Welded joint and manufacturing method thereof

The described method enhances spot welding of four steel plates by positioning a mild steel plate on the outermost side and applying pressure around the electrode tips to promote thickness-direction melting, achieving high joint strength and preventing dust, addressing the limitations of conventional methods.

JP7556834B2Active Publication Date: 2024-09-26KOBE STEEL LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021148140
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-09-10
Publication Date
2024-09-26
Estimated Expiration
2041-09-10

Smart Images

  • Figure 0007556834000004
    Figure 0007556834000004
  • Figure 0007556834000005
    Figure 0007556834000005
  • Figure 0007556834000003
    Figure 0007556834000003
Patent Text Reader

Abstract

To provide a weld joint having high joint strength by superimposing four steel plates including a soft steel plate and a high strength steel plate and performing spot welding.SOLUTION: A weld joint is obtained by superimposing four steel plates and performing spot welding, wherein the four steel plates include at least one soft steel plate having tensile strength of 270 MPa or more and less than 590 MPa, and at least two high strength steel plates having tensile strength of 980 MPa or more. The first soft steel plate is arranged on the outermost side of the four steel plates, the high strength steel plate is superimposed and arranged on one side of the first soft steel plate, a nugget formed by spot welding satisfies an expression (1) and a plate thickness retention rate defined by an expression (2) is 84% or more. Expression (1): dN / √t1≥3.0. In the expression, dN(mm) is a nugget diameter on a contact surface where the soft steel plate and the high strength steel plate are brought into contact with each other, and t1(mm) is a plate thickness of the soft steel plate brought into contact with the high strength steel plate. Expression (2): plate thickness retention rate (%)=(minimum thickness of weld joint) / (total plate thickness of four steel plates)×100.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to welded joints and methods for making the same. [Background technology]

[0002] The body of an automobile is made up of a structure made of steel plates joined together, so the technology for joining steel plates is extremely important. Spot welding is used as a method for joining steel plates, in which overlapping steel plates are sandwiched between electrodes and joined by melting the steel plates using Joule heat generated by passing an electric current through them.

[0003] For example, Patent Document 1 describes a lap resistance spot welding method in which a sheet assembly of three or more overlapping steel sheets is clamped and pressed by a pair of welding electrodes while passing current through them to weld the contact points of each steel sheet. The method of Patent Document 1 includes a step of assembling and welding the thinnest of the steel sheets so that it contacts one of the pair of welding electrodes, and a phosphate treatment film, chromate treatment film, organic film, or inorganic film is formed at least on the overlapping surfaces of the thinnest steel sheet and the steel sheet adjacent to the thinnest steel sheet.

[0004] Patent Document 2 describes a manufacturing method for manufacturing a resistance spot welded joint by resistance spot welding a plate assembly made of overlapping multiple metal plates. In the manufacturing method of Patent Document 2, the plate assembly is a plate assembly having a plate thickness ratio of 5 or more, in which a thin plate is overlapped on at least one of two or more overlapping thick plates. The resistance spot welding is performed in three stages, a first stage, a second stage, and a third stage, and the second stage welding is performed with a higher pressure, a lower current or the same current, and a longer current flow time or the same current flow time compared to the first stage welding, and further the third stage repeatedly passes a current higher than that of the second stage.

[0005] Patent Document 3 describes a manufacturing method for a resistance spot welded joint similar to that of Patent Document 2, and is the same as Patent Document 2 except that the third stage welding is repeated by applying a higher pressure and a higher current than the second stage.

[0006] Patent Document 4 describes a lap welding method for steel plates in which two or more steel plates are overlapped and welded, and a lap welded joint for steel plates. In the lap welding method of Patent Document 4, the two or more steel plates include a surface side steel plate having a plate thickness in the range of 0.3 to 1 mm, and one or more thick steel plates having a plate thickness greater than that of the surface side steel plate. The ratio of the plate thickness of the surface side steel plate to the total plate thickness of the surface side steel plate and the one or more thick steel plates (total plate thickness / plate thickness of surface side steel plate) is 5 or more. Then, the two or more steel plates are overlapped so that the surface side steel plate is disposed on the surface side, and then welded using a combination of laser welding and spot welding.

[0007] Patent Document 5 describes a spot welding method in which a welding current is applied to the overlapping portion of two or more overlapping metal sheets to join them. In the method of Patent Document 5, by controlling the pressure applied to a part of the outer periphery of a pair of electrodes that applies current to the overlapping portion using a pressure member separate from the electrodes, it is possible to suppress the generation of spatter even when the welding current is increased, and to achieve a large nugget diameter.

[0008] Patent Document 6 discloses a welded joint formed by spot welding two overlapping steel plates having thicknesses of t1 and t2, in which the diameter of the nugget formed by spot welding is 3√{(t1+t2) / 2} or more (nugget diameters, t1 and t2 are all in mm) and the radius of curvature of both radial ends of the nugget in a cross section in the plate thickness direction is 0.3(t1+t2) or more. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent No. 4884958 [Patent Document 2] JP 2010-240739 A [Patent Document 3] JP 2010-240740 A [Patent Document 4] JP 2010-264503 A [Patent Document 5] JP 2014-28392 A [Patent Document 6] JP 2014-180686 A Summary of the Invention [Problem to be solved by the invention]

[0010] Generally, spot welding is only permitted for welding up to three steel plates. For example, when spot welding four overlapping steel plates, the overlapping surface between the second and third steel plates melts first. On the other hand, the overlapping surfaces between the first and second steel plates and the overlapping surfaces between the third and fourth steel plates are less likely to melt because they are strongly affected by the cooling caused by the electrode tip. As a result, the welding of these overlapping surfaces becomes insufficient, and the joint strength of the welded joint is insufficient.

