Separator for non-aqueous secondary battery and non-aqueous secondary battery
The separator for non-aqueous secondary batteries, featuring a phenyl group-containing acrylic resin and butadiene-acrylonitrile resin, addresses the challenge of electrode adhesion in wet heat press processes, enhancing manufacturing efficiency and battery performance.
Patent Information
- Application Number
- JP2023028672
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-02-27
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2043-02-27
AI Technical Summary
Existing separators for non-aqueous secondary batteries face challenges in achieving strong adhesion to electrodes during manufacturing, particularly in wet heat press processes at low temperatures and pressures, which are necessary for larger battery designs.
A separator for non-aqueous secondary batteries comprising a porous layer with inorganic particles and a binder resin, incorporating a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin, with specific molar ratios of monomer units, to enhance adhesion through a well-mixed adhesive layer.
The separator achieves excellent adhesion to electrodes at low temperatures and pressures, facilitating efficient battery production and improving safety and energy density.
Smart Images

Figure 0007557563000005 
Figure 0007557563000006 
Figure 0007557563000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a separator for a nonaqueous secondary battery and a nonaqueous secondary battery. [Background technology]
[0002] Patent Document 1 discloses an adhesive for bonding components that constitute a lithium ion secondary battery together, the adhesive containing a particulate polymer having a core-shell structure.
[0003] Patent Documents 2 and 3 disclose a separator for a non-aqueous secondary battery, which includes an adhesive layer provided on one or both sides of a laminate of a porous substrate and a porous layer, the adhesive layer being formed by adhering adhesive resin particles to the laminate. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2015 / 005145 [Patent Document 2] International Publication No. 2019 / 130994 [Patent Document 3] International Publication No. 2020 / 246497 Summary of the Invention [Problem to be solved by the invention]
[0005] In order to prevent short circuits in the battery, the separator is required to have adhesive properties to the electrodes. In order to bond the separator to the electrodes more strongly, a separator impregnated with an electrolyte is placed on the electrodes and heat-pressed (this is called "wet heat pressing") during battery production. As batteries become larger, the heat pressing equipment used for wet heat pressing becomes larger and more complex. Therefore, there is a need for the development of a separator that has excellent adhesion to electrodes even when wet heat pressed at relatively low temperatures and pressures.
[0006] It is against the above background that the present disclosure has been made. An object of the present disclosure is to provide a separator for a nonaqueous secondary battery that has excellent adhesion to electrodes when subjected to a low-temperature, low-pressure wet heat press. [Means for solving the problem]
[0007] Specific means for solving the above problems include the following aspects. <1> a porous layer containing inorganic particles and a binder resin; An adhesive layer containing a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin, in which the amount of butadiene units in the total amount of acrylic units, styrene units, butadiene units, and acrylonitrile units contained in both resins is 3 mol % to 50 mol %; A separator for a non-aqueous secondary battery comprising: <2> Further comprising a porous substrate, The porous layer is provided on one or both sides of the porous substrate, The adhesive layer is provided on one or both sides of a laminate of the porous substrate and the porous layer. <1> The non-aqueous secondary battery separator according to claim 1 . <3> The adhesive layer contains resin particles, The resin particles contain at least one of a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin. <1> or <2> The non-aqueous secondary battery separator according to claim 1 . <4> The average primary particle size of all the resin particles contained in the adhesive layer is 0.1 μm to 1.0 μm. <3> The non-aqueous secondary battery separator according to claim 1 . <5> The mass ratio of the phenyl group-containing acrylic resin to the butadiene-acrylonitrile resin contained in the adhesive layer is 60:40 to 95:5. <1> ~ <4> 10. The separator for a non-aqueous secondary battery according to claim 9, <6> The phenyl group-containing acrylic resin has a styrene unit and an acrylic unit, the molar ratio of the styrene-based unit to the acrylic unit is 30:70 to 50:50; <1> ~ <5> 10. The separator for a non-aqueous secondary battery according to claim 9, <7> The glass transition temperature of the entire resin contained in the adhesive layer is 58°C to 100°C. <1> ~ <6> 10. The separator for a non-aqueous secondary battery according to claim 9, <8> The adhesive layer has a basis weight of 0.05 g / m per one side of the nonaqueous secondary battery separator. 2 ~1.0g / m 2 That is, <1> ~ <7> 10. The separator for a non-aqueous secondary battery according to claim 9, <9> The average primary particle size of all the inorganic particles contained in the porous layer is 0.01 μm to 1.0 μm. <1> ~ <8> 10. The separator for a non-aqueous secondary battery according to claim 9, <10> The binder resin includes at least one selected from the group consisting of polyamide-based resins, acrylic-based resins, fluorine-based resins, and styrene-butadiene-based resins. <1> ~ <9> 10. The separator for a non-aqueous secondary battery according to claim 9, <11> A positive electrode, a negative electrode, and a conductive material disposed between the positive electrode and the negative electrode. <1> ~ <10> and a non-aqueous secondary battery separator according to any one of the above items, Electromotive force is obtained by doping and dedoping lithium ions. Non-aqueous secondary battery. Effect of the Invention
[0008] According to the present disclosure, there is provided a non-aqueous secondary battery separator that exhibits excellent adhesion to electrodes by low-temperature, low-pressure wet heat pressing. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a schematic cross-sectional view of an example of a separator according to the present disclosure. [Diagram 2] FIG. 2 is a schematic cross-sectional view of an example of a separator according to the present disclosure. [Diagram 3] FIG. 2 is a schematic cross-sectional view of an example of a separator according to the present disclosure. [Figure 4] FIG. 2 is a schematic cross-sectional view of an example of a separator according to the present disclosure. [Diagram 5] FIG. 2 is a schematic cross-sectional view of an example of a separator according to the present disclosure. [Figure 6] FIG. 2 is a schematic cross-sectional view of an example of a separator according to the present disclosure. [Figure 7] FIG. 2 is a schematic cross-sectional view of an example of a separator according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, embodiments of the present disclosure will be described. These descriptions and examples are merely illustrative of the embodiments, and are not intended to limit the scope of the embodiments.
[0011] In the present disclosure, a numerical range indicated using "~" indicates a range that includes the numerical values before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples.
[0012] In the present disclosure, the term "step" includes not only an independent step, but also a step that cannot be clearly distinguished from other steps as long as the purpose of the step is achieved.
[0013] In the present disclosure, when referring to the amount of each component in a composition, in cases where multiple substances corresponding to each component are present in the composition, unless otherwise specified, it means the total amount of those multiple substances present in the composition. In the present disclosure, the particles corresponding to each component may include multiple types. When multiple types of particles corresponding to each component are present in the composition, the particle size of each component means the value for a mixture of the multiple types of particles present in the composition, unless otherwise specified.
[0014] In the present disclosure, MD (Machine Direction) means the longitudinal direction of a separator produced in a long shape, and TD (Transverse Direction) means the direction perpendicular to MD in the plane direction of the separator. In the present disclosure, TD is also referred to as "width direction."
[0015] In the present disclosure, when the stacking relationship of each layer constituting a separator is expressed as "upper" and "lower", the layer closer to the porous substrate is referred to as "lower" and the layer farther from the porous substrate is referred to as "upper".
[0016] In the present disclosure, the volume of the porous layer excluding the pores is referred to as the "solids volume."
[0017] In the present disclosure, performing a heat press treatment after impregnating a separator with an electrolyte is referred to as "wet heat press", and performing a heat press treatment without impregnating a separator with an electrolyte is referred to as "dry heat press".
[0018] In the present disclosure, the term "(meth)acrylic" means either "acrylic" or "methacrylic".
[0019] In the present disclosure, the term "monomer unit" of a polymer or resin means a structural unit of a polymer or resin, which is formed by polymerization of a monomer. In the present disclosure, a constituent unit formed by polymerization of an acrylic monomer is referred to as an "acrylic unit", a constituent unit formed by polymerization of a styrene monomer is referred to as a "styrene unit", a constituent unit formed by polymerization of butadiene is referred to as a "butadiene unit", and a constituent unit formed by polymerization of acrylonitrile is referred to as an "acrylonitrile unit".
[0020] <Separator for non-aqueous secondary batteries> The nonaqueous secondary battery separator of the present disclosure (also simply referred to as "separator" in the present disclosure) comprises a porous layer containing inorganic particles and a binder resin, and an adhesive layer containing a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin, in which the amount of butadiene units in the total amount of acrylic units, styrene units, butadiene units, and acrylonitrile units contained in both resins is 3 mol % to 50 mol %.
[0021] The phenyl group-containing acrylic resin and the butadiene-acrylonitrile resin may be contained in the adhesive layer as two types of resins as separate molecules, or may be contained in the adhesive layer in a linked state.
[0022] The separator of the present disclosure contains a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin, and has an adhesive layer in which the amount of butadiene units in the total amount of acrylic units, styrene units, butadiene units, and acrylonitrile units contained in these two resins is 3 mol % to 50 mol %, thereby providing excellent adhesion to electrodes by low-temperature, low-pressure wet heat pressing.The mechanism is presumed to be as follows.
[0023] The phenyl group-containing acrylic resin is a resin that easily adheres to electrodes by applying heat. On the other hand, the butadiene-acrylonitrile resin is a resin that has excellent affinity with the electrolyte. It is presumed that the amount of butadiene units in the total amount of acrylic units, styrene units, butadiene units, and acrylonitrile units contained in both resins is 3 mol% to 50 mol%, so that the two resins can be mixed together without being separated. It is presumed that the adhesive layer adheres well to the electrodes even in a low-temperature, low-pressure wet heat press when both resins are mixed together and contained in the adhesive layer.
[0024] If the amount of butadiene units in the total amount of acrylic units, styrene units, butadiene units and acrylonitrile units contained in the phenyl group-containing acrylic resin and the butadiene-acrylonitrile resin is less than 3 mol%, the adhesive layer has low affinity for the electrolyte. From the viewpoint of sufficiently impregnating the adhesive layer with the electrolyte, the amount of butadiene units is 3 mol% or more, preferably 3.2 mol% or more, and more preferably 3.5 mol% or more. If the amount of butadiene units in the total amount of acrylic units, styrene units, butadiene units, and acrylonitrile units contained in the phenyl group-containing acrylic resin and the butadiene-acrylonitrile resin exceeds 50 mol%, the phenyl group-containing acrylic resin and the butadiene-acrylonitrile resin are difficult to mix together. From the viewpoint of mixing the two resins well, the amount of butadiene units is 50 mol% or less, preferably 40 mol% or less, and more preferably 30 mol% or less.
