 of the FeNi alloy are not solid-dissolved with each other and are in contact with each other via grain boundaries as shown in Fig. 4. In Example 1, the relative permeability μr is 500, and the saturation magnetic flux density Bs is 1.3 T.
[0059] In the simulation, in the magnetic ribbon 40 in Example 2, the metal magnetic body 45 of the FeNi alloy was in a bulk state in which the metal magnetic particles of the precursor were dissolved in each other and sintered together as shown in Fig. 5. In Example 2, the relative permeability μr was 7000, and the saturation magnetic flux density Bs was 1.3 T. Therefore, the relative permeability μr in Example 2 was much larger than that in Example 1.
[0060] In the simulation, the element body 20 in the comparative example was in a state in which a metal composite material of powder-like metal magnetic particles made of an FeNi alloy and an organic resin was contained at a filling rate of 70%. Therefore, in the comparative example, the relative permeability μr was 24, and the saturation magnetic flux density Bs was 0.91 T.
[0061] Next, the characteristic index calculated by the simulation will be described. The unit of inductance L is nH, and the unit of DC bias characteristic Isat is A. The DC bias characteristic Isat is the current value Idc at which the inductance L decreases by 20% from the initial inductance Lin, which is the inductance L at a current value Idc of 0.001A.
[0062] As shown in FIG. 6, in Example 1, Example 2, and Comparative Example, the current value Idc was changed within a range of 0.001 A to 80 A, and the obtained inductance L was calculated by simulation.
[0063] 7, the initial inductance Lin in Example 1 was 14.7 nH, and the initial inductance Lin in Example 2 was 16.2 nH. On the other hand, the initial inductance Lin in the comparative example was 13.6 nH. Therefore, the initial inductance Lin in the example was larger than the initial inductance Lin in the comparative example.
[0064] Moreover, the DC bias characteristic Isat in Example 1 was 55 A, and the DC bias characteristic Isat in Example 2 was 45 A. On the other hand, the DC bias characteristic Isat in the comparative example was 30 A. Therefore, the DC bias characteristic Isat in the example was larger than the DC bias characteristic Isat in the comparative example.
[0065] (Operation of the First Embodiment) Next, the operation of the first embodiment will be described. In the first embodiment, the magnetic ribbon 40 is made of a sintered magnetic material. In a sintered body, the metal magnetic particles are more densely packed together than in a powder state. Therefore, the amount of metal magnetic particles contained per unit volume increases compared to before sintering. As a result, the effective magnetic permeability of the entire element body 20 can be increased.
[0066] In addition, the metal magnetic body 45 included in the magnetic ribbon 40 may be distorted before sintering. Even if the metal magnetic body 45 is distorted, the metal magnetic body 45 is fired in the sintering process, and such distortion is eliminated. An oxide layer may be formed on the surface of the metal magnetic body 45 during pre-sintering or sintering. This oxide layer becomes an insulating material 46 containing O element after sintering. The "distortion of the magnetic ribbon 40" is not limited to visible distortion, but also includes microscopic distortion such as a crystal structure or an intermolecular structure.
[0067] (Effects of the first embodiment) Next, the effects of the first embodiment will be described. (1-1) According to the first embodiment, the magnetic ribbon 40 is a sintered body. By using a sintered body as the magnetic ribbon 40, it is possible to alleviate distortion of the magnetic ribbon 40 during the sintering process. As a result, it is possible to prevent the magnetic properties of the magnetic ribbon 40, such as the magnetic permeability and coercive force, from being deteriorated during the manufacturing process.
[0068] Therefore, crystalline metal magnetic particles having a large magnetostriction constant but a high saturation magnetic flux density Bs can be used, and a high saturation magnetic flux density Bs can be obtained for the entire element body 20. As a result, both the initial inductance Lin and the DC bias characteristic Isat, which are characteristic indicators, are larger than when the entire element body 20 is made of a metal composite material of powder-like metal magnetic particles and organic resin. Therefore, according to the first embodiment, it is possible to improve the characteristics of the inductor component 10.
[0069] (1-2) According to the first embodiment, the magnetic ribbon 40, which is a sintered body, has an alloy containing Fe and Ni. The alloy containing Fe and Ni can achieve high magnetic permeability μ. Therefore, the initial inductance Lin and the DC bias characteristic Isat, which are characteristic indexes, can be increased.
[0070] (1-3) According to the first embodiment, in the magnetic ribbon 40, the metal magnetic bodies 45, which are a plurality of metal magnetic particles, are bonded via the insulating material 46. Therefore, it is possible to reduce eddy current loss and suppress leakage current and short circuits due to the conductive path in which the metal magnetic bodies 45 are connected to each other.
[0071] (1-4) According to the first embodiment, the insulating material 46 contains an O element. That is, the insulating material 46 is an oxide. Therefore, the insulating material 46 can be formed by oxidizing grain boundaries of a plurality of metal magnetic particles during pre-sintering treatment or sintering treatment. Therefore, in order to provide the insulating material 46, it is not necessary to use a material other than the precursor constituting the metal magnetic body 45.
[0072] (1-5) According to the above embodiment, the first virtual straight line VL1 passes through the first range AR1 of the second magnetic ribbon 41A. Therefore, among the magnetic flux generated when a current flows through the inductor wiring 30, most of the magnetic flux oriented along the first virtual straight line VL1 passes through a portion of the second magnetic ribbon 41A except for the end in the direction along the first axis X in the vicinity of the first wiring end IP1 of the inductor wiring 30. That is, among the magnetic flux generated when a current flows through the inductor wiring 30, the magnetic flux passing through the end in the direction along the second magnetic ribbon 41A is reduced. Therefore, it is possible to suppress the magnetic flux from being disturbed or being locally concentrated. According to such a positional relationship between the second magnetic ribbon 41A and the inductor wiring 30, the inductance L is large regardless of the filling rate of the magnetic material.
[0073] (1-6) According to the above embodiment, the multiple magnetic ribbons 40 are continuously stacked in the direction along the second axis Z with respect to the inductor wiring 30. In a cross-sectional view perpendicular to the central axis CA, the first virtual straight line VL1 passes through the first range AR1 of two or more magnetic ribbons 40 continuously stacked including the second magnetic ribbon 41A. Therefore, depending on the positional relationship between not only the second magnetic ribbon 41A but also the other magnetic ribbons 40 and the inductor wiring 30, the characteristic index can be further increased.
[0074] (1-7) According to the above embodiment, in a cross-sectional view perpendicular to the central axis CA, the first virtual straight line VL1 passes through the first range AR1 of all the magnetic ribbons 40 continuously stacked on the second magnetic ribbon 41A. Therefore, the first virtual straight line VL1 does not pass through the ends of the magnetic ribbons 40 in the direction along the first axis X, and the characteristic index can be further increased.
