Secondary battery and electric device
By designing a multi-pole structure and optimizing the electrolyte composition, the problem of slow charging speed and temperature rise of lithium-ion batteries under fast charging conditions is solved, the dynamics and cycle performance are improved, and the demand for super fast charging is met.
Patent Information
- Application Number
- CN202380020507.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-09
- Publication Date
- 2024-10-11
AI Technical Summary
Existing lithium-ion batteries have slow charging speeds, elevated temperatures, and insufficient kinetic and cycle performance under fast charging conditions, making it difficult to meet the needs of super-fast charging.
By designing the structure of the positive electrode tab and the negative electrode tab, regulating the coating weight of the positive electrode active material layer and the negative electrode active material layer, optimizing the composition and content of the electrolyte, increasing the transmission speed of lithium ions, and reducing the internal resistance and charging temperature rise of the battery .
It achieves high charging speed and low charging temperature rise of lithium-ion batteries under fast charging conditions, improves dynamic performance and cycle performance, and meets the requirements of super fast charging.
Smart Images

Figure CN118765451A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of electrochemical technology, and in particular to a secondary battery and an electrical device. Background Art
[0002] Lithium-ion batteries have the characteristics of high specific energy, high operating voltage, low self-discharge rate, small size and light weight. They are widely used in various fields such as energy storage, portable electronic devices and electric vehicles.
[0003] With the continuous iterative development of consumer lithium-ion batteries in recent years, the market has higher and higher requirements for their charging speed and charging rate. Therefore, how to reduce the impedance of various components of lithium-ion batteries and increase the charging speed of lithium-ion batteries to meet the requirements of super fast charging while keeping the temperature rise low has become a technical problem that needs to be urgently solved by technical personnel in this field. Summary of the invention
[0004] The purpose of the present application is to provide a secondary battery, which improves the charging speed of the secondary battery while taking into account the low charging temperature rise of the secondary battery, thereby improving the dynamic performance and cycle performance of the secondary battery, and at the same time provides an electrical device using the secondary battery.
[0005] It should be noted that in the invention content of this application, lithium-ion batteries are used as an example of secondary batteries to explain this application, but the secondary batteries of this application are not limited to lithium-ion batteries, but can also be applied to secondary batteries such as sodium-ion batteries. The specific technical solutions are as follows:
[0006] The first aspect of the present application provides a secondary battery, the secondary battery comprises a positive electrode sheet, a negative electrode sheet and an electrolyte, the positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer, the negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer; the coating weight of the positive electrode active material layer is W z , the coating weight of the negative electrode active material layer is W f , W z and W f Between: 1.6W f ≤W z ≤2.2W f 、3.25mg / cm 2 ≤W f ≤5.84mg / cm 2. The positive electrode current collector extends integrally to form a plurality of positive electrode tabs, and the negative electrode current collector extends integrally to form a plurality of negative electrode tabs. The electrolyte includes an organic solvent, a lithium salt and an additive, and the organic solvent includes a chain carboxylic acid ester compound. Based on the mass of the electrolyte, the mass percentage of the chain carboxylic acid ester compound is 6% to 56%. By adopting the structural design of the positive electrode tab and the negative electrode tab, multiple current channels can be generated on the positive electrode sheet and the negative electrode sheet during the secondary battery cycle, thereby reducing the internal resistance of the secondary battery, making the voltage polarization of the secondary battery small under fast charging conditions, reducing the charging temperature rise of the secondary battery, and shortening the charging time of the secondary battery.
[0007] By regulating the coating weight of the positive electrode active material layer and the negative electrode active material layer within the above range, the thickness of the positive electrode active material layer and the negative electrode active material layer can be reduced, and while taking into account the processing performance and energy density of the secondary battery, the transmission distance of lithium ions inside the positive electrode sheet and the negative electrode sheet can be reduced, thereby reducing the ohmic polarization and concentration polarization of the secondary battery, improving the fast charging performance, and making the secondary battery have higher dynamic performance. In order to adapt to the high dynamic performance of the secondary battery, higher requirements are put forward for the electrolyte in the secondary battery. The lithium ion transmission speed in the conventional electrolyte is slow under the high dynamic system of the secondary battery, resulting in a slow charging speed of the secondary battery, and lithium is easily precipitated during the cycle, resulting in reduced cycle performance of the secondary battery. By regulating the composition and content in the electrolyte, the electrolyte has high conductivity and low viscosity, which can accelerate the transmission speed of lithium ions and further reduce the electrochemical polarization and concentration polarization of the secondary battery. The present application optimizes the electrochemical system by combining the structural design of the positive electrode tab and the negative electrode tab, the coating weight of the positive electrode active material layer and the negative electrode active material layer, and the composition and content of the electrolyte. It can improve the charging speed of the secondary battery while taking into account the low charging temperature rise of the secondary battery, thereby improving the kinetic performance and cycle performance of the secondary battery.
[0008] In some embodiments of the present application, 6.49 mg / cm 2 ≤W z ≤11.69mg / cm 2 The present application adjusts the coating weight of the positive electrode active material layer within the scope of the present application, while taking into account the processing performance and energy density of the secondary battery, shortens the transmission distance of lithium ions and electrons on the positive electrode sheet, reduces the impedance of the secondary battery, and enables the secondary battery to have good cycle performance.
[0009] In some embodiments of the present application, N is provided between two adjacent positive electrode tabs. 1 There is a positive electrode sheet, and N is set between two adjacent negative electrode tabs. 2 Layer negative electrode, N 1 and N 2Each is independently selected from 0, 1, 2 or 3. In the present application, through the above configuration, there are multiple current channels on the positive electrode sheet and the negative electrode sheet, so that the impedance of the secondary battery is reduced, the voltage polarization of the secondary battery during fast charging is small, the charging temperature rise is reduced, and the charging time is shortened, so that the secondary battery has good dynamic performance and cycle performance. It can be understood that N 1 and N 2 Adjusting N to 0 can provide more current channels on the positive and negative electrodes, further reduce the internal resistance of the secondary battery, further reduce the charging temperature rise of the fast-charged secondary battery, and further shorten the charging time, thereby further improving the dynamic performance of the fast-charged secondary battery while taking into account the cycle performance and mechanical reliability. However, this will reduce the energy density of the battery to a certain extent. 1 and N 2 Adjusting it to 1, 2 or 3 will reduce the number of tabs and increase the internal resistance to a certain extent, but it can improve the battery energy density.
[0010] In some embodiments of the present application, the chain carboxylic acid ester compound includes at least one of methyl formate, methyl acetate, ethyl formate, ethyl acetate, propyl acetate, ethyl propionate, methyl propionate, n-propyl propionate, isopropyl propionate, n-butyl propionate, isobutyl propionate, n-pentyl propionate, isopentyl propionate, ethyl butyrate, n-propyl butyrate, propyl isobutyrate, n-pentyl butyrate, n-pentyl isobutyrate, n-butyl butyrate, isobutyl isobutyrate, and n-pentyl valerate. Preferably, the chain carboxylic acid ester compound includes at least one of methyl formate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, or ethyl butyrate. By selecting the above-mentioned chain carboxylic acid ester compounds, the obtained electrolyte has high conductivity and low viscosity, which is conducive to the rapid transmission of lithium ions, thereby reducing the impedance of the secondary battery, reducing the charging temperature rise during fast charging of the secondary battery, shortening the charging time, and having good dynamic performance and cycle performance.
[0011] In some embodiments of the present application, the organic solvent further comprises at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone or tetrahydrofuran, and the mass percentage of the organic solvent is 60% to 80% based on the mass of the electrolyte. By regulating the type and mass percentage of the organic solvent within the scope of the present application, it is beneficial to improve the stability of the electrolyte, thereby improving the kinetic performance and cycle performance of the secondary battery.
[0012] In some embodiments of the present application, the mass percentage of lithium salt is 10% to 20% based on the mass of the electrolyte. When the mass percentage of lithium salt is controlled within the above range, the lithium salt has a higher solubility in the electrolyte, so that the electrolyte has a higher conductivity, thereby improving the kinetic performance and cycle performance of the secondary battery.
[0013] In some embodiments of the present application, the lithium salt includes at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium perchlorate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(oxalatoborate) or lithium difluorooxalatoborate. The above-mentioned types of lithium salts can make the electrolyte have a higher conductivity, thereby improving the kinetics and cycle performance of the secondary battery.