[0025] The types and molar ratios of monomer units contained in the phenyl group-containing acrylic resin and the butadiene-acrylonitrile resin are identified by nuclear magnetic resonance (NMR). Specifically, the following measurements are performed.
[0026] The adhesive layer peeled off from the separator or the resin material used to form the adhesive layer is used as a sample. If the resin material used to form the adhesive layer is a resin particle dispersion, the resin particle dispersion is air-dried to use as a sample. After the sample was swollen with deuterated chloroform, it was measured at room temperature at 600 MHz using an NMR device (JNM-ECA600 manufactured by JEOL) and a semi-solid probe (FGMAS probe manufactured by JEOL). 1 H-NMR spectrum (MAS rotation speed 6 kHz, observation width 15 ppm, number of points 32 k, pulse repetition waiting time 4 seconds) was measured at 150 MHz. 13 Measure the C-NMR spectrum. 13 C-NMR spectra are accumulated approximately 33,000 times in quantitative mode (inverse gated decoupling method, MAS rotation speed 6 kHz, observation width 250 ppm, number of points 32 k, pulse repetition waiting time 12 seconds).
[0027] In the above measurement, it does not matter whether the acrylic unit, styrene unit, butadiene unit, and acrylonitrile unit are contained in a phenyl group-containing acrylic resin or a butadiene-acrylonitrile resin. For example, when a butadiene-acrylonitrile resin has a styrene unit, the styrene unit is also quantified. In the above measurement, acrylonitrile units are not included in acrylic units, i.e., acrylonitrile units are not quantified as acrylic units in duplicate. In the above measurement, it is possible that the styrene-based unit is not detected. For example, when the phenyl group-containing acrylic resin is a resin having a phenyl (meth)acrylate unit and not having a styrene-based unit, and the butadiene-acrylonitrile resin is a resin having not a styrene-based unit, the styrene-based unit is not detected.
[0028] The separator of the present disclosure may be in a form including only a porous layer and an adhesive layer, or may further include a porous substrate. From the viewpoint of increasing the mechanical strength of the separator and imparting a shutdown function to the separator, the separator of the present disclosure preferably includes a porous substrate. The porous substrate is a sheet that does not contain inorganic particles, and is distinguished from the porous layer in that it does not contain inorganic particles.
[0029] When the separator of the present disclosure includes a porous substrate, the separator includes a porous layer on one or both sides of the porous substrate, and an adhesive layer on one or both sides of a laminate of the porous substrate and the porous layer.
[0030] In the separator of the present disclosure, the adhesive layer is preferably an adhesive layer containing resin particles from the viewpoint of ion permeability. The resin particles may be attached to the porous layer or the porous substrate due to the adhesiveness of the resin particles, or may be included in the adhesive layer together with a binder resin. That is, the adhesive layer may be an adhesive layer in which the resin particles are attached to the porous layer or the porous substrate, or an adhesive layer containing the resin particles and the binder resin.
[0031] When the adhesive layer contains resin particles, the resin particles preferably contain at least one of a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin. That is, the resin particles may be any of phenyl group-containing acrylic resin particles, butadiene-acrylonitrile resin particles, resin particles containing a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin, and a combination of two or three of these resin particles.
[0032] The layer structure of the separator of the present disclosure will be described with reference to the drawings.
[0033] 1 to 7 are schematic cross-sectional views of embodiments of the separator of the present disclosure. Fig. 1 to Fig. 7 are schematic cross-sectional views mainly for explaining the stacking order of layers, and the structure of each layer is omitted or simplified. In Fig. 1 to Fig. 7, layers having similar functions are described with the same reference numerals.
[0034] The separator 101 shown in FIG. 1 is a separator in which an adhesive layer 50 is disposed on one surface of a porous layer 30 .
[0035] 2 is a separator in which adhesive layers 50 are disposed on both sides of a porous layer 30. One adhesive layer 50 and the other adhesive layer 50 may be the same or different in components and / or composition.
[0036] 3 is a separator in which a porous layer 30 is disposed on one side of a porous substrate 20, and an adhesive layer 50 is disposed on one side of a laminate 40 of the porous substrate 20 and one porous layer 30. In the separator 103, the adhesive layer 50 is disposed on the surface of the porous layer 30.
[0037] 4 is a separator in which a porous layer 30 is disposed on one side of a porous substrate 20, and an adhesive layer 50 is disposed on one side of a laminate 40 of the porous substrate 20 and one porous layer 30. In the separator 104, the adhesive layer 50 is disposed on the surface of the porous substrate 20.
[0038] 5 is a separator in which a porous layer 30 is disposed on one side of a porous substrate 20, and adhesive layers 50 are disposed on both sides of a laminate 40 of the porous substrate 20 and one porous layer 30. One adhesive layer 50 and the other adhesive layer 50 may be the same or different in terms of components and / or composition.
[0039] 6 is a separator in which porous layers 30 are disposed on both sides of a porous substrate 20, and an adhesive layer 50 is disposed on one side of a laminate 40 of the porous substrate 20 and two porous layers 30. One porous layer 30 and the other porous layer 30 may be the same or different in components and / or composition.
[0040] The separator 107 shown in Fig. 7 is a separator in which a porous layer 30 is disposed on both sides of a porous substrate 20, and adhesive layers 50 are disposed on both sides of a laminate 40 of the porous substrate 20 and two porous layers 30. One porous layer 30 and the other porous layer 30 may be the same or different in terms of components and / or composition. One adhesive layer 50 and the other adhesive layer 50 may be the same or different in terms of components and / or composition.
[0041] From the viewpoint of bonding the separator to both opposing electrodes, it is preferable that both surfaces of the separator are adhesive layers 50. From this viewpoint, separator 102, separator 105, and separator 107 are preferable.
[0042] In the separators 103 to 107, the porous layer 30 is a layer disposed on the surface of the porous substrate 20. The porous layer 30 may be on only one surface of the porous substrate 20, or may be on both surfaces of the porous substrate 20. When the porous layer 30 is on both surfaces of the porous substrate 20, the heat resistance of the separator is more excellent, and the safety of the battery can be further improved. In addition, the separator is less likely to curl, and the handling during battery production is excellent. When the porous layer 30 is on only one surface of the porous substrate 20, the ion permeability of the separator is more excellent. In addition, the thickness of the entire separator can be reduced, and a battery with a higher energy density can be produced.
[0043] The adhesive layer 50 is a layer disposed on the surface of the porous substrate 20 or the porous layer 30, and exists as the outermost layer of the separator.
[0044] From the viewpoint of ion permeability, the adhesive layer 50 is preferably a layer containing resin particles 52. From the viewpoint of superior adhesion to the electrode, the adhesive layer 50 preferably has a structure in which a large number of resin particles 52 are arranged adjacent to each other on the surface of the porous substrate 20 or the porous layer 30, and from the viewpoint of increasing the energy density of the battery, the resin particles 52 preferably have a structure of one layer in the thickness direction. However, the structure of the adhesive layer 50 is not limited to the above structure, and the resin particles 52 may have a structure in which a large number of resin particles 52 are scattered on the surface of the porous substrate 20 or the porous layer 30, or may have a structure in which multiple layers of the resin particles 52 are overlapped in the thickness direction.
[0045] In a separator adhered to an electrode, the resin particles 52 contained in the adhesive layer 50 may melt in part or in whole when heat is applied to adhere the separator to the electrode, causing adjacent resin particles 52 to connect to each other, and some or all of the resin particles may not retain their particle shape.
[0046] The porous substrate, the porous layer, and the adhesive layer of the separator of the present disclosure will be described in detail below.
[0047] [Porous base material] In the present disclosure, the porous substrate means a substrate having pores or gaps therein. Examples of such substrates include microporous membranes; porous sheets such as nonwoven fabrics and paper made of fibrous materials; composite porous sheets obtained by laminating one or more other porous layers on these microporous membranes or porous sheets; and the like. In the present disclosure, a microporous membrane is preferred from the viewpoint of thinning and strength of the separator. The microporous membrane means a membrane having a large number of micropores therein, a structure in which the micropores are connected, and which allows gas or liquid to pass from one surface to the other surface.
[0048] The material of the porous substrate is preferably an electrically insulating material.
[0049] The porous substrate preferably contains a thermoplastic resin in order to provide the porous substrate with a shutdown function. The shutdown function refers to a function in which, when the battery temperature rises, the constituent material dissolves and blocks the pores of the porous substrate, thereby blocking the movement of ions and preventing thermal runaway of the battery. The thermoplastic resin is preferably a thermoplastic resin having a melting point of less than 200°C. Examples of the thermoplastic resin include polyesters such as polyethylene terephthalate; polyolefins such as polyethylene and polypropylene; and the like, and among these, polyolefins are preferred.
[0050] The porous substrate is preferably a microporous membrane containing polyolefin (referred to as a "polyolefin microporous membrane" in the present disclosure). Examples of the polyolefin microporous membrane include polyolefin microporous membranes used in conventional battery separators, and it is preferable to select one having sufficient mechanical properties and ion permeability from these.
[0051] From the viewpoint of exhibiting a shutdown function, the polyolefin microporous membrane is preferably a microporous membrane containing polyethylene, and the polyethylene content is preferably 95% by mass or more based on the total mass of the polyolefin microporous membrane.
[0052] The polyolefin microporous film is preferably a microporous film containing polypropylene, from the viewpoint of heat resistance such that the film does not easily break when exposed to high temperatures.
[0053] From the viewpoint of having a shutdown function and heat resistance that does not easily break when exposed to high temperatures, the polyolefin microporous film is preferably a polyolefin microporous film containing polyethylene and polypropylene. An example of a polyolefin microporous film containing polyethylene and polypropylene is a microporous film in which polyethylene and polypropylene are mixed in one layer. From the viewpoint of achieving both the shutdown function and heat resistance, the microporous film preferably contains 95% by mass or more of polyethylene and 5% by mass or less of polypropylene. Also, from the viewpoint of achieving both the shutdown function and heat resistance, a polyolefin microporous film having a laminated structure of two or more layers, at least one layer containing polyethylene and at least one layer containing polypropylene, is also preferred.
