Highly concentrated and highly dispersed slurry composition and method for producing same

Cross-flow filtration in slurry composition production ensures high filler concentration and dispersion without aggregation, addressing sedimentation issues and maintaining stability.

JP7557300B2Active Publication Date: 2024-09-27ADMATECHS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020128736
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-29
Publication Date
2024-09-27
Estimated Expiration
2040-07-29

AI Technical Summary

Technical Problem

Conventional slurry compositions with high filler concentrations face challenges in achieving uniform dispersion and stability due to sedimentation and aggregation, leading to concentration gradients and reduced stability over time.

Method used

A method involving cross-flow filtration to remove dispersion medium from a highly dispersed slurry composition, maintaining conditions that prevent filler aggregation, resulting in a highly concentrated and dispersed state.

Benefits of technology

The method produces a slurry composition with high filler content and improved dispersibility, reducing the amount of dispersion medium and minimizing sedimentation, thereby enhancing stability and uniformity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557300000004
    Figure 0007557300000004
  • Figure 0007557300000007
    Figure 0007557300000007
  • Figure 0007557300000006
    Figure 0007557300000006
Patent Text Reader

Abstract

To provide a manufacturing method of a highly concentrated highly dispersed slurry composition, the method enabling increase of a filler content in a slurry composition.SOLUTION: A manufacturing method of a highly concentrated highly dispersed slurry composition is provided, comprising: a dispersion step of preparing highly dispersed slurry composition by dispersing a filler material constituted of a spherical inorganic material having a volume average particle size of 0.1 μm or larger and 3.0 μm or smaller in a dispersion medium being liquid in such a manner that a solid content is 52 vol.% or less based on a total mass; and a separation and concentration step of continuously circulating the highly concentrated highly dispersed slurry composition to a cross-flow filter to separate a part of the dispersion medium by filtration to concentrate until the solid content becomes over 52 vol.% based on a total mass, wherein the separation and concentration step is performed under the condition that coagulation is not generated on a filter membrane surface of the cross-flow filter.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a highly concentrated and highly dispersed slurry composition in which a filler composed of an inorganic material or the like is dispersed, and a method for producing the same. [Background technology]

[0002] Conventionally, resin compositions in which inorganic particulate materials composed of inorganic materials are dispersed as fillers in resin materials have been widely used. Such resin compositions have superior mechanical properties compared to resin materials and are widely used as semiconductor encapsulation materials, substrate materials, etc.

[0003] Incidentally, when dispersing a filler in a resin material, in addition to using a dry filler, a slurry composition in which the filler is dispersed in a dispersion medium may be used (Patent Document 1, etc.). This is because it may be difficult to uniformly disperse a dry filler in the resin material.

[0004] The slurry composition can be mixed and dispersed as it is in a resin material, for example, to disperse the filler material in the resin material. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 3920582 Summary of the Invention [Problem to be solved by the invention]

[0006] The resin composition obtained by mixing the slurry composition into the resin material contains a dispersion medium derived from the slurry composition. The amount of the dispersion medium contained in the resin composition is preferably small, and in order to reduce the amount of the dispersion medium contained in the resin material, it is effective to increase the concentration of the slurry composition and reduce the amount of the dispersion medium contained.

[0007] In addition, a low-concentration slurry composition is easy to disperse, but has a problem that the sedimentation rate of the filler material is high, and therefore the sedimentation stability over time is low. When the filler material settles in the slurry composition, a concentration gradient occurs, so it is necessary to stir and re-disperse the filler material before the process of using the slurry composition. In addition, when the sedimentation proceeds excessively, the filler material is in a compacted state, and re-dispersion by stirring may be difficult.

[0008] Such a high-concentration slurry composition has the advantage that the amount of dispersion medium contained can be reduced, and furthermore, the settling rate of the filler material is slow, so that the generation of a concentration gradient in the slurry composition due to settling is slow, and thus the composition has high stability over time.

[0009] However, a slurry composition containing a silica particle material at a high concentration of more than 75% by mass (52% by volume) has a high viscosity, and it is difficult to disperse the silica particle material to a high degree using a conventional dispersing machine, so there is no practical production method. Even if a high-concentration slurry composition in which a filler material is dispersed at a high concentration can be prepared, if the dispersion is insufficient, the filler material will exist as aggregates in the high-concentration slurry composition, and the aggregates, which are large particles, will settle quickly, causing a concentration gradient and resulting in insufficient stability over time.

[0010] The present invention was completed in consideration of the above-mentioned circumstances, and an object of the present invention is to provide a high-concentration, highly-dispersed slurry composition which contains a large amount of filler and is highly dispersed, and a method for producing a high-concentration, highly-dispersed slurry composition which can increase the filler content in the slurry composition and disperse the filler to a high degree. [Means for solving the problem]

[0011] In order to solve the above problems, the inventors conducted extensive research and discovered a method for producing a high-concentration, highly dispersed slurry composition having a high filler content and high dispersion, in which a relatively low-concentration slurry composition capable of increasing dispersibility is prepared and then the dispersion medium is removed to increase the concentration.

