By optimizing the nitrogen concentration gradient and specific element composition, the electromagnetic soft iron achieves enhanced magnetic properties and stability, addressing the demand for improved performance in electromagnetic control components.
Patent Information
- Application Number
- JP2024533914
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-02-03
- Filing Date
- 2024-01-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-01-30
AI Technical Summary
Existing technologies, such as those described in Patent Documents 1 and 2, fail to meet the increased demand for improved magnetic properties in electromagnetic control components, particularly in electromagnetic soft iron, especially for bar steel applications.
The composition of electromagnetic soft iron is optimized by controlling the difference in nitrogen concentration between the surface and inside, with specific limits on elements like C, Si, Mn, P, S, Al, and N, along with additional elements like B, Se, Ca, Pb, Bi, Mg, Zr, REM, O, Cr, Mo, Cu, Ni, Ti, Nb, V, Sb, and Sn, to enhance magnetic properties and grain size stability.
The solution results in electromagnetic soft iron with excellent magnetic properties, suitable for bar steel, particularly in electromagnetic valves and solenoid valves, by stabilizing grain size and improving machinability.
Smart Images

Figure 0007558478000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an electromagnetic soft iron having excellent magnetic properties, which is used for motor cores, solenoid valves, etc. [Background technology]
[0002] In recent years, the importance of electronic and electromagnetic control parts has been increasing with the advancement of vehicle control technology for automobiles, etc. Among them, electromagnetic soft iron with excellent magnetic properties is used in solenoid valves used for controlling hydraulic pressure, etc., in order to control hydraulic pressure quickly and stably.
[0003] For example, Patent Document 1 proposes a soft magnetic steel material having improved magnetic properties and cold forgeability by setting the ferrite grain size number to 9.1 or less and further controlling the dispersion state of carbonitrides.
[0004] Furthermore, Patent Document 2 proposes a soft magnetic steel material having a ferrite grain size number of 7 or less by controlling the Cu+Cr content and the Mn / S ratio, as well as a method for manufacturing soft magnetic steel parts by annealing in a vacuum or in an inert gas atmosphere. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 6262599 [Patent Document 2] Patent No. 5416452 Summary of the Invention [Problem to be solved by the invention]
[0006] However, in recent years, there has been a growing trend toward computerization and electrification of automobiles and the like, and thus there is a demand for further improvement in the magnetic properties of electronic and electromagnetic control parts. However, the techniques described in Patent Documents 1 and 2 above have the problem of being unable to meet the increased demand for improved magnetic properties.
[0007] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide electromagnetic soft iron having excellent magnetic properties, particularly electromagnetic soft iron suitable for use in steel bars. [Means for solving the problem]
[0008] In order to achieve the above object, the inventors have conducted extensive research into the effects of material factors on magnetic properties, and have found that the difference in N concentration between the surface and the interior is closely related to magnetic properties when used in magnetic soft iron, particularly magnetic soft iron bar steel.
[0009] The present invention has been completed based on the above findings. That is, the gist of the present invention is as follows. 1. A soft electromagnetic iron comprising C: 0.010% by mass or less, Si: 0.010% by mass or less, Mn: 0.01 to 0.50% by mass, P: 0.050% by mass or less, S: 0.050% by mass or less, and Al: 0.021 to 0.100% by mass, with a N concentration satisfying the following formula, and the remainder being Fe and unavoidable impurities. N mat -N sur ≧0.0010% by mass however, N mat is the N concentration (mass%) at a position 1 mm below the surface N sur is the N concentration (mass%) at a position 0.1 mm below the surface
[0010] 2. The electromagnetic soft iron according to 1 above, further comprising one or more components selected from the group consisting of B: 0.0100% by mass or less, Se: 0.300% by mass or less, Ca: 0.0500% by mass or less, Pb: 0.300% by mass or less, Bi: 0.300% by mass or less, Mg: 0.0500% by mass or less, Zr: 0.2000% by mass or less, REM: 0.010% by mass or less, and O: 0.0250% by mass or less.
[0011] 3. The electromagnetic soft iron according to 1 or 2, further comprising one or more selected from the group consisting of Cr: 2.0% by mass or less, Mo: 1.00% by mass or less, Cu: 1.0% by mass or less, Ni: 1.0% by mass or less, Ti: 0.10% by mass or less, Nb: 0.10% by mass or less, and V: 0.30% by mass or less.