[0054] The polyolefin contained in the polyolefin microporous membrane is preferably a polyolefin having a weight average molecular weight (Mw) of 100,000 to 5,000,000. When the Mw of the polyolefin is 100,000 or more, the microporous membrane can be imparted with sufficient mechanical properties. On the other hand, when the Mw of the polyolefin is 5,000,000 or less, the microporous membrane has good shutdown properties and is easy to mold.
[0055] Examples of methods for producing a polyolefin microporous membrane include a method in which a molten polyolefin resin is extruded through a T-die to form a sheet, which is crystallized, stretched, and then heat-treated to form a microporous membrane; a method in which a molten polyolefin resin together with a plasticizer such as liquid paraffin is extruded through a T-die, cooled to form a sheet, stretched, the plasticizer is extracted, and then heat-treated to form a microporous membrane; and the like.
[0056] Examples of the porous sheet made of a fibrous material include porous sheets such as nonwoven fabrics and papers made of fibrous materials such as polyesters such as polyethylene terephthalate; polyolefins such as polyethylene and polypropylene; heat-resistant resins such as wholly aromatic polyamide, polyamideimide, polyimide, polyethersulfone, polysulfone, polyetherketone, and polyetherimide; and cellulose.
[0057] In the present disclosure, a heat-resistant resin refers to a resin having a melting point of 200° C. or higher, or a resin having no melting point and a decomposition temperature of 200° C. or higher. In other words, a heat-resistant resin in the present disclosure refers to a resin that does not melt or decompose in a temperature range below 200° C.
[0058] The composite porous sheet may be a sheet in which a functional layer is laminated on a porous sheet made of a microporous membrane or a fibrous material. Such a composite porous sheet is preferable from the viewpoint of enabling further addition of functions by the functional layer. For example, from the viewpoint of imparting heat resistance, the functional layer may be a porous layer made of a heat-resistant resin. The heat-resistant resin may be one or more heat-resistant resins selected from wholly aromatic polyamide, polyamideimide, polyimide, polyethersulfone, polysulfone, polyetherketone, and polyetherimide. Examples of the composite method include a method of coating a functional layer on a microporous membrane or a porous sheet, a method of bonding a microporous membrane or a porous sheet to a functional layer with an adhesive, and a method of thermocompression bonding a microporous membrane or a porous sheet to a functional layer.
[0059] The surface of the porous substrate may be subjected to various surface treatments in order to improve wettability with the coating liquid for forming the porous layer, as long as the properties of the porous substrate are not impaired. Examples of the surface treatments include corona treatment, plasma treatment, flame treatment, and ultraviolet irradiation treatment.
[0060] -Characteristics of porous substrate- From the viewpoint of increasing the energy density of the battery, the thickness of the porous substrate is preferably 15 μm or less, more preferably 12 μm or less, and even more preferably 10 μm or less, and from the viewpoint of the production yield of the separator and the production yield of the battery, the thickness is preferably 3 μm or more, more preferably 5 μm or more, and even more preferably 7 μm or more.
[0061] The thickness of the porous substrate is measured using a contact thickness meter at 20 points within a 10 cm square and the average is calculated.
[0062] From the viewpoint of suppressing short circuits in the battery, the air permeability of the porous substrate is preferably 30 sec / 100 mL or more, more preferably 50 sec / 100 mL or more, and even more preferably 70 sec / 100 mL or more. The air permeability of the porous substrate is preferably 200 sec / 100 mL or less, more preferably 180 sec / 100 mL or less, and even more preferably 160 sec / 100 mL or less, from the viewpoint of ion permeability and from the viewpoint of preventing the porous structure from being blocked at the boundary between the porous substrate and the porous layer or adhesive layer when exposed to high temperatures.
[0063] The air permeability (sec / 100 mL) of the porous substrate is measured using a digital Oken air permeability tester in accordance with JIS P8117:2009.
[0064] [Porous layer] The porous layer has a structure in which a large number of minute pores are connected inside, and is a layer through which gas or liquid can pass from one surface to the other.
[0065] When the separator of the present disclosure includes a porous substrate, the porous layer may be present on only one side of the porous substrate, or on both sides of the porous substrate. When the porous layer is present on both sides of the porous substrate, the separator is less likely to curl, and handling during battery production is excellent. When the porous layer is present on only one side of the porous substrate, the ion permeability of the separator is more excellent. In addition, the thickness of the entire separator can be reduced, and a battery with a higher energy density can be produced.
[0066] The porous layer included in the separator of the present disclosure contains at least inorganic particles and a binder resin.
[0067] -Inorganic particles- Examples of inorganic particles include metal hydroxide particles, metal oxide particles, metal sulfate particles, metal carbonate particles, metal nitride particles, and clay mineral particles.
[0068] Examples of metal hydroxides constituting the metal hydroxide particles include magnesium hydroxide, aluminum hydroxide, calcium hydroxide, chromium hydroxide, zirconium hydroxide, cerium hydroxide, nickel hydroxide, and boron hydroxide, with magnesium hydroxide being preferred. Examples of metal oxides constituting the metal oxide particles include silica, alumina, boehmite (alumina monohydrate), titania, zirconia, magnesium oxide, and barium oxide, with alumina being preferred. Examples of metal sulfates constituting the metal sulfate particles include barium sulfate and calcium sulfate, with barium sulfate being preferred. Examples of metal carbonates constituting the metal carbonate particles include calcium carbonate, magnesium carbonate, and barium carbonate. Examples of metal nitrides constituting the metal nitride particles include boron nitride and aluminum nitride. Examples of clay mineral particles include calcium silicate and talc.
[0069] The inorganic particles may be surface-modified with a silane coupling agent or the like.
[0070] The inorganic particles may be used alone or in combination of two or more kinds.
[0071] From the viewpoints of stability in the electrolyte and electrochemical stability, the inorganic particles are preferably at least one type selected from the group consisting of metal hydroxide particles, metal oxide particles, and metal sulfate particles.
[0072] The particle shape of the inorganic particles is not limited, and may be any of spherical, elliptical, plate-like, needle-like, and amorphous. From the viewpoint of suppressing short circuits in the battery, the inorganic particles contained in the porous layer are preferably plate-like particles or non-aggregated primary particles.
[0073] From the viewpoint of ion permeability of the porous layer, the average primary particle size of all the inorganic particles contained in the porous layer is preferably 0.01 μm or more, more preferably 0.02 μm or more, and even more preferably 0.03 μm or more. The average primary particle size of all the inorganic particles contained in the porous layer is preferably 1.0 μm or less, more preferably 0.9 μm or less, and even more preferably 0.8 μm or less, from the viewpoint of suppressing interlayer delamination between the porous layer and the porous substrate or adhesive layer and maintaining adhesion of the separator to the electrodes.
[0074] The average primary particle size of inorganic particles is determined by measuring the long diameter of 100 inorganic particles randomly selected in observation with a scanning electron microscope (SEM) and averaging the long diameters of the 100 particles. The sample used for SEM observation is inorganic particles that are materials forming the porous layer, or inorganic particles extracted from the porous layer. There is no limitation on the method for extracting inorganic particles from the porous layer. The method includes, for example, a method in which the porous layer peeled off from the separator is immersed in an organic solvent that dissolves the binder resin, and the inorganic particles are extracted by dissolving the binder resin with the organic solvent; a method in which the porous layer peeled off from the separator is heated to about 800°C to eliminate the binder resin and extract the inorganic particles; and the like.
[0075] From the viewpoint of achieving a good balance between the heat resistance and ion permeability of the porous layer, and the adhesion of the porous layer to the porous substrate, the content of the inorganic particles is preferably 60% by mass to 99% by mass, more preferably 65% by mass to 98% by mass, and even more preferably 68% by mass to 96% by mass, relative to the total mass of the porous layer.
[0076] When porous layers are present on both sides of a porous substrate, the type or amount of inorganic particles contained in one porous layer may be the same as or different from the type or amount of inorganic particles contained in the other porous layer.
[0077] -Organic particles- The porous layer may contain organic particles. Examples of the organic particles include particles made of crosslinked polymers such as crosslinked poly(meth)acrylic acid, crosslinked poly(meth)acrylic acid ester, crosslinked polysilicone, crosslinked polystyrene, crosslinked polydivinylbenzene, styrene-divinylbenzene copolymer crosslinked product, melamine resin, phenol resin, and benzoguanamine-formaldehyde condensate; particles made of heat-resistant polymers such as polysulfone, polyacrylonitrile, aramid, and polyacetal; and the like. The resin constituting the organic particles may be a mixture, modified product, derivative, copolymer (random copolymer, alternating copolymer, block copolymer, graft copolymer) or crosslinked product of the above-exemplified materials.
[0078] The organic particles may be used alone or in combination of two or more kinds.
[0079] -Binding resin- The binder resin contained in the porous layer has the function of binding the inorganic particles contained in the porous layer together, as well as the function of adhering the porous layer to the porous substrate, the function of adhering the porous layer to the electrode, and the function of improving the heat resistance of the porous layer.
[0080] When porous layers are present on both sides of a porous substrate, the type or amount of binder resin contained in one porous layer may be the same as or different from the type or amount of binder resin contained in the other porous layer.
[0081] Examples of binder resins include polyamide resins, acrylic resins, fluorine resins, styrene-butadiene resins, homopolymers or copolymers of vinyl nitrile compounds (acrylonitrile, methacrylonitrile, etc.), carboxymethyl cellulose, hydroxyalkyl cellulose, polyvinyl alcohol, polyvinyl butyral, polyvinylpyrrolidone, polyethers (polyethylene oxide, polypropylene oxide, etc.), polysulfones, polyketones, polyether ketones, polyether sulfones, and mixtures thereof.
[0082] As the binder resin, from the viewpoint of suppressing interlayer delamination between the porous layer and the adhesive layer, a resin having excellent affinity with the adhesive layer is preferable, and specifically, at least one resin selected from the group consisting of polyamide-based resins, acrylic-based resins, fluorine-based resins, and styrene-butadiene-based resins is preferable.
[0083] As the binder resin, from the viewpoint of the heat resistance of the porous layer, a polyamide resin is preferable. Examples of the polyamide resin include fully aromatic polyamide, polyamideimide, poly-N-vinylacetamide, polyacrylamide, copolymerized polyether polyamide, polyimide, and polyetherimide. These resins may be used alone or in combination of two or more.