[0012] The spherical filler material can improve dispersibility and be made highly dispersed when it is made into a slurry composition having a normal concentration (solids concentration) (for example, a solids concentration of 52 volume% or less based on the total volume: hereinafter, when a percentage in a slurry composition is stated without indicating a standard, the value is based on the entire slurry composition).

[0013] A method was investigated, which is described in detail in the examples, for concentrating the filler material concentration by producing a highly dispersible slurry composition having a normal concentration and containing the filler material at a concentration lower than the target concentration, and then removing the dispersion medium.

[0014] As a result of the investigation, it was found that when the particle size of the filler material is equal to or less than a predetermined value and conditions are adopted that cause local concentration of the highly dispersed slurry composition in the concentration process for removing the dispersion medium, the filler material will aggregate in the area where the local concentration has progressed, and the composition will no longer be a highly dispersed slurry. Based on this knowledge, the investigation into the concentration process of the highly dispersed slurry composition was carried out, and it was found that it is possible to concentrate the composition without causing aggregation to progress by adopting specific conditions.

[0015] Specifically, by filtering and removing the dispersion medium from a highly dispersed slurry composition having a normal concentration using cross-flow filtration, it is possible to produce a highly concentrated, highly dispersed slurry composition by increasing the concentration of the highly dispersed slurry composition without causing localized concentration that accompanies aggregation of the filler material.

[0016] It has been found that localized thickening of the highly dispersed slurry composition is facilitated by localized removal of the dispersion medium. Note that the amount of dispersion medium removed must be carefully controlled, since once aggregates of the filler material have formed they cannot be easily redispersed by adding more dispersion medium.

[0017] Examples of the concentration method in which the dispersion medium is locally removed include a method of evaporating the dispersion medium from the surface of the highly dispersed slurry composition, total filtration, etc. In addition, even if cross-flow filtration is used, if the rate at which the dispersion medium is removed is too high, the filler material may be agglomerated, so it has been found that it is necessary to adopt appropriate filtration conditions. In particular, when the concentration of the highly dispersed slurry composition is low, the filler material is unlikely to agglomerate even if the rate at which the dispersion medium is removed is increased, so a lower limit value for the concentration of the highly dispersed slurry composition at which the method of the present invention works effectively has been set.

[0018] (1) Based on the above findings, the present inventors have completed the following invention. That is, the method for producing a highly concentrated and highly dispersed slurry composition of the present invention comprises a dispersing step of preparing a highly dispersed slurry composition by dispersing a filler material composed of a spherical inorganic material having a volume average particle size of 0.1 μm or more and 3.0 μm or less in a liquid dispersion medium so that the solid content is 52 volume % or less based on the total volume; a separation and concentration step in which the highly dispersed slurry composition is continuously circulated through a cross-flow filter to separate a portion of the dispersion medium by filtration, and the composition is concentrated to a solid content of more than 52% by volume based on the total volume to obtain a highly dispersed slurry composition; having The separation and concentration step is a method for producing a highly concentrated and highly dispersed slurry composition, which is carried out under conditions in which no aggregation occurs on the surface of the filtration membrane of the crossflow filter.

[0019] In particular, the condition for no aggregation to occur on the surface of the filtration membrane in the separation and concentration step is preferably that the flow rate of the highly dispersed slurry composition on the surface of the filtration membrane is equal to or higher than a predetermined value, and that at least one of the following (A) and (B) is satisfied. If the condition (A) or (B) is not satisfied, aggregates of the filler material are generated, and even if the condition is satisfied by adding a dispersion medium thereafter, the generated aggregates may not be redispersed. Therefore, in the method for producing a highly concentrated, highly dispersed slurry composition of this embodiment, it is preferable to always continue to satisfy both of these conditions (A) and (B). (A) The amount of the dispersion medium separated has not reached an amount at which the filler material would agglomerate if further separated. (B) The concentration of the filler material in the circulating highly dispersed slurry composition has not yet reached a concentration at which the filler material would agglomerate if the concentration were to increase any further.

[0020] (2) The above-mentioned method for producing a highly concentrated, highly dispersed slurry composition of the present invention makes it possible to produce a highly concentrated, highly dispersed slurry composition that could not be produced in the past, and makes it possible to provide the following inventions.

[0021] That is, the high-concentration, high-dispersion slurry composition of the present invention that solves the above problems comprises a filler material composed of a spherical inorganic material having a volume average particle size of 0.1 μm or more and 3.0 μm or less, a dispersion medium that is a liquid that disperses the filler material; The solid content is more than 52% by volume based on the total volume, The particle size distribution of the filler material dispersed in the dispersion medium, as measured by a laser diffraction method, is such that, based on the total volume, particles having a particle size of two times or more of the mode diameter are 15% by volume or less, particles having a particle size of three times or more of the mode diameter are 5% by volume or less, and particles having a particle size of four times or more of the mode diameter are 1% by volume or less, After being left in a cylindrical transparent container with a diameter of 35 mm for 300 hours with a liquid depth of 90 mm, the supernatant distance is 10 mm or less.

