How to prepare blocks of polyurethane / polyisocyanurate foam for tank insulation slabs
The method ensures uniform distribution of long fibers in polyurethane and polyisocyanurate foams by controlled impregnation and expansion, resulting in lightweight foams with enhanced mechanical and thermal properties and reduced material waste.
Patent Information
- Application Number
- JP2021541020
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-01-15
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-01-15
AI Technical Summary
Existing methods struggle to produce fiber-reinforced polyurethane and polyisocyanurate foams with uniform distribution of long fibers, leading to non-uniform density and mechanical inefficiencies, and result in significant material loss during cutting.
A method involving the impregnation of long fibers with a mixture of chemical components under controlled conditions, ensuring complete and uniform penetration, followed by constrained or free expansion to form homogeneous fiber-reinforced foams with optimized mechanical and thermal properties.
The method achieves lightweight, easily handled fiber-reinforced foams with good mechanical properties and insulation performance, minimizing material loss and ensuring uniform fiber content across the foam block.
Smart Images

Figure 0007556862000006 
Figure 0007556862000007 
Figure 0007556862000008
Abstract
Description
[Technical field]
[0001] The subject of the present invention is a method for preparing blocks of fiberized polyurethane (PUR) and / or polyisocyanurate (PIR) foam (containing long to continuous fibers) from at least one polyisocyanate and at least one polyol, for use in tanks integrated into support or self-supporting structures of type B or type C, in particular for containing very cold fluids, called cryogenic fluids, such as liquefied natural gas (LNG) or liquefied petroleum gas (LPG).
[0002] The invention also relates to a block of fiber-reinforced PUR and / or PIR foam, which must be as economical as possible to manufacture whilst exhibiting fairly finely specified mechanical and thermal characteristics in view of its specific application.
[0003] Finally, the invention more particularly relates to a sealed, insulated tank using the above-mentioned foam directly obtained by this preparation method, and to a ship equipped with said tank. [Background technology]
[0004] Polyurethane PUR foams are cellular insulations composed of microscopic cells that store gases that may have low thermal conductivity. PUR foams are used in a great many applications, such as in the automotive industry as flexible PUR foams or for insulation as rigid PUR foams. The formation of polyurethane type foams is known to those skilled in the art. It requires a multi-component reaction between polyols (compounds bearing at least two hydroxyl groups), polyisocyanates (compounds bearing at least two isocyanate-NCO functional groups), and blowing agents, also described as "blowing agents". This condensation reaction is catalyzed in particular by compounds with basic and / or nucleophilic properties, such as tertiary amines or metal-carboxylate coordination complexes, such as tin or bismuth salts. The polyols commonly used in the production of PUR foams are polyether polyols or polyester polyols. Thus, a large number of compounds are required for the formation of PUR foams.
[0005] Polyisocyanurate (PIR) and polyurethane / polyisocyanurate (PUR-PIR) foams are also used in the building industry (construction / renovation) and offer the advantage of better fire resistance properties and greater compressive strength than PUR. The process for the formation of these foams is similar to that for the formation of PUR foams, since obtaining PUR, PIR and PUR-PIR foams depends on the isocyanate / polyol ratio.
[0006] The documents FR2882755 and KR20000010021 are known from the prior art, which describe fiber-reinforced PUR or PIR foams and their preparation. In these two documents, the PUR or PIR foams have a high density.
[0007] Although obtaining PUR, PIR and PUR-PIR foams is known to those skilled in the art, the addition of fibers nevertheless entails certain technical problems, especially when it is desired to obtain fiber-reinforced PUR, PIR or PUR-PIR foams in which long to continuous fibers, i.e. long fibers of at least 5 centimeters, are uniformly distributed in the foam volume.
[0008] In particular, low density fiber reinforced PUR, PIR and PUR-PIR foams, i.e. 50 kg / m 3 If one wishes to obtain a foam with a density less than 0.05 mm, the incorporation of fibers is very difficult and often results in a foam with a non-uniform fiber distribution. This is because in order to obtain such low density fiber reinforced foams, a high proportion of blowing agent must be used with simultaneous rapid and uniform impregnation of the fibers. This results in the blowing agent no longer being completely dissolved in the polyol, but rather in the formation of an emulsion of blowing agent in saturated polyol, which must be stabilized and efficiently mixed with the isocyanate. In the situation of pouring the prepolymer mixture onto the fibers (under the action of simple gravity), one solution to the above problem is to increase the amount of nucleating gas during polyol / isocyanate mixing, but this leads to a high viscosity, which results in the top of the block being devoid or practically devoid of fibers, making it difficult or impossible to obtain good penetration of the polyurethane / polyisocyanurate foam into the fibers and thus a uniform fiber reinforced foam block.
[0009] Thus, increasing the blowing agent can result in foams with non-uniform structure (with respect to the fibers) or non-uniform density, and the resulting fiber reinforced foams are thermally inefficient and have poor mechanical qualities.
[0010] Furthermore, increasing the amount of blowing agent requires the use of more reactive chemical components to compensate for the endothermic phenomenon associated with significant evaporation of the physical blowing agent, which reduces the cream time and does not allow good impregnation of the fibers for controlled expansion.
[0011] A further challenge lies in the production of economical foam blocks, i.e. blocks that do not require cutting to obtain uniform fiber-reinforced foam blocks, the material losses associated with this cutting being conventionally in the order of 15%, and in practice exceeding 20%, which is totally insufficient for industrial processes.
[0012] Thus, at present, it is only possible to obtain blocks with low densities (50 kg / m2) that exhibit very good mechanical properties, in particular due to the inhomogeneity of the fiber content in the block. 3 No method exists for preparing blocks of fiber reinforced polyurethane and / or polyisocyanurate foam of less than 100 mm diameter. Summary of the Invention
[0013] In this context, the Applicant Company has succeeded in developing a method for producing polyurethane (PUR) and / or polyisocyanurate (PIR) foams containing a significant amount of continuous fibres from long fibres, which makes it possible at the same time to obtain fibre-reinforced foams which are light in weight, easy to handle and exhibit excellent mechanical properties, whilst at the same time maintaining, indeed even improving, their excellent thermal insulation performance qualities. Advantageously, according to preferred embodiments, a considerable reduction in the production costs for fibre-reinforced foams is possible, due to the perfect homogeneity of the latter (so that material losses from the foam block are minimal and can even be neglected in practice).
[0014] The term "block" according to the present invention is a non-limiting term, the "block" can have any shape and is not necessarily cut.
[0015] The present invention therefore aims to overcome the drawbacks of the prior art by providing an easy to implement and particularly effective solution for industrially obtaining low-density fiber-reinforced PUR / PIR foams with optimal mechanical properties.
[0016] The Applicant Company, after various studies and analyses, has discovered a method for the preparation of blocks of fibre-reinforced polyurethane (PUR) and / or polyisocyanurate (PIR) foams with long to continuous fibres, which allows, for the first time, to solve the technical problems in the current preparation, with a view to the specific objectives related to the end use of the blocks of low density foams.