[0084] Among polyamide resins, fully aromatic polyamides are preferred from the viewpoint of durability. Fully aromatic polyamides refer to polyamides whose main chains are composed only of benzene rings and amide bonds. However, a small amount of aliphatic monomers may be copolymerized in fully aromatic polyamides. Fully aromatic polyamides are also called aramids.
[0085] The wholly aromatic polyamide may be meta-type or para-type. Among the wholly aromatic polyamides, meta-type wholly aromatic polyamides (also called meta-type aramids) are preferred from the viewpoint of easy formation of a porous layer and excellent oxidation-reduction resistance in electrode reactions. Specifically, the wholly aromatic polyamide is preferably polymetaphenylene isophthalamide or polyparaphenylene terephthalamide, and more preferably polymetaphenylene isophthalamide.
[0086] When the porous layer contains a wholly aromatic polyamide, the content of the wholly aromatic polyamide is preferably 85% by mass to 100% by mass, more preferably 90% by mass to 100% by mass, and even more preferably 95% by mass to 99% by mass, based on the total amount of all resins contained in the porous layer.
[0087] Examples of the acrylic resin include homopolymers or copolymers of acrylic monomers, and copolymers of acrylic monomers and styrene monomers. These resins may be used alone or in combination of two or more.
[0088] Examples of the acrylic monomer of the acrylic resin include (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, isobornyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. As the acrylic monomer, (meth)acrylic acid alkyl ester is preferred. The alkyl group of the ester moiety of the (meth)acrylic acid alkyl ester is preferably an alkyl group having 1 to 10 carbon atoms, and more preferably an alkyl group having 1 to 8 carbon atoms. The acrylic monomer may be used alone or in combination of two or more kinds.
[0089] Examples of styrene monomers for acrylic resins include styrene, α-methylstyrene, alkyl-substituted styrenes such as 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, and 4-ethylstyrene, halogen-substituted styrenes such as 2-chlorostyrene, 3-chlorostyrene, and 4-chlorostyrene, and fluorine-substituted styrenes such as 4-fluorostyrene and 2,5-difluorostyrene. As styrene monomers, styrene and α-methylstyrene are preferred, and styrene is more preferred. The styrene monomers may be used alone or in combination of two or more.
[0090] Examples of fluorine-based resins include polyvinylidene fluoride-based resins. Examples of polyvinylidene fluoride-based resins include homopolymers of vinylidene fluoride (i.e., polyvinylidene fluoride); copolymers of vinylidene fluoride and halogen-containing monomers such as hexafluoropropylene, tetrafluoroethylene, trifluoroethylene, chlorotrifluoroethylene, vinyl fluoride, and trichloroethylene; copolymers of vinylidene fluoride and other monomers other than halogen-containing monomers; copolymers of vinylidene fluoride, halogen-containing monomers, and other monomers other than halogen-containing monomers; and mixtures thereof. These resins may be used alone or in combination of two or more.
[0091] Styrene-butadiene resins are copolymers of styrene monomers and butadiene. Examples of styrene monomers include styrene, α-methylstyrene; alkyl-substituted styrenes such as 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, and 4-ethylstyrene; halogen-substituted styrenes such as 2-chlorostyrene, 3-chlorostyrene, and 4-chlorostyrene; and fluorine-substituted styrenes such as 4-fluorostyrene and 2,5-difluorostyrene. Examples of styrene monomers include styrene and α-methylstyrene, and more preferably styrene. One type of styrene monomer may be used alone, or two or more types may be used in combination.
[0092] A small amount of an acrylic monomer may be copolymerized in the styrene-butadiene resin. The acrylic monomer is preferably a (meth)acrylic acid alkyl ester. The alkyl group at the ester moiety of the (meth)acrylic acid alkyl ester is preferably an alkyl group having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 8 carbon atoms. Specific examples of the acrylic monomer include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. The acrylic monomer may be used alone or in combination of two or more kinds.
[0093] From the viewpoint of achieving a good balance between the heat resistance and ion permeability of the porous layer, and the adhesion of the porous layer to the porous substrate, the content of the binder resin is preferably 1% by mass to 40% by mass, more preferably 2% by mass to 35% by mass, and even more preferably 4% by mass to 32% by mass, relative to the total mass of the porous layer.
[0094] -Other ingredients- The porous layer may contain additives such as a dispersant such as a surfactant, a wetting agent, an antifoaming agent, and a pH adjuster. The dispersant is added to the coating liquid for forming the porous layer for the purpose of improving dispersibility, coatability, or storage stability. The wetting agent, the antifoaming agent, and the pH adjuster are added to the coating liquid for forming the porous layer for the purpose of improving compatibility with the porous substrate, suppressing air entrapment in the coating liquid, or adjusting the pH, for example.
[0095] -Characteristics of the porous layer- From the viewpoint of heat resistance, the thickness of each porous layer is preferably 0.5 μm or more, more preferably 1.0 μm or more, and even more preferably 1.5 μm or more, and from the viewpoint of ion permeability and battery energy density, the thickness is preferably 5.0 μm or less, more preferably 4.0 μm or less, and even more preferably 3.5 μm or less.
[0096] When the porous layer is present on both sides of the porous substrate, the thickness of the porous layer, calculated as the total thickness of both sides, is preferably 1.0 μm or more, more preferably 2.0 μm or more, and even more preferably 2.5 μm or more, and is preferably 10.0 μm or less, more preferably 8.0 μm or less, and even more preferably 6.0 μm or less.
[0097] The thickness of the porous layer is the thickness of the flat membrane after removing the adhesive layer from the separator minus the thickness of the porous substrate. The thickness of the flat membrane after peeling the adhesive layer from the separator is measured at 20 points within a 10 cm square using a contact thickness meter and the average is calculated.
[0098] [Adhesive layer] The adhesive layer is a layer disposed on the surface of the porous layer or the porous substrate, and exists as the outermost layer of the separator. The adhesive layer has a large number of gaps or fine pores, and allows gas or liquid to pass from one surface to the other.
[0099] From the viewpoint of ion permeability, the adhesive layer is preferably an adhesive layer containing resin particles. The adhesive layer containing resin particles has excellent ion permeability due to the presence of gaps between the resin particles. The resin particles preferably maintain their shape in the electrolyte and are electrochemically stable.
[0100] The resin particles preferably contain at least one of a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin. That is, the resin particles may be any of phenyl group-containing acrylic resin particles, butadiene-acrylonitrile resin particles, resin particles containing a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin, and a combination of two or three of these resin particles.
[0101] When the adhesive layer contains resin particles, the adhesive layer may further contain a non-granular resin. The resin functions, for example, as a binder resin between the resin particles, or between the resin particles and the porous layer or the porous substrate. The resin is preferably at least one of a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin.
[0102] When the adhesive layer contains resin particles, the average primary particle size of all the resin particles contained in the adhesive layer is preferably 0.1 μm or more, more preferably 0.2 μm or more, and even more preferably 0.3 μm or more, from the viewpoint of ion permeability of the adhesive layer. The average primary particle size of all the resin particles contained in the adhesive layer is preferably 1.0 μm or less, more preferably 0.9 μm or less, and even more preferably 0.8 μm or less, from the viewpoint of preventing the resin particles from falling off.
[0103] The average primary particle size of resin particles is determined by measuring the long diameter of 100 randomly selected resin particles during observation with a scanning electron microscope (SEM) and averaging the long diameters of the 100 particles. The samples used for SEM observation are resin particles that are the material forming the adhesive layer, or resin particles removed from the adhesive layer.
[0104] The adhesive layer contains a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin. The phenyl group-containing acrylic resin and the butadiene-acrylonitrile resin contained in the adhesive layer may be two types of resins in the form of separate molecules, two types of resins in the form of molecules connected together, or a mixture thereof.
[0105] The phenyl group-containing acrylic resin and butadiene-acrylonitrile resin contained in the adhesive layer have a butadiene unit content of 3 mol% to 50 mol%, preferably 3.2 mol% to 40 mol%, and more preferably 3.5 mol% to 30 mol%, of the total amount of acrylic units, styrene units, butadiene units, and acrylonitrile units contained in both resins.
[0106] The mass ratio of the phenyl group-containing acrylic resin to the butadiene-acrylonitrile resin contained in the adhesive layer (phenyl group-containing acrylic resin:butadiene-acrylonitrile resin) is preferably 60:40 to 95:5, more preferably 55:45 to 92:8, and even more preferably 51:49 to 90:10, from the viewpoint of ease of bonding of the adhesive layer to the electrode by wet heat press.
[0107] -Phenyl group-containing acrylic resin- There is no limitation on the polymerization component that gives the phenyl group to the phenyl-group-containing acrylic resin, and examples of the polymerization component that gives the phenyl group include phenyl (meth)acrylate and styrene monomers.
[0108] The phenyl-containing acrylic resin preferably has a styrene-based unit from the viewpoint of facilitating adhesion of the resin to an electrode by wet heat pressing, i.e., the phenyl-containing acrylic resin preferably contains at least an acrylic monomer and a styrene-based monomer as polymerization components.
[0109] When the phenyl group-containing acrylic resin contains an acrylic monomer and a styrene monomer as polymerization components, it may be a random copolymer, an alternating copolymer, a block copolymer, or a graft copolymer of these two monomers. For example, the phenyl group-containing acrylic resin may be a block copolymer or a graft copolymer of an acrylic monomer and a styrene monomer, and the acrylic unit may be arranged in the core of the phenyl group-containing acrylic resin particle, and the styrene unit may be arranged in the shell.
[0110] The acrylic monomer is preferably at least one selected from the group consisting of (meth)acrylic acid, (meth)acrylic acid salts, and (meth)acrylic acid esters. The acrylic monomer may be used alone or in combination of two or more.
[0111] Examples of the (meth)acrylate salt include sodium (meth)acrylate, potassium (meth)acrylate, magnesium (meth)acrylate, and zinc (meth)acrylate. Examples of the (meth)acrylic acid ester include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, isobornyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-(diethylamino)ethyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, and phenyl (meth)acrylate.
[0112] The acrylic monomer is preferably a (meth)acrylic acid alkyl ester. The alkyl group at the ester moiety of the (meth)acrylic acid alkyl ester is preferably an alkyl group having 1 to 10 carbon atoms, and more preferably an alkyl group having 1 to 8 carbon atoms.