[0075] (1-8) The magnetic flux generated when a current flows through the inductor wiring 30 in a direction along the central axis CA includes magnetic flux that penetrates into the magnetic ribbon 40 in a direction along the second axis Z. The magnetic flux that penetrates in this way generates an eddy current in the magnetic ribbon 40. Moreover, when viewed from the direction along the second axis Z, the larger the area of each magnetic ribbon 40, the larger this eddy current becomes. When an eddy current occurs, the energy of the magnetic flux is lost as heat energy, resulting in a loss.
[0076] According to the first embodiment, two magnetic ribbons 40 are arranged in the direction along the first reference axis and two magnetic ribbons 40 are arranged in the direction along the second reference axis at the same position along the second axis Z. Therefore, the area of the magnetic ribbon 40 when viewed from the direction along the second axis Z is smaller than when there is one magnetic ribbon 40 at the same position along the second axis Z. Therefore, the eddy current generated in one magnetic ribbon 40 is smaller.
[0077] (1-9) According to the first embodiment, two magnetic ribbons 40 are arranged in the direction along the first axis X at the same position along the second axis Z. Therefore, the second magnetic ribbon 41A through which the first virtual straight line VL1 passing through the first wiring end IP1 of the inductor wiring 30 passes and the third magnetic ribbon 41B through which the third virtual straight line VL3 passing through the second wiring end IP2 of the inductor wiring 30 passes are different magnetic ribbons 40. Therefore, while ensuring a certain degree of size as the dimension of the inductor wiring 30 in the direction along the first axis X, the positional relationship described above can be realized as the positional relationship between the inductor wiring 30 and the second magnetic ribbon 41A.
[0078] (1-10) According to the first embodiment, the element body 20 has nonmagnetic portions 60 made of a nonmagnetic material that is a sintered body. The nonmagnetic portions 60 are located between adjacent magnetic ribbons 40 in the direction along the first reference axis and between adjacent magnetic ribbons 40 in the direction along the second reference axis. In this case, the nonmagnetic portions 60 that are located at the same position on the second axis Z as the magnetic ribbons 40 can be sintered in the same process that converts the magnetic ribbons 40 into a sintered body.
[0079] (1-11) According to the first embodiment, the element body 20 has the interlayer nonmagnetic parts 50 made of a nonmagnetic material of a sintered body. The interlayer nonmagnetic parts 50 are located between adjacent magnetic ribbons 40 in the stacking direction of the magnetic ribbons 40. In this case, the magnetic ribbons 40 stacked in the stacking direction can be sintered in the same process as the process of making a sintered body.
[0080] (1-12) According to the first embodiment, the dimensions of the multiple magnetic ribbons 40 in the direction along the second axis Z are all equal. Therefore, the magnetic flux density in each magnetic ribbon 40 is uniform, and the magnetic flux is less likely to concentrate and saturate at a specific location. As a result, the magnetic flux density in the entire element body 20 is improved.
[0081] (1-13) According to the first embodiment, the interlayer nonmagnetic parts 50 all have the same dimension in the direction along the second axis Z. This makes it possible to uniformize the disturbance of the magnetic flux occurring at the interface between the interlayer nonmagnetic parts 50 and the magnetic ribbons 40.
[0082] <Second embodiment> (Inductor components) An inductor component 110 in the second embodiment has a different configuration of a second portion P2 from inductor component 10 in the first embodiment. The differences from inductor component 10 in the first embodiment will be described below.
[0083] As shown in FIG. 8, the second portion P2 is composed of an inductor wiring 30 and two composite parts 80. The composite part 80 is composed of powder-like magnetic particles 81 made of a magnetic material, and a non-magnetic base material 82 made of a non-magnetic material. The magnetic particles 81 are metal magnetic particles containing, for example, Fe, Ni, Co, Cr, Cu, Al, Si, B, P, etc. In this embodiment, the magnetic particles 81 are metal particles of an alloy containing Fe, Si, and Cr. The non-magnetic base material 82 is, for example, an inorganic sintered body such as glass or alumina.
[0084] The composite part 80 has a rectangular shape when viewed along the second axis Z. When viewed along the second axis Z, the long side of the composite part 80 is parallel to the central axis CA. The dimension of the composite part 80 in the direction along the second axis Z is parallel to the inductor wiring 30.
[0085] 1, in the second portion P2, the two composite parts 80 are located on both sides in a first positive direction X1 and a first negative direction X2 along the first axis X when viewed from the inductor wiring 30. That is, in the second portion P2, the two composite parts 80 are lined up in a direction along the first axis X, with the inductor wiring 30 between them.
[0086] (Manufacturing method for inductor components) Next, a method for manufacturing the inductor element 110 will be described. As shown in FIG. 9, the manufacturing method of the inductor component 110 includes a first sheet preparation step S11, a second sheet preparation step S12, a lamination step S13, a pressure bonding step S14, a singulation step S15, a sintering step S16, and a coating process step S17.
[0087] First, a first sheet preparation step S11 is performed. The first sheet 210 has a non-magnetic layer 211 and a magnetic layer 212 containing a metal magnetic powder 212M, which is a magnetic material. As shown in FIG. 10, in manufacturing the first sheet 210, a film made of PET is first prepared as a first base material 91. The first base material 91 may be a substrate made of PET, alumina, or ferrite that is removed when the part is completed, or may be a non-magnetic layer 211 made of glass that remains. In the following description, the two main surfaces of the first base material 91 are arranged so as to be perpendicular to the second axis Z, and a cross section perpendicular to the central axis CA is shown. In addition, in FIG. 10 to FIG. 18, the dimensional ratio is greatly changed from that in FIG. 8 for ease of understanding.
[0088] A nonmagnetic paste made of a nonmagnetic and insulating nonmagnetic material is applied to a main surface of the first base material 91 facing the second positive direction Z1 along the second axis Z and formed into a sheet shape. This forms the nonmagnetic layer 211. The nonmagnetic layer 211 is made of a nonmagnetic material containing, for example, alumina, silica, crystallized glass, amorphous glass, etc.
[0089] 11, a metal magnetic paste containing metal magnetic powder 212M, which is a magnetic material, is applied to the surface of non-magnetic layer 211 facing second positive direction Z1 along second axis Z. In this embodiment, metal magnetic powder 212M is an FeNi alloy containing Fe and Ni elements. This forms magnetic layer 212. Magnetic layer 212 is made of metal magnetic paste in which resin 92 contains metal magnetic powder 212M.