[0017] The present invention therefore relates to a method for preparing a block of fibre-reinforced polyurethane / polyisocyanurate foam for an insulating slab of a closed insulating tank, said block of fibre-reinforced polyurethane / polyisocyanurate foam being made up of cells for storing gas and having a density of 50 kg / m 3 and the fiber content is less than C f represents at least 4% by weight of the block of fiber reinforced foam, and the method of preparing comprises: a) mixing the chemical components necessary to obtain a polyurethane / polyisocyanurate foam, including reactants for obtaining the polyurethane / polyisocyanurate, optionally at least one reaction catalyst, optionally at least one emulsifier, and at least one blowing agent; b) impregnating a plurality of fiber reinforcements with the mixture of chemical components by gravity flow; wherein the fibers are long to continuous fibers arranged in overlapping layers, the plurality of fiber reinforcements extend primarily along a direction perpendicular to the direction of the gravitational flow, and the plurality of fiber reinforcements are intimately connected to the mixture of chemical components. 2 The permeability K is expressed as c But, K c =(r f 2 ×p 3 ) / (k×τ 2 x4xV f 2 ) in which: r f = the radius of the fiber, expressed in meters (m), The porosity (dimensionless) of the fiber, p=0 to 1; k=form factor (dimensionless) depending on the nature of the fiber reinforcement, k=1 for fiber woven fabrics, k=6 for fiber mats; τ = tortuosity (dimensionless) depending on the arrangement of the fibers, V f = 0 to 1, the volume fraction of the fiber (the proportion of fibers in the volume of the fiber reinforcement), and c) forming and expanding the fiber-reinforced polyurethane / polyisocyanurate foam. A feature of the method according to the invention is that the mixture of the above chemical components is applied to the fibers during the impregnation step b) for a period of time t i The cream time of polyurethane / polyisocyanurate foam c The dynamic viscosity η is less than the fiber impregnation time t i t i =(η×e m 2 ) / (K c ×ΔP), and ΔP=(M sd ×g T ×k p ) in which η = viscosity in Pascals × seconds (Pa s), e m = the total average thickness of the fiber reinforcement in meters (m), ΔP = hydraulic gradient or pressure difference expressed in Pascals (Pa), M sd = weight per unit area (kg / m 2 the surface density of the mixture of chemical components (12) represented by g T = Gravity (force de gravitation terrestre), which is considered to be equal to 9.8 N / kg; k p = 0.5 is the average water pressure factor.
[0018] The term "cells storing gas" is understood to mean that the polyurethane / polyisocyanurate foam exhibits closed cells containing a gas, preferably exhibiting low thermal conductivity, originating from a gas poured during the nucleation step of the reaction mixture or originating directly or indirectly from a chemical or physical blowing agent.
[0019] The term "fibrous reinforcement" is understood to refer to the fact that the fibers can be provided in either of two distinct forms: - a form of weaving of at least one fibre, in which the fibres are perfectly aligned along at least one direction, in other words the fibres show at least one preferred direction of fibres. The term "weaving of fibres" refers to a clear technical definition, known per se to the person skilled in the art. or in the form of a mat of at least one fiber, in which the fibers do not exhibit a defined orientation, in other words the fibers are oriented isotropically mainly along the main surface of the layer of the mat. Again, the term "mat of fibers" refers to a clear technical definition known per se to the person skilled in the art.
[0020] According to one embodiment, the expression "gas having (advantageously) low thermal conductivity" is understood to mean either the gas resulting from the blowing agent by chemical reaction of the blowing agent, when the blowing agent is a "chemical substance", i.e. traditionally carbon dioxide (CO2) when the chemical blowing agent consists of water, or the gas resulting from the blowing agent by physical blowing agents, such as molecular nitrogen (N2), molecular oxygen (O2), carbon dioxide, hydrocarbons, chlorofluorocarbons, hydrochlorocarbons, hydrofluorocarbons, hydrochlorofluorocarbons and mixtures thereof. Physical blowing agents, such as molecular nitrogen N2, molecular oxygen O2 or CO2, are in the form of a gas. These gases are dispersed in the liquid mass of the copolymer under high pressure, for example using a static mixer. By reducing the pressure in the system, a cellular structure is generated by nucleation and growth of the bubbles.
[0021] The expression "the fiber reinforcement extends mainly along a direction perpendicular to the direction of the gravitational flow of the mixture of chemical components" is understood to mean the fact that this fiber reinforcement is provided during the impregnation step b) in the form of a layer of small thickness extending along a plane perpendicular to the direction of flow of said mixture of components. Thus, as seen in FIG. 1, a number of fiber reinforcements arranged as superposed layers with a width L are entrained in a longitudinal direction l, while the mixture of chemical components is deposited on the fiber reinforcement from a dispenser that allows / makes the flow of the mixture of chemical components by gravity. In other words, the mixture of chemical components leaving the dispenser, optionally under pressure, falls at least by its own weight onto the mat of stacked fibers, thereby performing impregnation from the top layer of the fiber reinforcement to the bottom layer.
[0022] "r" for the radius of the fiber, expressed in meters (m) f " refers to the radius of the fibers in the reinforcement, or more conventionally, the radius or quasi-radius taken by the aggregate of a set of fibers that locally form an aggregate fiber that represents the average radius (and this is r f The radius r of this fiber is understood to mean f This data on the fiber reinforcement is defined as one of its main physicochemical characteristics and can optionally be characterized by its linear density (g / km) or tex, which is a measure of the count (linear density) of yarns and spun yarns, known to those skilled in the art, and from which the radius r of the fiber can be calculated. f is obtained, and the average radius r f The radius of the
[0023] In other words, the radius of the fiber, r f is equal to the radius of a fiber in the reinforcement if the fiber does not form part of an agglomerated fiber, or equal to the radius of the agglomerated fiber if several fibers are agglomerated.
[0024] The expression "the fibres are filamentary to continuous" (or "filamentary to continuous") is understood to mean that the fibres, or, where appropriate, aggregate fibres (fibers bonded or fixed to one another), when considered alone or in an aggregated state forming the equivalent of a single fibre, all or at least 90% of the fibres, with respect to the total mass of fibres, have a length of at least 5 centimetres (cm).
[0025] Similarly, the fiber porosity p and tortuosity τ are quantities characteristic of the fiber reinforcement under consideration, i.e. the values of these quantities are known to define the fiber reinforcement. Thus, although these values are conventionally given as defining the fiber reinforcement, they can of course be measured by conventional techniques such as measuring the unidirectional or radial non-turbulent quiescent flow of a calibrated fluid (e.g. air, silicone oil) through a given stack of glass reinforcement by applying Darcy's law.
[0026] To measure the porosity of the fibers used in the context of the present invention, whether the fibers are provided in the form of a fiber fabric or a fiber mat, one can use, for example, a sliding caliper, ideally a digital caliper, measuring the thickness of a sample of a fiber fabric or a fiber mat stack, for example of the order of 10. Considering the width / length dimension of the fiber fabric / fiber mat sample and also knowing the density of the fibers under consideration (glass, basalt, carbon, hemp, etc.), the thickness (or height) is measured at several points / locations that constitute the thickness extremes in the fiber fabric or fiber mat stack, thus determining the average thickness of the fiber reinforcement under consideration (fabric or mat) and thus the volume occupied by the fibers in this fiber fabric or fiber mat (the density of air is considered to be zero in this case). As mentioned above, this porosity is dimensionless, between 0 and 1, i.e. it represents the percentage or proportion of voids in the fiber reinforcement under consideration (fabric or mat), which can be translated as "fiber porosity".
[0027] It is noted that the density of the fibers is a property known or accessible to the person skilled in the art. It is expressly understood that, typically, the subject of the present invention uses accessible or commercially available materials / products, the properties of which are available in the specifications for the material / product under consideration, in particular those related to their density or (dynamic) viscosity.
[0028] The tortuosity τ of a fiber reinforcement corresponds to the average tortuosity of the fibers that make up the fiber reinforcement, the tortuosity of the fibers being equal to the ratio Le / L, where Le is the effective path length, i.e. the length of the curve formed by the fibers, and L is the surface distance over which the fibers are curved, i.e. the distance between the two ends of the fibers.
[0029] Methods for determining the tortuosity of fibers or aggregates of fibers (referred to above as "aggregate fibers") are in particular described in the paper "Permeability Properties of Continuous Filament Mats for Resin Transfer Molding" by R. Pomeroy (2009) (available in particular in the Semantic Scholar database).
[0030] The form factor k is also a constant defined by the nature of the fibre reinforcement under consideration: thus, as mentioned above, in the context of the present invention the fibre reinforcement can consist of a fibre woven fabric or a fibre mat, and the value of this form factor k is given in each of these two cases, k=1 for a fibre woven fabric, for example carbon fibres, and k=6 for a fibre mat, for example a mat of continuous glass fibres.