[0014] In some embodiments of the present application, the additive includes at least one of succinonitrile, glutaronitrile, pimelonitrile, 1,2-bis(2-cyanoethoxy)ethane, 1,2-bis(2-cyanoethoxy)propane or 1,2,3-tri(2-cyanoethoxy)propane, and the mass percentage of the additive is 2% to 10% based on the mass of the electrolyte. By regulating the type and mass percentage of the additive within the scope of the present application, it is beneficial to form a protective electrolyte membrane (CEI) on the surface of the positive electrode sheet, thereby improving the structural stability of the positive electrode sheet, reducing the occurrence of side reactions in the electrolyte, and thus improving the high temperature safety performance of the secondary battery.
[0015] The second aspect of the present application provides an electric device, which comprises the secondary battery in any one of the above embodiments. Therefore, the electric device has good performance.
[0016] Beneficial effects of this application:
[0017] The present application provides a secondary battery and an electrical device, wherein the electrochemical system is optimized by combining the structural design of the positive electrode tab and the negative electrode tab, the coating weight of the positive electrode active material layer and the negative electrode active material layer, and the composition and content of the electrolyte, so that the structural design of the positive electrode tab and the negative electrode tab, the coating weight of the positive electrode active material layer and the negative electrode active material layer, and the electrolyte have good synergy, and the charging speed of the secondary battery can be improved while taking into account the low charging temperature rise of the secondary battery, thereby improving the dynamic performance and cycle performance of the secondary battery. The electrical device of the present application has good performance in use. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The drawings described herein are used to provide further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute improper limitations on the present application.
[0019] Figure 1 A schematic diagram of the structure of an electrode assembly according to an embodiment of the present application;
[0020] Figure 2 A schematic diagram of the structure of an electrode assembly according to another embodiment of the present application;
[0021] Figure 3 A schematic diagram of the positional relationship between the positive electrode sheet and the negative electrode sheet along the thickness direction of the positive electrode sheet in one embodiment of the present application;
[0022] Figure 4 A schematic diagram of the structure of a positive electrode sheet according to an embodiment of the present application;
[0023] Figure 5 This is a schematic diagram of the structure of a negative electrode plate according to an implementation scheme of the present application.
[0024] Figure numerals: electrode assembly 001; positive electrode plate 10; positive electrode current collector 11; positive electrode active material layer 12; positive electrode tab 13; negative electrode plate 20; negative electrode current collector 21; negative electrode active material layer 22; negative electrode tab 23; isolation membrane 30; positive electrode tab region 111; positive electrode main body region 112; negative electrode tab region 211; negative electrode main body region 212. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical scheme, and advantages of the present application more clearly understood, the present application is further described in detail with reference to the accompanying drawings and examples. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by those skilled in the art based on the present application belong to the scope of protection of the present application.
[0026] It should be noted that in the invention content of the present application, lithium ion batteries are used as an example of secondary batteries to explain the present application, but the secondary batteries of the present application are not limited to lithium ion batteries, and can also be applied to secondary batteries such as sodium ion batteries.
[0027] The first aspect of the present application provides a secondary battery, the secondary battery comprising a positive electrode sheet, a negative electrode sheet and an electrolyte, the positive electrode sheet comprising a positive electrode current collector and a positive electrode active material layer, the negative electrode sheet comprising a negative electrode current collector and a negative electrode active material layer. The coating weight of the positive electrode active material layer is W z , the coating weight of the negative electrode active material layer is W f , W z and W f Between: 1.6W f ≤W z ≤2.2W f 、3.25mg / cm 2 ≤W f ≤5.84mg / cm 2 For example, W f 3.25mg / cm 2 、3.5mg / cm 2 、3.75mg / cm 2 , 4mg / cm 2, 4.25mg / cm 2 , 4.5mg / cm 2 , 4.75mg / cm 2 , 5mg / cm 2 , 5.25mg / cm 2 , 5.5mg / cm 2 , 5.84mg / cm 2 Or a range consisting of any two of the values. The positive electrode current collector extends integrally to form a plurality of positive electrode tabs, and the negative electrode current collector extends integrally to form a plurality of negative electrode tabs. The electrolyte includes an organic solvent, a lithium salt and an additive, and the organic solvent includes a chain carboxylate compound. Based on the mass of the electrolyte, the mass percentage of the chain carboxylate compound is 6% to 56%, for example, the mass percentage of the chain carboxylate compound is 6%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 56% or a range consisting of any two of the values.
[0028] In this application, for ease of understanding, the positive electrode sheet is defined as having a length direction of X, a width direction of Y, and a thickness direction of Z in the unfolded state. It can be understood that the length direction, width direction, and thickness direction of the negative electrode sheet and the separator are the same as those of the positive electrode sheet in the unfolded state. After the positive electrode sheet, the separator, and the negative electrode sheet are wound to form an electrode assembly with a wound structure, the winding direction of the electrode assembly is W. Figures 1 to 5 As shown, along the winding direction W of the electrode assembly 001, the electrode assembly 001 includes a positive electrode sheet 10, a negative electrode sheet 20 and a separator 30. Along the thickness direction Z of the positive electrode sheet, the positive electrode sheet 10 includes a positive electrode collector 11 and a positive electrode active material layer 12 located on both surfaces of the positive electrode collector. The negative electrode sheet 20 includes a negative electrode collector 21 and a negative electrode active material layer 22 located on both surfaces of the negative electrode collector. The separator 30 is located between the positive electrode sheet 10 and the negative electrode sheet 20. Figure 4 As shown, the positive electrode sheet 10 includes a positive electrode collector 11, and the positive electrode collector 11 extends integrally to form a plurality of positive electrode tabs 12, wherein the positive electrode collector 11 includes a positive electrode tab region 111 and a positive electrode main region 112. It can be understood that the positive electrode tab region 111 is a region where the positive electrode tab 12 is provided, and the positive electrode main region 112 refers to the region of the positive electrode collector 11 other than the positive electrode tab region 111. Figure 5As shown, the negative electrode plate 20 includes a negative electrode current collector 21, and the negative electrode current collector 21 extends integrally to form a plurality of negative electrode tabs 22, wherein the negative electrode current collector 21 includes a negative electrode tab region 211 and a negative electrode main body region 212. It can be understood that the negative electrode tab region 211 refers to a region where the negative electrode tab 22 is provided, and the negative electrode main body region 212 refers to a region of the negative electrode current collector 21 other than the negative electrode tab region 211. In the present application, the above-mentioned "integrated extension" refers to the integral molding of the current collector and the tabs. For example, a plurality of tabs can be cut out on the current collector by die-cutting or laser, rather than connecting the tabs to the current collector by welding or other means. It should be noted that Figure 1 , Figure 2 , Figure 4 and Figure 5 The number, shape and size of the positive pole tabs and the negative pole tabs are only illustrative, and the present application is not limited thereto. In the present application, the above-mentioned "multiple" refers to two or more. In one embodiment of the present application, multiple refers to 2 to the same number as the number of pole sheet layers. Exemplarily, multiple can be 2, 3, 4, 5, 6, 7, 10, 15, 20, 25, 30.