[0090] 12, a groove 212H is formed in the magnetic layer 212 by laser processing. The groove 212H penetrates the magnetic layer 212. When viewed from the direction along the second axis Z, a part of the nonmagnetic layer 211 is exposed from the groove 212H in the second positive direction Z1 along the second axis Z. When viewed from the direction along the second axis Z, the groove 212H divides the magnetic layer 212 in the direction along the first reference axis and the direction along the second reference axis.
[0091] Next, as shown in Fig. 13, grooves 212H formed in magnetic layer 212 are filled with nonmagnetic paste made of a nonmagnetic and insulating material by printing or the like. This forms groove nonmagnetic portions 213. At the same time, magnetic layer 212 is divided in the direction along the first reference axis and in the direction along the second reference axis to form a plurality of divided magnetic layers 212D. Furthermore, first sheets 210 are prepared by forming divided magnetic layers 212D into sheets. The first sheets 210 are prepared in the same number as the number of stacked magnetic ribbons 40 of inductor component 10 to be manufactured.
[0092] Next, a second sheet preparation step S12 is performed. The second sheet 220 has a wiring pattern 221 and a negative pattern 222. First, in manufacturing the second sheet 220, a second base material 93 is prepared as shown in FIG. 14. The second base material 93 may be a substrate made of PET, alumina, or ferrite that is removed when the part is completed, or may be a substrate that remains, such as a nonmagnetic layer 211 made of glass. In the following description, it is assumed that the two main surfaces of the second base material 93 are disposed so as to be perpendicular to the second axis Z.
[0093] A nonmagnetic paste made of a nonmagnetic and insulating nonmagnetic material is applied to a main surface of the second base material 93 facing the second positive direction Z1 along the second axis Z and formed into a sheet. In this way, the nonmagnetic layer 211 is formed.
[0094] Next, a conductive paste is applied partially by printing or the like to a main surface of the nonmagnetic layer 211 facing the second positive direction Z1 along the second axis Z. This forms the wiring pattern 221. The wiring pattern 221 is made of a conductive material. For example, it is made of a conductive paste of Ag or Cu.
[0095] The method for forming the wiring pattern 221 may be a printing method such as screen printing, a photolithography method using a photosensitive material, a plating method such as semi-additive, a transfer method for transferring a wiring pattern formed on a separate sheet, etc. In the case of a plating method or a transfer method, a metal film that does not contain resin may be used as the material for the wiring pattern 221, instead of a conductive paste.
[0096] 15, of the main surface of the nonmagnetic layer 211 facing the second positive direction Z1 along the second axis Z, a negative paste is filled and applied by printing or the like to the portion where the wiring pattern 221 is not applied. In this way, a negative pattern 222 is formed. Although not shown, the negative pattern 222 contains magnetic particles 81 and nonmagnetic powder that is the raw material of the nonmagnetic base material 82. In this way, a second sheet 220 is prepared. In this embodiment, the nonmagnetic layer 211 serves as a sheet-like base material for forming the wiring pattern 221 and the negative pattern 222.
[0097] Next, a lamination step S13 is performed in which the prepared first sheet 210 and second sheet 220 are laminated. As shown in FIG. 16, first, the first base material 91 is peeled off from the first sheet 210, and the sheet is placed on a predetermined jig table (not shown) with the sheet in the up-down direction. Then, the surface of the wiring pattern 221 and the negative pattern 222 in the second sheet 220 facing the opposite direction to the surface on which the nonmagnetic layer 211 is applied is bonded to the surface of the nonmagnetic layer 211 in the first sheet 210 facing the opposite direction to the surface on which the magnetic layer 212 is applied. As a result, the first sheet 210 is laminated in the second positive direction Z1 along the second axis Z of the second sheet 220.
[0098] Similarly, the first base material 91 is peeled off from another first sheet 210. Then, a surface of the first sheet 210 laminated on the second sheet 220 facing in the opposite direction to the surface adhered to the second sheet 220 is faced and adhered to a surface of the nonmagnetic layer 211 of the other first sheet 210 facing in the opposite direction to the surface on which the magnetic layer 212 is applied. Although not shown in the drawings, the first sheets 210 are laminated by the number of magnetic ribbons 40 to be laminated on the third portion P3 of the inductor component 10.
[0099] Next, second base material 93 is peeled off from second sheet 220. Then, a surface of nonmagnetic layer 211 of second sheet 220 facing in the opposite direction to the surface on which wiring pattern 221 is applied is placed face to face with a surface of magnetic layer 212 of first sheet 210 facing in the opposite direction to the surface on which nonmagnetic layer 211 is applied, and they are adhered together. Then, first base material 91 is peeled off from first sheet 210.
[0100] Similarly, a surface of the nonmagnetic layer 211 of the first sheet 210 laminated on the second sheet 220 facing the opposite side to the surface on which the magnetic layer 212 is applied is placed face to face with a surface of the magnetic layer 212 of another first sheet 210 facing the opposite side to the surface on which the nonmagnetic layer 211 is applied, and bonded to the surface. Although not shown, the first sheets 210 are laminated by the same number of magnetic ribbons 40 to be laminated on the first portion P1 of the inductor component 10. In this manner, the first sheets 210 are repeatedly laminated on both main surfaces of the second sheet 220. That is, when forming the laminate 200, a plurality of split magnetic layers 212D are laminated.
[0101] Next, a pressure bonding step S14 is performed. The first sheet 210 and the second sheet 220 laminated in the lamination step S13 are pressure bonded by pressing such as WIP. In this way, the laminate 200 is formed.
[0102] Next, a singulation step S15 is performed. As shown in FIG. 17, for example, the laminate 200 is singulated by dicing at a predetermined break line DL. As a result, the laminate 200 is singulated to form individual pieces 201. The individual pieces 201 are composed of a wiring pattern 221 and a divided magnetic layer 212D. The multiple individual pieces 201 are arranged in a matrix in the laminate 200 so as to be aligned in a direction along the first reference axis and a direction along the second reference axis. In this embodiment, the individual piece 201 has one wiring pattern 221.
[0103] Next, the sintering step S16 is performed. As shown in FIG. 18, the individual parts 201 of the laminate 200 that have been singulated in the singulation step S15 are sintered by firing for a predetermined time. As a result, the wiring pattern 221 becomes the inductor wiring 30 of the sintered body. The negative pattern 222 becomes the composite part 80 of the sintered body. The non-magnetic layer 211 becomes the interlayer non-magnetic part 50 of the sintered body. The non-magnetic part 213 in the groove becomes the non-magnetic part 60 of the sintered body. The metal magnetic powder 212M of the magnetic layer 212 becomes the metal magnetic body 45 of the sintered body made of a magnetic material. Meanwhile, the resin contained in the individual parts 201 of the laminate 200 is vaporized by heating.