[0113] Specifically, the acrylic monomer is preferably methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, or 2-ethylhexyl (meth)acrylate. These acrylic monomers may be used alone or in combination of two or more.
[0114] Examples of styrene-based monomers include styrene, α-methylstyrene, alkyl-substituted styrenes such as 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, and 4-ethylstyrene, halogen-substituted styrenes such as 2-chlorostyrene, 3-chlorostyrene, and 4-chlorostyrene, and fluorine-substituted styrenes such as 4-fluorostyrene and 2,5-difluorostyrene, etc. One type of styrene-based monomer may be used alone, or two or more types may be used in combination.
[0115] As the styrene-based monomer, styrene and α-methylstyrene are preferred, and styrene is more preferred.
[0116] From the viewpoint of the resin being easily bonded to an electrode by wet heat pressing, the phenyl group-containing acrylic resin has a styrene unit and an acrylic unit, and the molar ratio of both units (styrene unit:acrylic unit) is preferably 30:70 to 50:50, more preferably 35:65 to 45:55, and even more preferably 37:63 to 43:57. The molar ratio is determined by nuclear magnetic resonance (NMR). The details of NMR are as described above.
[0117] The phenyl group-containing acrylic resin may contain a monomer other than the acrylic monomer and the styrene monomer in the polymerization component. Examples of such monomers include acid group-containing monomers. Examples of the acid group-containing monomers include monomers having a carboxy group such as crotonic acid, maleic acid, fumaric acid, and itaconic acid; monomers having a sulfonic acid group such as vinyl sulfonic acid, methyl vinyl sulfonic acid, (meth)allyl sulfonic acid, (meth)acrylic acid-2-ethyl sulfonate, 2-acrylamido-2-methylpropanesulfonic acid, and 3-allyloxy-2-hydroxypropanesulfonic acid; monomers having a phosphoric acid group such as 2-(meth)acryloyloxyethyl phosphate, methyl-2-(meth)acryloyloxyethyl phosphate, and ethyl-(meth)acryloyloxyethyl phosphate; monomers having a hydroxyl group such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; and the like. The acid group-containing monomer may be used alone or in combination of two or more kinds.
[0118] The phenyl group-containing acrylic resin may contain a crosslinkable monomer in the polymerization component. The crosslinkable monomer may be a polyfunctional monomer having two or more polymerizable groups. Examples of the polyfunctional monomer include divinyl compounds such as divinylbenzene; di(meth)acrylic acid ester compounds such as diethylene glycol dimethacrylate, ethylene glycol dimethacrylate, diethylene glycol diacrylate, and 1,3-butylene glycol diacrylate; tri(meth)acrylic acid ester compounds such as trimethylolpropane trimethacrylate and trimethylolpropane triacrylate; ethylenically unsaturated monomers containing epoxy groups such as allyl glycidyl ether and glycidyl methacrylate; and the like. The polyfunctional monomer may be used alone or in combination of two or more kinds.
[0119] -Butadiene-acrylonitrile resin- The butadiene-acrylonitrile resin may be a resin composed only of butadiene units and acrylonitrile units, or may be a resin composed of butadiene units, acrylonitrile units, and other monomer units. In other words, the butadiene-acrylonitrile resin may be a binary copolymer of butadiene and acrylonitrile, or may be a copolymer of butadiene, acrylonitrile, and other monomers. Examples of other monomers include styrene monomers and acrylic monomers.
[0120] Examples of the styrene monomer include styrene, α-methylstyrene, alkyl-substituted styrene such as 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, and 4-ethylstyrene, halogen-substituted styrene such as 2-chlorostyrene, 3-chlorostyrene, and 4-chlorostyrene, and fluorine-substituted styrene such as 4-fluorostyrene and 2,5-difluorostyrene. Examples of the styrene monomer include styrene and α-methylstyrene, and more preferably styrene. The styrene monomer may be used alone or in combination of two or more.
[0121] Examples of the acrylic monomer include (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, isobornyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. The acrylic monomer is preferably an alkyl (meth)acrylate. The alkyl group at the ester moiety of the alkyl (meth)acrylate is preferably an alkyl group having 1 to 10 carbon atoms, and more preferably an alkyl group having 1 to 8 carbon atoms. The acrylic monomer may be used alone or in combination of two or more kinds.
[0122] The molar ratio of butadiene units and acrylonitrile units (butadiene units:acrylonitrile units) contained in the butadiene-acrylonitrile resin is preferably 60:40 to 1:99, more preferably 50:50 to 10:90, from the viewpoint of excellent affinity with the phenyl group-containing acrylic resin. The molar ratio is determined by nuclear magnetic resonance (NMR). The details of NMR are as described above.
[0123] -Other resins- The adhesive layer may contain other resins than the phenyl group-containing acrylic resin and the butadiene-acrylonitrile resin. Examples of other resins include polyvinylidene fluoride resins, fluorine-based rubbers, homopolymers or copolymers of vinyl nitrile compounds (acrylonitrile, methacrylonitrile, etc.), carboxymethyl cellulose, hydroxyalkyl cellulose, polyvinyl alcohol, polyvinyl butyral, polyvinyl pyrrolidone, polyethers (polyethylene oxide, polypropylene oxide, etc.), or mixtures of two or more of these. These resins may be contained in the form of resin particles, or may be contained as a binder resin for the resin particles.
[0124] The mass ratio of other resins to the total resin in the adhesive layer is preferably 10 mass % or less, more preferably 5 mass % or less, even more preferably 1 mass % or less, and particularly preferably substantially none is contained. The total mass proportion of the phenyl group-containing acrylic resin and the butadiene-acrylonitrile resin in the total resin of the adhesive layer is preferably 90 mass% or more, more preferably 95 mass% or more, even more preferably 99 mass% or more, and particularly preferably 100 mass%.
[0125] The glass transition temperature of the entire resin contained in the adhesive layer is preferably 58°C or higher, more preferably 58.5°C or higher, and even more preferably 59°C or higher, from the viewpoint of excellent adhesion to the electrode, although the detailed mechanism is unknown. The upper limit of the glass transition temperature of the entire resin contained in the adhesive layer is not limited, but is preferably 100° C. or lower, more preferably 95° C. or lower, and even more preferably 94° C. or lower.
[0126] The glass transition temperature of a resin can be controlled by adjusting the types and copolymerization ratio of monomers that are polymerization components, using the FOX formula as a guideline.
[0127] The glass transition temperature of a resin is determined from a differential scanning calorimetry (DSC) curve obtained by DSC measurement. In the DSC curve, the intersection point of the low-temperature baseline and the tangent to the curve of the stepwise change portion is defined as intersection point (1), and the intersection point of the high-temperature baseline and the tangent to the curve of the stepwise change portion is defined as intersection point (2). The glass transition temperature is determined as the midpoint between intersection points (1) and (2).
[0128] -Other ingredients- The adhesive layer may contain additives such as a dispersant such as a surfactant, a wetting agent, an antifoaming agent, and a pH adjuster. The dispersant is added, for example, to the resin particle dispersion liquid for forming the adhesive layer for the purpose of improving dispersibility, coatability, or storage stability. The wetting agent, antifoaming agent, and pH adjuster are added, for example, to the resin particle dispersion liquid for forming the adhesive layer for the purpose of improving compatibility with the porous layer or porous substrate, for the purpose of suppressing air entrapment in the resin particle dispersion liquid, or for the purpose of pH adjustment.
[0129] -Characteristics of the adhesive layer- The adhesive layer's basis weight (mass per unit area) is set to 0.05 g / m per side of the separator from the viewpoint of adhesion to the electrode. 2 More than 0.07 g / m is preferable. 2 More preferably, 0.1 g / m or more 2 The above is more preferable. From the viewpoint of ion permeability, the weight of the adhesive layer is set to 1.0 g / m per side of the separator. 2 Less than 0.8 g / m is preferred. 2 Less than 0.6 g / m is more preferable. 2 The following is even more preferred:
[0130] When the adhesive layer is on both sides of the separator, the total weight of both sides is 0.1g / m 2 ~2.0g / m 2 is preferred, and 0.14 g / m 2 ~1.6g / m 2 More preferably, 0.2 g / m 2 ~1.2g / m 2is more preferred.
[0131] The basis weight of the adhesive layer is calculated by cutting the separator to a size of 20cm x 20cm, measuring the mass of the layer corresponding to the adhesive layer, and dividing the mass by the area to obtain the total for both sides. If the adhesive layer is formed equally on both sides of the separator, half of the total for both sides is the basis weight (g / m2) per side. 2 )
[0132] [Separator characteristics] From the viewpoint of the mechanical strength of the separator, the thickness of the separator is preferably 5 μm or more, more preferably 7 μm or more, and even more preferably 9 μm or more, and from the viewpoint of the energy density of the battery, the thickness is preferably 22 μm or less, more preferably 20 μm or less, and even more preferably 18 μm or less.
[0133] The thickness of the separator is measured at 20 points within a 10 cm square using a contact thickness meter and the average is calculated.
[0134] From the viewpoint of suppressing a short circuit in the battery, the air permeability of the separator is preferably 60 sec / 100 mL or more, more preferably 70 sec / 100 mL or more, and even more preferably 80 sec / 100 mL or more. From the viewpoint of ion permeability, the air permeability of the separator is preferably 260 sec / 100 mL or less, more preferably 250 sec / 100 mL or less, and even more preferably 240 sec / 100 mL or less.
[0135] The air permeability (sec / 100 mL) of the separator is measured using a digital Oken air permeability tester in accordance with JIS P8117:2009.
[0136] [Separator manufacturing method] The separator of the present disclosure is manufactured, for example, by the following manufacturing method A or manufacturing method B. Manufacturing methods A and B are methods for manufacturing a separator including a porous substrate. By replacing the porous substrate in manufacturing methods A and B with a release sheet and peeling off the release sheet at an appropriate time, it is possible to manufacture a separator including only a porous layer and an adhesive layer.
[0137] In the manufacturing method A and the manufacturing method B, the porous layer is formed on the porous substrate by a wet coating method. In the present disclosure, the wet coating method is a method in which the coating layer is solidified in a coagulating liquid, and the dry coating method is a method in which the coating layer is solidified by drying.