[0029] At present, the market mostly adopts the embedded single-pole ear design, that is, there is only one positive electrode ear and one negative electrode ear in the secondary battery. The positive electrode ear is welded to the positive electrode sheet, and the negative electrode ear is welded to the negative electrode sheet, which leads to crowding of the current channel in the positive electrode sheet or the negative electrode sheet, which is not conducive to the conduction of current, resulting in excessive internal resistance of the lithium-ion battery, increased temperature rise during fast charging of the lithium-ion battery, and poor dynamic performance. Compared with the conventional single-pole ear structure, the present application integrally forms a plurality of positive electrode current collector positions in the empty foil area of the positive electrode sheet, and integrally forms a plurality of negative electrode current collector positions in the empty foil area of the negative electrode sheet. Through the above-mentioned arrangement, multiple current channels are generated on the positive electrode sheet and the negative electrode sheet, so that the impedance of the secondary battery is reduced, the voltage polarization during fast charging of the secondary battery is smaller, the charging temperature rise of the secondary battery is reduced, the charging time of the secondary battery is shortened, and the requirements of fast charging are met. The coating weight of the positive active material layer is less than 1.6W f The coating weight of the negative electrode active material layer is too large relative to the coating weight of the positive electrode active material layer. When the potential of the secondary battery is reached, the lithium removal rate of the positive electrode increases significantly, resulting in a very high actual potential of the positive electrode and easy destruction of the structure. The positive electrode decays rapidly, resulting in the inability of the secondary battery to cycle normally; the coating weight of the positive electrode active material layer is greater than 2.2W f The coating weight of the positive electrode active material layer is too large relative to the coating weight of the negative electrode active material layer. Excessive lithium ions are released, and the negative electrode cannot accept all the lithium ions released from the positive electrode. The lithium ions cannot be normally embedded in the negative electrode sheet, which will cause lithium deposition on the negative electrode sheet and affect the cycle dynamics performance of the secondary battery. The coating weight of the negative electrode active material layer is less than 3.25 mg / cm2 , the energy density of the secondary battery is reduced, the service life is reduced, and it is difficult to meet the process requirements of the secondary battery; the coating weight of the negative electrode active material layer is greater than 5.84 mg / cm 2 , the transmission distance of lithium ions inside the positive electrode sheet and / or the negative electrode sheet increases, and the impedance of the secondary battery increases. By regulating the coating weight of the positive electrode active material layer and the negative electrode active material layer within the above range, the thickness of the positive electrode active material layer and the negative electrode active material layer can be reduced, the porosity of the positive electrode active material layer and the negative electrode active material layer can be increased, and the transmission distance of lithium ions and electrons inside the positive electrode sheet and the negative electrode sheet can be shortened, thereby reducing the ohmic polarization and concentration polarization of the secondary battery, improving the fast charging performance, and making the secondary battery have higher kinetic performance. In order to adapt to the high kinetic performance of the secondary battery, higher requirements are put forward for the electrolyte in the secondary battery. The lithium ion transmission speed in the conventional electrolyte is slow under the high kinetic system of the secondary battery, resulting in a slow charging speed of the secondary battery, and lithium is easily precipitated during the cycle, resulting in reduced cycle performance of the secondary battery. By regulating the composition of the electrolyte and the mass percentage of the chain carboxylic acid ester compound within the scope of the present application, the electrolyte has high conductivity and low viscosity, which can accelerate the transmission speed of lithium ions, further reduce the electrochemical polarization and concentration polarization of the secondary battery, and improve the cycle performance while taking into account the high kinetic performance of the secondary battery.
[0030] The present application optimizes the electrochemical system by combining the structural design of the positive and negative electrode tabs, the coating weight of the positive and negative electrode active material layers, and the composition and content of the electrolyte. On the basis of increasing the charging speed of the secondary battery, the low charging temperature rise of the secondary battery is taken into account, and the fast charging dynamics requirements of the secondary battery are met while improving the cycle performance. The present application can adjust the mass percentage of the chain carboxylate compound by adjusting the amount of the chain carboxylate compound added to the electrolyte.
[0031] The secondary battery of the present application can be used under fast charging conditions, specifically, can be used at a charging rate of 5C to 15C. For example, the charging rate of the secondary battery is 5C, 8C, 10C, 12C, 15C or a range consisting of any two of these values.
[0032] In some embodiments of the present application, 6.49 mg / cm 2 ≤W z ≤11.69mg / cm 2 For example, W z 6.49 mg / cm 2 、7.00mg / cm 2 、7.50mg / cm 2 、8.00mg / cm 2、8.50mg / cm 2 、9.00mg / cm 2 , 9.50mg / cm 2 、10.00mg / cm 2 、10.50mg / cm 2 、11.00mg / cm 2 、11.69mg / cm 2 Or a range consisting of any two of the values. The present application adjusts the coating weight of the positive electrode active material layer within the scope of the present application, while taking into account the processing performance and energy density of the secondary battery, shortens the transmission distance of lithium ions and electrons on the positive electrode sheet, which is beneficial to reducing the ohmic polarization and concentration polarization of the secondary battery, thereby reducing the impedance of the secondary battery and making the secondary battery have good cycle performance.
[0033] In some embodiments of the present application, N is provided between two adjacent positive electrode tabs. 1 There is a positive electrode sheet, and N is set between two adjacent negative electrode tabs. 2 Layer negative electrode, N 1 and N 2 Each is independently selected from 0, 1, 2 or 3. Figure 1 As shown, in the wound electrode assembly, two adjacent positive electrode tabs or two adjacent negative electrode tabs are distributed on different layers. From the top to the bottom of the figure, no positive electrode sheet 10 is set between two adjacent positive electrode tabs 12, and no negative electrode sheet 20 is set between two adjacent negative electrode tabs 22. Figure 2 As shown, in the wound electrode assembly, two adjacent positive pole ears or two adjacent negative pole ears are distributed on different layers. From the top to the bottom of the figure, one layer of positive electrode sheet 10 and two layers of positive electrode sheet 10 are respectively arranged between two adjacent positive pole ears 12, and zero layer of negative electrode sheet 20 and three layers of negative electrode sheet 20 are respectively arranged between two adjacent negative pole ears 22. Through the above arrangement, the present application has a sufficient number of positive pole ears and negative pole ears on the positive pole sheet and the negative pole sheet, so that there are multiple current channels on the positive pole sheet and the negative pole sheet, so that the internal resistance of the secondary battery is reduced, the voltage polarization of the secondary battery is smaller during high-rate fast charging, the charging temperature rise is reduced, and the charging time is shortened, so that the secondary battery has good dynamic performance and cycle performance. It can be understood that N 1 and N 2 Adjusting N to 0 can provide more current channels on the positive and negative electrodes, further reduce the internal resistance of the secondary battery, further reduce the charging temperature rise of the fast-charged secondary battery, and further shorten the charging time, thereby further improving the dynamic performance of the fast-charged secondary battery while taking into account the cycle performance and mechanical reliability. However, this will reduce the energy density of the secondary battery to a certain extent. 1 and N2 Adjusting it to 1, 2 or 3 will reduce the number of tabs and increase the internal resistance to a certain extent, but it can increase the battery energy density.
[0034] In one embodiment of the present application, N is provided between two adjacent positive electrode tabs. 1 There is a positive electrode sheet, and N is set between two adjacent negative electrode tabs. 2 Layer negative electrode, N 1 and N 2 Each is independently selected from 0. Figure 1 As shown, in the wound electrode assembly, from top to bottom in the figure, no positive electrode sheet 10 is provided between two adjacent positive electrode tabs 12, and no negative electrode sheet 20 is provided between two adjacent negative electrode tabs 22. 1 and N 2 When the voltage is adjusted to 0, each layer of the positive electrode sheet and the negative electrode sheet in the secondary battery can have a positive electrode ear and a negative electrode ear, so that the positive electrode sheet and the negative electrode sheet have more current channels, which can further reduce the internal resistance of the secondary battery, further reduce the charging temperature rise of the secondary battery, and further shorten the charging time, so that the secondary battery can take into account the cycle performance while further improving its dynamic performance. In this application, N is set between two adjacent positive electrode ears. 1 A layer positive electrode sheet refers to a positive electrode sheet with a double-sided positive electrode active material layer between two adjacent positive electrode tabs, and the number of layers is N. 1 N layer is provided between two adjacent negative electrode tabs. 2 A negative electrode sheet is a sheet with N layers of negative electrode active material layers on both sides between two adjacent negative electrode tabs. 2 layer.
[0035] In some embodiments of the present application, the chain carboxylic acid ester compound includes at least one of methyl formate, methyl acetate, ethyl formate, ethyl acetate, propyl acetate, ethyl propionate, methyl propionate, n-propyl propionate, isopropyl propionate, n-butyl propionate, isobutyl propionate, n-pentyl propionate, isopentyl propionate, ethyl butyrate, n-propyl butyrate, propyl isobutyrate, n-pentyl butyrate, n-pentyl isobutyrate, n-butyl butyrate, isobutyl isobutyrate, and n-pentyl valerate. Preferably, the chain carboxylic acid ester compound includes at least one of methyl formate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, or ethyl butyrate. By selecting the above-mentioned types of chain carboxylic acid ester compounds, the obtained electrolyte has high conductivity and low viscosity, which is conducive to the rapid transmission of lithium ions, reduces the electrochemical polarization and concentration polarization of the secondary battery, reduces the charging temperature rise and shortens the charging time during fast charging of the secondary battery, and has good kinetic performance and cycle performance.