[0031] fraction V f With respect to V, this fraction is the volume fraction of the fibers (the volume fraction of the constituent material of the fibers in the bulk volume of the reinforcement), i.e. a value between 0 and 1, in other words, the percentage by volume of the fibers in the reinforcement (defined by the volume enclosed by the edges / ends of the reinforcement). This value V f is known as an intrinsic characteristic of the fiber reinforcement under consideration, and the value V f is, for example, the surface density (g / m) known to those skilled in the art. 2), from which the fiber volume fraction V f Optionally, this fiber volume fraction V can be calculated using the international standard ISO 14127:2008. f can be measured.
[0032] e m The term represents the sum of the average thicknesses of the fiber reinforcements expressed in meters (m), in other words, the average thickness of each fiber reinforcement is measured and the term is derived by adding up the average thicknesses of each of the fiber reinforcements. m The expression "average thickness" is understood to mean the average of the distances between two local extremes of the reinforcement, i.e. the distance between the two most distant points of the fiber reinforcement, which are located substantially opposite each other with respect to the extension plane of the fiber reinforcement, the measurement of this distance between these two points being repeated in several zones of the reinforcement in order to determine the average thickness of the fiber reinforcement as accurately as possible. In other words, the average thickness of the fiber reinforcement corresponds to the average of the distances between several pairs of local extremes of the fiber reinforcement, which are arranged at a distance from each other along the thickness direction of the fiber reinforcement.
[0033] The term ΔP represents the hydraulic pressure gradient, expressed in Pascals (Pa), i.e. the pressure difference between the upper layer(s) of fiber reinforcement(s) impregnated by the mixture of chemical components and the lower layer(s) of fiber reinforcement(s) not yet impregnated by the mixture of chemical components, therefore at a pressure substantially equal to atmospheric pressure. As can be seen from the third formula, this term ΔP is proportional to the surface density M sd , i.e. the amount of material formed by the mixture per unit area (in this case kg / m 2 (expressed as:
[0034] Therefore, all the terms and descriptions used to define the preparation method according to the invention and their respective values, more particularly the impregnation time t i is data known per se or can be determined / measured by techniques known to those skilled in the art.
[0035] The expression "cream time" is understood to mean the time, counted from the mixing of the chemical components, that is necessary for the chemical components to start the polymerization reaction and for the mixture of components to start the expansion and crosslinking step c) (= formation of fiber-reinforced PUR / PIR foam). This cream time is a data known to the person skilled in the art. In other words, the cream time is the time until the mixture turns white under the effect of the nucleation of bubbles (cells that store gas) and the expansion of the foam after mixing of the chemical components at ambient temperature. The cream time can be determined visually or by using an ultrasonic sensor that detects the change in thickness that reflects the formation of the foam.
[0036] By a particular selection of the characteristics of the fiber reinforcement and the viscosity of the mixture of chemical components, a block of low density fiber reinforced PUR / PIR foam is obtained which shows perfect uniformity with respect to the fibers, in other words the fiber content C f is the same or within a range of ±35%, and in practice advantageously the same or within a range of ±20%, in all parts of the foam block. This important feature makes it possible to obtain blocks of fibre-reinforced foam which can be easily made light and well proportioned in terms of size and shape, and which exhibit excellent mechanical properties, as will later be demonstrated by tests carried out by the Applicant Company.
[0037] The blocks of fibre-reinforced foam obtained according to the invention are therefore characterised by their controlled and homogeneous structure and by their mechanical properties, in particular their fatigue strength, their tensile strength in the plane perpendicular to the expansion (measured according to standard ISO 1926) and their low thermal contraction coefficient in this same plane (measured according to standard ASTM E 228), which make them suitable for use in tanks integrated into a supporting structure, but also advantageously for tanks of type B or type C according to the IGC regulations (IMO), i.e. as external insulation in connection with self-supporting tanks for the storage and / or transport of very cold liquids, such as LNG or LPG.
[0038] Finally, the thermal properties of the block of fibre reinforced foam are at least equal to those of a block of low density non-fibre reinforced foam of the prior art, more precisely the block of foam has a thermal conductivity at a thickness E of less than 30 mW / (m·K) (milliwatts per metre per Kelvin), i.e. 0.03 W / (m·K), measured at 20°C, preferably less than 25 mW / (m·K) and even more preferably less than 23 mW / (m·K).
[0039] In the compositions according to the invention, the use of chemical blowing agents can be combined with the use of physical blowing agents, which in this case are preferably mixed with the foamable (co)polymer composition in liquid or supercritical form and then converted to the gas phase during the expansion process of the PUR / PIR foam.
[0040] Chemical and physical blowing agents are known to those skilled in the art, and they will select the appropriate amounts of both depending on the PUR / PIR foam they wish to obtain.
[0041] The term "polyol" is understood to mean any carbon-based structure having at least two OH groups.
[0042] PUR, PIR and PUR-PIR foams are obtained according to the isocyanate / polyol ratio, so PUR, PIR or PUR-PIR foams are obtained according to this ratio. When the ratio of the polyol component to the isocyanate component is 1:1 to 1:1.3, polyurethane PUR foam is obtained, when it is 1:1.3 to 1:1.8, polyurethane PUR-PIR foam is obtained, and when it is 1:1.8 to 1:2.8, polyurethane PIR foam is obtained.
[0043] Polyisocyanates suitable for forming PUR, PIR and PUR-PIR foams are known to those skilled in the art and include, for example, aromatic, aliphatic, cycloaliphatic and arylaliphatic polyisocyanates and mixtures thereof, preferably aromatic polyisocyanates.
[0044] Examples of suitable polyisocyanates within the scope of the present invention include aromatic isocyanates such as the 4,4'-, 2,4'- and 2,2'-isomers of diphenylmethane diisocyanate (MDI), any compounds resulting from the polymerization of these isomers, toluene 2,4- and 2,6-diisocyanate (TDI), m- and p-phenylene diisocyanate, naphthalene 1,5-diisocyanate; aliphatic, cycloaliphatic or arylaliphatic isocyanates such as 1,6-hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), 4,4'-dicyclohexylmethane diisocyanate (H12MDI), 1,4-cyclohexane diisocyanate (CHDI), bis(isocyanatomethyl)cyclohexane (H6XDI,DDI) and tetramethyxylylene diisocyanate (TMXDI). It is also possible to use any mixture of these diisocyanates. Advantageously, the polyisocyanates are the isomers of 4,4'-, 2,4'- and 2,2'-diphenylmethane diisocyanate (MDI).
[0045] It is generally known, during the formation of PUR, PIR or PUR-PIR foams, to add to the mixture comprising the polyol, the polyisocyanate and the blowing agent a reaction catalyst which may be selected, for example, from tertiary amines such as N,N-dimethylcyclohexylamine or N,N-dimethylbenzylamine, or from organometallic compounds based on bismuth, potassium or tin.
[0046] Other advantageous features of the present invention are briefly summarized below.
[0047] Advantageously, the impregnation time t i is a polyurethane / polyisocyanurate foam cream time c Regarding the formula t i +0.1t i <t c <2t i Meet the following.
[0048] According to a preferred embodiment of the invention, the expansion of the fiber reinforced polyurethane / polyisocyanurate foam is physically constrained by the walls of a double belt laminator (DBL) forming a tunnel, advantageously having a rectangular cross section and with a distance between the laterally disposed walls equal to L and a distance between the horizontally disposed walls equal to E, thus encasing the expandable fiber reinforced foam, thereby obtaining a block of said fiber reinforced polyurethane / polyisocyanurate foam.
[0049] Thus, in this embodiment with DBL, the method according to the invention allows considerable savings, as the block of fiber reinforced foam is uniform and inherently exhibits the desired excellent mechanical properties, especially along the plane perpendicular to the axis of thickness E, and there is no reason to later cut this block along this same direction to remove ends where there are no fibers and / or the ovoid cells are not oriented along the axis E. Thus, the amount of material loss in the method of preparation according to the invention is between 0% and 10%, and more often less than 5%.