[0012] 4. The electromagnetic soft iron according to any one of 1 to 3 above, wherein the component composition of the electromagnetic soft iron further contains one or more selected from the group consisting of Sn: 0.1000 mass % or less and Sb: 0.1000 mass % or less. Effect of the Invention
[0013] INDUSTRIAL APPLICABILITY According to the present invention, it is possible to provide electromagnetic soft iron, in particular electromagnetic soft iron steel bar, having excellent magnetic properties, which is extremely useful industrially. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present invention will be specifically described below. First, the basic components of the electromagnetic soft iron of the present invention will be described. C: 0.010% by mass or less If the C content exceeds 0.010 mass%, the core loss deteriorates due to magnetic aging, so the C content is limited to 0.010 mass% or less. On the other hand, although there is no particular lower limit for the C content, it is preferably 0.001 mass% or more in order to suppress an increase in refining costs.
[0015] Si: 0.010% by mass or less Although Si is effective as a deoxidizer, if it exceeds 0.010% by mass, it reduces workability, so it is limited to 0.010% by mass or less. It is preferably 0.005% by mass or less, and more preferably 0.003% by mass or less. On the other hand, there is no particular lower limit for the Si content, but an excessive reduction leads to an increase in refining costs, so it is preferably 0.001% by mass or more.
[0016] Mn:0.01~0.50% by mass Mn is an element that improves machinability by combining with S to form sulfides, and in order to obtain this effect, it is necessary to add at least 0.01% by mass. However, excessive addition reduces magnetic properties, so the upper limit of the Mn content is limited to 0.50% by mass. The content is preferably 0.10% by mass or more, and more preferably 0.20% by mass or more. The content is also preferably 0.40% by mass or less, and more preferably 0.35% by mass or less.
[0017] P: 0.050% by mass or less P has the effect of improving machinability. It may be added to obtain this effect, but in this case, the effect may not be evident unless 0.001 mass% or more of P is added. On the other hand, the addition of more than 0.050 mass% reduces the toughness of the steel, so the upper limit of the P content is set to 0.050 mass%.
[0018] S: 0.050% by mass or less S exists as sulfide-based inclusions and is an effective element for improving machinability. To obtain this effect, it is preferable to add at least 0.001% by mass. On the other hand, adding more than 0.050% by mass of S reduces the hot workability of the steel and increases surface cracking during continuous casting. Therefore, the S content is limited to a range of 0.050% by mass or less. It is preferably 0.040% by mass or less, and more preferably 0.035% by mass or less. It is also preferably 0.005% by mass or more, more preferably 0.010% by mass or more, and even more preferably 0.021% by mass or more.
[0019] Al:0.021~0.100% by mass Al combines with N to form fine nitrides. These nitrides have a pinning force that inhibits the movement of grain boundaries and suppresses grain growth, but by controlling their dispersion, it is possible to coarsen the grain size and consistently obtain excellent magnetic properties. In particular, the present invention is characterized in that the N concentration within 0.1 mm below the surface (on the steel surface side) is reduced to a predetermined concentration, and in order to utilize this characteristic, when Al is added, it is necessary to add at least 0.021 mass%. This is because it increases the amount of nitrides and effectively increases the pinning force. On the other hand, even if excessively added in excess of 0.100 mass%, the effect simply becomes saturated. Therefore, the Al content is limited to the range of 0.021 to 0.100 mass%, preferably 0.025 mass% or more, more preferably 0.030 mass% or more, and more preferably 0.090 mass% or less, more preferably 0.080 mass% or less.
[0020] N mat -N sur ≧0.0010% by mass however, N mat is the N concentration (mass%) at a position 1 mm below the surface N sur is the N concentration (mass%) at a position 0.1 mm below the surface N combines with Al to form nitrides. Nitrides have a pinning force that inhibits the movement of grain boundaries, and the finer and more dispersed they are, the stronger the pinning force. The grain size corresponds to the strength of the pinning force, and the stronger the pinning force, the finer the grain size. Therefore, when there is a difference in N concentration between the surface and the interior of a steel material, there is a difference in the crystal grain size between the surface and the interior of the steel material. When there is such a difference in crystal grain size between the surface and the interior, abnormal grain growth occurs in which coarse crystal grains eat away at fine crystal grains, resulting in the formation of extremely coarse crystal grains, which contributes to improving the magnetic properties.