[0104] Next, a coating process step S17 is performed. The surface including the break lines DL diced in the singulation process S15 is covered with a nonmagnetic film 70, which is a nonmagnetic insulator. As a result, the individual portions 201 become inductor components 110. Note that the volume of the inductor components 110 becomes smaller than the volume of the individual portions 201 by the sintering process S16.
[0105] (Operation of the second embodiment) According to the inductor component 110 of the second embodiment, the metal magnetic powder 212M of the magnetic layer 212 becomes a sintered body made of a magnetic material through the sintering step S16.
[0106] (Effects of the second embodiment) The second embodiment is different from the first embodiment in that the magnetic ribbon 40 and the interlayer nonmagnetic portion 50 in the second portion P2 are configured as a composite portion 80. Therefore, the configurations of the magnetic ribbon 40 and the interlayer nonmagnetic portion 50 in the first portion P1 and the third portion P3 are similar to those in the first embodiment. Therefore, the inductor component 110 in the second embodiment has a tendency similar to that of the simulation result of the inductor component 10 in the first embodiment. Therefore, according to the second embodiment, in addition to the effects (1-1) to (1-13) in the first embodiment, the following effects are obtained.
[0107] (2-1) In the second embodiment, the magnetic material of the magnetic ribbon 40 is permendur made of Fe and Co. Such a crystalline metal magnetic material has an extremely high saturation magnetic flux density Bs among metal magnetic materials. Therefore, from the viewpoint of the DC bias characteristic Isat, it is suitable as a material for the element body 20 in a power inductor or the like used at a high current value Idc.
[0108] However, crystalline metal magnetic materials such as permendur, which is made of Fe and Co elements, have a very large magnetostriction constant. That is, crystalline metal magnetic materials are materials that undergo a large amount of dimensional change when a magnetic field is generated. When forming the element body 20, for example, when pressure is applied, the stress tends to cause residual distortion of the crystalline metal magnetic material. If such distortion caused by processing remains, the magnetic permeability μ may decrease, or a large coercive force may be required to return the material to an unmagnetized state.
[0109] Here, in the second embodiment, residual strain caused by processing can be relaxed in the sintering step S16. In this way, the recovery characteristics can be increased by relaxing the strain, so that the effect of using a sintered body as a crystalline metal magnetic material is greatly exhibited.
[0110] (2-2) According to the second embodiment, the portion of the second portion P2 that is not the inductor wiring 30 is composed of the composite portion 80. In the composite portion 80, the magnetic particles 81 are randomly dispersed. Therefore, when the magnetic flux generated in the direction along the second axis Z penetrates into the magnetic material of the second portion P2, the eddy current generated in the composite portion 80 becomes small.
[0111] (2-3) If the sintered magnetic ribbons 40 were to be stacked one by one in one inductor component 10, it would be time-consuming. According to the second embodiment, the laminate 200 having a plurality of individual parts 201 is formed. The laminate 200 is then separated into individual parts to form the individual parts 201. The individual parts 201 are then sintered to manufacture the inductor component 10. Therefore, the individual parts 201 in which a plurality of magnetic ribbons 40 are stacked can be efficiently manufactured.
[0112] (2-4) According to the second embodiment, the first sheet 210 is prepared by forming the divided magnetic layer 212D into a sheet shape. The second sheet 220 is prepared by forming the wiring pattern 221 on the nonmagnetic layer 211 as a sheet-shaped base material. The first sheet 210 and the second sheet 220 are then pressure-bonded to form the laminate 200. Therefore, the laminate 200 can be formed by a process of preparing two types of sheets, a process of stacking, and a process of pressure-bonding.
[0113] (2-5) According to the second embodiment, the laminate 200 is formed by forming the split magnetic layer 212D on the wiring pattern 221. The position of the split magnetic layer 212D can be adjusted with reference to the wiring pattern 221.
[0114] (2-6) According to the second embodiment, in preparing second sheet 220, negative pattern 222 is formed on nonmagnetic layer 211 as a sheet-like base material in a portion where wiring pattern 221 is not formed. This makes it easy to adjust the position of composite portion 80 in inductor component 110.
[0115] (2-7) According to the second embodiment, a plurality of split magnetic layers 212D are stacked when forming the laminate 200. This makes it easy to adjust the number of magnetic ribbons 40 stacked in the stacking direction in the inductor component 110.
[0116] <Other embodiments> The above-described embodiments may be modified as follows: The above-described embodiments and the following modifications may be combined and implemented within the scope of technical compatibility.
[0117] In each of the above embodiments, the shape of the element body 20 is not limited to the examples of each of the above embodiments. For example, when viewed from a direction along the second axis Z, the shape of the element body 20 may be a rectangle, or a polygon other than a rectangle. Furthermore, for example, when viewed from a direction along the second axis Z, the shape of the element body 20 may be a circle such as an ellipse. Furthermore, the shape of the element body 20 may be a rectangular parallelepiped, a cube, a polygonal prism, a cylinder, or the like, in which the dimensions of the first reference axis and the second reference axis are different.
[0118] In each of the above embodiments, the shape of the inductor wiring 30 can be appropriately changed as long as it can generate a magnetic flux in the element body 20 when a current flows, thereby imparting inductance L to the inductor component 10. For example, as in the above simulation, both ends of the inductor wiring 30 may protrude from the element body 20.
[0119] 19, the inductor wiring 330 is elliptical in a cross section perpendicular to the central axis CA. A virtual rectangle VR2 is drawn that circumscribes the inductor wiring 330 and has a first side along the first axis X and a second side along the second axis Z, and has a minimum area. In this case, the first side of the virtual rectangle VR2 is longer than the second side of the virtual rectangle VR2. In this way, it is more preferable that the long side of the virtual rectangle VR2 is parallel to the first axis X, because the end of the wiring cross section in the direction along the first axis X, where the magnetic flux is more concentrated, corresponds to a region of the first magnetic ribbon 41 with a small demagnetizing field.
[0120] In the above embodiment, the shape of the inductor wiring 30 in a cross section perpendicular to the central axis CA may be such that the second side along the second axis Z is longer than the first side along the first axis X. Even in this case, magnetic flux is concentrated at the first wiring end IP1, which is the end of the inductor wiring 30 in the first positive direction X1. Therefore, it is more preferable that the first wiring end IP1 in the wiring cross section where the magnetic flux is more concentrated corresponds to a region of the first magnetic ribbon 41 with a small demagnetizing field.
