Joined structure and joining method
The bonded structure addresses the issue of reduced bonding strength by incorporating recessed joint surfaces to store intermetallic compounds, improving the bonding strength of dissimilar metals through reduced exposure.
Patent Information
- Application Number
- JP2020170292
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-08
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2040-10-08
AI Technical Summary
Existing bonded structures of dissimilar metals, such as those described in Patent Document 1, face a risk of decreased bonding strength due to the exposure of intermetallic compounds at the joint ends, necessitating improved joining methods.
A bonded structure design featuring recessed joint surfaces with a main surface extending across the recess, allowing intermetallic compounds to be stored within the recesses, reducing the exposed area of these compounds by applying a voltage and pressing the joint surfaces together.
This configuration minimizes the exposed area of intermetallic compounds, thereby enhancing the bonding strength and ensuring proper joining of dissimilar metals.
Smart Images

Figure 0007557331000009 
Figure 0007557331000010 
Figure 0007557331000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a joint structure and a joining method. [Background technology]
[0002] As a conventional joint structure, for example, Patent Document 1 describes a welded joint in which an iron-based metal member and an aluminum-based metal member are joined via a molten layer. This welded joint suppresses a decrease in joint strength by specifying the volume fraction and size of the intermetallic compound contained in the molten layer. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-126824 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, the joint structure described in the above-mentioned Patent Document 1 may have a reduced joint strength in the intermetallic compound exposed from the end of the molten layer, for example, and there is room for further improvement in this regard.
[0005] Therefore, the present invention has been made in consideration of the above, and an object of the present invention is to provide a joint structure and a joining method capable of properly joining dissimilar metals. [Means for solving the problem]
[0006] In order to solve the above-mentioned problems and achieve the object, the bonded structure of the present invention comprises a first metal member having a first bonding surface, a second metal member which is a metal member different from the first metal member and has a second bonding surface, and a liquid phase bonded portion formed by liquid phase bonding the first bonding surface and the second bonding surface which face each other along a facing direction, wherein at least one of the first bonding surface and the second bonding surface has a recessed portion formed by being recessed along the facing direction, and a bonding main surface which extends along a cross direction which intersects the facing direction and surrounds the recessed portion, wherein the distance between the recessed portion and the other of the first bonding surface and the second bonding surface in the facing direction is longer than the distance between the bonding main surface and the other, and an intermetallic compound generated by the liquid phase bonding is stored in the recessed portion.
[0007] The joining method according to the present invention includes a joining step in which a first joining surface of a first metal member and a second joining surface of a second metal member, which is a metal member different from the first metal member, are pressed against each other, and a voltage is applied to the first metal member and the second metal member to perform liquid phase joining, wherein at least one of the first joining surface and the second joining surface has a recessed portion formed by being recessed along the opposing direction, and a main joining surface extending along a cross direction that intersects the opposing direction and surrounding the recessed portion, and the recessed portion is characterized in that a distance between the recessed portion and the other of the first joining surface and the second joining surface in the opposing direction is longer than a distance between the main joining surface and the other, and the recessed portion stores an intermetallic compound produced by the liquid phase joining. Effect of the Invention
[0008] In the joined structure and joining method according to the present invention, the joining surface to be liquid phase joined has a recess and a main joining surface surrounding the recess, so that the area of the exposed end face of the intermetallic compound can be reduced, and as a result, dissimilar metals can be properly joined. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a cross-sectional view showing an example of the configuration of a joint structure according to an embodiment. [Diagram 2]FIG. 2 is a perspective view showing an example of the configuration of the aluminum plate and the copper plate according to the embodiment. [Diagram 3] FIG. 3 is a schematic diagram showing an example of the configuration of a welding machine according to an embodiment. [Figure 4] FIG. 4 is a cross-sectional view showing an aluminum plate and a copper plate before being joined together according to the embodiment. [Diagram 5] FIG. 5 is a cross-sectional view showing an aluminum plate and a copper plate being joined together according to the embodiment. [Figure 6] FIG. 6 is a flowchart showing steps of the bonding method according to the embodiment. [Figure 7] FIG. 7 is a cross-sectional view showing a configuration example of a joint structure according to a modified example of the embodiment. [Figure 8] FIG. 8 is a perspective view showing an example of the configuration of an aluminum plate and a copper plate according to a modified example of the embodiment. [Figure 9] FIG. 9 is a cross-sectional view showing an example of the configuration of an aluminum plate and a copper plate before being joined together according to a modified example of the embodiment. [Figure 10] FIG. 10 is a cross-sectional view showing a configuration example of an aluminum plate and a copper plate being joined together according to a modified example of the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The form (embodiment) for carrying out the present invention will be described in detail with reference to the drawings. The present invention is not limited to the contents described in the following embodiment. Furthermore, the components described below include those that a person skilled in the art can easily imagine and those that are substantially the same. Furthermore, the configurations described below can be appropriately combined. Furthermore, various omissions, substitutions, or modifications of the configurations can be made without departing from the gist of the present invention.