[0050] According to this preferred embodiment of the invention, advantageously, the positioning of the walls of the tunnel of the double belt laminator is determined in such a way that the volume of the fiber reinforced polyurethane / polyisocyanurate foam at the outlet of the double belt laminator due to the constraint on the expansion of the fiber reinforced polyurethane / polyisocyanurate foam is 85% to 99%, preferably 90% to 99%, of the expansion volume of this same fiber reinforced polyurethane / polyisocyanurate foam in case of free expansion without the constraint of the walls of such double belt laminator. In this case, the foam obtained has its ovoid cells preferentially oriented along the axis E, which results in advantageous properties such as resistance to crushing along this direction E (measured according to standard ISO 844) in conjunction with the already described properties in the plane perpendicular to this axis E. Tests and experiments have been carried out by the applicant company to determine the above-mentioned broad and preferred ranges, but are not presented here for the sake of clarity and conciseness.
[0051] On the one hand, the above-mentioned specific parameterization of the constraints on the expansion of the fiber-reinforced PUR / PIR foam in the DBL results in a block of low-density fiber-reinforced PUR / PIR foam in which at least 60%, more often 80%, and indeed even 90% of the cells storing the gas with low thermal conductivity extend longitudinally along an axis parallel to the axis of the thickness E of the block of foam, which, besides the specific selection related to the characteristics of the fiber reinforcement and the viscosity of the mixture of chemical components, contributes to a perfect homogeneity of the block of fiber-reinforced foam. These two characteristics (cell orientation and fiber content in the block C f The uniformity of the thickness E (compressive strength) makes it possible to obtain a block of fiber-reinforced foam that exhibits excellent mechanical properties along the thickness E (compressive strength) and in the plane perpendicular to the thickness direction (tensile strength and low thermal shrinkage coefficient).
[0052] According to another embodiment of the invention, the expansion of the fiber reinforced polyurethane / polyisocyanurate foam is free, i.e., not limited by the volume of a closed section.
[0053] In this case, unlike the embodiment of the preparation according to the invention using a DBL, the preparation of the fiber reinforced polyurethane / polyisocyanurate foam is said to be by "free rise", i.e., unlike a mould defining a finite volume, the expansion of the fiber reinforced foam is unconstrained on at least one side or at least one face of the expansion and is free on this side or face. Conventionally, free rise is achieved by omitting the (top) cover and allowing the foam to expand naturally upwards, possibly beyond the top of these side walls, with side walls preventing the foam from spilling over the sides.
[0054] Advantageously, following the step of free rise of the fibre reinforced polyurethane / polyisocyanurate foam, said fibre reinforced foam is cut in order to obtain blocks of said fibre reinforced polyurethane / polyisocyanurate foam.
[0055] According to one of the possibilities provided by the invention, not shown in the attached drawings, immediately after the step of impregnation of the fiber reinforcement, a system for applying pressure (which can be for example a system of rollers of the type of dedicated "nip rolls") is applied to the mixture of components to be impregnated (penetrated into the fibers) and at least the foaming agent, configured to apply pressure to the upper surface of the assembly consisting of said mixture and the fibers. This pressure system makes it possible on the one hand to create the upper surface of this assembly and contributes to accelerating the impregnation of the fibers in said mixture by the pressure applied to the assembly. This pressure system can consist of a single or double roller, the relative position of which is adjusted so as to spread the liquid assembly perfectly evenly above and possibly below the foam support. Doing this therefore results in an equal amount of liquid assembly at any point of the cross section defined by the distance between the two rollers or between the upper roller and the conveyor belt. In other words, the main purpose of this pressure system is to complement the liquid dispenser in that it contributes to making the liquid assembly uniform in thickness / width before the main part of its expansion.
[0056] Preferably, the viscosity η of the mixture of the above components is between 30 mPa·s and 3000 mPa·s (or between 0.03 Pa·s and 3 Pa·s), preferably between 50 mPa·s and 1500 mPa·s (or between 0.05 Pa·s and 1.5 Pa·s), under standard temperature and pressure conditions (STPC) (corresponding to a temperature of 25° C. and a pressure of 1015 mPa).
[0057] The viscosity of the mixture of the components can be determined, for example, using a Brookfield type viscometer or a rheometer, for example using standard ISO 2555.
[0058] Advantageously, at least 60% of the cells for storing the gas, advantageously having said low thermal conductivity, exhibit an elongated or elongated shape along an axis parallel to the axis of thickness E of the block of fiber reinforced polyurethane / polyisocyanurate foam.
[0059] More advantageously, at least 80%, preferably at least 90%, of the cells for storing the gas advantageously having said low thermal conductivity exhibit an elongated or elongated shape along an axis parallel to the axis of thickness E of the block of fiber reinforced polyurethane / polyisocyanurate foam.
[0060] An elongated or elongated shape may be defined by a shape that has an extended length, i.e., one dimension (its length) is greater than the other dimensions (its width and thickness).
[0061] Here, the features relating to the elongated shape of the cells for storing a gas advantageously having a low thermal conductivity and their content / proportion in the block according to the invention are particularly directed to the context of carrying out the preparation method with DBL, but are immediately understood to be absolutely not limited to this scenario, since such a preferential orientation of the cells for storing a gas advantageously having a low thermal conductivity is also obtained in the case of free expansion, more particularly in the absence of a top wall / cover limiting the expansion of the fiber-reinforced foam.
[0062] In one embodiment of the invention, the long to continuous fibres consist of glass fibres, carbon fibres or any other organic or inorganic material, preferably glass fibres, typically polymeric, metallic, ceramic, glass fibres of glassy, inorganic or organic nature, such as natural fibres, preferably made of glass fibres, for example hemp or flax.
[0063] Preferably, the fiber reinforcement is arranged over the entire width L, and the impregnation of the fibers with the mixture of components and blowing agent to obtain a fiber reinforced polyurethane / polyisocyanurate foam in step b) is carried out simultaneously over the entire width L via a controlled liquid dispenser.
[0064] The term "simultaneously" is understood to mean the fact that the liquid mixture (reactants and at least the blowing agent) reaches the fibers over a section of width L and all along this section at the same time, so that the impregnation of the different fiber reinforcements is started or carried out at the same time or at the same speed for one and the same section of width along the thickness (or height) of the block of foam.
[0065] Advantageously, the blowing agent consists of a physical blowing agent and / or a chemical blowing agent, preferably a combination of these two types.
[0066] Preferentially, the physical expansion agents are selected from alkanes and cycloalkanes having at least 4 carbon atoms, dialkyl ethers, esters, ketones, acetals having 1 to 8 carbon atoms, fluoroalkanes, fluoroolefins, tetraalkylsilanes having 1 to 3 carbon atoms in the alkyl chain, in particular tetramethylsilane, and mixtures thereof.
[0067] Under this assumption, examples of compounds may be propane, n-butane, isobutane, cyclobutane, n-pentane, isopentane, cyclopentane, cyclohexane, dimethyl ether, methyl ethyl ether, methyl butyl ether, methyl formate, acetone and fluoroalkane substances, and the fluoroalkanes selected are those that do not degrade the ozone layer, such as trifluoropropane, 1,1,1,2-tetrafluoroethane, difluoroethane and heptafluoropropane.Examples of fluoroolefins include 1-chloro-3,3,3-trifluoropropene or 1,1,1,4,4,4-hexafluorobutene (e.g. HFO FEA1100, sold by DuPont).
[0068] According to a preferred embodiment of the invention, the physical blowing agent selected is 1,1,1,3,3-pentafluoropropane or HFC-245fa (sold by Honeywell), 1,1,1,3,3-pentafluorobutane or 365mfc (e.g. Solkane® 365mfc, sold by Solvay), 2,3,3,3-tetrafluoroprop-1-ene, 1,1,1,2,3,3,3-heptafluoropropane (also known internationally as HFC-227ea, sold by DuPont), 1,1,1,4,4,4-hexafluorobutene (e.g. HFO FEA1100, sold by DuPont), trans-1-chloro-3,3,3-trifluoropropene (Solstice LBA - Honeywell) or mixtures thereof.