[0011] In particular, when considering the structure of a car body, there are cases where multiple high-strength steel plates capable of withstanding a collision are arranged inside the car body, and mild steel plates (e.g., galvanized steel plates) that cover the car body are arranged on the outermost surface of the car body. In such steel plate assemblies, the high-strength steel plates in the interior have a higher electrical resistance than the mild steel plates on the outermost surface, and therefore heat up and melt preferentially. On the other hand, mild steel plates with relatively low electrical resistance are less likely to heat up and melt. In this way, the mild steel plate arranged on the outermost surface is prone to insufficient welding between the adjacent high-strength steel plates due to the effect of cooling by the electrode tip and insufficient heat generation caused by its relatively low electrical resistance.

[0012] In order to promote the welding of the outermost mild steel plate, it is considered effective to increase the welding current of the spot welding. However, if the welding current becomes too high, a phenomenon called "flash" occurs in which molten metal splashes. If flash occurs, the metal at the spot weld is reduced, and the joint strength may become insufficient. In addition, the molten metal splashes due to the flash, contaminating the surroundings of the weld, and the molten metal may damage the welding equipment and the worker. Therefore, the welding current can only be increased to a level where flash does not occur, and there are cases where the welding of the outermost mild steel plate cannot be sufficiently improved.

[0013] Patent Documents 1 to 6 do not specifically disclose spot welding of four overlapping mild steel plates and four high-strength steel plates, and do not consider the need to improve the welding of the outermost mild steel plate.

[0014] Therefore, an object of one embodiment of the present invention is to provide a welded joint having high joint strength, which is formed by overlapping and spot welding four steel plates, including a mild steel plate arranged on at least one outermost surface and two or more high-strength steel plates arranged on one side of the mild steel plate.Another embodiment of the present invention is to provide a manufacturing method capable of manufacturing such a welded joint. [Means for solving the problem]

[0015] Aspect 1 of the present invention is A welded joint made by overlapping four steel plates and spot welding them together, The four overlapping steel plates include at least one mild steel plate having a tensile strength of 270 MPa or more and less than 590 MPa, and at least two high-strength steel plates having a tensile strength of 980 MPa or more, The first mild steel plate is disposed on the outermost side of the four steel plates; The at least two high strength steel plates are arranged in a superimposed manner on one side of the first mild steel plate, The nugget formed by spot welding satisfies the following formula (1), and This is a welded joint having a thickness retention rate of 84% or more, as defined by the following formula (2). d N / √t1≧3.0 (1) where d N (mm) is the nugget diameter at the contact surface where the mild steel plate and the high strength steel plate are in contact with each other, t1 (mm) is the plate thickness of the mild steel plate in contact with the high strength steel plate. Plate thickness retention rate (%) = (minimum thickness of welded joint) / (total thickness of four steel plates) x 100 (2)

[0016] Aspect 2 of the present invention is The welded joint according to aspect 1, wherein a plate thickness t1 of the mild steel plate is smaller than a plate thickness of the high-strength steel plate in contact with the mild steel plate.

[0017] Aspect 3 of the present invention is The welded joint according to aspect 1 or 2, wherein the four steel plates are composed of the first mild steel plate and three high-strength steel plates arranged in a superimposed manner on one side of the first mild steel plate.

[0018] A fourth aspect of the present invention is A method for manufacturing a welded joint by spot welding overlapping portions of four steel plates, comprising the steps of: A step of stacking four steel plates including at least one mild steel plate having a tensile strength of 270 MPa or more and less than 590 MPa and at least two high-strength steel plates having a tensile strength of 980 MPa or more, overlapping the four steel plates such that a first of the mild steel plates is disposed on the outermost side of the four steel plates and the at least two high strength steel plates are disposed on one side of the first mild steel plate; A process of pressing and clamping the overlapping portion of the steel plate with a pair of electrodes and a pair of pressure members provided so as to surround the electrode tips of the electrodes, The pressure member is configured to apply pressure over a range of 180° or more in a circumferential direction centered on the tip of the electrode, The distance between the pressing tip of the pressing member and the electrode tip is 0.1 mm or more and 10.0 mm or less, A pressurizing and clamping step in which the overlapping portion is pressurized by the electrode tip with an electrode load of 1.5 kN or more and is pressurized by the pressing tip with a peripheral load of 0.1 to 1.0 times the electrode load; and welding the overlapping portion by passing a welding current of 5 kA or more and 15 kA or less through the pair of electrodes.