[0011] [Embodiment] A bonded structure 1 and a bonding method according to an embodiment will be described with reference to the drawings. The bonded structure 1 is formed by liquid phase bonding of dissimilar metals using a bonding method. Here, liquid phase bonding refers to bonding by applying a voltage to a bonding portion in a state where the metals to be bonded are combined with each other, and melting the metals at the bonding portion. As shown in Figs. 1 and 2, the bonded structure 1 includes an aluminum plate 10 as a first metal member, a copper plate 20 as a second metal member, and a liquid phase bonding portion 30. In this example, the aluminum plate 10 and the copper plate 20 are each formed in a rectangular shape.
[0012] In the following description, the direction along the short sides of the aluminum plate 10 and the copper plate 20 is referred to as the short side direction (cross direction) X, the direction along the long sides of the aluminum plate 10 and the copper plate 20 is referred to as the long side direction (cross direction) Y, and the direction in which the aluminum plate 10 and the copper plate 20 face each other is referred to as the facing direction Z. The short side direction X, the long side direction Y, and the facing direction Z cross each other and are typically perpendicular to each other.
[0013] The aluminum plate 10 is made of aluminum and is formed into a rectangular plate shape (see FIG. 2). The aluminum plate 10 has a first bonding surface 11. The first bonding surface 11 is formed into a planar shape and is perpendicular to the facing direction Z. In other words, the first bonding surface 11 is parallel to the short side direction X and the long side direction Y. The first bonding surface 11 faces the copper plate 20 in the facing direction Z, and is a portion that is liquid-phase bonded to a second bonding surface 21 of the copper plate 20, which will be described later. In this example, the first bonding surface 11 is provided within a predetermined range on one side of the aluminum plate 10 in the long side direction Y.
[0014] The copper plate 20 is a metal member different from the aluminum plate 10, and is made of copper. The copper plate 20 is formed into a rectangular plate shape (see FIG. 2), and in this example, is formed into the same shape as the aluminum plate 10, but is not limited to this. The copper plate 20 has a second bonding surface 21. The second bonding surface 21 faces the aluminum plate 10 in the facing direction Z, and is a portion that is liquid-phase bonded to the first bonding surface 11 of the aluminum plate 10. In this example, the second bonding surface 21 is provided within a predetermined range on one side of the copper plate 20 in the long side direction Y. The second bonding surface 21 has a recessed portion 21a and a bonding main surface 21b.
[0015] The recessed portion 21a is a portion recessed on the opposite side to the aluminum plate 10 along the facing direction Z, and one recessed portion is provided. The recessed portion 21a is formed, for example, by press processing using a mold, and in this example, as shown in FIG. 2, is formed in a curved surface shape (for example, a spherical shape). The recessed portion 21a has a certain depth along the facing direction Z. That is, as shown in FIG. 1, the distance H1 between the recessed portion 21a and the first bonding surface 11 in the facing direction Z is longer than the distance H2 between the bonding main surface 21b and the first bonding surface 11. The recessed portion 21a includes a space portion having this certain depth, and the intermetallic compound C generated by liquid phase bonding is stored in a solidified state in the space portion. The recessed portion 21a faces the first bonding surface 11 of the aluminum plate 10, and is liquid phase bonded to the first bonding surface 11 in a state in which the intermetallic compound C is stored. Incidentally, the intermetallic compound C is a compound made of a relatively hard and brittle material.