[0121] Furthermore, in a cross section perpendicular to the central axis CA, the shape of the inductor wiring 30 may be a shape that does not have symmetry, such as line symmetry or rotational symmetry, for example, when it includes one or more protruding parts. In this way, when symmetry is lost in a cross section perpendicular to the central axis CA, a place where the magnetic flux is concentrated more than other places occurs. It is preferable to determine the positional relationship of the second magnetic ribbon 41A so that the place where the magnetic flux is concentrated more than other places, such as a protruding part, becomes the first wiring end IP1.
[0122] Also, for example, in a cross section perpendicular to the central axis CA, the shape of the inductor wiring 30 may be a square or a perfect circle. In this case, a virtual rectangle VR drawn in a cross section perpendicular to the central axis CA is a square, and the first side of the virtual rectangle VR does not have to be longer than the second side of the virtual rectangle VR.
[0123] The first magnetic ribbon 41, the second magnetic ribbon 41A, and the third magnetic ribbon 41B are determined according to the shape of the inductor wiring 30 in a cross section perpendicular to the central axis CA. In the modification shown in FIG. 19, among the magnetic ribbons 40 stacked in the direction along the second axis Z with respect to the inductor wiring 330, the magnetic ribbon 40 having the shortest distance along the second axis Z from the first wiring end IP1 is one of the magnetic ribbons 40 included in the second part P2. Also, the first magnetic ribbon 41 is the magnetic ribbon 40 closest to the inductor wiring 30 among the magnetic ribbons 40 stacked with respect to the inductor wiring 30. Therefore, the first magnetic ribbon 41 is the magnetic ribbon 40 closest to the inductor wiring 30 in the first part P1 and the magnetic ribbon 40 closest to the inductor wiring 30 in the third part P3. That is, in the modification shown in FIG. 19, the second magnetic ribbon 41A is not the first magnetic ribbon 41.
[0124] In each of the above embodiments, the position of the inductor wiring 30 in the direction along the first axis X is not limited to the examples in each of the above embodiments. For example, the center of the inductor wiring 30 in the direction along the first axis X does not have to coincide with the center of the element body 20 in the direction along the first axis X.
[0125] In each of the above embodiments, the shape of the inductor wiring 30 is not limited to a straight line. It is sufficient that the inductor wiring 30 extends along the main surface MF of the magnetic ribbon 40, and may be, for example, a curved shape or a meandering shape as a whole. If the inductor wiring 30 extends on the same plane, it is easy to adjust the arrangement of the first wiring end IP1 of the inductor wiring 30 and the second magnetic ribbon 41A.
[0126] In each of the above embodiments, the material of the inductor wiring 30 is not limited to the examples of the above embodiments as long as it is a conductive material. For example, the material of the inductor wiring 30 may be a conductive resin.
[0127] In each of the above embodiments, the central axis CA and the first reference axis may not coincide with each other. The second reference axis may not coincide with the first axis X. For example, when the inductor wiring 30 has a meandering shape as described above, the central axis CA extends in a meandering shape. In this case, the first reference axis may be perpendicular to the second axis Z, and the second reference axis may be perpendicular to the second axis Z and intersect with the first reference axis. Even in this case, if a plurality of magnetic ribbons 40 are arranged in a direction along the first reference axis or a plurality of magnetic ribbons 40 are arranged in a direction along the second reference axis, the area of the magnetic ribbon 40 when viewed from a direction along the second axis Z is smaller than the case where one magnetic ribbon 40 is arranged at the same position along the second axis Z. Therefore, the eddy current generated in one magnetic ribbon 40 is smaller.
[0128] The positional relationship between the first virtual straight line VL1 passing through the first wiring end IP1 and the first range AR1 of the second magnetic ribbon 41A described in each of the above embodiments may be satisfied in any one of the cross sections of the inductor wiring 30 perpendicular to the central axis CA. That is, the positional relationship between the first virtual straight line VL1 and the first range AR1 of the second magnetic ribbon 41A may not be satisfied in all areas of the inductor wiring 30. It is not necessary that there is even one cross section that satisfies the positional relationship between the first virtual straight line VL1 passing through the first wiring end IP1 and the first range AR1 of the second magnetic ribbon 41A. That is, the position of the first wiring end IP1 of the inductor wiring 30 in the direction along the first axis X may not be within the first range AR1 of the second magnetic ribbon 41A, and may coincide with the end of the second magnetic ribbon 41A in the direction along the first axis X.
[0129] In each of the above embodiments, external electrodes may be connected to the portion of the inductor wiring 30 exposed from the element body 20. For example, external electrodes may be formed by coating, printing, plating, or the like on both end faces of the inductor wiring 30 in the direction along the central axis CA and both end faces of the element body 20 in the direction along the central axis CA.
[0130] In each of the above embodiments, the direction in which the magnetic ribbon 40 and the interlayer nonmagnetic portion 50 are stacked may not be perpendicular to the central axis CA and the first axis X due to manufacturing errors, etc. In each of the above embodiments, the magnetic ribbon 40, etc. are "stacked in the direction along the second axis Z" to allow for such manufacturing errors, etc.
[0131] In each of the above embodiments, the number of magnetic ribbons 40 stacked in the direction along the second axis Z may be two or more. In this case, the inductor wiring 30 and the interlayer nonmagnetic portion 50 may be disposed between the two magnetic ribbons 40.
[0132] In each of the above embodiments, the magnetic ribbons 40 and the interlayer nonmagnetic portions 50 do not have to be completely alternately stacked. In each of the above embodiments, the inductor wiring 30 does not have to be configured as a single layer, and the inductor wiring 30 may be configured as multiple layers.
[0133] In each of the above embodiments, the material of the magnetic ribbon 40 is not limited to the examples of the above embodiments as long as it is a magnetic material. For example, it may be Fe or Ni. It may also be an alloy containing Fe and Co. It may also be an alloy containing at least two of Fe, Ni, Co, Cr, Cu, Al, Si, B, and P. It may also be a mixture containing at least two of Fe, Ni, Co, Cr, Cu, Al, Si, B, and P. A magnetic material with a large magnetic permeability μ is suitable for improving the initial inductance Lin of the inductor component.
[0134] In each of the above embodiments, the metal magnetic body 45 of the magnetic ribbon 40 is not limited to an alloy of Fe and Ni, and may be Fe or Ni. It may also be an alloy containing Fe and Co. It may also be an alloy containing at least two of Fe, Ni, Co, Cr, Cu, Al, Si, B, and P. It may also be a mixture containing at least two of Fe, Ni, Co, Cr, Cu, Al, Si, B, and P. It may be changed as appropriate according to the characteristics required for the inductor component and the conditions of the sintering step S16.