[0019] A fifth aspect of the present invention is A method for producing a welded joint according to aspect 4, wherein a plate thickness t1 of the mild steel plate is smaller than a plate thickness of the high-strength steel plate in contact with the mild steel plate. Effect of the Invention

[0020] According to the welded joint of one embodiment of the present invention, a welded joint having high joint strength can be realized. Also, according to the method for manufacturing a welded joint of another embodiment of the present invention, the welded joint of one embodiment can be manufactured. [Brief description of the drawings]

[0021] [Figure 1] 1A and 1B are diagrams showing a schematic configuration of an electrode and a pressure member for spot welding, in which FIG. 1A is a bottom view and FIG. 1B is a cross-sectional view taken along line AA in FIG. 1A. [Diagram 2] 2(a) and 2(b) are schematic cross-sectional views of an electrode and a pressure terminal for spot welding. [Diagram 3] FIG. 3(a) is a schematic perspective view showing a state in which four steel plates are welded together, and FIG. 3(b) is a schematic cross-sectional view taken along line XX in FIG. 3(a). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The inventors have noticed that when a welded joint is formed by spot welding a plate assembly in which four steel plates including a mild steel plate and a high-strength steel plate are stacked, if the mild steel plate is placed on the outermost surface, poor welding occurs between the mild steel plate and the adjacent high-strength steel plate, or the desired joint strength cannot be obtained, and have studied the cause. As a result, it has been found that if the molten pool is expanded in the thickness direction so as to melt the mild steel plate placed on the outermost surface, the molten pool expands in the lateral direction before it expands sufficiently in the thickness direction, and molten metal erupts from the gap between the plates, generating flash. When spot welding is performed, welding is performed at an electrode current below which flash does not occur, making it difficult to expand the molten pool in the thickness direction. As a result of extensive research by the inventors into how to expand the molten pool in the thickness direction while suppressing the generation of spatter, they discovered that by applying an appropriate amount of pressure to the overlapping portion around the spot welding electrodes, it is possible to block the route through which molten metal sprays out, suppressing the generation of spatter, and also to efficiently concentrate the heat generated by the passage of electricity between the electrodes, thereby suppressing the progression of melting in the lateral direction and the generation of spatter, and promoting melting in the thickness direction, which led to the completion of an embodiment of the present invention.

[0023] The manufacturing method of a welded joint according to an embodiment of the present invention is a method of spot welding overlapping portions of four steel plates, A step of stacking four steel plates including at least one mild steel plate having a tensile strength of 270 MPa or more and less than 590 MPa and at least two high-strength steel plates having a tensile strength of 980 MPa or more, overlapping the four steel plates such that a first of the mild steel plates is disposed on the outermost side of the four steel plates and the at least two high strength steel plates are disposed on one side of the first mild steel plate; A process of pressing and clamping the overlapping portion of the steel plate with a pair of electrodes and a pair of pressure members provided so as to surround the electrode tips of the electrodes, The pressure member is configured to apply pressure over a range of 180° or more in a circumferential direction centered on the tip of the electrode, The distance between the pressing tip of the pressing member and the electrode tip is 0.1 mm or more and 10.0 mm or less, A pressurizing and clamping step in which the overlapping portion is pressurized by the electrode tip with an electrode load of 1.5 kN or more and is pressurized by the pressing tip with a peripheral load of 0.1 to 1.0 times the electrode load; and welding the overlapping portion by passing a welding current of 5 kA or more and 15 kA or less through the pair of electrodes.

[0024] The manufacturing method for the welded joint makes it possible to spot weld four steel plates, including a mild steel plate on the outermost surface, which was not possible to weld sufficiently using conventional spot welding methods, by setting the pressure application range by the pressure member to 180° or more in the circumferential direction (more than 50% of the entire circumference), setting the electrode load to 1.5 kN or more, and setting the peripheral load to 0.1 to 1.0 times the electrode load. The welded joints obtained by this manufacturing method have the following characteristics:

[0025] The welded joint according to the embodiment of the present invention is formed by welding a mild steel plate having a tensile strength (TS) of 270 MPa or more and less than 590 MPa to a high-strength steel plate having a tensile strength of 980 MPa or more. The reason why the lower limit of the TS of the mild steel plate is set to 270 MPa is because the TS of a general mild steel plate is specified to be 270 MPa or more, and the reason why the upper limit is set to less than 590 MPa is that high-strength steel plates are not included. The reason why the lower limit of the TS of the high-strength steel plate is set to 980 MPa is that the high-strength steel plate is in the range of high strength levels that are difficult to spot weld, among high-strength steel plates, and the upper limit is not particularly limited, but is currently about 1900 MPa.

[0026] A welded joint according to an embodiment of the present invention is formed by overlapping four steel plates and spot welding them. When overlapping the four steel plates, one mild steel plate (referred to as a "first mild steel plate") is disposed as the outermost of the four steel plates, and at least two high-strength steel plates are disposed on one side of the first mild steel plate. Note that another steel plate may be disposed between the first mild steel plate and the at least two high-strength steel plates.

[0027] The four steel plates are composed of at least one mild steel plate and at least two high-strength steel plates. Specific combinations of the steel plates include a case where the four steel plates are composed of one mild steel plate and three high-strength steel plates (Pattern 1) and a case where the four steel plates are composed of two mild steel plates and two high-strength steel plates (Pattern 2). We will explain in detail specific examples of the order in which four steel plates are stacked (plate assembly) in two patterns: Pattern 1 and Pattern 2.

[0028] (Pattern 1: When the four steel plates consist of one mild steel plate and three high-strength steel plates) In pattern 1, one type of board assembly (board assembly (1-1)) is assumed. [Board group (1-1)] One mild steel plate (first mild steel plate) is placed on the outermost side of the four steel plates, and three high-strength steel plates are placed on one side of the first mild steel plate. When stacked in this way, the four steel plates are stacked in the following order: (i) first mild steel plate - (ii) high-strength steel plate - (iii) high-strength steel plate - (iv) high-strength steel plate.