[0016] The bonding principal surface 21b is a portion surrounding the periphery of the recessed portion 21a. In other words, the bonding principal surface 21b is a portion extending from the edge of the recessed portion 21a to the outside of the recessed portion 21a along the short side direction X and the long side direction Y. In other words, when a virtual plane perpendicular to the facing direction Z is taken as a virtual plane, the bonding principal surface 21b extends from the edge of the recessed portion 21a to the outside of the recessed portion 21a along the virtual plane. The bonding principal surface 21b faces the first bonding surface 11 of the aluminum plate 10 and is liquid-phase bonded to the first bonding surface 11.
[0017] The bonding principal surface 21b has a tapered portion 21c. The tapered portion 21c is inclined from the outside toward the recessed portion 21a with respect to the short side direction X and the long side direction Y. That is, the tapered portion 21c is inclined downward from the outside toward the recessed portion 21a with respect to the imaginary plane. In other words, the distance between the tapered portion 21c and the imaginary plane gradually increases from the outside toward the recessed portion 21a. The tapered portion 21c is formed, for example, from the end of the second bonding surface 21 in the short side direction X to the edge of the recessed portion 21a when viewed from the long side direction Y.
[0018] The liquid phase bonding portion 30 is a portion where the first bonding surface 11 and the second bonding surface 21 are liquid-phase bonded. That is, the liquid phase bonding portion 30 is a portion between the first bonding surface 11 and the second bonding surface 21. In other words, the liquid phase bonding portion 30 is a portion between the bonding main surface 21b and the first bonding surface 11, and a portion between the inner surface of the recessed portion 21a and the first bonding surface 11. The liquid phase bonding portion 30 is configured to include an intermetallic compound C generated by liquid phase bonding. The liquid phase bonding portion 30 is formed so that the thickness of the exposed end surface 31 of the intermetallic compound C exposed to the outside in the facing direction Z is relatively thin. The liquid phase bonding portion 30 is formed so that the thickness of the exposed end surface 31 is, for example, 3 μm or less, and preferably, the thickness of the exposed end surface 31 is 1 μm or less.
[0019] Next, a joining method for joining an aluminum plate 10 and a copper plate 20 by a resistance welding machine 100 will be described. The welding machine 100 includes a positive electrode 101, a negative electrode 102, and a power source 104 that is connected to the positive electrode 101 and the negative electrode 102 via an electric wire 103 and supplies power. As shown in Fig. 6, the joining method includes a condition setting step (step S1) and a joining step (step S2).
[0020] In the condition setting step (step S1), processing conditions such as the power supplied from the power source 104 and the time for which the power is supplied are set in the welding machine 100. After the condition setting step (step S1), the process proceeds to a joining step (step S2).
[0021] In the joining process (step S2), a voltage is applied to the aluminum plate 10 and the copper plate 20 while the first joining surface 11 of the aluminum plate 10 and the second joining surface 21 of the copper plate 20 are pressed against each other to perform liquid phase joining. For example, in the joining process, the aluminum plate 10 and the copper plate 20 are set between the positive electrode 101 and the negative electrode 102 of the welding machine 100 with the first joining surface 11 of the aluminum plate 10 and the second joining surface 21 of the copper plate 20 facing each other along the facing direction Z (see FIG. 4). In the joining process, a voltage is applied from the positive electrode 101 while a pressing force F (see FIG. 3) is applied by the welding machine 100 along the facing direction Z. As a result, in the joining process, parts of the first joining surface 11 and the second joining surface 21 are melted by heat generated by resistance to perform liquid phase joining. At this time, an intermetallic compound C is generated in the joining process. 5, in the joining process, the generated intermetallic compound C is poured from the outside along the tapered portion 21c of the joining main surface 21b toward the recessed portion 21a and stored in the recessed portion 21a. In the joining process, the application of the voltage from the positive electrode 101 is stopped to solidify the intermetallic compound C stored in the recessed portion 21a and to join the first joining surface 11 and the second joining surface 21 to form the joined structure 1.