[0036] In some embodiments of the present application, the organic solvent also includes at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone or tetrahydrofuran, and the mass percentage of the organic solvent is 60% to 80% based on the mass of the electrolyte. For example, the mass percentage of the organic solvent is 60%, 65%, 70%, 75%, 80% or a range consisting of any two of the values. By regulating the type and mass percentage of the organic solvent within the scope of the present application, it is beneficial to improve the solubility of the additive and the lithium salt, while taking into account the kinetic performance of the secondary battery and improving the stability of the electrolyte, thereby improving the kinetic performance and cycle performance of the secondary battery. The present application can regulate the mass percentage of the organic solvent by regulating the amount of the organic solvent added to the electrolyte. The mass percentage of non-chain carboxylic acid ester compounds in the organic solvent = the mass percentage of the organic solvent - the mass percentage of the chain carboxylic acid ester compounds.
[0037] In some embodiments of the present application, the mass percentage of the lithium salt is 10% to 20% based on the mass of the electrolyte. For example, the mass percentage of the lithium salt is 10%, 12%, 14%, 16%, 18%, 20% or a range consisting of any two of these values. The mass percentage of the lithium salt is regulated within the above range, and the lithium salt has a higher solubility in the electrolyte, so that the electrolyte has a higher conductivity, thereby improving the kinetic performance and cycle performance of the secondary battery. The present application can regulate the mass percentage of the lithium salt by regulating the amount of lithium salt added to the electrolyte.
[0038] In some embodiments of the present application, the lithium salt includes at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium perchlorate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(oxalatoborate) or lithium difluorooxalatoborate. The above-mentioned types of lithium salts can make the electrolyte have a higher conductivity, thereby improving the kinetics and cycle performance of the secondary battery.
[0039] In some embodiments of the present application, the additive includes at least one of succinonitrile, glutaronitrile, pimelonitrile, 1,2-bis(2-cyanoethoxy)ethane, 1,2-bis(2-cyanoethoxy)propane or 1,2,3-tris(2-cyanoethoxy)propane, and the mass percentage of the additive is 2% to 10% based on the mass of the electrolyte. For example, the mass percentage of the additive is 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or a range consisting of any two of the values. By regulating the type and mass percentage of the additive within the scope of the present application, the cyano group in the nitrile compound can be complexed with the transition metal element ions in the positive electrode sheet to form a CEI film on the surface of the positive electrode sheet, thereby improving the structural stability of the positive electrode sheet and reducing the side reactions between the positive active material and the electrolyte, thereby improving the high temperature safety performance of the secondary battery. The present application can regulate the mass percentage of the additive by regulating the amount of the additive added to the electrolyte.
[0040] The present application has no particular restrictions on the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the positive electrode current collector may include aluminum foil, aluminum alloy foil or a composite current collector (such as an aluminum-carbon composite current collector), etc. The positive electrode active material layer of the present application includes positive electrode active materials. The present application has no particular restrictions on the type of positive electrode active materials, as long as the purpose of the present application can be achieved. For example, the positive electrode active material may include lithium nickel cobalt manganese oxide (NCM811, NCM622, NCM523, NCM111), lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide (LiCoO 2)、at least one of lithium manganate, lithium iron manganese phosphate, or lithium titanate, etc. In the present application, the positive electrode active material may further contain a non-metal element. For example, the non-metal element includes at least one of fluorine, phosphorus, boron, chlorine, silicon, or sulfur. In the present application, there is no particular limitation on the thickness of the positive electrode current collector and the positive electrode active material layer, as long as the object of the present application can be achieved. For example, the thickness of the positive electrode current collector is 5 μm to 20 μm, preferably 6 μm to 18 μm. The thickness of the single-sided positive electrode material layer is 30 μm to 120 μm. In the present application, the positive electrode active material layer may further include a conductive agent and a binder. The present application has no particular limitation on the type of the binder in the positive electrode active material layer, as long as the object of the present application can be achieved. For example, the binder may include, but is not limited to, at least one of polyvinylidene fluoride, copolymer of vinylidene fluoride - hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate salt, polyvinylpyrrolidone, polyethylene ether, polymethyl methacrylate, polytetrafluoroethylene, or polyhexafluoropropylene. The present application has no particular limitation on the type of the conductive agent in the positive electrode active material layer, as long as the object of the present application can be achieved. For example, the conductive agent may include, but is not limited to, at least one of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon fiber, flake graphite, Ketjen black, graphene, metal material, or conductive polymer. The above carbon nanotubes may include, but are not limited to, single-walled carbon nanotubes and / or multi-walled carbon nanotubes. The above carbon fiber may include, but is not limited to, vapor grown carbon fiber (VGCF) and / or nanofiber. The above metal material may include, but is not limited to, metal powder and / or metal fiber. Specifically, the metal may include, but is not limited to, at least one of copper, nickel, aluminum, or silver. The above conductive polymer may include, but is not limited to, at least one of polyphenylene derivatives, polyaniline, polythiophene, polyacetylene, or polypyrrole. The present application has no particular limitation on the mass ratio of the positive electrode active material, conductive agent, and binder in the positive electrode active material layer. Those skilled in the art can select according to actual needs as long as the object of the present application can be achieved.
[0041] The present application has no particular limitation on the negative electrode current collector, as long as the object of the present application can be achieved. For example, the negative electrode current collector may include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, or composite current collector (such as lithium copper composite current collector, carbon copper composite current collector, nickel copper composite current collector, titanium copper composite current collector, etc.). The negative electrode active material layer of the present application contains a negative electrode active material. The present application has no particular limitation on the type of the negative electrode active material, as long as the object of the present application can be achieved. For example, the negative electrode active material may include natural graphite, artificial graphite, mesophase microcarbon microbeads (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composite, SiO x (0 < x < 2), Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO 2, spinel structure lithium titanate Li 4 Ti 5 O 12 , Li-Al alloy or at least one of metallic lithium. In the present application, there is no particular restriction on the thickness of the negative electrode current collector and the negative electrode material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the negative electrode current collector is 4μm to 20μm, and the thickness of the negative electrode active material layer is 30μm to 130μm. Optionally, the negative electrode active material layer may also include a conductive agent and a binder. The present application does not particularly limit the type of conductive agent in the negative electrode active material layer, as long as the purpose of the present application can be achieved. For example, the conductive agent may be the same type as the conductive agent in the above-mentioned positive electrode active material layer. The present application does not particularly limit the type of binder in the negative electrode active material layer, as long as the purpose of the present application can be achieved. For example, the binder may be the same type as the binder in the above-mentioned positive electrode active material layer. The present application does not particularly limit the mass ratio of the negative electrode active material, the conductive agent and the binder in the negative electrode active material layer, as long as the purpose of the present application can be achieved.
[0042] There is no particular restriction on the isolation membrane in the secondary battery of the present application, as long as the purpose of the present application can be achieved. For example, the isolation membrane includes at least one of polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polyimide (PI) or aramid. For example, polyethylene includes at least one selected from high-density polyethylene, low-density polyethylene and ultra-high molecular weight polyethylene. The isolation membrane of the present application may have a porous structure. The present application does not particularly limit the size of the pore size of the porous structure of the isolation membrane, as long as the purpose of the present application can be achieved. For example, the size of the pore size can be 0.01μm to 1μm. The present application does not particularly limit the thickness of the isolation membrane, as long as the purpose of the present application can be achieved. For example, the thickness of the isolation membrane can be 5μm to 500μm.
[0043] The secondary battery of the present application also includes a packaging bag for containing a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, as well as other components known in the art in the secondary battery, and the present application does not limit the above other components. The present application does not specifically limit the packaging bag, and it can be a packaging bag known in the art, as long as it can achieve the purpose of the present application.
[0044] The secondary battery of the present application is not particularly limited, and may include any device that undergoes an electrochemical reaction. In one embodiment of the present application, the electrochemical device may include, but is not limited to, a lithium ion secondary battery (lithium ion battery), a lithium polymer secondary battery, or a lithium ion polymer secondary battery.