[0029] (Pattern 2: When the four steel plates consist of two mild steel plates and two high-strength steel plates) In pattern 2, two types of board sets (board set (2-1) and board set (2-2)) are assumed. [Board group (2-1)] Two high-strength steel plates are sandwiched between two mild steel plates. In other words, one mild steel plate (first mild steel plate) is disposed on the outermost side of the four steel plates, and the other mild steel plate (referred to as the "second mild steel plate") is disposed on the outermost side of the four steel plates opposite the first mild steel plate. Then, two high-strength steel plates are placed in a stacked manner between the first mild steel plate and the second mild steel plate. When stacked in this manner, the four steel plates are stacked in the following order: (i) first mild steel plate - (ii) high-strength steel plate - (iii) high-strength steel plate - (iv) second mild steel plate.

[0030] [Board group (2-2)] Two mild steel plates are stacked, and two high-strength steel plates are stacked on one side of one of the mild steel plates. In other words, a first mild steel plate is placed on the outermost side of the four steel plates, two high-strength steel plates are stacked on one side of the first mild steel plate, and another mild steel plate (second mild steel plate) is placed between the first mild steel plate and the two high-strength steel plates. When stacked in this way, the four steel plates are stacked in the following order: (i) first mild steel plate - (ii) second mild steel plate - (iii) high-strength steel plate - (iv) high-strength steel plate. Since the second mild steel plate is present between the first mild steel plate and the high-strength steel plate, the first mild steel plate and the high-strength steel plate do not come into direct contact with each other.

[0031] In the welded joint according to the embodiment of the present invention, the nugget diameter (mm) at the contact surface between the mild steel plate and the high-strength steel plate adjacent to the mild steel plate satisfies formula (1). d N / √t1≧3.0 (1) where d N (mm) is the nugget diameter at the contact surface where the mild steel plate and the high strength steel plate are in contact with each other, t1 (mm) is the plate thickness of the mild steel plate in contact with the high strength steel plate.

[0032] Generally, joints formed by welding have N The larger the value of / √t1, the better the welded joint (e.g., the higher the joint strength). In this embodiment, as shown in formula (1), N By specifying that / √t1 is 3 or more, it is possible to obtain a welded joint with sufficiently high cross tensile strength.

[0033] The nugget diameter (diameter of the molten and solidified portion (nugget) generated in the molten portion), which is the most important factor for the weld strength (joint strength) of the welded portion, is generally required to be several times or more the square root of the plate thickness. In the embodiment of the present invention, it is considered that it is particularly important to control the nugget diameter formed on the surface of the mild steel plate which is difficult to melt, and the nugget diameter d N(mm) must be 3√t1 or more (t1 (mm) is the thickness of the mild steel plate), i.e., formula (1) must be satisfied. The nugget diameter is preferably 4√t1 or more, more preferably 5√t1 or more, and even more preferably 6√t1 or more.

[0034] The "nugget diameter" is based on the method for measuring the nugget diameter in a two- or three-layer lap weld described in "JIS Z3139:2009 Cross-sectional test method for spot, projection and seam welds." The method for measuring the nugget diameter in the embodiment of the present invention will be described in detail with reference to Figs. 3(a) and (b). FIG. 3(a) is a schematic perspective view showing an example of a plate assembly (corresponding to the above-mentioned [Plate assembly (1-1)]) including one mild steel plate and three high-strength steel plates. This figure shows, from above, a state in which four steel plates, consisting of one mild steel plate P1 and three high-strength steel plates P2, P3, and P4 stacked in this order, are welded together by a welded joint WJ. FIG. 3(b) is a schematic cross-sectional view of a plane (cross-section along line XX) passing through the vicinity of the center of the welded joint WJ in FIG. 3(a). As shown in FIG. 3(b), the diameter (width of nugget N) of the nugget N at the contact surface (or interface) between the mild steel plate P1 and the high-strength steel plate P2 is measured, and this is called the nugget diameter d N It is defined as:

[0035] Furthermore, for another plate combination, the nugget diameter d N " will be explained. In the case of the plate combination (2-1), there are two contact surfaces where the mild steel plate and the high strength steel plate are in contact with each other (the contact surface between the first mild steel plate and the high strength steel plate, and the contact surface between the second mild steel plate and the high strength steel plate). In this case, the nugget diameter d N is measured on both of the two contact surfaces. In the embodiment of the present invention, the nugget diameter d N By satisfying formula (1), a welded joint with sufficiently high cross tensile strength can be obtained.

[0036] In the case of the plate combination (2-2), there is one contact surface where the mild steel plate and the high strength steel plate are in contact (the contact surface between the second mild steel plate and the high strength steel plate). Nugget diameter d Nis measured at the interface between the second mild steel plate and the high strength steel plate.

[0037] The welded joint according to the embodiment of the present invention has a plate thickness retention rate defined by the formula (2) of 84% or more. Plate thickness retention rate (%) = (minimum thickness of the welded joint) / (total thickness of the four steel plates) × 100 (2)

[0038] The "minimum thickness of the weld joint" in formula (2) is the thinnest part of the weld joint WJ in the cross section passing through the weld joint WJ, and is indicated by the symbol t in Figure 3(b). WJ This refers to the thickness indicated by the symbol.