[0069] Advantageously, the chemical leavening agent consists of water.
[0070] Advantageously, during step a) of mixing the chemical components, a nucleating gas is incorporated in the at least one polyol compound, preferably using a static / dynamic mixer under a pressure of 20-250 bar, the nucleating gas being between 0% and 50% by volume of the polyol volume, preferably between 0.05% and 20% by volume of the polyol volume.
[0071] Preferably, during step a) of mixing the chemical components, the temperature of each of the reactants to obtain the polyurethane / polyisocyanurate is between 10°C and 40°C, preferably between 15°C and 30°C.
[0072] Preferably, according to a preferred embodiment of the present invention, the final mixing of the polyol, isocyanate and / or blowing agent streams is carried out in a mixhead at low pressure (less than 20 bar) or high pressure (more than 50 bar) using a dynamic or static mixer.
[0073] According to one possibility offered by the invention, in step a) an organic phosphorus flame retardant, advantageously triethyl phosphate (TEP), tris(2-chloroisopropyl)phosphate, tris(1,3-dichloroisopropyl)phosphate (TDCP), tris(2-chloroethyl)phosphate or tris(2,3-dibromopropyl)phosphate, or mixtures thereof, or an inorganic flame retardant, advantageously red phosphorus, expandable graphite, aluminium oxide hydrate, antimony trioxide, arsenic oxide, ammonium polyphosphate, calcium sulfate or cyanuric acid derivatives, or mixtures thereof, is additionally added to the mixture.
[0074] It is also possible to envisage using flame retardants such as diethyl ethane phosphonate (DEEP), triethyl phosphate (TEP), dimethyl propyl phosphonate (DMPP) or diphenyl cresyl phosphate (DPC).
[0075] The flame retardant, when present in the composition according to the invention, is present in an amount of from 0.01% to 25% by weight of the PUR / PIR foam.
[0076] Preferably, the fiber content C f is 7% to 15% by weight of the block of fiber-reinforced foam. f is a maximum of 30% by mass of the fiber-reinforced foam block.
[0077] The invention also relates to a block of fiber-reinforced polyurethane / polyisocyanurate foam for an insulating slab of a closed insulating tank, directly obtained by the method briefly shown above, the block of fiber-reinforced polyurethane / polyisocyanurate foam being made up of cells for storing a gas which advantageously has a low thermal conductivity and has a density of 50 kg / m 3 and the fiber content is less than C f is at least 4% by weight of the block of fiber reinforced foam.
[0078] The foam block has fibers uniformly distributed in the fiber-reinforced polyurethane / polyisocyanurate foam block and has a content of C in all or part of the fiber-reinforced polyurethane / polyisocyanurate foam block. f is characterized in that it is configured to vary by ±35%, and preferably in practice to vary within an even more limited range, i.e. on the order of ±20%.
[0079] Thus, for example, the fiber content in the block C f is equal to 4%, i.e. on average in the block, this means that the fiber content can vary from 2.8% to 5.2% (and preferentially from 3.2% to 4.8%) depending on the zone of the block, and if this average fiber content C f has a value of 15%, the fiber content can vary between 10.5% and 19.5% (and preferentially between 12% and 18%) depending on the zone of the block.
[0080] Such foam blocks exhibit essentially different characteristics than those prepared according to conventional preparation techniques. It should be noted that the characteristics concerning the nature or amounts of the various elements mentioned above in connection with the method of preparation of the fiber-reinforced foam block can, if necessary, more precisely define the fiber-reinforced PUR / PIR foam block according to the invention.
[0081] Advantageously, the density of the foam block is between 20 and 50 kg / m 3 and preferably 30 to 45 kg / m 3 It is.
[0082] The present invention also relates to a sealed, insulated tank integrated into a support structure, said tank comprising: a tank integrated in a support structure, comprising a sealed, insulated tank, the sealed, insulated tank comprising at least one sealed metal membrane made up of a plurality of metal strakes or metal plates, which may include at least a corrugation and an insulating slab, and an insulating slab comprising at least one insulating barrier adjacent to said membrane, or - Tanks of type B or type C as defined by the IGC Code, containing at least one insulating slab.
[0083] The tank according to the invention is characterized in that the insulating slab comprises a block of the fibre reinforced polyurethane / polyisocyanurate foam outlined above.
[0084] The reference "IGC Code" is understood to mean the "International Code for the Construction and Equipment of Ships for the Carriage of Liquefied Gases in Bulk", known to those skilled in the art, in which tank types B and C are listed.
[0085] It should be noted that, inter alia, the IGC Code allows the use of the expression "membrane tank" instead of "integral tank" to denote one and the same category of tank, which tank is fitted on certain tankers transporting and / or storing at least partially liquefied gas. "Membrane tanks" are integral to a supporting structure, whereas Type B or Type C tanks are said to be self-supporting.
[0086] This tank contains a number of blocks of fiber reinforced polyurethane / polyisocyanurate foam obtained directly by the preparation method described above.
[0087] Finally, the invention also relates to a vessel for the transportation of cold liquid products, comprising at least one hull and a sealed, insulated tank as described above arranged within the hull.
[0088] Advantageously, when the tank consists of a tank integrated in a support structure (membrane tank), such a vessel comprises at least one above-mentioned sealed and insulated tank, which tank comprises two successive sealing barriers, one of which is a primary sealing barrier in contact with the product contained in the tank and the other of which is a secondary sealing barrier arranged between the primary barrier and a support structure, preferably formed by at least a part of the vessel's wall, these two sealing barriers alternating with two insulating barriers or with one insulating barrier arranged between the primary barrier and the support structure.
[0089] Such tanks are conventionally designated as integral tanks by International Maritime Organization (IMO) regulations, e.g. tanks of type NO, including NO96®, NO96L03®, NO96L03+® or NO96Max®, or preferably tanks of type NO, Mark III®.
[0090] Preferably the tanks, being of membrane type or type B or type C, contain liquefied natural gas (LNG) or liquefied gas (LG).
[0091] The following description is given by way of example only and not by way of limitation with reference to the accompanying figures. [Brief description of the drawings]
[0092] [Figure 1] 1 is a schematic diagram showing the different steps of the preparation method according to the invention; [Diagram 2] 1 is a schematic diagram of an embodiment of a controlled liquid dispenser according to the present invention; [Diagram 3] FIG. 2 shows two sets of insulating panels fixed together, each forming a primary and secondary insulating space for a tank, the panels being formed from blocks of fiber reinforced polyurethane / polyisocyanurate foam according to the present invention. [Figure 4]FIG. 4 is a cutaway view of an LNG tanker tank and a loading / unloading terminal for the tank, the tank being fitted with two sets of insulation panels of the type shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0093] Preferably, the preparation of the fiber-reinforced PUR / PIR according to the invention is carried out in the presence of a catalyst making it possible to accelerate the isocyanate / polyol reaction. Such compounds are described, for example, in the prior art document entitled "Kunststoffhandbuch, Volume 7, Polyurethane" published by Karl Hanser (3rd edition, 1993, chapter 3.4.1). These compounds include amine-based catalysts and catalysts based on organic compounds.
[0094] Preferably, the preparation of the fiber reinforced PUR / PIR according to the invention is carried out in the presence of one or more stabilizers intended to promote the formation of an ordered cellular structure during foam formation. These compounds are known to those skilled in the art and may, for example, be mentioned foam stabilizers containing silicones such as siloxane-oxyalkylene copolymers and other organopolysiloxanes.
[0095] The skilled artisan knows the amount of stabilizer to be used depending on the reactants envisaged, between 0.5% and 4% by weight of the PUR / PIR foam.
[0096] According to one possibility offered by the invention, in step a), the mixture of chemical components can comprise a plasticizer, for example a polybasic ester, preferably a dibasic ester, of a carboxylic acid with a monohydric alcohol, or can consist of a polymeric plasticizer, such as a polyester of adipic, sebacic and / or phthalic acid. The skilled person knows the envisaged amounts of plasticizer, depending on the reactants used, which are customarily between 0.05% and 7.5% by weight of the polyurethane / polyisocyanurate foam.