[0045] The present application has no particular restrictions on the preparation method of the positive electrode sheet, as long as the purpose of the present application can be achieved. For example, the preparation method of the positive electrode sheet includes but is not limited to the following steps: (1) preparing a positive electrode slurry; (2) coating the positive electrode slurry on one surface of the positive electrode main region of the positive electrode current collector, and after drying, forming a positive electrode active material layer on one surface of the positive electrode main region of the positive electrode current collector; (3) coating the positive electrode slurry on the other surface of the positive electrode main region of the positive electrode current collector, and after drying, forming a positive electrode active material layer on each of the two surfaces of the positive electrode main region of the positive electrode current collector; (4) die-cutting the positive electrode ear region of the positive electrode current collector after cold pressing, so that the positive electrode current collector extends integrally to form multiple positive electrode ears; (5) cutting the positive electrode sheet. The present application has no particular restrictions on the content and type of each component in the positive electrode slurry in the above step (2), and those skilled in the art can choose according to actual conditions, as long as the purpose of the present application can be achieved. The present application has no particular restrictions on the solid content of the positive electrode slurry in the above step (1), as long as the coating weight of the obtained positive electrode active material layer is within the scope of the present application and the purpose of the present application can be achieved. The present application has no particular restrictions on the time and temperature of the drying in the above steps (2) and (4), as long as the purpose of the present application can be achieved. The present application has no particular restrictions on the process parameters of the cold pressing in the above step (4), as long as the purpose of the present application can be achieved.
[0046] The present application has no particular restrictions on the method for preparing the negative electrode sheet, as long as the purpose of the present application can be achieved. For example, the method for preparing the negative electrode sheet includes but is not limited to the following steps: (1) preparing the negative electrode slurry; (2) coating the negative electrode slurry on one surface of the negative electrode main region of the negative electrode current collector, and after drying, forming a negative electrode active material layer on one surface of the negative electrode main region of the negative electrode current collector; (3) coating the negative electrode slurry on the other surface of the negative electrode main region of the negative electrode current collector, and after drying, forming a negative electrode active material layer on each of the two surfaces of the negative electrode main region of the negative electrode current collector; (4) die-cutting the negative electrode tab region of the negative electrode current collector after cold pressing, so that the negative electrode current collector extends integrally to form multiple negative electrode tabs; (5) after stripping, the negative electrode sheet is obtained. The present application has no particular restrictions on the content and type of each component in the negative electrode slurry in the above step (1), and those skilled in the art can choose according to actual conditions, as long as the purpose of the present application can be achieved. The present application has no particular restrictions on the solid content of the negative electrode slurry in the above step (1), as long as the coating weight of the obtained negative electrode active material layer is within the scope of the present application and the purpose of the present application can be achieved. The present application has no particular restrictions on the drying time and temperature in the above steps (2) and (3), as long as the purpose of the present application can be achieved. The present application has no particular restrictions on the process parameters of the cold pressing in the above step (4), as long as the purpose of the present application can be achieved.
[0047] The present application does not particularly limit the preparation method of the secondary battery, and a preparation method known in the art can be selected as long as the purpose of the present application can be achieved. For example, the preparation method of the secondary battery includes but is not limited to the following steps: stacking the separator, the positive electrode sheet, the separator and the negative electrode sheet in order, and winding and folding them as needed to obtain an electrode assembly with a wound structure, spot welding multiple positive electrode tabs and multiple negative electrode tabs, placing the electrode assembly in a shell, injecting the electrolyte into the shell and sealing it to obtain a secondary battery.
[0048] The second aspect of the present application provides an electric device, which comprises the secondary battery in any one of the above embodiments. Therefore, the electric device has good performance.
[0049] The electric device of the present application is not particularly limited, and it can be used for any electronic device known in the prior art. For example, the electronic device can include but is not limited to a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery, and a lithium-ion capacitor.
[0050] Example
[0051] Hereinafter, the embodiments of the present application will be described in more detail with reference to Examples and Comparative Examples. Various tests and evaluations were performed according to the following methods.
[0052] Test methods and equipment:
[0053] Coating Weight Test:
[0054] (1) Coating weight W of positive electrode active material layer z test:
[0055] The lithium-ion battery was discharged at 0.5C to 3.0V and then disassembled to obtain the positive electrode sheet. The positive electrode sheet was immersed in dimethyl carbonate (DMC) solution for 4 hours and then dried. The area A mm was cut. 2 The positive electrode sample is placed on a balance and weighed, recorded as p 1 Then wash the positive electrode active material layer on the positive electrode sheet and put the positive electrode current collector on a balance to weigh the weight, which is recorded as p 2 ;
[0056] If the positive electrode sheet is coated with a positive electrode active material layer on one side, Wz =(p 1 -p 2 ) / A.
[0057] If it is a positive electrode sheet with a positive electrode active material layer coated on both sides, W z =(p 1 -p 2 ) / 2A.
[0058] (2) Coating weight W of negative electrode active material layer f test:
[0059] The lithium-ion battery was discharged at 0.5C to 3.0V and then disassembled to obtain the negative electrode sheet. The negative electrode sheet was immersed in DMC solution for 4 hours and then dried. The area B mm was cut. 2 The negative electrode sample is placed on a balance and weighed, recorded as q 1 Then wash the negative electrode active material layer on the negative electrode sheet and put the negative electrode current collector on a balance to weigh the weight, which is recorded as q 2 ;
[0060] If the negative electrode sheet is coated with a negative electrode active material layer on one side, W f =(q 1 -q 2 ) / B.
[0061] If it is a negative electrode sheet with negative electrode active material layer coated on both sides, W f =(q 1 -q 2 ) / 2B.
[0062] Dynamic performance test:
[0063] The lithium ion batteries in the embodiments and comparative examples were subjected to a dynamic performance test under a charging rate of 10C, and the specific steps are as follows:
[0064] The test temperature was adjusted to a constant temperature of 25°C, and the temperature sensing line of the multi-channel thermometer was placed at the center of the surface of the lithium-ion battery. The following steps were performed: (1) 10C constant current charging to 4.20V; (2) 8C constant current charging to 4.35V; (3) 5C constant current charging to 4.45V; (4) 4.45V constant voltage charging to 0.05C; (5) standing for 30 minutes; (6) 1C constant current discharge to 3.0V; (7) standing for 30 minutes; end.
[0065] Charging speed: the time from step (1) to step (4) in step (1);
[0066] Charging temperature rise: the difference between the maximum temperature of the process from step (1) to step (2) in step (1) recorded by the temperature sensing line on the surface of the lithium-ion battery and the room temperature.
[0067] The kinetic performance is characterized by charging speed, charging temperature rise and lithium-ion battery impedance. Among them, the lower the lithium-ion battery impedance, the shorter the charging time and the smaller the charging temperature rise, the better the kinetic performance.
[0068] Cycle performance test:
[0069] The lithium ion batteries in the embodiments and comparative examples were subjected to a cycle performance test under a charging rate of 10C, and the specific steps are as follows:
[0070] Adjust the test temperature to 25°C and start the test: (1) 10C constant current charging to 4.20V; (2) 8C constant current charging to 4.35V; (3) 6C constant current charging to 4.40V; (4) 4.40V constant voltage charging to 0.05C; (5) stand for 5 minutes; (6) 1C constant current discharge to 3.0V; (7) stand for 5 minutes; (8) process steps (1) to (7) cycle 1000 times (cls); end;
[0071] Capacity retention rate (%) = discharge capacity after 1000 cycles / first cycle discharge capacity × 100%.
[0072] Example 1-1
[0073] <Preparation of positive electrode sheet>
[0074] The positive electrode active material is lithium cobalt oxide, the positive electrode conductive agent is superconducting carbon (Super P), and the positive electrode binder is polyvinylidene fluoride (PVDF, Mw = 70 × 10 5 ) are mixed in a mass ratio of 95:2.5:2.5, N-methylpyrrolidone (NMP) is added as a solvent, and stirred under the action of a vacuum mixer until the solid content is 75wt% and the system is uniform. The positive electrode slurry is evenly coated on the positive electrode main body area on one surface of the positive electrode current collector aluminum foil with a thickness of 13μm, and dried at 95°C to obtain a positive electrode sheet coated with a single-sided positive electrode active material layer. After that, the above steps are repeated on the positive electrode main body area on the other surface of the aluminum foil to obtain a positive electrode sheet coated with a double-sided positive electrode active material layer. After cold pressing, die-cutting, and slitting, after slitting, it is dried at 85°C for 4h to obtain a positive electrode sheet with a specification of 60mm×1580mm for standby use. Among them, the single-layer thickness of the positive electrode active material layer is 38.5μm, and the thickness of the positive electrode sheet is 90μm. The positive electrode ear area of the positive current collector is integrally formed by die-cutting (see the structure Figure 4 , but not Figure 4 20 positive electrode tabs are formed, and the coating weight of the positive electrode active material layer is W z 9.08mg / cm 2 .