[0039] In the example of the plate set (1-1) shown in FIG. 3(b), the “total plate thickness of the four steel plates” in formula (2) is the sum (= t1 + t2 + t3 + t4) of the thickness t1 of the mild steel plate P1 and the thicknesses t2, t3, and t4 of the high-strength steel plates P2, P3, and P4. In the case of the plate set (2-1) and the plate set (2-2), the "total plate thickness of the four steel plates" also refers to the total thickness of each of the four steel plates.

[0040] As mentioned above, in general spot welding, the number of overlapping steel sheets is limited to three. Therefore, in order to overlap four steel sheets to create a welded joint, it is necessary to increase the welding current as much as possible. If a welding current that is too high is applied, the strength of the steel sheets is excessively reduced during welding, and the pressure applied by the electrode causes significant plastic deformation in the welded part. In some cases, spatter is generated from the welded part, causing a significant reduction in the plate thickness in the welded part directly below the electrode. As a result, the volume of the nugget in the welded part, which contributes to the strength of the joint, is reduced, which is assumed to be a factor in reducing and varying (instability) the strength of the joint.

[0041] In an embodiment of the present invention, the ratio of the plate thickness of the welded portion (= the minimum thickness of the spot-welded joint) to the total plate thickness before welding (= the total plate thickness of the steel plates before welding) is defined as the "plate thickness retention rate" in equation (2), and a plate thickness retention rate of 84% or more is determined to be a sound welded joint. The thickness retention is preferably 85% or more, and more preferably 87% or more.

[0042] The thickness of each of the four overlapping steel plates is arbitrary, but for example, the plate thickness t1 of the first mild steel plate provided on the outermost surface of the body of an automobile may be made smaller than that of the high-strength steel plate inside the body. Even in the case of steel plates of the same steel type, when overlapping and spot welding in the order of thin plate-thick plate-thick plate-thick plate, the overlapping surface between the thick plates melts preferentially, and melting does not occur at the overlapping surface between the thin plates-thick plates. This is because the thin plates are more strongly affected by the cooling by the electrode tip than the thick plates. Therefore, in the example of plate set (1-1), when the mild steel plates are thin and the high-strength steel plates are thick, they are overlapped in the order of "(i) the first mild steel plate as a thin plate-(ii) the high-strength steel plate as a thick plate-(iii) the high-strength steel plate as a thick plate-(iv) the high-strength steel plate as a thick plate." When such overlapping steel sheets are welded by conventional spot welding, the weld may be insufficient at the contact surface between (i) the thin first mild steel sheet and (ii) the thick high strength steel sheet.

[0043] However, the welded joint according to the embodiment of the present invention satisfies the above formula (1) and has a plate thickness retention rate defined by formula (2) of 84% or more, and therefore can achieve sufficient joint strength, so that even if the plate thickness t1 of the first mild steel plate on the outermost surface is thin, the welded joint can have sufficient joint strength. Therefore, the welded joint according to the embodiment of the present invention is also suitable for welding overlapping steel plates including thin mild steel plates.

[0044] Regarding the provision of formula (2), the action and effect in the welded joint in the case of plate assembly (1-1) has been explained. The welded joints in the cases of plate assembly (2-1) and plate assembly (2-2) also have the first mild steel plate provided on the outermost surface, so that by satisfying formula (2), the same action and effect can be achieved.

[0045] Next, a preferred method for producing a welded joint will be described. The method of manufacturing a welded joint by spot welding the overlapping parts of four steel plates is as follows: A step of stacking four steel plates including at least one mild steel plate having a tensile strength of 270 MPa or more and less than 590 MPa and at least two high-strength steel plates having a tensile strength of 980 MPa or more; a step of pressing and clamping the overlapping portion of the steel plate with a pair of electrodes and a pair of pressure members provided so as to surround the electrode tips of the electrodes; and welding the overlapping portion by passing a welding current of 5 kA or more and 15 kA or less through the pair of electrodes.

[0046] (1. Layering process) Four steel plates are prepared, including at least one mild steel plate having a tensile strength of 270 MPa or more and less than 590 MPa, and at least two high-strength steel plates having a tensile strength of 980 MPa or more. The four steel plates are overlapped such that one mild steel plate (first mild steel plate) is disposed on the outermost side of the four steel plates, and at least two high-strength steel plates are disposed overlapping on one side of the first mild steel plate. This makes it possible to form an overlapping portion of four steel plates with a mild steel plate disposed on at least one outermost surface. The thickness of each of the four overlapping steel plates may be any thickness, but the plate thickness t1 of the first mild steel plate provided on the outermost surface may be smaller than that of the high-strength steel plate in contact with the first mild steel plate.

[0047] (2. Process of clamping the overlapping portion under pressure) The overlapping portions of the steel plates are pressed and clamped by a pair of electrodes and a pair of pressure members provided so as to surround the electrode tips of the electrodes. Four overlapping steel plates are pressed from above and below with electrodes while an electric current is passed through them, causing the interface between the plates to melt due to Joule heat between the plates. In preparation for this, the steel plates are pressed and fixed in place in the welding device before the current is passed through. The steel plates are clamped and pressed between the electrodes and the pressure member. By applying pressure around the electrodes, the pressure member can suppress the lateral growth of the molten pool and promote its growth in the thickness direction.