[0097] Organic and / or inorganic fillers, especially reinforcing fillers, may also be envisaged in the mixture of chemical components, such as siliceous minerals, metal oxides (e.g. kaolin, titanium or iron oxides) and / or metal salts, etc. The amount of this filler, if present in the mixture, is customarily 0.5% to 15% by weight of the PUR / PIR foam.
[0098] It should be noted that the present invention is not intended to add any technical teaching to the formation of PUR / PIR foams, both with regard to the nature of the essential chemical components and the nature of the optional functional agents and their respective amounts. The skilled person knows how to obtain different types of fiber reinforced PUR / PIR foams, and the preparation according to the present invention is based on the specific selection of the permeability characteristics of the fiber reinforcement and of the foam viscosity during the impregnation of said reinforcement, as well as the impregnation time t , taking into account the relatively high or high content of long to continuous fibers. i However, the cream time of the polymer foam under consideration c It relates to performing something so that it is slightly or only slightly less than
[0099] Thus, the present invention is not targeted at creating new fiber reinforced PUR / PIR foams as described herein, but rather at creating new blocks of fiber reinforced PUR / PIR foams, where the specific characteristics of the permeability of the fiber reinforcement and the viscosity / cream time of the PUR / PIR foam are such that i <t c The rule is preferably 0.50<(t i / t c ) < 0.91 rule, in other words t i +0.1t i <t c <2t i The goal is to create a foam that is impregnated into the fibers by pouring, in accordance with the rules of the 1990s.
[0100] Thus, as can be seen in Figure 1, a number of fiber reinforcements 10 are unwound and moved in parallel alignment with one another on or above a conveyor belt 11 configured to transport said reinforcements 10 and the components that form the PUR / PIR foam, since the impregnation of the fiber reinforcement 10 is carried out in the context of the present invention by gravity, i.e. the mixture 12 of chemical components, blowing agent(s) and optional other functional agents used to obtain the PUR / PIR foam is poured directly onto the fiber reinforcement 10 from a liquid dispenser located above the fiber reinforcement 10.
[0101] Therefore, whether the fiber reinforcement 10 is one or more mats or one or more woven fabrics, the cream time t is set so that the initiation of expansion of the PUR / PIR foam occurs immediately or soon after the moment when complete impregnation of the fiber reinforcement 10 with the mixture 12 has occurred (i.e., the mixture 12 has completely penetrated into the fiber reinforcement 10). c The impregnation of the mixture 12 into all of the fiber reinforcement 10 must be very uniform throughout the entire volume of the block of PUR / PIR foam. In doing so, by observing the characteristics of the fiber reinforcement and the PUR / PIR foam defined according to the invention, the expansion of the PUR / PIR foam is carried out while maintaining a perfect uniformity of the fibers 10 within the volume of the block of PUR / PIR foam.
[0102] In the context of the present invention, the cream time of the components of the mixture 12 for forming the PUR / PIR foam is known to the person skilled in the art and is selected so that the assembly formed from the mixture of components 12, the blowing agent and the fibers 10 is moved by the conveyor belt 11, for example to a double belt laminator not shown in the attached drawings, just when the expansion of the foam has just started, in other words so that the expansion of the PUR / PIR foam is finished at the double belt laminator.
[0103] In such an embodiment with a double belt laminator (DBL), a pressure system using one or two rollers is optionally placed before the double belt laminator, i.e. between the zone for impregnation with the mixture on the fibers and the double belt laminator. When using a DBL, the expansion of the foam volume is carried out in the laminator when the expansion volume of this foam reaches 30% to 60% of the expansion volume of this same foam if the expansion remains free (i.e. without any constraints). In doing this, the double belt laminator can constrain the expansion of the PUR / PIR foam to its second expansion phase when it is close or relatively close to its maximum expansion, i.e. when its expansion brings it close to all the walls forming the rectangular or square cross-section tunnel of the double belt laminator. According to a different way of presenting a particular option of the preparation according to the invention, the gel point of the mixture of components, i.e. the moment when at least 60% of the polymerization of the mixture of components is reached, in other words the maximum volume expansion of the mixture is 70%-80%, is forced to occur in the double belt laminator, possibly in the latter part of the length of the double belt laminator (i.e. closer to the laminator outlet than to the laminator inlet).
[0104] As regards the function of simultaneous dispensing of the mixture 12 of chemical components and blowing agent over the entire width L of the fiber reinforcement 10, it is provided by a controlled liquid dispenser 15, shown in Fig. 2. Such a dispenser 15 comprises a supply channel 16 for the assembly formed of the mixture 12 of chemical components and at least the blowing agent from a reservoir (not shown) forming a reactant mixer, where, on the one hand, all the chemical components and the blowing agent are mixed, and on the other hand, the nucleation, in particular of such a mixture, actually heating, occurs. This liquid assembly formed of the mixture 12 of chemical components and blowing agent is then dispensed under pressure into two channels 17 extending laterally to end in two identical dispensing plates 18 (each having a length substantially equal to L / 2) extending along the width L, which dispensing plates 18 comprise a number of nozzles 19 for flowing the mixture 12 over the fiber reinforcement 10. These flow nozzles 19 consist of orifices with a calibrated cross section presenting a predetermined length. The length of these flow nozzles 19 is therefore predetermined in such a way that the liquid leaves with equal flow rates between all the nozzles 19, so that the impregnation of the fibre reinforcement 10 takes place at the same time, i.e. simultaneously, over a section of width L of the fibre reinforcement 10, and so that the surface density of the liquid deposited perpendicular to each nozzle is equal. In doing this, if a section of width L of the fibre 10 is taken into account, the impregnation of the fibre 10 takes place simultaneously, so that the impregnation of the layer of fibre 10 with the mixture 12 takes place in the same way at all points of this section, which contributes to obtaining a perfectly homogeneous block of fibre reinforced foam at the outlet of the double belt laminator.
[0105] This controlled liquid dispenser 15 shown in figure 2 is an exemplary embodiment in which two identical dispensing plates 18 are used, but different designs can be envisaged, as long as the function of simultaneous dispensing of liquid over a width section of the fibre 10 is achieved. Of course, the main technical feature used in this case consists in the different lengths of the flow nozzles 19, which are longer or shorter depending on the route or path of the liquid mixture 12 from the supply duct 16 of the dispenser 15 to the flow nozzle 19 under consideration.
[0106] PUR / PIR foam cream time c One of the key aspects to achieve good impregnation of the immediate fiber reinforcement 10 lies in the selection of a specific viscosity of the liquid (consisting of the mixture of chemical components and blowing agent 12) linked to the specific characteristics of the fiber reinforcement. The selected viscosity range and the penetration characteristics of the fiber reinforcement must allow good penetration of the liquid into the first layer of fibers 10 so that the immediately following liquid reaches the final layer (the layer below the fibers 10, i.e. the lowest layer in the stack of fiber reinforcements), resulting in a short impregnation time t i Cream Time c The viscosity of the mixture of ingredients 12 is selected, for example, by heating and / or by greater or less nucleation of plasticizer additives, so that the impregnation of all the fibers 10 with the mixture of chemical ingredients and blowing agent 12 over a section of width L is obtained just before the cream time, i.e. just before or slightly before the start of the expansion of the PUR / PIR foam.
[0107] The block of fiber-reinforced foam is intended to be used in a rather specific environment and must therefore guarantee specific mechanical and thermal characteristics. The block of fiber-reinforced foam obtained by the preparation according to the invention therefore conventionally forms part of an insulating slab 30, i.e. in the example used in Fig. 3, in the upper or primary panel 31 and / or the lower or secondary panel 32 of the insulating slab 30 of a tank 71 arranged to contain a cryogenic liquid such as LNG or LPG. Such a tank 71 may comprise, for example, a land tank, a floating barge, etc. (such as an FSRU "Floating Storage and Regasification Unit" or FLNG "Floating Liquefied Natural Gas") or it may comprise a vessel transporting this high-energy liquid between two ports, such as, for example, an LNG tanker.