[0022] In particular, the solid content is preferably 68% by volume or less.Furthermore, it is preferable that the filler material is surface-treated with a silane compound. Effect of the Invention

[0023] The high-concentration, high-dispersion slurry composition of the present invention has a higher concentration than conventional ones, so that it is possible to reduce the proportion of the dispersion medium contained. Furthermore, the method for producing the high-concentration, high-dispersion slurry composition of the present invention makes it possible to produce such a high-concentration, high-dispersion slurry composition. [Brief description of the drawings]

[0024] [Figure 1] 1 is a particle size distribution of the slurry composition of Example 1. [Diagram 2] 1 is a particle size distribution of the slurry composition of Example 2. [Diagram 3] 1 is a particle size distribution of the slurry composition of Example 3. [Figure 4] 1 is a particle size distribution of the slurry composition of Example 4. [Diagram 5] 1 shows the particle size distribution of the slurry composition of Comparative Example 1. [Figure 6] 1 shows the particle size distribution of the slurry composition of Comparative Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] The high-concentration, high-dispersion slurry composition and the manufacturing method thereof according to the present embodiment will be described in detail below based on the embodiment. The high-concentration, high-dispersion slurry composition according to the present embodiment is a high-concentration, high-dispersion slurry composition in which a filler material is dispersed in a liquid dispersion medium. The high-concentration, high-dispersion slurry composition according to the present embodiment is a dispersion liquid that is a uniform fluid throughout.

[0026] (Highly concentrated and highly dispersed slurry composition) The high-concentration, high-dispersion slurry composition of this embodiment has a filler material and a dispersion medium that disperses the filler material. It may further have other components. Examples of other components include a dispersant and a resin. Although the presence of a dispersant can suppress the aggregation of the filler material, it is preferable that the number of components other than the filler material is as small as possible, so that the amount of dispersant is small, and in particular, it is preferable that there is no dispersant. The resin may be polymerized by polymerization. The dispersant and resin are preferably dissolved in the dispersion medium, and even if they are not dissolved, they may have a particulate form having a particle size similar to that of the filler material and be dispersed in the dispersion medium.

[0027] The filler material is composed of a spherical inorganic material with a volume average particle size of 0.1 μm or more and 3.0 μm or less. The volume average particle size of the filler material is a value measured in a state where it is separated into primary particles. The lower limit of the volume average particle size can be 0.11 μm, 0.12 μm, 0.13 μm, 0.2 μm, or 0.3 μm, and the upper limit can be 2.9 μm, 2.8 μm, 2.7 μm, 2.5 μm, 2.0 μm, 1.5 μm, or 1.0 μm. These lower and upper limits can be combined arbitrarily. The particle size of the filler material is controlled as necessary.

[0028] The inorganic material constituting the filler material is not particularly limited, but examples include silica, alumina, titania, zirconia, mixtures thereof, and composite oxides. Any crystal type can be used. It is preferable that the content of uranium, thorium, etc., which emit α-rays, is low, and it is also preferable that the content of alkali metals and alkaline earth metals is low.

[0029] The filler material is spherical, and the sphericity of 0.95 or more, 0.98 or more, or 0.99 or more can be used. The greater the sphericity, the better the filling property tends to be, and the lower the viscosity of the high-concentration, high-dispersion slurry composition tends to be. The sphericity is measured by taking a photograph with an SEM, and using the area and perimeter of the observed particles, (sphericity) = {4π × (area) ÷ (perimeter)} 2 The closer to 1, the closer to a perfect sphere. Specifically, the average value measured for 100 particles using image analysis software (Asahi Kasei Engineering Corporation: A-zo-kun) is used.

[0030] The filler material may be surface-treated. By performing the surface treatment, the surface properties of the filler material can be made preferable. For example, when mixed into a resin material, the filler material can be hydrophobized (phenyl group, hydrocarbon group, etc.) to improve affinity with the resin material, or functional groups reactive with the resin (vinyl group, epoxy group, acrylic group, methacrylic group, etc.) can be introduced. The amount of surface treatment is not particularly limited, but the surface can be treated so as to achieve the desired properties. In addition, when the surface treatment agent is a substance that reacts with the functional groups (OH groups, etc.) on the surface of the filler material, the amount of the surface treatment agent can be selected according to the amount of functional groups present on the surface of the filler material (the total amount, half amount, etc. of the functional groups on the surface).

[0031] A silane compound can be used as a surface treatment agent for performing the surface treatment. Examples of the silane compound include so-called silane coupling agents having SiH, SiOH, and SiOR (R is a hydrocarbon group) and silazanes such as hexamethylenedisilazane, and examples of the silane compound include those in which any functional group is bonded to Si.

[0032] The optional functional group may be a hydrocarbon group (an alkyl group (e.g., a methyl group, an ethyl group, a propyl group, a butyl group), an alkenyl group (e.g., a vinyl group, an ethenyl group, a propenyl group), a phenyl group, an amino group, a phenylamino group, an acrylic group, a methacrylic group, an epoxy group, a styryl group, a silicone, or a combination of these. As the silane compound, one type may be used for treatment, or two or more types may be used in combination for treatment. When two or more types are used in combination for surface treatment, multiple types of surface treatment agents may be mixed and used for surface treatment, or multiple types of surface treatment agents may be used sequentially for surface treatment.