[0048] The electrodes and the pressure members will be described in detail with reference to FIGS. FIG. 1 is a diagram showing a schematic configuration of an electrode 1 for spot welding and a pressing member 2, where (a) is a bottom view and (b) is a cross-sectional view taken along line AA in FIG. 1(a). 1 only shows the electrode 1 and pressure member 2 that are placed on the upper side of the overlapped steel sheets, and when welding, a similar electrode 1 and pressure member 2 with the top and bottom reversed are also placed on the lower side of the overlapped steel sheets. As will be described later, the overlapped portion of the steel sheets is pressed between the upper and lower electrodes and between the upper and lower pressure members.

[0049] The electrode 1 shown in FIG. 1 is a cylindrical smooth-tip electrode, and the diameter of the electrode tip 1x is D. The electrode 1 is composed of an upper electrode shown in FIG. 1(b) and a lower electrode not shown, forming a pair of electrodes. The pair of electrodes holds the overlapping portion of four stacked steel sheets from both sides, and a current is passed through the overlapping portion. The shape of the electrode 1 can be a smooth-tip type as shown in FIG. 1(b), or an electrode shape commonly used in spot welding, such as a DR type.

[0050] The pressure member 2 is a member provided so as to surround the electrode tip 1x of the electrode 1. The pressure tip 2x of the pressure member 2 comes into contact with the overlapping steel plates and applies pressure thereto. The pressure tip 2x may be, for example, ring-shaped or may have another shape. As long as the steel plates are not locally deformed when softened during welding, the pressure tip 2x may be in a form in which a part of the ring shape is cut out to provide a non-pressure portion. For example, the pressure tip 2x may be in a C-shape with one part cut out, or in a shape divided into multiple arcs with two or more parts cut out (for example, a shape divided into three arcs as shown in FIG. 1(a)).

[0051] The configuration of the pressure member 2 shown in FIGS. 1(a) and 1(b) will be described in detail below. As shown in Fig. 1(a), the pressing member 2 is composed of three pressing parts 21, 22, and 23. The three pressing parts 21, 22, and 23 are arranged so as to surround the periphery of the electrode tip 1x of the electrode 1. The pressing parts 21, 22, and 23 each have a sector-shaped pressing tip 2x with a thickness of t and a central angle of a1, a2, or a3 in the circumferential direction centered on the electrode tip 1x. Adjacent pressing parts 21, 22, and 23 are separated from each other by a gap with a central angle of b1, b2, or b3 in the circumferential direction centered on the electrode tip 1x.

[0052] The pressure member 2 is designed to be able to apply pressure over a range of 180° or more (50% of the entire circumference) in the circumferential direction centered on the electrode tip 1x. Here, "180° or more" means that when the pressure member 2 is divided into multiple (three) pressure parts 21, 22, 23 as shown in Fig. 1(a), the sum of the central angles a1, a2, a3 of the pressure tips 2x of each of the pressure parts 21, 22, 23 is 180° or more. In other words, the sum of the central angles b1, b2, b3 of the gaps is 180° or less. If the angular range over which pressure can be applied by the pressure member 2 is 180° or more, the generation of spatter can be suppressed even when a relatively large welding current is applied to weld four steel plates. The angular range over which pressure can be applied by the pressure member 2 is preferably 270° or more (75% or more of the entire circumference), and more preferably 360° (100% of the entire circumference, which corresponds to the case where the pressure tip 2x of the pressure member 2 is ring-shaped).

[0053] As shown in FIG. 1(b), the pressure tip 2x of each of the pressure parts 21, 22, and 23 and the electrode tip 1x of the electrode 1 are separated by a clearance CL. In the embodiment of the present invention, the clearance CL is set to 0.1 mm or more and 10.0 mm or less. If the clearance CL between the pressure tip 2x and the electrode tip 1x is too narrow, the electrode 1 and the pressure member 2 come into contact with each other, current flows from the pressure member 2 to the electrode 1, and the effect of suppressing the lateral spread of the molten pool cannot be obtained. If the clearance CL is too wide, the effect of pressing the overlapping portion around the electrode 1 with the pressure member 2 decreases, and the effect of suppressing the generation of spatter cannot be fully obtained. The lower limit of the clearance CL is preferably 0.5 mm, more preferably 1.0 mm, and the upper limit of the clearance CL is preferably 8.0 mm, more preferably 6.0 mm.

[0054] The overlapping portion of the steel sheets is pressed between the electrode tips 1x of a pair of upper and lower electrodes 1. Furthermore, the periphery of the portion of the overlapping portion pressed by the electrode tips 1x is pressed between the pressing tips 2x of pressing members 2 arranged above and below.

[0055] When the load applied to the overlapping portion by the electrode 1 (referred to as the "electrode load") is high, it is highly effective in suppressing deformation of the steel plates caused by heating and melting during welding, and in suppressing the occurrence of flash. However, if the electrode load is too high, the welded portion may be crushed and deformed during welding, which may reduce the remaining plate thickness rate. If the electrode load is too low, the amount of heat generated in the welded portion during welding that is dissipated through the electrode 1 decreases, making surface flash more likely to occur. The lower limit of the electrode load is 1.5 kN, preferably 2.0 kN. The electrode load should not be excessively high, and the upper limit is preferably 7.0 kN, more preferably 6.0 kN.