[0135] In the above-mentioned embodiments, the insulating material 46 of the magnetic ribbon 40 is not limited to an oxide containing O element, which is a metal contained in the metal magnetic powder 212M before sintering. For example, the metal magnetic powder 212M before sintering may contain a small amount of Si element, and the Si element may be vitrified during sintering of the metal magnetic powder 212M and extruded onto the surface of the metal magnetic body 45 to become the insulating material 46 after sintering. In this case, the insulating material 46 contains Si element. For example, if the metal magnetic body 45 is an alloy containing Fe element, Si element, and Cr element, the metal magnetic body 45 is an FeSiCr alloy, and the Si element and the Cr element are present at the grain boundary. In other words, among the elements contained in the metal magnetic powder 212M before sintering, those having a high diffusion rate are present at the grain boundary. In this way, the gaps between the metal magnetic bodies 45 are filled with the components contained in the metal magnetic powder 212M that have a high diffusion rate compared to the magnetic material, and a sintered body with a higher density is obtained. In this case, the insulating material 46 contains Si element and Cr element. Furthermore, the insulating material 46 may not be present at the grain boundaries of the metal magnetic body 45 .
[0136] In each of the above embodiments, the material of the interlayer nonmagnetic portion 50 is not limited to the examples of the above embodiments, so long as it is a nonmagnetic material. The interlayer nonmagnetic portion 50 may be partially made of resin, such as acrylic resin, epoxy resin, or silicon resin. The same applies to the nonmagnetic portion 60 and the nonmagnetic film 70. The materials of the interlayer nonmagnetic portion 50, the nonmagnetic portion 60, and the nonmagnetic film 70 may be different from each other or may be partially different from each other, so long as they are nonmagnetic materials. In these cases, this can be achieved by coating the outer surface of the individual portion 201 with resin or filling the space with resin from the outside after the sintering step S16. In addition, when the interlayer nonmagnetic portion 50 is formed of a sintered body as in the manufacturing method described in the second embodiment, a material that can be sintered, such as alumina, silica, crystallized glass, or amorphous glass, is suitable as the nonmagnetic paste. Furthermore, the materials of the interlayer nonmagnetic portion 50, the nonmagnetic portion 60 and the nonmagnetic film 70 may be nonmagnetic ceramics other than alumina or glass, or nonmagnetic inorganic substances containing these, or mixtures of these including voids.
[0137] Furthermore, when the nonmagnetic paste is resin, the gaps between the magnetic ribbons 40 are formed due to scattering of the resin, but for example, the gaps may be the interlayer nonmagnetic parts 50. Furthermore, after the magnetic layer 212 is fired in sheets, the sheets may be bonded together with a resin layer, which is an adhesive, and the interlayer nonmagnetic parts 50 may be made of resin.
[0138] In the above embodiment, the interlayer nonmagnetic portion 50, the nonmagnetic portion 60, and the nonmagnetic film 70 may be integrated or may be separate members. For example, the interlayer nonmagnetic portion 50 may be hollow, or may be configured with an oxide film formed by oxidizing the surface of the magnetic ribbon 40 serving as an insulator.
[0139] In the above embodiment, the interlayer nonmagnetic portions 50 may be omitted. In this case, the magnetic ribbons 40 adjacent to each other in the direction along the second axis Z may be in direct contact with each other. In the above embodiment, the nonmagnetic portion 60 may be omitted. In this case, the magnetic ribbons 40 aligned in the direction along the first reference axis or the second reference axis may be in direct contact with each other. The nonmagnetic portion 60 may be present between the inductor wiring 30 and the magnetic ribbon 40. In this case, the nonmagnetic portion 60 can ensure insulation between the inductor wiring 30 and the magnetic ribbon 40.
[0140] Note that "multiple magnetic ribbons 40 are stacked" and "multiple magnetic ribbons 40 are arranged" specifically refer to the case where adjacent magnetic ribbons 40 are completely or partially insulated from each other or the case where a microscopic physical boundary exists. For example, this does not include a state where the magnetic ribbons 40 are sintered and completely integrated with each other.
[0141] In each of the above embodiments, as long as the second magnetic ribbon 41A exists in at least one of the first portion P1 and the third portion P3, the configurations of the magnetic ribbon 40, the interlayer nonmagnetic portion 50, and the nonmagnetic portion 60 can be changed. For example, the entire portion of the second portion P2 except for the inductor wiring 30 may be composed of the magnetic ribbon 40 or the interlayer nonmagnetic portion 50.
[0142] According to each of the above embodiments, two magnetic ribbons 40 are arranged in the direction along the first axis X at the same position along the second axis Z, and two are arranged in the direction along the central axis CA, i.e., the first reference axis. That is, when "M" and "N" are positive integers, "M" magnetic ribbons 40 are arranged in the direction along the first reference axis at the same position along the second axis Z, and "N" magnetic ribbons 40 are arranged in the direction along the first axis X, i.e., the second reference axis, and both "M" and "N" are 2. In each of the above embodiments, "M", which is the number of magnetic ribbons 40 arranged in the direction along the second reference axis, may be 1 or 3 or more. Also, "N", which is the number of magnetic ribbons 40 arranged in the direction along the central axis CA, may be 1 or 3 or more. When at least one of "M" and "N" is 2 or more, the area of each magnetic ribbon 40 when viewed from the second axis Z can be reduced, making it easier to reduce loss due to eddy current.
[0143] In each of the above embodiments, the dimensions of the magnetic ribbons 40 in the direction along the second axis Z may be different. When the dimension of the magnetic ribbon 40 in the direction along the second axis Z is small, a manufacturing error of about 20% may occur depending on the manufacturing method. Therefore, the dimension of the magnetic ribbon 40 in the direction along the second axis Z can be considered to be approximately equal if it is 80% or more and 120% or less of the average value of the dimensions of the magnetic ribbons 40 in the direction along the second axis Z. Note that the dimension of one magnetic ribbon 40 in the direction along the second axis Z is the smallest dimension in the direction along the second axis Z of one image enlarged by an electron microscope at a magnification between 1000 times and 10000 times. Also, the dimension of the magnetic ribbons 40 in the direction along the second axis Z is the average value of the dimensions of one magnetic ribbon 40 in the direction along the second axis Z measured in one image in which five or more magnetic ribbons 40 are included in the electron microscope.