[0033] The dispersion medium is a liquid, and examples of the dispersion medium include water and organic solvents. Examples of organic solvents include alkanes (e.g., hexane), alcohols (e.g., methanol, ethanol, propanol), ketones (e.g., acetone, cyclohexanone), and aromatic hydrocarbons (e.g., benzene, toluene, ethylbenzene, xylene), which are used alone or in combination.

[0034] The filler material contained in the high-concentration, high-dispersion slurry composition of this embodiment is based on the mode diameter calculated from the particle size distribution measured by the laser diffraction method, and has 15 vol % or less of particles having a particle size of 2 times or more of the mode diameter, 5 vol % or less of particles having a particle size of 3 times or more of the mode diameter, and 1 vol % or less of particles having a particle size of 4 times or more of the mode diameter. If this condition is met, it can be treated as if no aggregates exist, and the measurement object is judged to be a homogeneous fluid as a whole and to maintain the high dispersibility of the present invention.

[0035] The measurement of particle size distribution by the laser diffraction method in this specification is performed without ultrasonic irradiation. Specifically, the measurement is performed using HORIBA's LA-750, and a dedicated flow cell for LA-750, which performs measurement while circulating liquid, is used as the cell. A small amount of high-concentration, high-dispersion slurry composition is poured into the cell in which the dispersion medium is circulating, and the measurement is performed in a state where the concentration is adjusted to a predetermined value. The predetermined concentration is a concentration at which the laser transmittance when the cell is irradiated with a laser is 60% to 90%. When measuring particle size distribution using the above device, ultrasonic irradiation is usually performed, but the measurement conditions in this specification are to measure the particle size distribution by circulating the dispersion medium only, without dispersing with ultrasonic waves or the like. The aggregates of the filler material formed in the slurry composition are not eliminated even when diluted, and are detected by the laser diffraction method. Therefore, the generation of aggregates can be detected by the laser diffraction method.

[0036] Furthermore, the high concentration, highly dispersed slurry composition of this embodiment has a supernatant distance of 10 mm or less after being left to stand for 300 hours at 90 mm in a cylindrical transparent container with a diameter of 35 mm. Here, the liquid length may be equal to or greater than the above-mentioned value. The supernatant distance is preferably 9 mm or less, 8 mm or less, 7 mm or less, 6 mm or less, 5 mm or less, 4 mm or less, 3 mm or less, 2 mm or less, or 1 mm or less.

[0037] The high-concentration, high-dispersion slurry composition of the present embodiment contains a high concentration of solids based on the total volume. Whether or not it is a high concentration is determined by whether or not the solids are contained in an amount of more than 52% by volume based on the total volume.

[0038] Preferable lower limits of the solid content concentration include 53 vol%, 54 vol%, 55 vol%, 56 vol%, 57 vol%, 58 vol%, 59 vol%, 60 vol%, 61 vol%, 62 vol%, 63 vol%, 64 vol%, and 65 vol%. Preferable upper limits of the solid content are not particularly limited as long as the slurry state can be maintained, and include values ​​such as 75 vol%, 73 vol%, 71 vol%, 70 vol%, 69 vol%, 68 vol%, and 67 vol%.

[0039] The solid content is assumed to be composed of the filler material, but solid materials other than the filler material are permitted to be contained as solid content. If the amount of solid content is specified based on the total mass, when the solid content is composed almost entirely of the filler material and the filler material is composed of silica, the specific gravity of silica is 2.20 g / cm 3 The specific gravity of organic solvents as typical dispersion media is 0.70 to 0.95 g / cm 3 (Methyl ethyl ketone: MEK, specific gravity 0.81 g / cm 3 ), the high-concentration, high-dispersion slurry composition of this embodiment contains more than 75 mass% of solids based on the total mass. Preferred lower limits include 76 mass%, 77 mass%, 78 mass%, 79 mass%, 80 mass%, 81 mass%, 82 mass%, 83 mass%, and 84 mass%. Preferred upper limits are not particularly limited as long as high dispersibility can be maintained, and include values ​​such as 90 mass%, 88 mass%, 86 mass%, and 85 mass%.

[0040] The solid content includes the filler material and other solid matter. If there is no solid matter other than the filler material, the content of the filler material is the solid content. Even if a component becomes solid when the dispersion medium is removed, if it is dissolved in the dispersion medium, it is not included in the solid content because it does not exist as a solid.

[0041] (Method for producing high-concentration, high-dispersion slurry composition) The method for producing a high-concentration, highly-dispersed slurry composition of the present embodiment is a method for producing a high-concentration, highly-dispersed slurry composition without forming aggregates of the filler material even at a concentration where the filler material is difficult to disperse in the dispersion medium at that concentration. After producing a highly-dispersed slurry composition in which the filler material is dispersed in the dispersion medium at a concentration lower than the concentration of the filler material contained in the high-concentration, highly-dispersed slurry composition to be produced, the method is a method for producing a high-concentration, highly-dispersed slurry composition having a higher concentration than the high-dispersed slurry composition and in which aggregation of the filler material is unlikely to progress by removing the dispersion medium while preventing aggregation of the filler material.