[0108] 4, a cutaway view of an LNG tanker 70 shows a sealed, insulated tank 71 having a prismatic overall shape mounted on the vessel's double hull 72. The walls of the tank 71 include a primary containment barrier configured to be in contact with the LNG contained within the tank, a secondary containment barrier disposed between the primary containment barrier and the vessel's double hull 72, and two insulating barriers disposed between the primary containment barrier and the secondary containment barrier and between the secondary containment barrier and the double hull 72, respectively.
[0109] An offloading pipe 73 located on the upper deck of the ship can be connected by suitable connectors to a shipping or port terminal in a manner known per se to transfer a cargo of LNG to or from the tank 71.
[0110] 4 represents an example of a shipping terminal comprising an unloading station 75, an underwater pipeline 76 and an onshore facility 77. The unloading station 75 is a fixed offshore facility comprising a movable arm 74 and a tower 78 supporting the movable arm 74. The movable arm 74 holds a bundle of insulated hoses 79 which can be connected to an unloading pipe 73. The pivoting movable arm 74 fits all sizes of LNG tankers. A connecting pipeline (not shown) extends inside the tower 78. The unloading station 75 allows unloading from the onshore facility 77 to the LNG tanker 70 or from the LNG tanker 70 to the onshore facility 77. The facility comprises a liquefied gas storage tank 80 and a connecting pipeline 81 connected to the unloading station 75 via the underwater pipeline 76. The underwater pipeline 76 allows the transport of liquefied gas over long distances, e.g. 5 km, between the offloading station 75 and the onshore facility 77, thereby enabling the LNG tanker 70 to be kept at a large distance from the shore during offloading operations.
[0111] To generate the pressure required for the transfer of the liquefied gas, on-board pumps within the vessel 70 and / or pumps provided with the onshore facility 77 and / or pumps provided with the offloading station 75 are used.
[0112] As mentioned above, the use or application of the subject matter of the present invention, i.e. the preferred embodiment of the blocks of fiber reinforced polyurethane / polyisocyanurate foam, is not intended to be limited to integral tanks in a supporting structure, but is also provided for tanks of types B and C of the IGC Code in force on the filing date of this patent application, but also in future versions of this Code (unless these significant amendments are applied to tanks of types B and C), and it is understood that other types of tanks may be applications that may be envisaged for the blocks of fiber reinforced PUR / PIR foam according to the invention, under the assumption that the IGC Code is amended.
[0113] Following is a description of some of the experiments and tests carried out by the Applicant Company in order to make it possible to evaluate the subject matter and scope of the invention, it being contemplated that other tests / experiments may be carried out and subsequently provided as necessary / requested.
[0114] Polyurethane foam compositions incorporating fibers in the form of a mat are used to demonstrate the invention, these fibers always being provided as long to continuous fibers, more precisely, the length of these fibers is exactly the same as in the compositions according to the invention and in the prior art. The Applicant Company has in particular tested the subject of the invention with fibers provided in the form of a woven fabric, and the results obtained are the same or substantially the same as those obtained with a mat of fibers, as shown below.
[0115] For each of these PUR foams, the fiber reinforcement either has characteristics that are defined as meeting the present invention (bold type in the table of results below) or characteristics that do not meet the definition of the present invention. More precisely, in the latter case, the impregnation time t i PU foam cream time c It is important to note that the fiber soaking time t i Cream Time c In other words, the cream time t c is the fiber soaking time t iIf it is longer than twice the length of (t c >2t i ) is excluded, since in this case the preparation method obviously cannot have any industrial realism.
[0116] Thus, other parameters of the preparation of the block of PUR foam are not modified or different between the preparation according to the invention and the preparation according to the prior art, to ensure that only the combination of the specific characteristics of the impermeability of the fiber reinforcement and the choice of the PUR foam indicates a specific cream time or suitable for the properties of said fiber reinforcement. As non-exhaustive examples, we can mention the fact that the nucleation, the amount of blowing agent, the reaction temperature, the nature and amount of the mixture of chemical components, the pouring method, the distance between the place where the mixture of chemical components is poured and the DBL, or, where appropriate, the device allowing free expansion, are strictly the same in the case according to the invention and in the case according to the prior art.
[0117] Of course, for clarity and brevity it has been chosen in this case to illustrate the invention using PIR foam, however the same or substantially the same results are obtained in PUR foam and PUR / PIR blends.
[0118] Similarly, although the preparation of the fiber reinforced foam (the results of which are presented below) uses a free rise technique, the applicant company has demonstrated that the same or substantially the same results can be obtained using DBL in terms of fiber reinforced foams according to the present invention and fiber reinforced foams according to the prior art.
[0119] It is further understood that all compositions tested in succession are considered to be under the same density condition, and that this density parameter is involved in the evaluation of performance qualities with respect to compressive strength.
[0120] The permeability of fiber reinforcement and cream time of PIR foam for the compositions according to the prior art c The characteristics are as follows:
[0121] [Table 1]
[0122] For the compositions according to the present invention, the permeability of the fiber reinforcement and the cream time of the PIR foam c The characteristics are as follows:
[0123] [Table 2]
[0124] PIR foam cream time t c It should be noted that are logically the same, since the forms used are the same in each case according to the prior art and according to the invention.
[0125] After conducting tests, some results are presented below in a simplified form to illustrate the findings of the applicant company when the fibrous reinforcement is provided in the form of at least one mat of glass fibers.
[0126] [Table 3]
[0127] As can be seen from the results shown in the table above, with regard to the three criteria considered for comparing the obtained fiber reinforced foams, those according to the invention show significantly better results than those of the fiber reinforced foams according to the prior art.
[0128] Furthermore, it should be noted that the fiber reinforced PUR / PIR foams according to the invention do not show any significant decrease in the properties related to the (very low) thermal conductivity. Thus, for example, the following thermal conductivity values are obtained with a fiber reinforced foam according to the invention having 10% by weight of fibers:
[0129] [Table 4]
[0130] Although the present invention has been described with reference to some specific embodiments, it is clear that the invention is in no way limited thereto, but includes all technical equivalents of the described means and combinations thereof, provided that these are within the scope of the invention.
[0131] Use of the verb "comprise" or "comprise" and its conjugations does not exclude the presence of other elements or steps than those stated in a claim.
[0132] In the claims, any reference signs placed between parentheses shall not be construed as limiting the claim.
Claims
1. 1. A method for preparing a block of fiber reinforced polyurethane / polyisocyanurate foam for an insulating slab of a closed insulated tank, comprising the steps of: The block of fiber-reinforced polyurethane / polyisocyanurate foam is made up of cells for storing gas and has a density of 50 kg / m 3 and the fiber content C f represents at least 4% by weight of the block of fiber-reinforced foam, The method of preparing includes: a) mixing the chemical components necessary to obtain a polyurethane / polyisocyanurate foam to obtain a chemical mixture, said chemical components comprising reactants for obtaining a polyurethane / polyisocyanurate, optionally at least one reaction catalyst, optionally at least one emulsifier, and at least one blowing agent; b) impregnating a plurality of fiber reinforcements (10) having fibers and selected from fiber woven fabrics and fiber mats by gravity flow of the chemical mixture; and c) forming and expanding the fiber reinforced polyurethane / polyisocyanurate foam, In the step b) of impregnating the plurality of fiber reinforcements (10), the fibers are at least 5 centimeters in length and are arranged in overlapping layers; the plurality of fiber reinforcements (10) extend primarily along a direction perpendicular to the direction of the gravitational flow; The plurality of fiber reinforcements (10) are 2 The permeability K is expressed as c But, K c = (r f 2 ×p 3 ) / (k × τ 2 x4xV f 2 ) in which: r f = the radius of the fiber, expressed in meters, p=the dimensionless porosity of the fibers (10), with values between 0 and 1, which represents the proportion of voids in the fiber reinforcement; k=a dimensionless form factor depending on the nature of the fiber reinforcement (10), for woven fiber fabrics k=1 and for fiber mats k=6; τ = dimensionless tortuosity depending on the arrangement of the fibers, V f = a volume fraction of the fibers in the plurality of fiber reinforcements, the volume fraction being a value between 0 and 1; The mixture of chemical components obtained in step a) is subjected to the impregnation step b) for a period of time t i The cream time of the polyurethane / polyisocyanurate foam is t c The viscosity η is less than The impregnation time t of the fibers i is, t i = (η × e m 2 ) / (K c ×ΔP), where ΔP = (M sd ×g T ×k p ) in which η = viscosity in Pascals x seconds, e m = the sum of the average thicknesses of the fiber reinforcement (10) expressed in meters, where the average thickness of each fiber reinforcement corresponds to the average of the distance between a plurality of pairs of local extremes of the fiber reinforcement (10) spaced apart from one another along the thickness direction of the fiber reinforcement, ΔP = pressure gradient expressed in Pascals (Pa), M sd = surface density of the mixture of chemical components obtained in step a) expressed in kilograms per square meter, g T = gravity, which is equal to 9.8 N / kg. k p = 0.5 is a constant average pressure factor.