[0022] As described above, the joint structure 1 according to the embodiment includes the aluminum plate 10, the copper plate 20, and the liquid phase bonding portion 30. The aluminum plate 10 has the first bonding surface 11. The copper plate 20 is a metal member different from the aluminum plate 10 and has the second bonding surface 21. The liquid phase bonding portion 30 is a portion where the first bonding surface 11 and the second bonding surface 21, which face each other along the facing direction Z, are liquid phase bonded. The second bonding surface 21 of the copper plate 20 has a recessed portion 21a and a bonding main surface 21b. The recessed portion 21a is a portion formed by recessing along the facing direction Z. The bonding main surface 21b is a portion that extends along the short side direction X and the long side direction Y and surrounds the periphery of the recessed portion 21a. In the opposing direction Z, the distance H1 between the recess 21a and the other of the first bonding surface 11 and the second bonding surface 21 is longer than the distance H2 between the bonding main surface 21b and the other, and the intermetallic compound C generated by liquid phase bonding is stored in the recess 21a.
[0023] With this configuration, the joint structure 1 can store the intermetallic compound C in the recessed portion 21a, thereby making the thickness of the intermetallic compound C present between the main joint surface 21b of the copper plate 20 and the first joint surface 11 of the aluminum plate 10 relatively thin. At this time, the recessed portion 21a of the joint structure 1 is not exposed to the outside because it is surrounded by the main joint surface 21b. As a result, the joint structure 1 can reduce the area of the exposed end surface 31 of the intermetallic compound C exposed to the outside from between the main joint surface 21b of the copper plate 20 and the first joint surface 11 of the aluminum plate 10. Therefore, the joint structure 1 can reduce the intermetallic compound C, which is a hard and brittle material, and can suppress a decrease in the joint strength at the exposed end surface 31 of the intermetallic compound C, and as a result, can properly join dissimilar metals.
[0024] In the above-mentioned joint structure 1, the joint main surface 21b has a tapered portion 21c that is inclined from the outside toward the recessed portion 21a with respect to the short side direction X and the long side direction Y. With this configuration, the joint structure 1 can promote the flow of the intermetallic compound C from the outside toward the recessed portion 21a by the tapered portion 21c, so that the area of the exposed end surface 31 of the intermetallic compound C exposed to the outside can be reduced.
[0025] The bonding method according to the embodiment includes a bonding step of applying a voltage to the aluminum plate 10 and the copper plate 20 to perform liquid phase bonding while pressing the first bonding surface 11 of the aluminum plate 10 against the second bonding surface 21 of the copper plate 20. This makes it possible to form a bonded structure 1 in which the area of the exposed end surface 31 of the intermetallic compound C exposed to the outside is reduced, thereby making it possible to properly bond dissimilar metals.
[0026] [Modifications] Next, a modified example of the embodiment will be described. In the modified example, the same components as those in the embodiment will be denoted by the same reference numerals, and detailed description thereof will be omitted. The joint structure 1A according to the modified example of the embodiment differs from the joint structure 1 according to the embodiment in that a plurality of recesses 21d are provided.
[0027] 7 and 8, the joint structure 1A includes an aluminum plate 10, a copper plate 20A, and a liquid phase joint 30. The copper plate 20A has a second joint surface 21A. The second joint surface 21A has a plurality of recesses 21d and a main joint surface 21e.
[0028] The recesses 21d are formed, for example, by press processing using a mold. In this example, as shown in Figs. 7 and 8, a knurling process is performed to form a plurality of fine recesses. That is, the recesses 21d are formed with a plurality of fine recesses along the short side direction X and the long side direction Y. The recesses 21d have a certain depth along the facing direction Z. That is, as shown in Fig. 7, the distance H3 between the recesses 21d and the first bonding surface 11 in the facing direction Z is longer than the distance H4 between the bonding main surface 21e and the first bonding surface 11. The recesses 21d include a space having a certain depth, and the intermetallic compound C generated by liquid phase bonding is stored in the space in a solidified state. The recesses 21d face the first bonding surface 11 of the aluminum plate 10, and are liquid phase bonded to the first bonding surface 11 in a state in which the intermetallic compound C is stored.