[0042] The method for producing a high-concentration, highly dispersed slurry composition of this embodiment includes a dispersion step and a separation and concentration step. The dispersion step is a step of preparing a highly dispersed slurry composition by dispersing a filler material in a dispersion medium so that the solid content is 52 volume % or less based on the total volume. The upper limit of the amount of solid content contained in the highly dispersed slurry composition is a concentration lower than the high concentration (more than 52 volume %) mentioned in the description of the highly concentrated, highly dispersed slurry composition described above.

[0043] Specifically, the amount of solids is not particularly limited as long as it is an amount that can form a highly dispersed slurry composition simply by mixing and dispersing in a dispersion medium. In order to remove excess dispersion medium, it is preferable that the amount of solids in the highly dispersed slurry composition is as large as possible. For example, the upper limit of the amount of solids (particularly the amount of filler material) can be about 50 volume %, 48 volume %, 46 volume %, or 44 volume % based on the total volume.

[0044] The explanation of the filler material and the dispersion medium is the same as that of the high-concentration, high-dispersion slurry composition described above, and therefore further explanation is omitted. Regarding the solid content, when a solid is contained other than the filler material, the contained components are also included, but when only the filler material is contained, the amount of the solid content and the amount of the filler material are the same.

[0045] The dispersion method in the dispersion step is not particularly limited, but examples thereof include stirring, ultrasonic irradiation, and applying shear force. The dispersion medium may be gradually added to the filler material to disperse it, or the filler material may be gradually added to the dispersion medium to disperse it, or the filler material and the dispersion medium may be mixed in their entirety and dispersed. When multiple types of dispersion medium are used, the dispersion medium may be added in sequence for each type.

[0046] The separation and concentration step is a step of concentrating the highly dispersed slurry composition by separating the dispersion medium from the highly dispersed slurry composition to prepare a highly concentrated, highly dispersed slurry composition. The highly dispersed slurry composition is concentrated until the solid content exceeds 52% by volume based on the total volume. The amount of solid content in the highly dispersed slurry composition finally produced by concentration is preferably as high as possible within the range in which no aggregates are formed.

[0047] Specifically, the separation and concentration step involves removing the dispersion medium from the highly dispersed slurry composition using a cross-flow filter. A cross-flow filter is a machine that filters the highly dispersed slurry composition while flowing it along a filter membrane. Cross-flow filtration can reduce the force applied to the contained filler material. In particular, the separation and concentration step is preferably a step that does not involve removal of the dispersion medium by evaporation (a step that is not primarily involved in removal of the dispersion medium by heating, decompression, etc.).

[0048] The filtration membrane may be in the form of a tube or a plate. When a tubular filtration membrane is used, the highly dispersed slurry composition is passed through the tube constituting the filtration membrane, and the dispersion is filtered out from the tube wall. When a plate-shaped filtration membrane is used, the filtration membrane is rotated at high speed while filtering, and the highly dispersed slurry composition flows relatively along the surface of the filtration membrane. The pore size of the filtration membrane is determined appropriately according to the particle size of the filler material. A pore size that does not allow the smallest particles of the inorganic particle material contained in the filler material to pass through can be adopted. For example, in order to prevent the passage of particles of a predetermined particle size (for example, 10 nm), a filtration membrane having a pore size of half the predetermined particle size or less (5 nm when the predetermined particle size is 10 nm) can be adopted, which can sufficiently prevent the passage of not only particles having the predetermined particle size but also particles having a particle size larger than the predetermined particle size. Furthermore, it is preferable that the pore size of the filtration membrane is close to uniform.

[0049] The separation and concentration process is a process carried out under conditions in which the filler material does not aggregate. In this process, "aggregation of the filler material occurs" means that the aggregated filler material is mixed into the concentrated highly dispersed slurry composition. In other words, even if the filler material aggregates in this process, it can be treated as "aggregation of the filler material occurs" if it is not ultimately mixed into the highly dispersed slurry composition.

[0050] The cross-flow filter separates the dispersion medium by the filter membrane while flowing the highly dispersed slurry composition in a direction along the filter membrane. Since the highly dispersed slurry composition flows in a direction along the filter membrane, the filler material contained in the highly dispersed slurry composition is prevented from accumulating on the filter membrane.

[0051] In the dead-end filtration, the filler material is deposited on the filtration membrane to form aggregates, but in the cross-flow filtration, the filler does not deposit, so the formation of aggregates is also suppressed. The speed at which the highly dispersed slurry composition flows on the filtration membrane surface is preferably set to a predetermined flow rate or more at a level at which the dispersion medium is removed by the filtration membrane and the filler material does not deposit. In addition, even when conditions are adopted that cause the deposition of the filler material on the surface of the filtration membrane, it is possible to suppress the incorporation of aggregates of the filler material into the produced high-concentration highly dispersed slurry composition by adopting conditions that do not allow the deposited filler material to return to the highly dispersed slurry composition, but it is preferable to adopt conditions that do not cause deposition as much as possible because the deposited filler material will be wasted.

[0052] The separation and concentration step is carried out under conditions that do not cause aggregation of the filler material, and specifically, at least one of the following conditions (A) and (B) can be adopted as preferable conditions. Condition (B) is easier to control because the concentration of the filler material is measured directly, but condition (A) is easier to measure.