[0021] To utilize this effect, the difference between the N concentration (mass%) at a position 1 mm below the surface and the N concentration (mass%) at a position 0.1 mm below the surface must be at least 0.0010 mass%. Preferably, this difference is 0.0020 mass% or more. On the other hand, there is no particular upper limit to this difference, but considering the N concentration that can be added to steel using existing technology, it is about 0.1000 mass% or less.
[0022] The amount of N in the steel is not particularly limited as long as it satisfies the above-mentioned formula relating to the concentration difference and is within a range in which a difference in crystal grain size occurs between the surface and the interior of the steel material, but is preferably in the range of about 0.0015 to 0.1000 mass%, more preferably 0.0025 mass% or more, and more preferably 0.0300 mass% or less. Here, in order to reduce the N concentration at a position within 0.1 mm below the surface, it is sufficient to carry out a heat treatment in which the nitrogen potential is controlled to a value smaller than that of the base material. For example, heat treatment in a vacuum (reduced pressure) can be applied.
[0023] In the present invention, a position 1 mm below the surface refers to a position 1 mm deep from any steel surface in the electromagnetic soft iron member or component. Also, a position 0.1 mm below the surface refers to a position 0.1 mm deep from any steel surface in the electromagnetic soft iron member or component. Note that in the present invention, both the position 1 mm below the surface and the position 0.1 mm below the surface may be positions that satisfy the depth requirements, and the positions perpendicular to the depth direction (for example, the position in the longitudinal or transverse direction of a rod-shaped member) may be positions selected at random. The effects of the present invention can be achieved by measuring and controlling the N concentration at such a position.
[0024] The basic components of the present invention have been described above. However, in the present invention, the following components can be further added as necessary. B: 0.0100% by mass or less B improves machinability by bonding with N to form nitrides. However, if the content exceeds 0.0100% by mass, there is a risk of degrading the magnetic properties, so the upper limit of the B content is preferably 0.0100% by mass. More preferably, it is 0.0050% by mass or less. Even more preferably, it is 0.0030% by mass or less. On the other hand, the lower limit of the B content is not particularly limited, but in order to obtain a sufficient effect of improving machinability, it is preferably 0.0005% by mass or more. More preferably, it is 0.0010% by mass or more.
[0025] Se: 0.300% by mass or less Se improves machinability by combining with Mn to form Se compounds. However, if the Se content exceeds 0.300% by mass, the magnetic properties may be deteriorated, so the upper limit of the Se content is preferably 0.300% by mass. More preferably, it is 0.100% by mass or less. Further preferably, it is 0.070% by mass or less. On the other hand, the lower limit of the Se content is not particularly limited, but in order to obtain a sufficient effect of improving machinability, it is preferably 0.001% by mass or more. More preferably, it is 0.005% by mass or more.
[0026] Ca: 0.0500% by mass or less Ca improves machinability by combining with S to form sulfides. However, if the Ca content exceeds 0.0500% by mass, the magnetic properties may be deteriorated, so the upper limit of the Ca content is preferably 0.0500% by mass. More preferably, it is 0.0300% by mass or less. Even more preferably, it is 0.0150% by mass or less. On the other hand, the lower limit of the Ca content is not particularly limited, but in order to obtain a sufficient effect of improving machinability, it is preferably 0.0005% by mass or more. More preferably, it is 0.0010% by mass or more.
[0027] Pb: 0.300 mass% or less, Bi: 0.300 mass% or less Pb and Bi improve machinability by miniaturizing chips during cutting. However, excessive addition will only saturate the effect, so it is preferable to set the upper limit of the Pb and Bi contents to 0.300 mass%. More preferably, both Pb and Bi contents are 0.250 mass% or less. Even more preferably, both are 0.150 mass% or less. On the other hand, there is no particular lower limit for the Pb and Bi contents, but in order to fully obtain the machinability improving effect, each is preferably 0.005 mass% or more. More preferably, each is 0.010 mass% or more.
[0028] Mg: 0.0500% by mass or less Mg has the effect of improving machinability, but if the content exceeds 0.0500% by mass, there is a risk of significant deterioration in magnetic properties. Therefore, the upper limit of the Mg content is preferably 0.0500% by mass. More preferably, it is 0.0300% by mass or less. Even more preferably, it is 0.0150% by mass or less. On the other hand, the lower limit of the Mg content is not particularly limited, but in order to obtain a sufficient effect of improving machinability, it is preferably 0.0010% by mass or more. More preferably, it is 0.0030% by mass or more.