[0138] Manufacturing method A (discontinuous manufacturing method): A porous layer is formed on a porous substrate unwound from a roll to obtain a laminate of the porous substrate and the porous layer, and the laminate is temporarily wound up on another roll. Next, an adhesive layer is formed on the laminate unwound from the roll to obtain a separator, and the completed separator is wound up on another roll.
[0139] Manufacturing method B (continuous manufacturing method): A porous layer and an adhesive layer are formed continuously or simultaneously on a porous substrate unwound from a roll, and the completed separator is wound up on another roll.
[0140] The production method B may be any one of the following modes B-1 to B-4.
[0141] Mode B-1: A coating liquid for forming a porous layer is applied onto a porous substrate, the coating layer is solidified by immersion in a coagulating liquid, and the substrate is pulled out of the coagulating liquid, washed with water, and dried. Next, a resin particle dispersion is applied onto the substrate, and the substrate is dried.
[0142] Configuration B-2: A coating liquid for forming a porous layer is applied onto a porous substrate, the coating layer is solidified by immersion in a coagulating liquid, and the substrate is pulled out of the coagulating liquid and washed with water. Next, a resin particle dispersion is applied onto the substrate, followed by drying.
[0143] Configuration B-3: Two layers of a coating liquid for forming a porous layer and a resin particle dispersion liquid are simultaneously applied onto a porous substrate, the substrate is immersed in a coagulating liquid to solidify the former coating layer, and then the substrate is removed from the coagulating liquid, washed with water, and dried.
[0144] Configuration B-4: A coating liquid for forming a porous layer is applied onto a porous substrate, the coating layer is solidified by immersing it in a coagulating liquid, and then the substrate is removed from the coagulating liquid and transported through a water bath containing resin particles to wash the substrate and adhere the resin particles thereto, and the substrate is removed from the water bath and dried.
[0145] The steps included in the production method will be described in detail below by taking Production Method B of Form B-1 as an example.
[0146] In the manufacturing method B of the embodiment B-1, a porous layer is formed on at least one surface of a porous substrate by a wet coating method to obtain a laminate of the porous substrate and the porous layer, and then an adhesive layer is formed on at least one surface of the laminate by a dry coating method. The manufacturing method B of the embodiment B-1 includes the following steps (1) to (7), which are carried out in sequence.
[0147] Step (1): Preparation of coating liquid for forming porous layer The coating liquid for forming the porous layer (hereinafter, referred to as "coating liquid" in the description of the production method) is prepared by dissolving or dispersing the binder resin and inorganic particles of the porous layer in a solvent. If necessary, other components than the binder resin and inorganic particles are dissolved or dispersed in the coating liquid.
[0148] The solvent used in preparing the coating liquid includes a solvent that dissolves the binder resin of the porous layer (hereinafter, also referred to as a "good solvent"). Examples of the good solvent include polar amide solvents such as N-methylpyrrolidone, dimethylacetamide, dimethylformamide, and dimethylformamide.
[0149] From the viewpoint of forming a porous layer having a good porous structure, the solvent used in preparing the coating liquid preferably contains a phase separation agent that induces phase separation. Therefore, the solvent used in preparing the coating liquid is preferably a mixed solvent of a good solvent and a phase separation agent. The phase separation agent is preferably mixed with the good solvent in an amount within a range that ensures a viscosity suitable for coating. Examples of the phase separation agent include water, methanol, ethanol, propyl alcohol, butyl alcohol, butanediol, ethylene glycol, propylene glycol, and tripropylene glycol.
[0150] From the viewpoint of forming a good porous structure, the solvent used for preparing the coating liquid is preferably a mixed solvent of a good solvent and a phase separation agent, containing 60% by mass or more of the good solvent and 5% by mass to 40% by mass of the phase separation agent.
[0151] The resin concentration in the coating liquid is preferably 1% by mass to 20% by mass in order to form a good porous structure, and the inorganic particle concentration in the coating liquid is preferably 0.5% by mass to 50% by mass in order to form a good porous structure.
[0152] Step (2): Preparation of resin particle dispersion The resin particle dispersion is prepared by dispersing resin particles in a suitable dispersion medium (e.g., water). A surfactant may be added to the resin particle dispersion to enhance the dispersibility of the resin particles in the dispersion medium. The resin particle dispersion may be a commercially available product or a diluted solution of a commercially available product.
[0153] From the viewpoint of coating suitability, the concentration of the resin particles in the resin particle dispersion is preferably 1% by mass to 60% by mass.
[0154] Step (3): Coating with coating fluid The coating liquid is applied to at least one surface of the porous substrate to form a coating layer on the porous substrate. Examples of the method for applying the coating liquid to the porous substrate include knife coating, Mayer bar coating, die coating, reverse roll coating, roll coating, gravure coating, screen printing, inkjet, and spraying. When forming a porous layer on both sides of the porous substrate, it is preferable to apply the coating liquid to both sides of the porous substrate at the same time from the viewpoint of productivity.
[0155] Step (4): Solidification of the coating layer The porous substrate on which the coating layer is formed is immersed in a coagulation liquid to induce phase separation in the coating layer while solidifying the binder resin, thereby forming a porous layer containing the binder resin and inorganic particles, thereby obtaining a laminate consisting of the porous substrate and the porous layer.
[0156] The solidification liquid generally contains the good solvent and phase separation agent used in preparing the coating liquid, and water. It is preferable from the viewpoint of productivity that the mixing ratio of the good solvent and the phase separation agent is the same as the mixing ratio of the mixed solvent used in preparing the coating liquid. The content of water in the solidification liquid is preferably 40% by mass to 90% by mass from the viewpoints of forming a porous structure and productivity. The temperature of the solidification liquid is, for example, 20°C to 50°C.
[0157] Step (5): Washing and drying the coating layer The laminate is pulled out of the coagulating liquid and washed with water. The coagulating liquid is removed from the laminate by washing with water. Furthermore, water is removed from the laminate by drying. The washing with water is performed, for example, by conveying the laminate in a water washing bath. The drying is performed, for example, by conveying the laminate in a high-temperature environment, by blowing air on the laminate, by bringing the laminate into contact with a heat roll, or the like. The drying temperature is preferably 40°C to 80°C.
[0158] Step (6): Coating of resin particle dispersion A resin particle dispersion is applied to at least one surface of the laminate by a method such as knife coating, gravure coating, Mayer bar coating, die coating, reverse roll coating, roll coating, screen printing, inkjet printing, spraying, etc.
[0159] Step (7): Drying the resin particle dispersion The resin particle dispersion on the laminate is dried to adhere the resin particles to the surface of the laminate. The drying is performed, for example, by conveying the laminate in a high-temperature environment or by exposing the laminate to wind. The drying temperature is preferably 40°C to 100°C.
[0160] The production method A or the production method B of Forms B-2 to B-4 can be carried out by partially omitting or modifying the above steps (1) to (7).
[0161] <Non-aqueous secondary battery> The nonaqueous secondary battery of the present disclosure is a nonaqueous secondary battery that obtains electromotive force by doping and dedoping lithium ions, and includes a positive electrode, a negative electrode, and the separator of the present disclosure. Doping means occlusion, support, adsorption, or insertion, and refers to the phenomenon in which lithium ions enter the active material of an electrode such as a positive electrode.
[0162] The nonaqueous secondary battery of the present disclosure has a structure in which, for example, a battery element in which a negative electrode and a positive electrode face each other with a separator interposed therebetween is enclosed in an exterior material together with an electrolyte solution. The nonaqueous secondary battery of the present disclosure is suitable for nonaqueous electrolyte secondary batteries, particularly lithium ion secondary batteries.
[0163] The nonaqueous secondary battery of the present disclosure has excellent productivity in terms of battery productivity because the separator of the present disclosure is well bonded to the electrodes by low-temperature, low-pressure wet heat pressing.
[0164] Hereinafter, examples of the positive electrode, negative electrode, electrolyte, and exterior material included in the nonaqueous secondary battery of the present disclosure will be described.
[0165] An example of the positive electrode is a structure in which an active material layer containing a positive electrode active material and a binder resin is formed on a current collector. The active material layer may further contain a conductive additive. Examples of the positive electrode active material include lithium-containing transition metal oxides, specifically LiCoO2, LiNiO2, LiMn 1 / 2 Ni 1 / 2 O2, LiCo 1 / 3 Mn 1 / 3 Ni 1 / 3 O2, LiMn2O4, LiFePO4, LiCo 1 / 2 Ni 1 / 2 O2, LiAl 1 / 4 Ni 3 / 4 Examples of the binder resin include polyvinylidene fluoride resin, styrene-butadiene copolymer, etc. Examples of the conductive assistant include carbon materials such as acetylene black, ketjen black, graphite powder, etc. Examples of the current collector include aluminum foil, titanium foil, stainless steel foil, etc., having a thickness of 5 μm to 20 μm.
[0166] An example of the negative electrode is a structure in which an active material layer containing a negative electrode active material and a binder resin is formed on a current collector. The active material layer may further contain a conductive assistant. The negative electrode active material may be a material capable of electrochemically absorbing lithium ions, specifically, for example, a carbon material; an alloy of lithium with silicon, tin, aluminum, or the like; Wood's alloy; and the like. The binder resin may be, for example, a polyvinylidene fluoride resin, a styrene-butadiene copolymer, and the like. The conductive assistant may be, for example, a carbon material such as acetylene black, ketjen black, graphite powder, or ultrafine carbon fiber. The current collector may be, for example, a copper foil, a nickel foil, a stainless steel foil, or the like having a thickness of 5 μm to 20 μm. In addition, instead of the above-mentioned negative electrode, a metallic lithium foil may be used as the negative electrode.
[0167] The electrolyte is a solution in which a lithium salt is dissolved in a non-aqueous solvent. Examples of the lithium salt include LiPF6, LiBF4, and LiClO4. Examples of the non-aqueous solvent include cyclic carbonates such as ethylene carbonate, propylene carbonate, fluoroethylene carbonate, difluoroethylene carbonate, and vinylene carbonate; chain carbonates such as dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, and fluorine-substituted derivatives thereof; and cyclic esters such as γ-butyrolactone and γ-valerolactone; which may be used alone or in combination. The electrolyte is preferably a solution in which a cyclic carbonate and a chain carbonate are mixed in a mass ratio (cyclic carbonate:chain carbonate) of 20:80 to 40:60, and a lithium salt is dissolved in the range of 0.5 mol / L to 1.5 mol / L.