[0053] (A) The amount of the dispersion medium separated has not reached an amount at which the filler material would agglomerate if further separated. This condition is met by measuring the amount of dispersion medium separated by the filtration membrane to determine whether or not the concentration of the filler material in the highly dispersed slurry composition is at a level at which aggregation occurs.

[0054] (B) The concentration of the filler material in the circulating highly dispersed slurry composition has not yet reached a concentration at which the filler material would agglomerate if the concentration were to increase any further. This condition is determined by actually measuring the filler concentration in the highly dispersed slurry composition to determine whether or not the concentration is such that aggregation occurs in the highly dispersed slurry composition. EXAMPLES

[0055] The highly concentrated and highly dispersed slurry composition and the method for producing the same of the present invention will be described in detail below with reference to examples.

[0056] Example 1 A high-concentration, high-dispersion slurry composition was prepared using a surface-treated filler material. The filler material used was a surface-treated inorganic particle material obtained by reacting a silane compound (N-phenyl-3-aminopropyltrimethoxysilane, KBM-573, Shin-Etsu Chemical Co., Ltd.) as a surface treatment agent with an inorganic particle material (sphericity 0.99, Admatechs, Admafine SO-C2) made of silica with an average particle size of 0.5 μm, synthesized by the VMC method (a method of producing metal oxide particles by putting metal particles into an oxidizing flame and causing a deflagration phenomenon). The surface treatment of the inorganic particle material was performed in an amount of 0.6% based on the mass of the inorganic particle material.

[0057] The highly concentrated and highly dispersed slurry composition in this example uses this surface-treated inorganic particulate material as a filler material and MEK as a dispersion medium.

[0058] 100 parts by mass of the above-mentioned surface-treated inorganic particle material and 42 parts by mass of MEK were premixed with a stirrer to form a coarse slurry composition, and then a highly dispersed slurry composition in which the filler material was uniformly dispersed was prepared using a disperser (dispersion step). The concentration of the solid content (filler material) in the highly dispersed slurry composition was about 70% by mass (46% by volume).

[0059] The obtained highly dispersed slurry composition was circulated through a cross-flow filter having a tubular filtration membrane (a ceramic filter with a filtration surface composed of nano-sized pores of 10 nm or less and 1 nm or more) until 24 parts by mass of MEK was removed, to obtain a highly concentrated, highly dispersed slurry composition with a filler material concentration of 84.7% by mass (67% by volume) (separation and concentration process), which was used as the test sample for this example.

[0060] Example 2 The high-concentration, high-dispersion slurry composition in this example uses the surface-treated inorganic particulate material used in Example 1 as a filler material, and methyl isobutyl ketone (MIBK) as a dispersion medium.

[0061] 100 parts by mass of the surface-treated inorganic particulate material used in Example 1 and 42 parts by mass of MIBK were premixed with a stirrer to form a coarse slurry composition, and then a highly dispersed slurry composition in which the filler material was uniformly dispersed was prepared using a disperser (dispersion step). The concentration of the solid content (filler material) in the highly dispersed slurry composition was about 70% by mass (46% by volume).

[0062] The obtained highly dispersed slurry composition was circulated through a cross-flow filter having the same filtration membrane as used in Example 1 until 22 parts by mass of MIBK was removed, thereby obtaining a highly concentrated, highly dispersed slurry composition of this example having a filler material concentration of 83.3% by mass (64% by volume) (separation and concentration process), which was used as the test sample of this example.

[0063] Example 3 The high-concentration, high-dispersion slurry composition in this example uses the surface-treated inorganic particulate material used in Example 1 as a filler material and MEK as a dispersion medium.

[0064] 100 parts by mass of the surface-treated inorganic particulate material used in Example 1 and 42 parts by mass of MEK were premixed with a stirrer to form a coarse slurry composition, and then a highly dispersed slurry composition in which the filler material was uniformly dispersed was prepared using a disperser (dispersion step). The concentration of the solid content (filler material) in the highly dispersed slurry composition was about 70% by mass (46% by volume).

[0065] The obtained highly dispersed slurry composition was circulated through a cross-flow filter having the same filtration membrane as used in Example 1 until 17 parts by mass of MEK was removed, thereby obtaining a highly concentrated, highly dispersed slurry composition of this example having a filler material concentration of 80% by mass (60% by volume) (separation and concentration process), which was used as the test sample of this example.

[0066] Example 4 The high-concentration, high-dispersion slurry composition in this example uses the surface-treated inorganic particulate material used in Example 1 as a filler material and MEK as a dispersion medium.

[0067] 100 parts by mass of the surface-treated inorganic particulate material used in Example 1 and 42 parts by mass of MEK were premixed with a stirrer to form a coarse slurry composition, and then a highly dispersed slurry composition in which the filler material was uniformly dispersed was prepared using a disperser (dispersion step). The concentration of the solid content (filler material) in the highly dispersed slurry composition was about 70% by mass (46% by volume).

[0068] The obtained highly dispersed slurry composition was circulated through a cross-flow filter having the same filtration membrane as used in Example 1 until 12 parts by mass of MEK was removed, thereby obtaining a highly concentrated, highly dispersed slurry composition of this example having a filler material concentration of 76.9% by mass (55% by volume) (separation and concentration process), which was used as the test sample of this example.