[0056] The load applied to the overlapping portion by the pressure member 2 (referred to as the "periphery load") is between 0.1 and 1.0 times the electrode load. If the peripheral load is too low, the effect of suppressing spattering cannot be obtained. Due to the limitations of the welding equipment, there is an upper limit to the total load of the peripheral load and electrode load. If the peripheral load is increased, the electrode load must be reduced, which reduces the amount of heat dissipated through the electrode 1 and makes surface spattering more likely to occur. For this reason, the peripheral load must be set appropriately so that sufficient electrode load can be secured. The lower limit of the peripheral load is preferably 0.2 times, more preferably 0.3 times, in terms of the ratio of the electrode load, and the upper limit of the peripheral load is preferably 0.8 times, more preferably 0.5 times, in terms of the ratio of the electrode load.

[0057] The electrode 1 may be made of any of the electrode materials commonly used in spot welding, such as pure copper, chromium copper, and alumina-dispersed copper. The material of the pressure member 2 may be either a non-conductive or conductive material. The material of the pressure member 2 must have a strength sufficient to prevent plastic deformation when pressure is applied.

[0058] (3. Process of welding overlapping parts) The overlapping portion is welded by passing a welding current of 5 A to 15 kA between the pair of electrodes. The upper limit of the welding current is preferably 13 kA, and more preferably 10 kA. EXAMPLES

[0059] - Welded test specimen A 270 MPa-class GA steel plate with a thickness of 0.6 mm was prepared as the mild steel plate, and a 1180 MPa-class uncoated steel plate (CR steel plate) with a thickness of 1.4 mm was prepared as the high-strength steel plate. The mild steel plate and the high-strength steel plate were stacked according to the plate combination shown in Table 1 to prepare a welded test specimen (a laminate of four steel plates).

[0060] Welding method The welding machine used was a DC inverter spot welding machine with an air cylinder type pressure mechanism. The electrode 1 used was a chromium copper electrode tip with a DR shape (electrode diameter 13.0 mm, tip diameter 6.0 mm) as shown in Figures 2(a) and (b). A pipe-shaped pressure member that covers the periphery of the electrode 1 was used as the pressure member 2. By using the pipe-shaped pressure member 2, a peripheral load can be applied in a range of 360° in the circumferential direction centered on the electrode tip 1x. In addition to the pressure mechanism for the electrode 1, an air cylinder for applying pressure to the pressure member 2 was prepared. A pipe-shaped pressure member 2 was pressed against the overlapping portion of the welded test pieces, and a peripheral load was applied to the periphery of the electrode tip 1x.

[0061] In order to confirm the effect of the clearance CL between the electrode 1 and the pressure member 2 on the welded joint, two types of pressure members 2 with different shapes of pressure tips 2x were used (Figs. 2(a) and (b)). The pressure member 201 shown in Fig. 2(a) has a diameter tapered toward the tip near the pressure tip 2x. The dimensions of the pressure member 2 are: inner diameter of the parallel portion (non-reduced portion) is 14.0 mm, inner diameter of the pressure tip 2x is 10.0 mm, and thickness of the pressure member is 1.0 mm. The clearance CL between the pressure tip 2x and the electrode tip 1x is 2.0 mm. The pressure member 202 shown in Fig. 2(b) has a constant diameter throughout. In other words, the pressure member 2 does not have a reduced diameter near the pressure tip 2x. The dimensions of the pressure member 2 are an inner diameter of 14.0 mm and a wall thickness of 1.0 mm. The clearance CL between the pressure tip 2x and the electrode tip 1x is 4.0 mm.

[0062] The plate-assembly welded test specimens shown in Table 1 were clamped under pressure under the conditions (electrode load by electrode 1, outer circumferential load by pressure member 2, and clearance CL between pressure tip 2x and electrode tip 1x) shown in Table 2. Note that a clearance CL of "2.0 mm" means that the pressure member 201 shown in Fig. 2(a) was used, and a clearance CL of "4.0 mm" means that the pressure member 202 shown in Fig. 2(b) was used. Also, for C1 to C4, the pressure member 2 was not used. Thereafter, spot welding was performed by passing a welding current between the electrodes as shown in Table 2. The current passing time was 320 ms (milliseconds).

[0063] For the welded test specimen after welding, the nugget diameter d N , the minimum thickness of the welded joint t WJ The nugget diameter d N The method for measuring the nugget diameter in two- or three-sheet welding was based on JIS Z3139:2009. In detail, as shown in Fig. 3(b), the diameter (width of nugget N) of the nugget N at the interface between the outermost mild steel sheet P1 and the high-strength steel sheet P2 was measured, and this was defined as the nugget diameter d N It was decided. Minimum thickness of welded joint t WJ is the thinnest part of the weld joint WJ in the cross section passing through the weld joint WJ. The cross section is observed macroscopically, and the thickness of the thinnest part in the center of the weld joint is measured to determine the minimum thickness t WJ (Figure 3(b)).

[0064] Measured nugget diameter d N Using the value of and the value of the thickness t1 of the mild steel plate, it was verified whether each example satisfied the formula (1). d N / √t1≧3.0 (1) where d N (mm) is the nugget diameter at the contact surface where the mild steel plate and the high strength steel plate are in contact with each other, t1 (mm) is the plate thickness of the mild steel plate in contact with the high strength steel plate. Table 2 shows the N When this value is 3.0 or more (i.e., formula (1) is satisfied), it is judged as "good", and when it is 4.0 or more, it is judged as "excellent".