[0029] The bonding principal surface 21e is a region surrounding the periphery of the plurality of recesses 21d. In other words, when the region in which the plurality of recesses 21d are formed is defined as a recess region T, the bonding principal surface 21e is a region surrounding the periphery of this recess region T. The bonding principal surface 21e faces the first bonding surface 11 of the aluminum plate 10, and is liquid-phase bonded to the first bonding surface 11.
[0030] The bonding principal surface 21e has a tapered portion 21f. The tapered portion 21f is inclined from the outside toward the multiple recessed portions 21d with respect to the short side direction X and the long side direction Y. That is, the tapered portion 21f is inclined downward from the outside toward the recessed portion 21a with respect to the imaginary plane. In other words, the distance between the tapered portion 21f and the imaginary plane gradually increases from the outside toward the multiple recessed portions 21d. The tapered portion 21f is formed, for example, from the end of the second bonding surface 21A in the short side direction X to the edge of the multiple recessed portions 21d when viewed from the long side direction Y.
[0031] In the copper plate 20A having the plurality of recesses 21d formed therein, a voltage is applied to the aluminum plate 10 and the copper plate 20A in a state where the first joint surface 11 of the aluminum plate 10 and the second joint surface 21A of the copper plate 20A are pressed against each other to perform liquid phase bonding. For example, in the bonding process, the aluminum plate 10 and the copper plate 20A are set between the positive electrode 101 and the negative electrode 102 of the welding machine 100 in a state where the first joint surface 11 and the second joint surface 21A face each other along the facing direction Z (see FIG. 9). Then, in the bonding process, a voltage is applied from the positive electrode 101 in a state where the welding machine 100 applies a pressing force F (see FIG. 3) along the facing direction Z. As a result, in the bonding process, a part of the first joint surface 11 and the second joint surface 21A melts due to heat generated by resistance to perform liquid phase bonding. At this time, an intermetallic compound C is generated between the first joint surface 11A and the second joint surface 21 in the bonding process. 10, in the joining process, the intermetallic compound C is poured from the outside along the tapered portion 21f of the joining main surface 21e toward the multiple recesses 21d, and the intermetallic compound C is stored in the multiple recesses 21d. In the joining process, when the application of the voltage from the positive electrode 101 is stopped, the intermetallic compound C stored in the multiple recesses 21d is solidified and the first joining surface 11 and the second joining surface 21A are joined to form the joined structure 1A.
[0032] As described above, the joint structure 1A according to the modified embodiment can relatively reduce the thickness of the intermetallic compound C between the main joint surface 21e of the copper plate 20A and the first joint surface 11 of the aluminum plate 10 by storing the intermetallic compound C in the multiple recesses 21d. At this time, the multiple recesses 21d of the joint structure 1A are not exposed to the outside because they are surrounded by the main joint surface 21e. As a result, the joint structure 1A can reduce the area of the exposed end surface 31 of the intermetallic compound C exposed to the outside from between the main joint surface 21e of the copper plate 20A and the first joint surface 11 of the aluminum plate 10. Therefore, the joint structure 1A can reduce the intermetallic compound C, which is a hard and brittle material, and can suppress the reduction in the joint strength at the exposed end surface 31 of the intermetallic compound C, and as a result, can properly join dissimilar metals.
[0033] In the above description, an example has been described in which the joining main surface 21b has the tapered portion 21c that is inclined from the outside toward the recessed portion 21a with respect to the short side direction X and the long side direction Y. However, this is not limited to this, and the joining main surface 21b may not have the tapered portion 21c.
[0034] Although an example has been described in which the bonding main surface 21e has the tapered portion 21f that is inclined from the outside toward the multiple recessed portions 21d with respect to the short side direction X and the long side direction Y, the bonding main surface 21e is not limited to this, and may not have the tapered portion 21f.
[0035] Although the first metal member is described as being made of aluminum as an example material, the present invention is not limited to this, and may be made of any other metal as long as it is different from the second metal member.
[0036] Although the second metal member is described as being made of copper as an example material, the present invention is not limited to this, and may be made of any other metal as long as it is different from the first metal member.