2. The impregnation time t i is the cream time of the polyurethane / polyisocyanurate foam. c For 0.50 < (t i / t c 2. The method of claim 1 , wherein the formula:
3. The expansion of the fiber reinforced polyurethane / polyisocyanurate foam is physically constrained by the walls of a double belt laminator forming a tunnel; 3. The method according to claim 1 or 2, wherein the tunnel has an advantageously rectangular cross section, the distance between the laterally disposed walls being equal to L and the distance between the horizontally disposed walls being equal to E, thereby being configured to encapsulate the expanding fiber-reinforced foam and obtain the block of fiber-reinforced polyurethane / polyisocyanurate foam.
4. The arrangement of the walls of the tunnel of the double belt laminator is as follows:
4. The method according to claim 3, wherein the constraint on the expansion of the fiber reinforced polyurethane / polyisocyanurate foam is determined such that the volume of the fiber reinforced polyurethane / polyisocyanurate foam at the outlet of the double belt laminator is 85% to 99%, preferably 90% to 99%, of the expanded volume of this same fiber reinforced polyurethane / polyisocyanurate foam in the case of free expansion without the constraint of the walls of such double belt laminator.
5. 3. The method of claim 1 or 2, wherein the expansion of the fiber reinforced polyurethane / polyisocyanurate foam is free, i.e., not constrained by the volume of a closed section.
6. 6. The method of claim 5, wherein after the step of allowing the fiber reinforced polyurethane / polyisocyanurate foam to freely rise, the fiber reinforced foam is cut to obtain blocks of the fiber reinforced polyurethane / polyisocyanurate foam.
7. 7. The method according to any one of claims 1 to 6, wherein the viscosity η of the mixture is between 30 mPa·s and 3000 mPa·s, preferably between 50 mPa·s and 1500 mPa·s, under standard temperature and pressure conditions.
8. At least 60% of the cells storing a gas having advantageously low thermal conductivity are parallel to the axis of thickness E of the block of fiber-reinforced polyurethane / polyisocyanurate foam. The method according to any one of claims 1 to 7, wherein the shape is elongated or elongated along an axis.
9. 9. The method according to any one of claims 1 to 8, wherein at least 80%, preferably at least 90%, of the cells storing a gas having advantageously low thermal conductivity have an elongated or elongated shape along an axis parallel to the axis of thickness E of the block of fibre reinforced polyurethane / polyisocyanurate foam.
10. A method according to any one of claims 1 to 9, wherein said long to continuous fibres consist of glass fibres, carbon fibres or any other organic or inorganic material, preferably glass fibres.
11. The fiber reinforcement (10) is disposed over the entire width L, 11. The method according to claim 1, wherein step b) of impregnating the fibers with the mixture of components and blowing agent to obtain the fiber reinforced polyurethane / polyisocyanurate foam is carried out simultaneously over the entire width L via a controlled liquid dispenser (15).
12. The method according to any one of the preceding claims, wherein the blowing agent consists of a physical blowing agent and / or a chemical blowing agent, preferably a combination of these two types.
13. 13. The method according to claim 12, wherein the physical expansion agent is selected from alkanes and cycloalkanes having at least 4 carbon atoms, dialkyl ethers, esters, ketones, acetals having 1 to 8 carbon atoms, fluoroalkanes, fluoroolefins, tetraalkylsilanes having 1 to 3 carbon atoms in the alkyl chain, in particular tetramethylsilane, and mixtures thereof.
14. The method of claim 12 , wherein the chemical leavening agent consists of water.
15. During step a) of mixing the chemical components, a nucleating gas is incorporated into at least one polyol compound under a pressure of 20 to 250 bar, preferably using a static / dynamic mixer, The method of claim 13, wherein the nucleating gas is from 0% to 50% by volume of the polyol, preferably from 0.05% to 20% by volume of the polyol.
16. 16. The method according to any one of the preceding claims, wherein during step a) of mixing the chemical components, the temperature of each of the reactants to obtain the polyurethane / polyisocyanurate is between 10°C and 40°C, preferably between 15°C and 30°C.
17. 17. The method according to any one of claims 1 to 16, wherein in step a) an organophosphorus flame retardant, preferably triethyl phosphate (TEP), tris(2-chloroisopropyl)phosphate (TCPP), tris(1,3-dichloroisopropyl)phosphate (TDCP), tris(2-chloroethyl)phosphate or tris(2,3-dibromopropyl)phosphate, or a mixture thereof, or an inorganic flame retardant, preferably red phosphorus, expandable graphite, aluminium oxide hydrate, antimony trioxide, arsenic oxide, ammonium polyphosphate, calcium sulfate or cyanuric acid derivatives, or a mixture thereof, is additionally added to the mixture.
18. The fiber content C f The method according to any one of claims 1 to 17, wherein said fiber reinforced foam block has a mass ratio of 7 to 15% by weight.
19. Thermal insulation of a closed, insulated tank, obtained directly by the method according to any one of claims 1 to 18. A block of fiber reinforced polyurethane / polyisocyanurate foam of a slab (30), The block of fiber-reinforced polyurethane / polyisocyanurate foam is composed of cells for storing gas, which advantageously has a low thermal conductivity and a density of 50 kg / m 3 and the fiber content C f represents at least 4% by weight of the block of fiber reinforced foam, the fibers having a length of at least 5 centimeters; The fiber content C f is uniformly distributed in the blocks of the fiber-reinforced polyurethane / polyisocyanurate foam, and the fiber content C f but varies by no more than ±35%, preferably no more than ±20%, over all or a portion of said fiber reinforced polyurethane / polyisocyanurate foam block.
20. A tank comprising a sealed, insulated tank integrated into a support structure, the tank comprising at least one sealed metal membrane made of a plurality of metal strakes or metal plates, which may include corrugations, and an insulating slab (30) comprising at least one insulating barrier adjacent to said sealed metal membrane, or It consists of a tank of type B or type C according to the definition given by the IGC Code, equipped with at least one insulating slab (30), 20. A sealed, insulated tank, wherein the insulating slab (30) comprises a block of the fiber reinforced polyurethane / polyisocyanurate foam of claim 19.
21. A vessel (70) for transporting cold liquid products, comprising at least one hull (72) and arranged within said hull a sealed, insulated tank (71) according to claim 20.
Citation Information
Patent Citations
Heat-insulating composite panel for membrane type liquified natural gas tank and its manufacturing method
JP2006214458A
Glass fiber-reinforced polyurethane / polyisocyanurate foamed article
JP2006241453A
Composition suitable for producing rigid polyurethane or rigid polyisocyanurate foams
JP2019518855A
Insulation boxes
WO2019108344A1