[0069] Comparative Example 1 The high-concentration, high-dispersion slurry composition in this comparative example uses the surface-treated inorganic particulate material used in Example 1 as a filler material and MEK as a dispersion medium.

[0070] 100 parts by mass of the surface-treated inorganic particulate material used in Example 1 and 25 parts by mass of MEK were premixed with a stirrer to form a crude slurry composition, which was then dispersed with a disperser until the dispersibility did not improve any further (corresponding to the dispersion step), but the resulting slurry composition did not reach a highly dispersed state. This slurry composition was used as the test sample of this comparative example. The concentration of solids (filler material) in this test sample was 80% by mass (60% by volume).

[0071] Comparative Example 2 The high-concentration, high-dispersion slurry composition in this comparative example uses the surface-treated inorganic particulate material used in Example 1 as a filler material and MEK as a dispersion medium.

[0072] 100 parts by mass of the surface-treated inorganic particle material used in Example 1 and 18 parts by mass of MEK were premixed with a stirrer, and then an attempt was made to disperse the mixture using a disperser, but the mixture did not even become a slurry. This composition was used as the test sample of this comparative example. The concentration of the solid content (filler material) in this test sample was 84.7% by mass (67% by volume).

[0073] Comparative Example 3 A slurry composition was prepared in the same manner as in Example 1 up to the dispersion step. After that, 17 parts by mass of MEK was removed from this slurry composition using an evaporator. The obtained slurry composition (concentration: about 80% by mass: 60% by volume) had aggregates that could be confirmed with the naked eye.

[0074] Comparative Example 4 A slurry composition was prepared as a test sample of this comparative example in the same manner as in Example 1 up to the dispersion step. The concentration of the obtained slurry composition was 70 mass % (46 volume %), and it was a highly dispersed slurry composition.

[0075] (Measurement of particle size distribution and evaluation of settling properties) The particle size distribution of the test samples of each of the Examples and Comparative Examples was measured by a laser diffraction method. Comparative Example 2 was not evaluated because it did not become a slurry, and Comparative Example 3 was evaluated because aggregates were observed with the naked eye.

[0076] The particle size distribution was measured using HORIBA's LA-750. The particle size distribution was measured by the laser diffraction method in a state where a small amount of the test sample was poured into a flow cell in which the dispersion medium was circulating and adjusted to a predetermined concentration. When circulating the dispersion medium, ultrasonic waves may be irradiated to disperse the sample, but in the present invention, ultrasonic irradiation was not performed and the sample was dispersed only by circulation and then measured.

[0077] The predetermined concentration is a concentration at which the transmittance of a laser when the cell is irradiated with the laser (He-Ne laser: wavelength 632.8 nm) is 60% to 90%.

[0078] The measured particle size distributions are shown in Figure 1 (Example 1), Figure 2 (Example 2), Figure 3 (Example 3), Figure 4 (Example 4), Figure 5 (Comparative Example 1), and Figure 6 (Comparative Example 4). Table 1 shows the results of calculating the volume of particles having a mode diameter calculated from the measured particle size distribution, and a particle diameter twice or more (components that are the mode diameter x 2 or more), three times or more (components that are the mode diameter x 3 or more), and four times or more (components that are the mode diameter x 4 or more) the particle diameter calculated from the mode diameter, and Table 2 shows the particle diameters of each test sample.

[0079] Settling property was evaluated for Examples 1 to 3 and Comparative Example 4. Comparative Examples 1 to 3 were not evaluated because they were clearly not suitable for practical use, with more than 15% by volume of particles twice the mode diameter or larger, failure to form a slurry, and large aggregates visible to the naked eye.

[0080] The sedimentation property was evaluated by leaving each test sample in a cylindrical transparent container with a diameter of 35 mm with a liquid depth of 90 mm for 300 hours, and then measuring the distance (skimming distance) of the transparent part (skimming layer) formed by the sedimentation of the filler material.

[0081] [Table 1]

[0082] [Table 2]

[0083] In Examples 1 to 4, the particles having a diameter of two or more times the mode diameter were 15% by volume or less, the particles having a diameter of three or more times the mode diameter were 5% by volume or less, and the particles having a diameter of four or more times the mode diameter were 1% by volume or less. The supernatant distance was 10 mm or less, which shows that the particles have better dispersibility than Comparative Example 1 and are in a highly dispersed state.

[0084] In this embodiment, particles with a volume average particle size of 0.5 μm are used to explain the present invention applicable to a volume average particle size range of 0.1 μm to 3.0 μm. This is because the present invention is an invention that mainly improves the properties related to sedimentation, and therefore results equivalent to those of particles with a volume average particle size of 0.5 μm can be obtained for a volume average particle size range of 0.1 μm to 3.0 μm.

[0085] Settling properties are mainly governed by viscosity in the range of 50 μm or less, and the influence of Brownian motion cannot be ignored in the range of less than 0.1 μm. It is known that settling properties governed by viscosity are well approximated by Stokes' law, and the range of volume average particle size of 0.1 μm to 3.0 μm, which is the range of application of this invention, is also a range that can be adequately approximated by Stokes' law, and this invention is fully supported by the results of particles with a volume average particle size of 0.5 μm.