[0029] Zr: 0.2000 mass% or less Zr has the effect of improving machinability, but if it exceeds 0.2000 mass%, there is a risk of significant deterioration in magnetic properties. Therefore, the upper limit of the Zr content is preferably 0.2000 mass%, more preferably 0.1000 mass% or less, and even more preferably 0.0500 mass% or less. On the other hand, the lower limit of the Zr content is not particularly limited, but in order to sufficiently obtain the effect of improving machinability, it is preferably 0.0010 mass% or more, and more preferably 0.0030 mass% or more.
[0030] REM: 0.010% by mass or less REM has the effect of improving machinability, but if the REM content exceeds 0.010% by mass, the magnetic properties may be significantly degraded. Therefore, the upper limit of the REM content is preferably 0.010% by mass. More preferably, it is 0.005% by mass or less. Even more preferably, it is 0.004% by mass or less. On the other hand, the lower limit of the REM content is not particularly limited, but in order to obtain a sufficient effect of improving machinability, it is preferably 0.001% by mass or more. More preferably, it is 0.002% by mass or more.
[0031] O: 0.0250% by mass or less O (oxygen) has the effect of improving machinability through the effect of coarsening sulfide-based inclusions, but excessive addition may lead to a decrease in the toughness of the steel material and cause early fracture of structural members. Therefore, the upper limit of the O content is preferably 0.0250 mass%, more preferably 0.0230 mass% or less, and even more preferably 0.0200 mass% or less. On the other hand, the lower limit of the O content is not particularly limited, but in order to sufficiently obtain the effect of improving machinability, it is preferably 0.0010 mass% or more, and more preferably 0.0050 mass% or more.
[0032] Cr: 2.0 mass% or less, Mo: 1.00 mass% or less, Cu: 1.0 mass% or less, Ni: 1.0 mass% or less, Ti: 0.10 mass% or less, Nb: 0.10 mass% or less, and V: 0.30 mass% or less Cr, Mo, Cu, Ni, Ti, Nb and V contribute to improving the strength of steel through solid solution strengthening and precipitation strengthening. These elements may be added to adjust the strength to match the required characteristics of the part, but since the effect will simply saturate if they are added in excess, it is preferable to specify the upper limit amounts as above. On the other hand, there is no particular restriction on the lower limit amounts of these elements, and each may be 0 mass%.
[0033] Sb: 0.0100 mass% or less, Sn: 0.1000 mass% or less Sb and Sn have the effect of improving the descaling properties during shot blasting and pickling performed before cold wire drawing, and can be added as necessary when these processes are included in the manufacturing of parts. However, even if Sb and Sn are added in excess of 0.0100 mass% and 0.1000 mass%, respectively, the effect of improving the descaling properties saturates, so the upper limits of the Sb and Sn amounts are set to 0.0100 mass% and 0.1000 mass%, respectively. On the other hand, there are no particular limitations on the lower limits of the Sb and Sn amounts, and both may be 0.0010 mass%.
[0034] The balance other than the elements described above is Fe and inevitable impurities. The inevitable impurities are those that are mixed in from raw materials such as ore and scrap, or from the manufacturing environment, during industrial production of steel material, and are allowed within a range that does not adversely affect the characteristics of the present embodiment.
[0035] The electromagnetic soft iron (electromagnetic soft iron steel bar) according to the present invention can be produced by any conventional method. As an example, the steel having the above-mentioned composition is melted by continuous casting, and then hot-rolled at a heating temperature in the range of 1250 to 920°C and air-cooled. Next, hot-rolled again at a heating temperature in the range of 1250 to 920°C to form into a specified shape such as a round bar. Then, heat treatment is performed in which the nitrogen potential is controlled to a value smaller than that of the base material to obtain the electromagnetic soft iron (electromagnetic soft iron bar) according to the present invention. Before the heat treatment in which the nitrogen potential is controlled to a value smaller than that of the base material, processing such as forging and cutting may be performed as necessary. This makes it possible to obtain electromagnetic soft iron with excellent magnetic properties, particularly electromagnetic soft iron suitable for use in steel bars. In addition, the shape of the present invention is not limited to steel bars, and may be steel plates, etc.