[0168] Examples of the exterior material include an aluminum laminate film pack, a metal can, etc. The shape of the battery may be rectangular, cylindrical, coin-shaped, etc., and the separator of the present disclosure is suitable for any shape.
[0169] The nonaqueous secondary battery of the present disclosure can be produced by producing a laminate in which the separator of the present disclosure is disposed between a positive electrode and a negative electrode, and then using this laminate, for example, by Production Method 1 or Production Method 2 described below.
[0170] Manufacturing method 1: The laminate is dry heat pressed to temporarily bond the electrodes and separator, then housed in an exterior material (e.g., an aluminum laminate film pack; the same applies below) and an electrolyte is injected into it. The laminate is then wet heat pressed from above the exterior material to bond the electrodes and separator and seal the exterior material.
[0171] Manufacturing method 2: The laminate is placed in an exterior material and an electrolyte is poured in. The laminate is then wet heat pressed onto the exterior material to bond the electrodes and the separator and seal the exterior material.
[0172] In the manufacturing method 1 and the manufacturing method 2, the pressing temperature of the wet heat press is preferably 50° C. to 80° C., and more preferably 60° C. to 70° C. The pressing pressure of the wet heat press is preferably 40 kPa to 200 kPa, and more preferably 50 kPa to 100 kPa. The pressing time of the wet heat press is preferably adjusted according to the pressing temperature and pressing pressure, and is adjusted, for example, in the range of 8 hours to 20 hours.
[0173] When manufacturing a laminate in which a separator is disposed between a positive electrode and a negative electrode, the method of disposing the separator between the positive electrode and the negative electrode may be a method of stacking at least one layer of a positive electrode, a separator, and a negative electrode in this order (a so-called stack method), or a method of stacking a positive electrode, a separator, a negative electrode, and a separator in this order and winding them up in the length direction. EXAMPLES
[0174] The separator and nonaqueous secondary battery of the present disclosure will be described in more detail below with reference to examples. The materials, amounts, ratios, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present disclosure. Therefore, the scope of the separator and nonaqueous secondary battery of the present disclosure should not be interpreted as being limited by the specific examples shown below.
[0175] In the following description, syntheses, treatments, manufactures, etc. were carried out at room temperature (25° C.±3° C.) unless otherwise specified.
[0176] <Measurement and evaluation methods> The measurement and evaluation methods applied in the examples and comparative examples are as follows.
[0177] [Air permeability of separator and porous substrate] The air permeability (sec / 100 mL) of the separator and the porous substrate was measured using a digital Oken air permeability tester (Asahi Seiko Co., Ltd., EGO1-55-1MR) in accordance with JIS P8117:2009.
[0178] [Thickness of separator and porous substrate] The thickness of the separator and the porous substrate was measured at 20 points within a 10 cm square using a contact thickness meter (Mitutoyo Corporation, LITEMATIC VL-50S) and the average was calculated. A spherical probe with a sphere radius of 10 mm (Mitutoyo Corporation) was used as the measurement terminal, and the load was adjusted so that 0.19 N was applied during the measurement.
[0179] [Porous layer thickness] The thickness of the flat membrane was calculated by subtracting the thickness of the porous substrate from the thickness of the flat membrane after removing the adhesive layer from the separator. The thickness of the flat membrane was measured at 20 points within a 10 cm square area using a contact thickness meter (Mitutoyo Corporation, LITEMATIC VL-50S) and calculated by averaging the measurements. A spherical probe with a sphere radius of 10 mm (Mitutoyo Corporation) was used as the measurement terminal, and the measurement was adjusted so that a load of 0.19 N was applied during measurement.
[0180] [Weight of adhesive layer] The separator was cut to a size of 20 cm x 20 cm, the mass of the layer corresponding to the adhesive layer was measured, and the mass was divided by the area to calculate the total basis weight (g / m2) of both sides. 2 In all of the examples and comparative examples, the adhesive layer was formed in equal amounts on both sides of the separator, so the basis weight per side (g / m2) was calculated by dividing the total basis weight of both sides by half. 2 ) was decided.
[0181] [Average primary particle size of inorganic particles] The inorganic particles used to form the porous layer were used as samples and observed with a scanning electron microscope (SEM) to determine the average primary particle size. Specifically, the major axis of 100 inorganic particles randomly selected during SEM observation was measured, and the average of the major axes of the 100 particles was taken as the average primary particle size (μm).
[0182] [Average primary particle size of resin particles] The dried resin particle dispersion liquid used to form the adhesive layer was used as a sample and observed by SEM to determine the average primary particle size. Specifically, the major axis of 100 randomly selected resin particles was measured during SEM observation, and the average of the major axis values of the 100 particles was taken as the average primary particle size (μm).
[0183] [Glass transition temperature of resin] A dry solid of the resin particle dispersion liquid used for forming the adhesive layer was used as a sample, and differential scanning calorimetry (DSC) was performed. A Q200 Differential Scanning Calorimeter (TA Instruments) was used as the DSC device, and the weight of the sample was 5 mg. The temperature was raised from -65°C to 150°C at a heating rate of 10°C / min, then quenched and heated again at the same heating rate to obtain a DSC curve. In the obtained DSC curve, the intersection point (1) between the low-temperature side baseline and the tangent to the curve of the stepwise change part, and the intersection point (2) between the high-temperature side baseline and the tangent to the curve of the stepwise change part were obtained, and the temperature in the middle between the intersection points (1) and (2) was determined as the glass transition temperature (Tg, °C).
[0184] [Resin composition] The monomer units contained in the resin constituting the adhesive layer were quantified by NMR. The dried resin particle dispersion liquid used to form the adhesive layer was used as a sample. The sample was swollen with deuterated chloroform, and then measured at room temperature at 600 MHz using an NMR device (JNM-ECA600 manufactured by JEOL Ltd.) and a semi-solid probe (FGMAS probe manufactured by JEOL Ltd.). 1 H-NMR spectrum (MAS rotation speed 6 kHz, observation width 15 ppm, number of points 32 k, pulse repetition waiting time 4 seconds) was measured at 150 MHz. 13 C-NMR spectrum was measured. 13 C-NMR spectra were accumulated approximately 33,000 times in quantitative mode (inverse gated decoupling method, MAS rotation speed 6 kHz, observation width 250 ppm, number of points 32 k, pulse repetition waiting time 12 seconds).
[0185] [Adhesive strength] A test secondary battery was prepared as described below. A compression type bending test (three-point bending measurement) was performed on the battery. The measurement was performed by attaching a compression type bending test jig to a Tensilon (A&D Co., Ltd., STB-1225S). The distance between the supports was 4 cm, and the battery was placed on the support so that the short side of the battery was parallel to the long direction of the indenter and the compression position during measurement was the center of the long direction of the electrode in the battery. The measurement was started by setting the displacement at 0 when the indenter was lowered until a load of 0.1 N was applied. The compression speed during measurement was 2 mm / min, and the measurement was performed up to a displacement of 2 mm. The yield point load (N) in the load displacement curve obtained from this result was taken as the adhesive strength. When the yield point load could not be observed, the maximum load (N) was taken as the adhesive strength. The results are shown in Table 3.
[0186] [Heat resistance] A test secondary battery was prepared as described below. The battery was charged at a constant current and constant voltage of 0.2C and 4.2V at room temperature. The battery was then placed in an oven at a temperature of 150°C, and a weight of about 500g was placed on the battery. After 60 minutes, the battery was removed from the oven and cooled to room temperature. The battery voltage was measured, and a short circuit was determined when it was 3.5V or less. The number of short circuits among the five batteries was classified as follows. The results are shown in Table 3. A:0 pieces B: 1~2 pieces C: 3~5 pieces
[0187] <Preparation of separator and battery> [Example 1] -Making the separator- A mixed solvent of dimethylacetamide (DMAc) and tripropylene glycol (TPG) (DMAc:TPG = 80:20 [mass ratio]) was prepared. Meta-aramid (polymetaphenylene isophthalamide, Teijin, Conex) was dissolved in the mixed solvent so that the resin concentration was 4 mass%, to obtain a resin solution. Magnesium hydroxide particles (average primary particle size 0.8 μm) were added to the resin solution in an amount such that the magnesium hydroxide particles:meta-aramid = 70:30 [mass ratio], and the mixture was stirred and mixed to obtain coating liquid (1).
[0188] Resin particle dispersion (1) (dispersion medium: water, solid content concentration 7% by mass) was prepared. The dried resin particle dispersion (1) was used as a sample, and the above-mentioned SEM observation, DSC and NMR were performed to analyze the particle size of the resin particles, the Tg of the resin and the composition of the resin. The results are shown in Table 2.
[0189] An appropriate amount of the coating liquid (1) was placed on a pair of Mayer bars, and a polyethylene microporous membrane (thickness 9 μm, air permeability 95 sec / 100 mL) was passed between the Mayer bars to coat both sides with the coating liquid (1) in equal amounts. This was immersed in a coagulation liquid (DMAc:TPG:water=30:8:62 [mass ratio], liquid temperature 40°C) to solidify the coating layer, and then washed in a water washing tank with a water temperature of 40°C and dried. Next, this was passed between a pair of bar coaters on which an appropriate amount of the resin particle dispersion liquid (1) was placed, and the resin particle dispersion liquid (1) was coated in equal amounts on both sides and dried. In this way, a separator in which a porous layer and an adhesive layer were formed on both sides of the polyethylene microporous membrane was obtained. When the obtained separator was observed with an SEM, it was found that the porous layer had a large number of micropores inside and a structure in which the micropores were connected, allowing gas or liquid to pass through from one side to the other.
[0190] - Preparation of positive electrode - 89.5 parts by mass of lithium cobalt oxide powder as a positive electrode active material, 4.5 parts by mass of acetylene black as a conductive assistant, 6 parts by mass of polyvinylidene fluoride as a binder resin, and an appropriate amount of N-methyl-2-pyrrolidone were mixed by stirring with a twin-arm mixer to prepare a positive electrode slurry. The positive electrode slurry was applied to both sides or one side of a 20 μm thick aluminum foil, dried, and pressed to obtain a positive electrode having a positive electrode active material layer on both sides or one side.