[0086] The following is a general explanation of Stokes' law. It is known that particles in the submicron to micron order exhibit settling properties according to Stokes' law. Based on Stokes' law, the settling velocity can be calculated by the following formula:

[0087] V = [(ρ1-ρ2)gD 2 ] / 18μ where V is the settling velocity of the particle [m / s], ρ1 is the density of the particle [kg / m 3 ], ρ2 is the density of the dispersion medium [kg / m 3 ], g is the gravitational acceleration [m / s 2 ], μ is the viscosity coefficient [Pa s], and D is the particle diameter [m].

[0088] However, the range within which the settling velocity obeys Stokes' law can be set by the dimensionless Reynolds number Re, which is expressed as the ratio of inertial force to viscous force.

[0089] Re = ρUL / μ where ρ is the density of the fluid [kg / m 3 ], U is the characteristic velocity of the fluid [m / s], L is the characteristic length [m], and μ is the viscosity coefficient of the fluid [Pa s].

[0090] The range in which the settling velocity follows Stokes' law is when Re<0.25, and Stokes' law only applies when the settling of particles is mainly governed by viscosity. When Re is greater than this value, the flow velocity of the boundary layer between the dispersion medium and the particles increases, causing the boundary layer to separate and generating vortex flows behind the settling particles. In this state, not only viscosity but also inertia comes into play in the settling of the particles, so the settling velocity can no longer be calculated using Stokes' law.

[0091] In reality, it is believed that particles with a diameter of approximately 50 μm or less settle according to Stokes' law, although this differs depending on the particle shape, density, density of the solvent, etc. Furthermore, for particles with a diameter of less than 0.01 μm, the Brownian motion of the particles becomes dominant, and the settling behavior does not follow Stokes' law.

[0092] (Definition of terms used in the Examples and Comparative Examples) Highly concentrated and highly dispersed slurry composition: a slurry composition containing a filler material at a concentration of more than 75% by mass and which is well dispersed.

[0093] Highly dispersed slurry composition: A slurry composition containing a filler material at a concentration of 75% by weight or less, and which is well dispersed.

[0094] Coarse slurry composition: A slurry composition in an insufficiently dispersed state obtained by premixing a filler material with a dispersion medium.

Claims

1. a filler material made of an inorganic material consisting of spherical silica having a volume average particle size of 0.1 μm or more and 3.0 μm or less; A dispersion medium that is a liquid that disperses the filler material, The solid content is more than 52% by volume based on the total volume; The particle size distribution of the filler material dispersed in the dispersion medium, as measured by a laser diffraction method without irradiating the filler with ultrasonic waves, is such that, based on the total volume, particles having a particle size of two times or more of the mode diameter are 3.4 vol % or less, particles having a particle size of three times or more of the mode diameter are 0.7 vol % or less, and particles having a particle size of four times or more of the mode diameter are 0 vol % or less, A highly concentrated and highly dispersed slurry composition, which has a supernatant distance of 10 mm or less after being allowed to stand for 300 hours in a cylindrical transparent container with a liquid length of 90 mm.

2. 2. The highly concentrated and highly dispersed slurry composition according to claim 1, wherein the solid content is 68% by volume or less.

3. 3. The highly concentrated and highly dispersed slurry composition according to claim 1, wherein the filler material is surface-treated with a silane compound.

4. A method for producing a highly concentrated and highly dispersed slurry composition according to any one of claims 1 to 3, comprising: A dispersion step of preparing a highly dispersed slurry composition by dispersing a filler material composed of a spherical inorganic material having a volume average particle size of 0.1 μm or more and 3.0 μm or less in a liquid dispersion medium so that the solid content is 52 volume % or less based on the total volume; a separation and concentration step of continuously circulating the highly dispersed slurry composition through a cross-flow filter to separate a portion of the dispersion medium by filtration and concentrate the composition until the solid content exceeds 52% by volume based on the total volume; having The method for producing a highly concentrated and highly dispersed slurry composition, wherein the separation and concentration step is carried out under conditions in which no aggregation occurs on the surface of the filtration membrane of the crossflow filter.

5. The method for producing a high-concentration, highly-dispersed slurry composition according to claim 4, wherein the condition for preventing aggregation on the surface of the filtration membrane in the separation and concentration process is that the flow rate of the highly-dispersed slurry composition on the surface of the filtration membrane is equal to or higher than a predetermined value, and at least one of the following (A) and (B) is satisfied. (A) The amount of the dispersion medium separated has not reached an amount at which the filler material would agglomerate if further separated. (B) The concentration of the filler material in the circulating highly dispersed slurry composition has not yet reached a concentration at which the filler material would agglomerate if the concentration were to increase any further.

Citation Information

Patent Citations

  • Wet type silica dispersion liquid and method of manufacturing the same

    JP2005231954A

  • Spherical silica powder, slurry using the same and resin composition

    JP2012240900A

  • Filler-containing slurry composition

    JP3920582B2

  • Sol-gel silica powder and method for producing same

    WO2018096876A1