[0036] The electromagnetic soft iron of the present invention can be suitably used for steel bars used in electromagnetic soft iron parts such as solenoid valves, etc. Taking advantage of its excellent magnetic properties, it can also be used for solenoid valves, voice coil motors, etc. EXAMPLES
[0037] The configuration and effects of the present invention will be described in more detail below with reference to examples. Note that the present invention is not limited to these examples, and can be modified as appropriate within the scope of the invention, and all such modifications are included in the technical scope of the present invention.
[0038] Steel having the chemical composition shown in Table 1 was formed into a round bar with a diameter of 50 mm by hot rolling, and then the bar was cut to form cylindrical (hereinafter also referred to as ring-shaped) test pieces with a hollow hole in the center and an outer diameter of 45 mm, an inner diameter of 33 mm, and a height of 30 mm. Further, the test pieces were heat-treated at 850°C for 30 minutes in a heating furnace in which the nitrogen potential in the atmosphere was controlled. Then, the N concentration at positions 0.1 mm and 1 mm below the surface of the outer diameter side of the ring-shaped test piece was measured by soft X-ray spectroscopy under the following measurement conditions: acceleration voltage: 8 kV, probe diameter: 10 μm, measurement current: 0.1 μA, and measurement time: 360 seconds.
[0039] The magnetic properties were measured in accordance with JIS C2504 by applying an excitation winding (primary winding 220 turns) and a detection winding (secondary winding 100 turns). A DC magnetization measuring device was used to measure the BH curve, and the magnetic flux density of 200A / m was evaluated during the magnetization process with a maximum magnetic field of 10,000A / m. In this test, a magnetic property of 1.45T or more can be said to be excellent. Similarly, the coercive force was measured and evaluated at a reversal magnetization force of ±400 A / m using a DC magnetic property tester. In this example, a coercive force of 45 A / m or less can be said to be excellent in magnetic properties. Table 1 also shows the evaluation results of the magnetic properties.
[0040] [Table 1]
[0041] As shown in Table 1, all of the examples according to the present invention have excellent magnetic properties.
[0042] In contrast, all of the comparative examples outside the scope of the present invention were inferior in magnetic properties.
Claims
1. C: 0.010% by mass or less, Si: 0.010% by mass or less, Mn: 0.01 to 0.50% by mass, P: 0.050% by mass or less, S: 0.050% by mass or less; and Al: 0.021 to 0.100 mass%; The magnetic soft iron has a composition in which the N concentration satisfies the following formula, and the remainder is Fe and unavoidable impurities. N mat -N sur ≧0.0010% by mass however, N mat is the N concentration (mass%) at a position 1 mm below the surface N sur is the N concentration (mass%) at a position 0.1 mm below the surface
2. The composition of the electromagnetic soft iron further includes: B: 0.0100% by mass or less, Se: 0.300% by mass or less, Ca: 0.0500% by mass or less, Pb: 0.300% by mass or less, Bi: 0.300% by mass or less, Mg: 0.0500% by mass or less, Zr: 0.2000% by mass or less, REM: 0.010% by mass or less, O: 0.0250% by mass or less, 2. The electromagnetic soft iron according to claim 1, comprising one or more selected from the following:
3. The composition of the electromagnetic soft iron further includes: Cr: 2.0% by mass or less, Mo: 1.00% by mass or less, Cu: 1.0% by mass or less, Ni: 1.0% by mass or less, Ti: 0.10% by mass or less, Nb: 0.10% by mass or less, V: 0.30% by mass or less, 3. The electromagnetic soft iron according to claim 1 or 2, comprising one or more selected from the following:
4. The composition of the electromagnetic soft iron further includes: Sn: 0.1000 mass% or less and Sb: 0.1000% by mass or less 3. The electromagnetic soft iron according to claim 1 or 2, comprising one or more selected from the following:
5. The composition of the electromagnetic soft iron further includes: Sn: 0.1000 mass% or less and Sb: 0.1000% by mass or less The electromagnetic soft iron according to claim 3, comprising one or more selected from the following:
Citation Information
Patent Citations
Production of thick nonoriented silicon steel plate excellent in magnetic property
JP1992333517A
Thick electromagnetic soft-iron superior in the inside property, and manufacturing method therefor
JP2003129195A
Soft magnetic steel
JP2006328461A
Preparation of dis*amnomethyl* cyclohexane
JP1979016452A
Electromagnetic wave shielding material
JP1987062599A