[0075] <Preparation of negative electrode sheet>
[0076] The negative electrode active material artificial graphite, negative electrode conductive agent Super P, stabilizer sodium carboxymethyl cellulose (CMC-Na, Mw = 7 × 10 5 ), negative electrode binder styrene butadiene rubber (SBR, Mw = 50 × 10 5 ) are mixed according to a mass ratio of 96:1.0:1.5:1.5, and then deionized water is added as a solvent, and stirred under the action of a vacuum mixer until the solid content is 51wt% and the system is uniform. The negative electrode slurry is evenly coated on the negative electrode main body area on one surface of the negative electrode current collector copper foil with a thickness of 10μm, and dried at 85°C to obtain a negative electrode pole piece coated with a single-sided negative electrode active material layer. After that, the above steps are repeated on the negative electrode main body area on the other surface of the copper foil to obtain a negative electrode pole piece coated with a negative electrode active material layer on both sides. After cold pressing, die cutting, and slitting, after slitting, it is dried at 110°C for 4h to obtain a negative electrode pole piece with a specification of 62mm×1600mm for standby use. Among them, the single layer thickness of the negative electrode active material layer is 58.5μm, and the thickness of the negative electrode pole piece is 127μm. The negative electrode ear area of the negative electrode current collector is integrally formed by die cutting (see the structure Figure 5 , but not Figure 5 20 negative electrode tabs are formed, and the coating weight of the negative electrode active material layer is W f 4.54 mg / cm 2 .
[0077] <Preparation of Electrolyte>
[0078] In a dry argon atmosphere glove box, a chain carboxylic acid ester compound n-propyl propionate and a non-chain carboxylic acid ester compound ethylene carbonate and diethyl carbonate were used as organic solvents, and lithium salt lithium hexafluorophosphate (LiPF 6 ) and the additive succinonitrile are dissolved and mixed uniformly to obtain an electrolyte. Based on the mass of the electrolyte, the mass percentage of n-propyl propionate is 40%, the mass percentage of the organic solvent is 80%, and the mass percentage of LiPF 6 The mass percentage of ethylene carbonate is 17%, the mass percentage of succinonitrile is 3%, and the mass percentage ratio of ethylene carbonate to diethyl carbonate is 1:1.
[0079] <Preparation of Separator Film>
[0080] A polypropylene film with a thickness of 5 μm was selected as the isolation membrane.
[0081] <Preparation of lithium-ion batteries>
[0082] Stack the separator, positive electrode sheet, separator, and negative electrode sheet in order, so that the separator is between the positive electrode sheet and the negative electrode sheet to play a role of isolation, and then wind to obtain an electrode assembly. The positive electrode tab is spot welded out with an aluminum tab, and the negative electrode tab is spot welded out with a nickel tab. Among them, after winding, there is one positive electrode tab on each layer of positive electrode sheet with positive electrode tabs, and one negative electrode tab on each layer of negative electrode sheet with negative electrode tabs, and N is set between two adjacent positive electrode tabs. 1 = 0 positive electrode sheet, N is set between two adjacent negative electrode tabs 2 = 0 negative electrode sheet (for the setting of positive and negative electrodes, see Figure 1 , but not Figure 1 limited).
[0083] The electrode assembly is placed in an aluminum-plastic film shell, and after drying, the electrolyte is injected, and the lithium-ion battery is obtained through vacuum packaging, standing, formation, capacity, degassing, trimming and other processes.
[0084] Example 1-2 to Example 1-12
[0085] Except for adjusting the relevant preparation parameters according to Table 1, the rest is the same as Example 1-1. When the content of the chain carboxylic acid ester compound in the electrolyte changes, the content of the organic solvent remains unchanged, and the content of the non-chain carboxylic acid ester compounds ethylene carbonate and diethyl carbonate in the organic solvent changes accordingly, wherein the mass percentage ratio of ethylene carbonate to diethyl carbonate remains unchanged at 1:1.
[0086] Examples 1-13
[0087] <Preparation of positive electrode sheet>
[0088] Except that the positive electrode tab region of the positive electrode current collector is integrally extended to form 10 positive electrode tabs, the rest is the same as Example 1-1.
[0089] <Preparation of negative electrode sheet>
[0090] Except that the negative electrode tab region of the negative electrode current collector is integrally extended to form 10 negative electrode tabs, the rest is the same as Example 1-1.
[0091] <Preparation of lithium-ion batteries>
[0092] In addition to the N 1 = 1 layer of positive electrode sheet, N is set between two adjacent negative electrode tabs 2 =1 layer of negative electrode sheet, the rest is the same as Example 1-1.
[0093] <Preparation of separator> and <Preparation of electrolyte> were the same as those in Example 1-1.
[0094] Examples 1-14
[0095] <Preparation of positive electrode sheet>
[0096] Except that the positive electrode tab region of the positive electrode current collector is integrally extended to form 6 positive electrode tabs, the rest is the same as Example 1-1.
[0097] <Preparation of negative electrode sheet>
[0098] Except that the negative electrode tab region of the negative electrode current collector is integrally extended to form 6 negative electrode tabs, the rest is the same as Example 1-1.
[0099] <Preparation of lithium-ion batteries>
[0100] In addition to the N 1 = 2 layers of positive electrode sheets, N is set between two adjacent negative electrode tabs 2 =2 layers of negative electrode sheets, the rest are the same as Example 1-1.
[0101] <Preparation of separator> and <Preparation of electrolyte> were the same as those in Example 1-1.
[0102] Example 2-1 to Example 2-8
[0103] Except for adjusting the relevant preparation parameters according to Table 2, the rest is the same as Example 1-1. Among them, when the type of non-chain carboxylic acid ester compounds in the organic solvent changes, the content ratio between the non-chain carboxylic acid ester compounds does not change. When the content of the organic solvent changes, the content of the chain carboxylic acid ester compounds in the organic solvent remains unchanged, and the content of the non-chain carboxylic acid ester compounds in the organic solvent changes accordingly, and the mass ratio of the two substances in the non-chain carboxylic acid ester compounds remains unchanged at 1:1.
[0104] Embodiment 2-9
[0105] Except that no additives are added in <Preparation of Electrolyte> and relevant preparation parameters are adjusted according to Table 2, the rest is the same as Example 1-1. Among them, when the content of the organic solvent changes, the content of the chain carboxylic acid ester compound in the organic solvent remains unchanged, and the content of the non-chain carboxylic acid ester compounds ethylene carbonate and diethyl carbonate in the organic solvent changes accordingly, wherein the mass percentage ratio of ethylene carbonate to diethyl carbonate remains unchanged at 1:1.
[0106] Embodiment 2-10
[0107] Except for adjusting the relevant preparation parameters according to Table 2, the rest is the same as Example 1-1.
[0108] Comparative Examples 1 to 4
[0109] Except for adjusting the relevant preparation parameters according to Table 1, the rest is the same as Example 1-1.
[0110] Comparative Example 5
[0111] Except that the following preparation steps are adopted for <Preparation of Electrolyte>, the rest is the same as Example 1-1.
[0112] <Preparation of Electrolyte>
[0113] In a dry argon atmosphere glove box, non-chain carboxylic acid ester compounds ethylene carbonate and diethyl carbonate were used as organic solvents, and lithium salt lithium hexafluorophosphate (LiPF 6 ) and the additive succinonitrile are dissolved and mixed uniformly to obtain an electrolyte. Based on the mass of the electrolyte, the mass percentage of the organic solvent is 80%, LiPF 6 The mass percentage of ethylene carbonate is 17%, the mass percentage of succinonitrile is 3%, and the mass percentage ratio of ethylene carbonate to diethyl carbonate is 1:1.
[0114] Comparative Example 6 to Comparative Example 7
[0115] Except for adjusting the relevant preparation parameters according to Table 1, the rest is the same as Example 1-1. When the content of the chain carboxylic acid ester compound in the electrolyte changes, the content of the organic solvent remains unchanged, and the content of the non-chain carboxylic acid ester compounds ethylene carbonate and diethyl carbonate in the organic solvent changes accordingly, wherein the mass percentage ratio of ethylene carbonate to diethyl carbonate remains unchanged at 1:1.