[0144] The dimensions of the multiple magnetic ribbons 40 in the direction along the second axis Z do not have to be identical to each other, and may vary by more than 20% from the average value. In each of the above embodiments, the dimensions of the interlayer nonmagnetic parts 50 in the direction along the second axis Z may be different. If the dimension of the interlayer nonmagnetic parts 50 in the direction along the second axis Z is small, a manufacturing error of about 20% may occur depending on the manufacturing method. Therefore, the dimension of the interlayer nonmagnetic parts 50 in the direction along the second axis Z can be considered to be approximately equal if it is 80% or more and 120% or less of the average dimension of the dimensions of the interlayer nonmagnetic parts 50 in the direction along the second axis Z. Note that the dimension of one interlayer nonmagnetic part 50 in the direction along the second axis Z is the smallest dimension in the direction along the second axis Z of a single image enlarged by an electron microscope at a magnification between 1000 times and 10000 times. In addition, the dimension of the multiple interlayer nonmagnetic portions 50 in the direction along the second axis Z is the average value of the dimension of one interlayer nonmagnetic portion 50 in the direction along the second axis Z measured using an electron microscope in a single image that contains five or more interlayer nonmagnetic portions 50.
[0145] The dimensions of the multiple interlayer nonmagnetic parts 50 in the direction along the second axis Z do not have to be identical to one another, and may vary by more than 20% from the average value. In each of the above embodiments, the number and positions of the nonmagnetic portions 60 are not limited to those in the above embodiments. The number and positions of the nonmagnetic portions 60 may be changed according to the number and positions of the magnetic ribbons 40 in the direction along the first axis X or the direction along the central axis CA. The size of the nonmagnetic portions 60 may also be changed appropriately according to the intervals between the magnetic ribbons 40 at the same positions in the direction along the second axis Z.
[0146] In each of the above embodiments, the non-magnetic film 70 may be omitted. When the non-magnetic film 70 is omitted, the coating process S17 may be omitted in the method for manufacturing the inductor component 110 in the second embodiment. In addition, in the coating process S17, the non-magnetic film 70 may be formed by applying the non-magnetic film 70 to the entire outer surface of the individual portion 201 and then partially scraping it off to expose the inductor wiring 30.
[0147] In the second embodiment, the configuration of the composite part 80 is not limited to the example of the second embodiment. For example, the non-magnetic base material 82 may be an insulating thermoplastic resin such as alumina, epoxy resin, or acrylic resin. The composite part 80 may be an integrally molded body, not a laminated structure like the magnetic ribbons 40 of the first part P1 and the third part P3. In manufacturing such a composite part 80, for example, after the sintering step S16 and before the coating step S17, a resin may be filled into the area constituting the composite part 80.
[0148] In the manufacturing method of the inductor component 110 in the second embodiment, a sheet lamination method in which a plurality of sheets are formed, then laminated and pressure-bonded is exemplified, but the method is not limited to this. For example, a print lamination method in which a plurality of sheets are formed and laminated in sequence may be used. In this case, the split magnetic layer 212D is formed on the wiring pattern 221, so that the split magnetic layer 212D is disposed above the wiring pattern 221.
[0149] In the method for manufacturing inductor component 110 in the second embodiment described above, second sheet 220 may include magnetic layer 212 or nonmagnetic layer 211 instead of negative pattern 222, or may include magnetic layer 212 and nonmagnetic layer 211. When magnetic layer 212, nonmagnetic layer 211, and in-groove nonmagnetic portion 213 are provided instead of negative pattern 222, inductor component 10 in the first embodiment can be manufactured. Furthermore, negative pattern 222 may include at least either a magnetic material or a nonmagnetic material.
[0150] In the manufacturing method of inductor component 110 in the second embodiment, singulation step S15 may be omitted. When first sheet 210 and second sheet 220 for only one individual portion 201 are prepared, singulation step S15 may be omitted.
[0151] In the manufacturing method of the inductor component 110 described in the second embodiment, the portion corresponding to the first portion P1 or the third portion P3 has a plurality of magnetic ribbons 40 and an interlayer nonmagnetic portion 50. Here, if the second sheet 220 is omitted, a laminated sheet is formed by laminating a plurality of first sheets 210. If this laminated sheet is sintered, a magnetic sheet in which the magnetic ribbons 40 are sintered can be manufactured. In this magnetic sheet, a plurality of magnetic ribbons 40 are laminated in a direction along the second axis Z, i.e., an orthogonal axis perpendicular to the main surface MF of the magnetic ribbons 40. Furthermore, two magnetic ribbons 40 are lined up at the same position along the orthogonal axis in a direction along the first axis X, i.e., a first parallel axis parallel to the main surface MF of the magnetic ribbons 40. Furthermore, two magnetic ribbons 40 are lined up at the same position along the orthogonal axis in a direction along the center axis CA, i.e., a second parallel axis perpendicular to the orthogonal axis and the first parallel axis.
[0152] In each of the above embodiments, the magnetic ribbons 40 do not have to be arranged regularly. In particular, the magnetic ribbons 40 may be arranged partially irregularly. In each of the above embodiments, the element body 20 may contain a composite body in addition to the magnetic ribbons 40. For example, the sintered individual portion 201 may be covered with a composite body containing a powdered magnetic material, so that the composite body is disposed on the outside of the sintered individual portion 201.
[0153] In the above embodiments, an inductor component is given as an example of an electronic component, but any electronic component, such as a multilayer capacitor component, may be used. Similarly, a method for manufacturing an inductor component is given as an example of a method for manufacturing an electronic component, but any electronic component may be used. In this case, the wiring does not need to be inductor wiring, and may be flat wiring like a capacitor, or may be wiring of other known shapes.
[0154] The element described in Patent Document 1 aims to improve the properties of the magnetic material, such as the saturation magnetic flux density Bs, by increasing the filling rate of the inorganic filler. However, the technology described in Patent Document 1 is premised on a structure in which inorganic filler particles are randomly dispersed, and no consideration is given to the structures of other magnetic materials.
[0155] Such a magnetic sheet is suitable as a sheet that is required to be permeable to magnetic flux and to have insulating properties, such as the element body 20 of the inductor component of each of the above embodiments. Moreover, with such a method for manufacturing a magnetic sheet, it is easy to efficiently manufacture a structure in which the magnetic ribbons 40, which are sintered bodies, are regularly arranged.
[0156] The technical ideas that can be understood from the above embodiments and modifications will be described below. <Appendix 1> The magnetic strips are laminated in a direction perpendicular to a main surface of the magnetic strips, and the magnetic strips are made of a sintered magnetic material. When "M" and "N" are positive integers and at least one of "M" and "N" is 2 or more, The magnetic ribbons are arranged in a number "M" in the direction along the first reference axis and in a number "N" in the direction along the second reference axis at each position in the stacking direction. Magnetic sheet.