[0065] In addition, the total plate thickness of the welded test piece was considered to be the sum of the plate thicknesses of the four steel plates, and the plate thickness retention rate defined by formula (2) was calculated using the minimum thickness of the measured welded joint. Plate thickness retention rate (%) = (minimum thickness of the welded joint) / (total thickness of the four steel plates) × 100 (2) A plate thickness retention rate of 84% or more was judged to be "passed."

[0066] In addition, cross tensile tests were conducted on some of the welded specimens to evaluate the joint strength of the welded joint between the outermost plate (mild steel plate) and the second plate (high strength steel plate). The cross tensile tests were conducted in accordance with JIS Z3140:2017. For cross tensile strength, 2.1 kN or more was judged as "good" and 3.0 kN or more was judged as "excellent."

[0067] The measurement results are shown in Table 2. In Table 2, underlined values ​​indicate values ​​outside the range defined in the embodiment of the present invention.

[0068] [Table 1]

[0069] [Table 2]

[0070] Consider the results in Table 2. In Nos. D-3, E-1, E-2, F-2 and F-3, in which the welded joints satisfy the manufacturing conditions of the embodiment of the present invention, the d of the welded joints N / √t1 was 3.0 or more, and the plate thickness retention rate was 84% ​​or more. As a result, it is believed that the joint strength will be high. In No. D-3 and F-3, where cross tensile tests were actually performed, the cross tensile strength of the welded joints was high. In particular, the d of the welded joint N It is believed that the joint strength of No. E-2, F-2 and F-3, which have a / √t1 of 4.0 or more, will be even higher. The cross tensile strength of the welded joint of No. F-3, which was actually subjected to a cross tensile test, was higher than that of No. D-3.

[0071] In Nos. C-1 to C-4, the pressure member 2 was not used, so the steel plate was not clamped under pressure during welding. N / √t1 was less than 3.0 and / or the plate thickness retention rate was less than 84%. As a result, it is believed that the joint strength will be low. In No. C-1 and C-3, where cross tensile tests were actually performed, the cross tensile strength of the welded joints was low.

[0072] No.D-1 and D-2 are d N / √t1 was less than 3.0. As a result, it is believed that the joint strength was low. In No. D-4, the plate thickness retention rate was less than 84%, which is thought to result in a decrease in joint strength. In No. E-3 and E-4, the plate thickness retention rate was less than 84%, which is considered to result in low joint strength. No.F-1 is d N / √t1 was less than 3.0. As a result, it is believed that the joint strength was low. In No. F-4, the plate thickness retention rate was less than 84%, which is considered to result in a low joint strength. [Explanation of symbols]

[0073] 1 electrode 2 Pressure terminal P1 mild steel plate P2, P3, P4 High strength steel plate WJ Welded joint N Nugget

Claims

1. A welded joint in which four steel plates are overlapped and spot welded, The four stacked steel plates include one mild steel plate having a tensile strength of 270 MPa or more and less than 590 MPa, and three high-strength steel plates having a tensile strength of 980 MPa or more, The one mild steel plate is disposed on the outermost side of the four steel plates, The three high-strength steel plates are arranged in a superimposed manner on one side of the one mild steel plate, The nugget formed by spot welding satisfies the following formula (1), and A welded joint having a plate thickness retention rate defined by the following formula (2) of 84% or more. d N / √t 1 ≧3.0 (1) Here, d N (mm) is the nugget diameter at the contact surface where the mild steel plate and the high strength steel plate are in contact with each other, t 1 (mm) is the plate thickness of the mild steel plate in contact with the high strength steel plate. Plate thickness retention rate (%) = (minimum thickness of welded joint) / (total thickness of four steel plates) × 100 (2)

2. The thickness t of the mild steel plate 1 is less than the thickness of the high strength steel plate in contact with the mild steel plate.

3. A method for manufacturing a welded joint by spot welding overlapping portions of four steel plates, comprising the steps of: A process of stacking four steel plates including one mild steel plate having a tensile strength of 270 MPa or more and less than 590 MPa and three high-strength steel plates having a tensile strength of 980 MPa or more, overlapping the four steel plates such that the one mild steel plate is disposed on the outermost side of the four steel plates and the three high strength steel plates are disposed on one side of the one mild steel plate; A process of pressing and clamping the overlapping portion of the steel plate with a pair of electrodes and a pair of pressure members provided so as to surround the electrode tips of the electrodes, The pressure member is configured to apply pressure over a range of 180° or more in a circumferential direction centered on the electrode tip, The distance between the pressing tip of the pressing member and the electrode tip is 0.1 mm or more and 10.0 mm or less, A pressurizing and clamping step in which the overlapping portion is pressurized by the electrode tip with an electrode load of 1.5 kN or more and is pressurized by the pressing tip with a peripheral load of 0.1 to 1.0 times the electrode load; and welding the overlapping portion by passing a welding current of 5 kA or more and 15 kA or less through the pair of electrodes.

4. The thickness t of the mild steel plate 1 The method for manufacturing a welded joint according to claim 3, wherein the thickness of the high strength steel plate in contact with the mild steel plate is smaller than the thickness of the high strength steel plate in contact with the mild steel plate.

Citation Information

Patent Citations

  • JP1973084958A

  • Welding and device therfor

    JP1979148151A

  • Method of manufacturing resistance spot welded joint

    JP2010240739A

  • Method of manufacturing resistance spot welded joint

    JP2010240740A

  • Lap welding method for steel sheet, and lap-welded joint of steel sheet

    JP2010264503A