[0116] Comparative Example 8
[0117] Except that the following preparation steps are adopted for <Preparation of positive electrode sheet>, <Preparation of negative electrode sheet>, and <Preparation of lithium-ion battery>, the rest are the same as Example 1-1.
[0118] <Preparation of positive electrode sheet>
[0119] The positive electrode active material is lithium cobalt oxide, the positive electrode conductive agent is superconducting carbon (Super P), and the positive electrode binder is polyvinylidene fluoride (PVDF, Mw = 70 × 10 5) are mixed in a mass ratio of 96:2:2, N-methylpyrrolidone (NMP) is added as a solvent, and stirred under the action of a vacuum mixer until the solid content is 75wt% and the system is uniform. The positive electrode slurry is evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 13μm, and dried at 95°C to obtain a positive electrode sheet with a single-sided positive electrode active material layer. After that, the above steps are repeated on the other surface of the aluminum foil to obtain a positive electrode sheet with a double-sided positive electrode active material layer. Then it is cold pressed, cut into pieces, and striped. After stripping, it is dried at 85°C for 4h, and a positive electrode aluminum ear is welded on the surface of the positive electrode collector to obtain a positive electrode sheet with a specification of 60mm×1580mm for standby use. Among them, the single layer thickness of the positive electrode active material layer is 38.5μm, and the thickness of the positive electrode sheet is 90μm. The coating weight W of the positive active material layer z 9.08mg / cm 2 .
[0120] <Preparation of negative electrode sheet>
[0121] The negative electrode active material artificial graphite, negative electrode conductive agent Super P, stabilizer sodium carboxymethyl cellulose (CMC-Na, Mw = 7 × 10 5 ), negative electrode binder styrene butadiene rubber (SBR, Mw = 50 × 10 5 ) are mixed according to a mass ratio of 96.5:1.0:1.0:1.5, and then deionized water is added as a solvent, and stirred under the action of a vacuum mixer until the solid content is 51wt% and the system is uniform. The negative electrode slurry is evenly coated on one surface of a negative electrode current collector copper foil with a thickness of 10μm, and dried at 85°C to obtain a negative electrode sheet with a single-sided negative electrode active material layer. After that, the above steps are repeated on the other surface of the copper foil to obtain a negative electrode sheet with a double-sided negative electrode active material layer. Then it is cold pressed, cut into pieces, and striped. After stripping, it is dried at 110°C for 4h, and a negative electrode ear nickel ear is welded on the surface of the negative electrode current collector to obtain a negative electrode sheet with a specification of 62mm×1600mm for standby use. Among them, the single layer thickness of the negative electrode active material layer is 58.5μm, and the thickness of the negative electrode sheet is 127μm. The coating weight W of the negative electrode active material layer f 4.54 mg / cm 2 .
[0122] <Preparation of lithium-ion batteries>
[0123] The separator, positive electrode sheet, separator, and negative electrode sheet are stacked in order, so that the separator is between the positive electrode sheet and the negative electrode sheet to play a role of isolation, and then wound to obtain an electrode assembly. The electrode assembly is placed in an aluminum-plastic film shell, and after drying, the electrolyte is injected, and the lithium-ion battery is obtained through vacuum packaging, standing, formation, capacity, degassing, trimming and other processes.
[0124] Comparative Example 9
[0125] Except that <Preparation of electrolyte> is the same as Comparative Example 5, the rest is the same as Comparative Example 8.
[0126] Comparative Example 10
[0127] Except for adjusting the relevant preparation parameters according to Table 1, the rest is the same as Comparative Example 5.
[0128] Comparative Example 11
[0129] Except for adjusting the relevant preparation parameters according to Table 1, the rest is the same as Comparative Example 9.
[0130] The preparation parameters and performance parameters of each embodiment and comparative example are shown in Tables 1 and 2.
[0131] Table 1
[0132]
[0133]
[0134] Note: “ / ” in Table 1 means there is no corresponding parameter.
[0135] It can be seen from Examples 1-1 to 1-14 and Comparative Examples 1 to 11 that the lithium-ion battery of the present application embodiment has a multi-electrode structure by providing a positive electrode current collector integrally extending to form a plurality of positive electrode tabs and a negative electrode current collector integrally extending to form a plurality of negative electrode tabs. At the same time, the coating weight W of the positive electrode active material layer is adjusted. z The coating weight W of the negative electrode active material layer f The ratio W z / W f and W f The value of is within the scope of the present application, and a chain carboxylate compound is added to the electrolyte to regulate the mass percentage of the chain carboxylate compound within the scope of the present application. The lithium-ion battery has lower impedance, shorter charging time (i.e., higher charging speed), lower charging temperature rise and higher capacity retention rate at a charging rate of 10C, indicating that the lithium-ion battery in the embodiment of the present application has better kinetic performance and cycle performance during fast charging.
[0136] In the lithium ion batteries of Comparative Examples 1 and 2, the coating weight W of the negative electrode active material layer is f Not within the scope of this application, the lithium ion batteries in Comparative Examples 3 to 4, the coating weight W of the positive electrode active material layer z The coating weight W of the negative electrode active material layer f The ratio W z / Wf It is not within the scope of this application. The coating weight W of the positive electrode active material layer of Comparative Example 1 z The coating weight W of the negative electrode active material layer f The obtained lithium-ion battery has a faster charging speed and lower impedance, but because the coating weight of the positive electrode active material layer and the negative electrode active material layer is too low, the cost of accurately controlling the coating weight in actual industrial production is too high, and the qualified rate of lithium-ion batteries obtained in large-scale production is too low and the energy density of the obtained lithium-ion batteries is too low, which cannot meet the needs of actual production and is not suitable for industrial production applications. The lithium-ion battery in Comparative Example 2 has a higher impedance, a longer charging time (that is, a lower charging speed), a higher charging temperature rise, and a lower capacity retention rate at a charging rate of 10C, indicating that the lithium-ion battery has poor kinetic performance and cycle performance during high-rate fast charging. The coating weight W of the positive electrode active material layer of Comparative Example 3 is z The coating weight of the negative electrode active material layer is too large relative to the coating weight of the positive electrode active material layer. When the potential of the secondary battery is reached, the lithium removal rate of the positive electrode increases significantly, resulting in a high actual potential of the positive electrode and easy destruction of the structure. The positive electrode decays rapidly, resulting in a very poor cycle life of the secondary battery. z Too large and with the coating weight W of the negative electrode active material layer f The ratio W z / W fToo large, resulting in a mismatch between the capacity of the positive electrode sheet and the negative electrode sheet. When the lithium-ion battery is fast charged, the lithium ions in the positive electrode sheet cannot be removed in time, and the lithium ions cannot be embedded in the negative electrode sheet in time, which cannot meet the charging speed requirements during fast charging, and is prone to lithium precipitation. The capacity retention rate is low, and the cycle performance of the lithium-ion battery is poor. The electrolyte in Comparative Example 5 does not add chain carboxylic acid ester compounds, and the mass percentage of chain carboxylic acid ester compounds in Comparative Examples 6 and 7 is not within the scope of this application. The lithium-ion batteries in Comparative Examples 5 and 6 have higher impedance, longer charging time (that is, lower charging speed), higher charging temperature rise and lower capacity retention rate at a charging rate of 10C, indicating that the lithium-ion battery has poor kinetic performance and cycle performance during fast charging. In Comparative Example 7, due to the excessively high mass percentage of chain carboxylic acid ester compounds, the battery system is too active, and side reactions are prone to occur during the cycle process, resulting in a decrease in capacity retention rate, and the cycle performance of the lithium-ion battery is poor. The lithium-ion battery in Comparative Example 8 has an embedded single-pole structure rather than the multi-pole structure of the present application. The obtained lithium-ion battery has a higher impedance, a longer charging time (that is, a lower charging speed), a higher charging temperature rise, and a lower capacity retention rate at a charging rate of 10C, indicating that the lithium-ion battery has poor kinetic performance and cycle performance during fast charging. The electrolyte in Comparative Example 9 does not add chain carboxylic acid ester compounds, and the lithium-ion battery has an embedded single-pole structure rather than the multi-pole structure of the present application. The obtained lithium-ion battery has a higher impedance, a longer charging time (that is, a lower charging speed), a higher charging temperature rise, and a lower capacity retention rate at a charging rate of 10C, indicating that the lithium-ion battery has poor kinetic performance and cycle performance during fast charging. For the lithium-ion battery in Comparative Example 10, the coating weight W of the positive electrode active material layer z The coating weight W of the negative electrode active material layer f The ratio W z / W f It is not within the scope of this application that the electrolyte does not add chain carboxylic acid ester compounds. The obtained lithium ion battery has higher impedance, longer charging time (i.e., lower charging speed), higher charging temperature rise and lower capacity retention rate at a charging rate of 10C, indicating that the lithium ion battery has poor kinetic performance and cycle performance during fast charging. In the lithium ion battery in Comparative Example 11, the coating weight W of the positive electrode active material layer is z The coating weight W of the negative electrode active material layer f The ratio W z / W fIt is not within the scope of the present application. The electrolyte does not add chain carboxylic acid ester compounds, and the lithium-ion battery has an embedded single-pole structure rather than the multi-pole structure of the present application. The obtained lithium-ion battery has higher impedance, longer charging time (i.e., lower charging speed), higher charging temperature rise and lower capacity retention rate at a charging rate of 10C, indicating that the lithium-ion battery has poor kinetic performance and cycle performance during fast charging.