[0157] <Appendix 2> forming a non-magnetic layer from a non-magnetic paste containing a non-magnetic material, forming a magnetic layer on the non-magnetic layer from a magnetic paste containing a magnetic material, dividing the magnetic layer by grooves, and filling the grooves with the non-magnetic paste containing a non-magnetic material to form divided magnetic layers; A plurality of the divided magnetic layers are stacked to form a divided magnetic layer group; The divided magnetic layer group is fired to form the nonmagnetic layers into interlayer nonmagnetic portions of the sintered body, and the magnetic layers into magnetic ribbons of the sintered body. A method for manufacturing a magnetic sheet. [Explanation of symbols]
[0158] 10, 110, 310...Inductor components 20…Base 30,330…Inductor wiring 40...Magnetic ribbon 41…First magnetic strip 41A…Second magnetic ribbon 45...Metal magnetic material 46...Insulating materials 50…Interlayer nonmagnetic part 60...Non-magnetic part 70...Nonmagnetic film 80…Composite section 210…1st sheet 211...Nonmagnetic layer 212...Magnetic layer 220…Second seat 221...Wiring pattern AR1: First range CA…Central axis MF: Main surface MP1...1st end MP2…2nd end VL: Virtual line VR: Virtual rectangle X…1st axis Z…Second axis S11: First sheet preparation process S12: Second sheet preparation process S13…Lamination process S14… Crimping process S15…Singulation process S16…Sintering process
Claims
1. an element body having a plurality of flat magnetic ribbons made of a sintered magnetic material, the plurality of magnetic ribbons being stacked in a stacking direction that is a direction perpendicular to a main surface of the magnetic ribbons; wiring extending along the main surface inside the element body; When "M" and "N" are positive integers, and at least one of "M" and "N" is 2 or more, and among the plurality of magnetic strips, the magnetic strip closest to the wiring in the stacking direction is defined as a first magnetic strip, the plurality of magnetic strips are arranged in the same position as the first magnetic strip in the stacking direction, in a direction along a first reference axis perpendicular to the stacking direction, in a number "M", and arranged in a direction along a second reference axis perpendicular to the stacking direction and the first reference axis, in a number "N", The element body has a non-magnetic portion made of a sintered non-magnetic material and located between the magnetic ribbons adjacent in the direction along the first reference axis or between the magnetic ribbons adjacent in the direction along the second reference axis. Electronic components.
2. The magnetic ribbons are arranged in a number "M" in the direction along the first reference axis and in a number "N" in the direction along the second reference axis at each position in the stacking direction. The electronic component according to claim 1 .
3. The magnetic ribbon contains at least one of Fe, Ni, an alloy containing Fe and Si, an alloy containing Fe and Ni, and an alloy containing Fe and Co. The electronic component according to claim 1 or 2.
4. In the magnetic ribbon, a plurality of metal magnetic particles are bonded via an insulating material. The electronic component according to any one of claims 1 to 3.
5. The insulating material contains an O element. The electronic component according to claim 4.
6. The insulating material contains Si element. The electronic component according to claim 4 or 5.
7. The insulating material contains Cr. The electronic component according to any one of claims 4 to 6.
8. When an axis along which the wiring extends is defined as a central axis, an axis along the main surface in a cross-sectional view perpendicular to the central axis is defined as a first axis, an axis perpendicular to the main surface in the cross-sectional view is defined as a second axis, and one of two directions along the first axis is defined as a first positive direction, In the cross-sectional view, an end of the wiring in the first positive direction is defined as a first wiring end; Among the magnetic ribbons stacked on the wiring in a direction along the second axis, the magnetic ribbon having the shortest distance from an end of the first wiring in a direction along the second axis is designated as a second magnetic ribbon, When a range of the second magnetic ribbon excluding both ends in a direction along the first axis is defined as a first range, When a virtual line is drawn passing through the first wiring end and extending in a direction along the second axis, the virtual line passes through the first range of the second magnetic ribbon. The electronic component according to any one of claims 1 to 7.
9. The dimension of the second magnetic strip in the stacking direction is 80% or more and 120% or less of the average dimension of the plurality of magnetic strips arranged in the stacking direction relative to the second magnetic strip. The electronic component according to claim 8.
10. an element body having a plurality of flat magnetic ribbons made of a sintered magnetic material, the plurality of magnetic ribbons being stacked in a stacking direction that is a direction perpendicular to a main surface of the magnetic ribbons; wiring extending along the main surface inside the element body; The element body has interlayer nonmagnetic portions made of a sintered nonmagnetic material and located between adjacent magnetic thin strips in the stacking direction of the plurality of magnetic thin strips. Electronic components.
11. the element body includes a plurality of the interlayer nonmagnetic portions, The dimension of one of the interlayer nonmagnetic portions in the stacking direction is 80% or more and 120% or less of the average dimension of the plurality of interlayer nonmagnetic portions in the stacking direction. The electronic component according to claim 10.
12. forming a non-magnetic layer from a non-magnetic paste containing a non-magnetic material, forming a magnetic layer on the non-magnetic layer from a magnetic paste containing a magnetic material, dividing the magnetic layer by grooves, and filling the grooves with the non-magnetic paste containing a non-magnetic material to form divided magnetic layers; forming a laminate by disposing the divided magnetic layer above a wiring pattern formed of a conductive paste containing a conductive material; By firing the laminate, the wiring pattern is converted into wiring of the sintered body, the nonmagnetic layer is converted into an interlayer nonmagnetic portion of the sintered body, and the magnetic layer is converted into a magnetic thin strip of the sintered body. A method for manufacturing electronic components.
13. preparing a first sheet by forming the divided magnetic layer into a sheet shape; preparing a second sheet by forming the wiring pattern on a sheet-like substrate; The first sheet and the second sheet are pressed together to form the laminate. The method for manufacturing an electronic component according to claim 12.
14. The laminate is formed by forming the divided magnetic layers on the wiring pattern. The method for manufacturing an electronic component according to claim 12.
15. The wiring pattern is formed on a substrate, and a negative paste containing at least one of a magnetic material and a non-magnetic material is filled in the substrate on which the wiring pattern is not formed, thereby forming a negative pattern. The method for manufacturing an electronic component according to any one of claims 12 to 14.
16. When forming the laminate, a plurality of the split magnetic layers are laminated. The method for manufacturing an electronic component according to any one of claims 12 to 15.
17. When forming the laminate, a plurality of individual pieces each formed by the wiring pattern and the divided magnetic layer are arranged in a matrix form; Dividing the laminate into individual pieces. The method for manufacturing an electronic component according to any one of claims 12 to 16.
Citation Information
Patent Citations
Production of laminated magnetic material parts
JP1993190367A
Magnetic material, method of producing the same, magnetic sheet using the same and antenna device
JP2006174223A
Inductor component, package component, and switching regulator
JP2019192920A
Inductance element and electronic apparatus
JP2020088289A