[0191] - Preparation of negative electrode - A negative electrode slurry was prepared by mixing 300 parts by mass of artificial graphite as a negative electrode active material, 7.5 parts by mass of a water-soluble dispersion containing 40% by mass of a modified styrene-butadiene copolymer as a binder resin, 3 parts by mass of carboxymethylcellulose as a thickener, and an appropriate amount of water with a twin-arm mixer. The negative electrode slurry was applied to both sides or one side of a copper foil with a thickness of 10 μm, dried, and pressed to obtain a negative electrode having a negative electrode active material layer on both sides or one side.
[0192] -Creating a battery for evaluating adhesive strength- The double-sided positive electrode and double-sided negative electrode were each cut into a rectangle of 30 mm x 70 mm. The separator was cut into a rectangle measuring TD 35 mm x MD 75 mm. These were stacked so that the positive and negative electrodes were alternated and a separator was sandwiched between the positive and negative electrodes, to produce a laminate consisting of three positive electrodes, three negative electrodes, and five separators. The laminate was inserted into a pack made of aluminum laminate film, and an electrolyte (1 mol / L LiPF6-ethylene carbonate:ethyl methyl carbonate [mass ratio 3:7]) was injected into the pack to allow the electrolyte to soak into the laminate. Next, the pack and the laminate were heat-pressed in the stacking direction using a heat press machine (wet heat press) to bond the electrodes and separators. The heat press conditions were a press temperature of 60°C, a press pressure of 50 kPa, and a press time of 17 hours. The test secondary battery thus obtained was subjected to the above-mentioned adhesion strength test.
[0193] -Creating a battery for evaluating heat resistance- The single-sided positive electrode and the single-sided negative electrode were each cut into a rectangle of 14 mm x 20 mm. The separator was cut into a rectangle measuring TD 20 mm x MD 26 mm. These were stacked so that the positive electrode active material layer and the negative electrode active material layer faced each other and the separator was sandwiched between the positive electrode and the negative electrode to produce a laminate consisting of one positive electrode, one negative electrode, and one separator. The laminate was inserted into a pack made of an aluminum laminate film, and an electrolyte (1 mol / L LiPF6-ethylene carbonate:ethyl methyl carbonate [mass ratio 3:7]) was injected into the pack to allow the electrolyte to soak into the laminate. Next, the pack and the laminate were heat-pressed in the stacking direction using a heat press machine (wet heat press) to bond the electrodes and the separator. The heat press conditions were a press temperature of 60°C, a press pressure of 50 kPa, and a press time of 17 hours. The test secondary battery thus obtained was subjected to the evaluation of heat resistance as described above.
[0194] [Example 2] Resin particle dispersion (2) (dispersion medium: water, solid content concentration 7% by mass) was prepared. The dried resin particle dispersion (2) was used as a sample, and the above-mentioned SEM observation, DSC and NMR were performed to analyze the particle size of the resin particles, the Tg of the resin and the composition of the resin. The results are shown in Table 2.
[0195] A separator was produced in the same manner as in Example 1, except that the resin particle dispersion liquid (1) was changed to the resin particle dispersion liquid (2). The basis weight of the adhesive layer is as shown in Table 2. When the obtained separator was observed with an SEM, it was found that the porous layer had a large number of micropores inside and a structure in which the micropores were connected, allowing gas or liquid to pass through from one side to the other.
[0196] [Comparative Example 1] Resin particle dispersion (3) (dispersion medium: water, solid content concentration 7% by mass) was prepared. The dried resin particle dispersion (3) was used as a sample, and the above-mentioned SEM observation, DSC and NMR were performed to analyze the particle size of the resin particles, the Tg of the resin and the composition of the resin. The results are shown in Table 2.
[0197] A separator was produced in the same manner as in Example 1, except that the resin particle dispersion liquid (1) was changed to the resin particle dispersion liquid (3). The basis weight of the adhesive layer is as shown in Table 2.
[0198] [Comparative Example 2] A separator was produced in the same manner as in Example 1, except that the resin particle dispersion liquid (1) was changed to liquid butadiene-acrylonitrile copolymer (hereinafter referred to as liquid NBR). The basis weight of the adhesive layer is as shown in Table 2.
[0199] [Comparative Example 3] The same procedure as in Example 1 was followed, except that the resin particle dispersion (1) was replaced with a mixture of the resin particle dispersion (1) and liquid NBR, and a separator was produced. The mixture ratio was the solid content of the resin particle dispersion (1): the liquid NBR = 15:85 [mass ratio]. The resin particles of the resin particle dispersion (1) and the liquid NBR were separated, and an adhesive layer could not be formed. In this example, the glass transition temperature was not measured. The particle size of the resin particles shown in Table 2 is the measurement value of the resin particle dispersion (1). The type and amount of the monomer unit shown in Table 2 are shown based on the measurement results of the resin particle dispersion (1) and the measurement results of the liquid NBR.
[0200] [Example 3] A separator was produced in the same manner as in Example 1, except that the magnesium hydroxide particles were changed to barium sulfate particles (average primary particle size: 0.03 μm). The composition of the porous layer and the basis weight of the adhesive layer are as shown in Tables 1 and 2. When the obtained separator was observed with an SEM, it was found that the porous layer had a large number of micropores inside and a structure in which the micropores were connected, allowing gas or liquid to pass through from one side to the other.
[0201] [Comparative Example 4] A separator was produced in the same manner as in Example 3, except that the resin particle dispersion (1) was changed to the resin particle dispersion (3). The composition of the porous layer and the basis weight of the adhesive layer are as shown in Tables 1 and 2.
[0202] [Example 4] A separator was produced in the same manner as in Example 1, except that the meta-aramid was changed to an acrylic resin and the magnesium hydroxide particles were changed to alumina particles (average primary particle size 1.0 μm). The composition of the porous layer and the basis weight of the adhesive layer are as shown in Tables 1 and 2. When the obtained separator was observed with an SEM, it was found that the porous layer had a large number of micropores inside and a structure in which the micropores were connected, allowing gas or liquid to pass through from one side to the other.
[0203] [Comparative Example 5] A separator was produced in the same manner as in Example 4, except that the resin particle dispersion (1) was changed to the resin particle dispersion (3). The composition of the porous layer and the basis weight of the adhesive layer are as shown in Tables 1 and 2.
[0204] [Example 5] A separator was produced in the same manner as in Example 1, except that the meta-aramid was changed to an acrylic resin and the magnesium hydroxide particles were changed to boehmite particles (average primary particle size 1.0 μm). The composition of the porous layer and the basis weight of the adhesive layer are as shown in Tables 1 and 2. When the obtained separator was observed with an SEM, it was found that the porous layer had a large number of micropores inside and a structure in which the micropores were connected, allowing gas or liquid to pass through from one side to the other.
[0205] The acrylic resin used to form the porous layer in Example 4, Comparative Example 5, and Example 5 was an n-butyl methacrylate / acrylonitrile copolymer.
[0206] The abbreviations in Tables 1 and 2 have the following meanings. PE: Polyethylene St: styrene MMA: Methyl methacrylate ·BMA: n-butyl methacrylate EHMA: 2-Ethylhexyl methacrylate Bt: Butadiene ·AN: Acrylonitrile
[0207] [Table 1]
[0208] [Table 2]
[0209] [Table 3]
[0210] All publications, patent applications, and standards mentioned in this specification are herein incorporated by reference to the same extent as if each individual publication, patent application, or standard was specifically and individually indicated to be incorporated by reference. [Explanation of symbols]
[0211] 101, 102, 103, 104, 105, 106, 107 Separators 20 Porous substrate 30 Porous layer 40 Laminate 50 Adhesive layer 52 Resin particles
Claims
1. a porous layer containing inorganic particles and a binder resin; an adhesive layer containing a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin, in which the amount of butadiene units in the total amount of acrylic units, styrene units, butadiene units and acrylonitrile units contained in both resins is 3 mol % to 50 mol %; A separator for a non-aqueous secondary battery comprising:
2. Further comprising a porous substrate, The porous layer is provided on one or both sides of the porous substrate, The adhesive layer is provided on one or both sides of a laminate of the porous substrate and the porous layer. The separator for a non-aqueous secondary battery according to claim 1 .
3. The adhesive layer contains resin particles, The resin particles contain at least one of a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin. The separator for a non-aqueous secondary battery according to claim 1 .
4. 4. The separator for a non-aqueous secondary battery according to claim 3, wherein the average primary particle size of all the resin particles contained in the adhesive layer is 0.1 μm to 1.0 μm.
5. 2. The separator for a non-aqueous secondary battery according to claim 1, wherein a mass ratio of the phenyl group-containing acrylic resin to the butadiene-acrylonitrile resin contained in the adhesive layer is 60:40 to 95:
5.
6. The phenyl group-containing acrylic resin has a styrene unit and an acrylic unit, The molar ratio of the styrene-based unit to the acrylic unit is 30:70 to 50:50; The separator for a non-aqueous secondary battery according to claim 1 .
7. 2. The separator for a non-aqueous secondary battery according to claim 1, wherein the glass transition temperature of the entire resin contained in the adhesive layer is 58° C. to 100° C.
8. The adhesive layer has a basis weight of 0.05 g / m per one side of the nonaqueous secondary battery separator. 2 ~1.0g / m 2 The separator for a non-aqueous secondary battery according to claim 1 ,
9. 2. The separator for a non-aqueous secondary battery according to claim 1, wherein the inorganic particles contained in the porous layer all have an average primary particle size of 0.01 μm to 1.0 μm.
10. 2. The separator for a non-aqueous secondary battery according to claim 1, wherein the binder resin comprises at least one resin selected from the group consisting of polyamide-based resins, acrylic-based resins, fluorine-based resins, and styrene-butadiene-based resins.
11. A non-aqueous secondary battery separator according to any one of claims 1 to 10, the separator being disposed between the positive electrode and the negative electrode; Electromotive force is obtained by doping and dedoping lithium ions. Non-aqueous secondary battery.
Citation Information
Patent Citations
Porous film composition for lithium ion secondary batteries, lithium ion secondary battery separator, electrode for lithium ion secondary batteries, and lithium ion secondary battery
JP2015026572A
Composite porous separator and electrochemical device
JP2015191886A
Separator for power storage device, and electrochemical element
JP2016072197A
Adhesive for lithium ion secondary batteries, separator for lithium ion secondary batteries, and lithium ion secondary battery
WO2015005145A1
Separator for non-aqueous secondary batteries, and non-aqueous secondary battery
WO2019130994A1