[0137] The coating weight W of the positive electrode active material layer z Usually it will affect the dynamic performance and cycle performance of lithium-ion batteries during high-rate fast charging. z The lithium-ion battery within the scope of the present application has lower impedance, shorter charging time (i.e., higher charging speed), lower charging temperature rise, and higher capacity retention rate at a charging rate of 10C, indicating that the lithium-ion battery has better kinetic performance and cycle performance during fast charging. The coating weight W of the positive electrode active material layer in Examples 1-6 is z The coating weight of the negative electrode active material layer is relatively low, and the coating weight of the positive electrode active material layer is slightly different from that of the positive electrode active material layer. When the potential of the secondary battery is reached, the delithiation rate of the positive electrode increases, which may lead to the occurrence of over-delithiation of the positive electrode, thereby reducing the capacity retention rate of the lithium-ion battery. Furthermore, although the charging speed of lithium-ion batteries is fast and the impedance is low, the energy density of lithium-ion batteries is low. In actual industrial production, it is difficult to control the coating weight of the positive electrode active material layer. In Examples 1-7, the coating weight W of the positive electrode active material layer is z The coating weight of the negative electrode active material layer is relatively high, and the coating weight of the positive electrode active material layer is quite different from that of the positive electrode active material layer. When the lithium-ion battery is fast charged, the lithium ions in the positive electrode sheet cannot be removed in time, and the lithium ions cannot be embedded in the negative electrode sheet in time, which easily leads to the occurrence of lithium precipitation, thereby reducing the capacity retention rate of the lithium-ion battery. The type of chain carboxylic acid ester compound usually affects the kinetics and cycle performance of lithium-ion batteries during high-rate fast charging. It can be seen from Example 1-1, Example 1-11 to Example 1-12 that the lithium-ion battery whose type of chain carboxylic acid ester compound is within the scope of this application has a lower impedance, a shorter charging time (that is, a higher charging speed), a lower charging temperature rise and a higher capacity retention rate at a charging rate of 10C, indicating that the lithium-ion battery has better kinetics during fast charging.
[0138] N 1 and N 2 The value of usually affects the dynamic performance and cycle performance of lithium-ion batteries during fast charging. 1 and N 2The lithium-ion battery whose value is within the scope of the present application has lower impedance, shorter charging time (i.e., higher charging speed), lower charging temperature rise and higher capacity retention rate at a charging rate of 10C, indicating that the lithium-ion battery has better kinetic performance and cycle performance during fast charging.
[0139] Table 2
[0140]
[0141] Note: “ / ” in Table 2 means there is no corresponding parameter.
[0142] The type and content of organic solvents usually affect the dynamic performance and cycle performance of lithium-ion batteries during fast charging. It can be seen from Examples 1-1, 2-1 to 2-5 that lithium-ion batteries whose types and contents of organic solvents are within the scope of this application have lower impedance, shorter charging time (i.e., higher charging speed), lower charging temperature rise and higher capacity retention rate at a charging rate of 10C, indicating that lithium-ion batteries have better dynamic performance and cycle performance during fast charging.
[0143] The type and content of lithium salts usually affect the kinetic performance and cycle performance of lithium-ion batteries during fast charging. It can be seen from Examples 1-1, 2-6 to 2-8 that lithium-ion batteries whose types and contents of lithium salts are within the scope of this application have lower impedance, shorter charging time (i.e., higher charging speed), lower charging temperature rise and higher capacity retention rate at a charging rate of 10C, indicating that lithium-ion batteries have better kinetic performance and cycle performance during fast charging.
[0144] The type and content of additives usually affect the dynamic performance and cycle performance of lithium-ion batteries during fast charging. It can be seen from Examples 1-1, 2-7 to 2-10 that lithium-ion batteries whose types and contents of additives are within the scope of this application have lower impedance, shorter charging time (i.e., higher charging speed), lower charging temperature rise and higher capacity retention rate at a charging rate of 10C, indicating that lithium-ion batteries have better dynamic performance and cycle performance during fast charging.
[0145] The terms "comprises," "comprising," or any other variations thereof are intended to cover a non-exclusive inclusion such that a process, method, or article that comprises a list of elements includes not only those elements but also includes other elements not expressly listed or that are inherent to such process, method, or article.
[0146] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.
[0147] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.
Claims
1. A secondary battery comprising a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer, and the negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer; the coating weight of the positive electrode active material layer is W z The coating weight of the negative electrode active material layer is W f , W z and W f Between: 1.6W f ≤W z ≤2.2W f 、3.25mg / cm 2 ≤W f ≤5.84mg / cm 2 ; The positive electrode current collector is integrally extended to form a plurality of positive electrode tabs; the negative electrode current collector is integrally extended to form a plurality of negative electrode tabs; The electrolyte includes an organic solvent, a lithium salt and an additive. The organic solvent includes a chain carboxylate compound. Based on the mass of the electrolyte, the mass percentage of the chain carboxylate compound is 6% to 56%.
2. The secondary battery according to claim 1, wherein 6.49mg / cm 2 ≤W z ≤11.69mg / cm 2 。 3. The secondary battery according to claim 1, wherein An N1 layer of positive electrode sheet is arranged between two adjacent positive electrode tabs, and an N2 layer of negative electrode sheet is arranged between two adjacent negative electrode tabs, and N1 and N2 are independently selected from 0, 1, 2 or 3.
4. The secondary battery according to claim 1, wherein The chain carboxylate compound includes at least one of methyl formate, methyl acetate, ethyl formate, ethyl acetate, propyl acetate, ethyl propionate, methyl propionate, n-propyl propionate, isopropyl propionate, n-butyl propionate, isobutyl propionate, n-pentyl propionate, isopentyl propionate, ethyl butyrate, n-propyl butyrate, propyl isobutyrate, n-pentyl butyrate, n-pentyl isobutyrate, n-butyl butyrate, isobutyl isobutyrate, and n-pentyl valerate.
5. The secondary battery according to claim 1, wherein The organic solvent further comprises at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone or tetrahydrofuran, and the mass percentage of the organic solvent is 60% to 80% based on the mass of the electrolyte.
6. The secondary battery according to claim 1, wherein Based on the mass of the electrolyte, the mass percentage of the lithium salt is 10% to 20%.
7. The secondary battery according to claim 1, wherein The additive includes at least one of succinonitrile, glutaronitrile, pimelonitrile, 1,2-bis(2-cyanoethoxy)ethane, 1,2-bis(2-cyanoethoxy)propane or 1,2,3-tris(2-cyanoethoxy)propane, and the mass percentage of the additive is 2% to 10% based on the mass of the electrolyte.
8. The secondary battery according to claim 1, wherein Satisfies at least one of the following characteristics: (1) The chain carboxylic acid ester compound includes at least one of methyl formate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate or ethyl butyrate; (2) The lithium salt includes at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium perchlorate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(oxalatoborate) or lithium difluorooxalatoborate. 9 . An electric device comprising the secondary battery according to claim 1 .
Citation Information
Cited By
Battery cell, battery device, and electric device
CN119153759A
Secondary battery and electronic device
CN119725782A
Battery cell, battery device, and electric device
CN119852495A
Battery cell, battery device, and electric device
CN119852496A
Battery cell, battery device, and electric device
CN120048981A