[0037] Although an example has been described in which the recessed portion 21a and the bonding main surface 21b are provided on the second bonding surface 21, the present invention is not limited to this example and the recessed portion 21a and the bonding main surface 21b may be provided on the first bonding surface 11. In addition, the recessed portion 21a and the bonding main surface 21b are not limited to the example in which they are provided on either the first bonding surface 11 or the second bonding surface 21, and may be provided on both the first bonding surface 11 and the second bonding surface 21.
[0038] Although an example has been described in which the tapered portion 21c is formed from the end of the second bonding surface 21 in the short side direction X to the edge of the recessed portion 21a when viewed from the long side direction, the present invention is not limited to this. For example, the tapered portion 21c may be formed from the end of the second bonding surface 21 in the short side direction X closer to the recessed portion 21a (for example, an intermediate position between the end of the second bonding surface 21 and the edge of the recessed portion 21a) to the edge of the recessed portion 21a when viewed from the long side direction Y.
[0039] Although an example has been described in which the tapered portion 21f is formed from the end of the second bonding surface 21A in the short side direction X to the edges of the multiple recesses 21d when viewed from the long side direction, the present invention is not limited to this. For example, the tapered portion 21f may be formed from the end of the second bonding surface 21A in the short side direction X closer to the multiple recesses 21d (for example, an intermediate position between the end of the second bonding surface 21A and the edges of the multiple recesses 21d) to the edges of the multiple recesses 21d when viewed from the long side direction Y.
[0040] Although the example in which the plurality of recessed portions 21d are knurled to form a plurality of fine recesses has been described, the present invention is not limited to this, and may be formed, for example, of a plurality of dots (point-like recesses). [Explanation of symbols]
[0041] 1, 1A bonded structure 10 Aluminum plate (first metal member) 11 First joint surface 20, 20A Copper plate (second metal member) 21, 21A 2nd joint surface 21a, 21d recess 21b, 21e Main surface of joint 21c, 21f tapered section 30 Liquid phase junction H1~H4 interval X Short side direction (cross direction) Y Long side direction (cross direction) Z Opposite Direction
Claims
1. a first metal member having a first bonding surface; a second metal member which is a metal member different from the first metal member and has a second bonding surface; a liquid phase bonding portion formed by liquid phase bonding the first bonding surface and the second bonding surface opposed to each other along an opposing direction, At least one of the first bonding surface and the second bonding surface has a recessed portion formed by being recessed along the opposing direction, and a bonding main surface extending along a cross direction intersecting the opposing direction and surrounding a periphery of the recessed portion, a distance between the recess and the other of the first bonding surface and the second bonding surface in the opposing direction is longer than a distance between the main bonding surface and the other of the first bonding surface and the second bonding surface, and an intermetallic compound generated by the liquid phase bonding is stored in the recess; The joining main surface has a tapered portion that is inclined from an outer side toward the recessed portion with respect to the intersecting direction, A joint structure, characterized in that the tapered portion is formed from an end portion of the joint main surface in a short side direction along the intersecting direction to an edge of the recessed portion.
2. a bonding process in which a voltage is applied to the first metal member and the second metal member to perform liquid phase bonding while a first bonding surface of a first metal member and a second bonding surface of a second metal member which is a metal member different from the first metal member are pressed against each other, At least one of the first bonding surface and the second bonding surface has a plurality of recessed portions formed by recessing along the opposing direction, and a bonding main surface extending along a cross direction intersecting the opposing direction and surrounding the periphery of the recessed portions, In the opposing direction, a distance between the recess and the other of the first bonding surface and the second bonding surface is longer than a distance between the main bonding surface and the other of the first bonding surface and the second bonding surface, and the recess stores an intermetallic compound generated by the liquid phase bonding, The joining main surface has a tapered portion that is inclined from an outer side toward the recessed portion with respect to the intersecting direction, The joining method, characterized in that the tapered portion is formed from an end portion of the joining main surface in a short side direction along the intersecting direction to an edge of the recessed portion.
Citation Information
Patent Citations
Spot welding method of dissimilar plates
JP2009226446A
Dissimilar material joining body and dissimilar material joining method
JP2018043279A
Weld joined body
JP2019126824A
Intruding feature in aluminum alloy workpiece to improve al-steel spot welding