Electrolyte and lithium-ion secondary battery
The use of a specific electrolytic solution with controlled molecular weight and distribution for lithium ion secondary batteries enhances electrode impregnation, thereby improving battery performance in terms of output and cycle characteristics.
Patent Information
- Application Number
- JP2020161070
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-25
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-09-25
AI Technical Summary
High viscosity of electrolytes containing high molecular weight methacrylic acid ester polymers leads to insufficient electrode impregnation, affecting battery characteristics such as cycle and output characteristics in lithium ion secondary batteries.
An electrolytic solution comprising an aprotic solvent, a supporting salt, and a copolymer of methyl methacrylate and (3-ethyloxetan-3-yl)methyl methacrylate with a weight average molecular weight of 100,000 to 300,000 and a molecular weight distribution less than 2, which includes LiPF6, LiBF4, LiAsF6, LiSbF6, and LiN(SO2F)2 as supporting salts, and a methacrylic acid ester polymer content of 1.5 to 2.5% by mass, facilitating better impregnation and gelation properties.
The electrolytic solution achieves low viscosity for effective electrode impregnation, improving both output and cycle characteristics of lithium ion secondary batteries.
Smart Images

Figure 0007558526000001 
Figure 0007558526000002 
Figure 0007558526000003
Abstract
Description
Technical Field
[0001] Embodiments of the present invention relate to an electrolytic solution and a lithium ion secondary battery using the same.
Background Art
[0002] In a lithium ion secondary battery, it is required to improve battery characteristics such as output characteristics and cycle characteristics. For example, Patent Documents 1 and 2 disclose that cycle characteristics are improved by using a polymer gel electrolyte containing a crosslinked body obtained by crosslinking a methacrylic acid ester polymer obtained by copolymerizing methyl methacrylate and (3-ethyloxetan-3-yl)methyl methacrylate.
Prior Art Documents
Patent Documents
[0003]
Patent Document 1
Patent Document 2
Summary of the Invention
Problems to be Solved by the Invention
[0004] In the methacrylic acid ester polymer described in Patent Documents 1 and 2, n representing the number of methyl methacrylate units satisfies 1800 < n < 3000, and m representing the number of (3-ethyloxetan-3-yl)methyl methacrylate units satisfies 350 < m < 600. Specifically, in the examples used, n = 2620, m = 420, and the molecular weight exceeds 300,000. In the examples, a polymer gel electrolyte is prepared using an electrolytic solution containing 2% by mass of such a high molecular weight methacrylic acid ester polymer. However, since this electrolytic solution is expected to have a high viscosity, for example, when injecting the electrolytic solution into the battery before injection, the impregnation of the electrolytic solution into the electrode may be insufficient, which may adversely affect battery characteristics such as cycle characteristics.
[0005] In view of the above, an object of the embodiments of the present invention is to provide an electrolyte solution capable of improving pourability while enabling good output characteristics and cycle characteristics to be obtained, and a lithium ion secondary battery using the electrolyte solution. [Means for solving the problem]
[0006] The present invention includes the embodiments set forth below. [1] An electrolyte solution comprising an aprotic solvent, a supporting salt, and a methacrylic acid ester polymer, which is a copolymer of methyl methacrylate and (3-ethyloxetan-3-yl)methyl methacrylate and has a weight average molecular weight of 100,000 or more and 300,000 or less and a molecular weight distribution of less than 2. [2] The electrolyte solution according to [1], wherein the aprotic solvent comprises at least one solvent selected from the group consisting of cyclic carbonates, chain carbonates, aliphatic carboxylic acid esters, γ-lactones, cyclic ethers, and chain ethers. [3] The electrolyte according to [1] or [2], containing at least one substance selected from the group consisting of LiPF6, LiBF4, LiAsF6, LiSbF6 and LiN(SO2F)2 as the supporting salt. [4] The electrolyte solution according to any one of [1] to [3], wherein the content of the methacrylic acid ester polymer is 1.5 to 2.5 mass % of the total amount of the electrolyte solution. [5] A lithium ion secondary battery comprising: a positive electrode; a negative electrode; and a polymer gel electrolyte obtained by crosslinking the methacrylic acid ester polymer using the electrolytic solution according to any one of [1] to [4]. [6] The lithium ion secondary battery according to [5], wherein the positive electrode contains a lithium-containing composite oxide as a positive electrode active material. [7] The lithium ion secondary battery according to [5] or [6], wherein the negative electrode contains, as a negative electrode active material, a material selected from the group consisting of materials capable of absorbing and releasing lithium. [8] The lithium ion secondary battery according to [7], wherein the material capable of absorbing and releasing lithium includes a carbon material. Effect of the Invention
[0007] According to an embodiment of the present invention, the viscosity of the electrolyte can be made low, and therefore the electrolyte can be easily impregnated into the electrodes during injection, improving the injection properties, and good output characteristics and cycle characteristics can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The electrolyte solution according to the embodiment is a non-aqueous electrolyte solution containing an aprotic solvent, a supporting salt, and a methacrylic acid ester polymer. The electrolyte solution is an electrolyte solution in which the supporting salt and the methacrylic acid ester polymer are dissolved in an aprotic solvent, and the methacrylic acid ester polymer is crosslinked to form a crosslinked body, thereby forming a polymer gel electrolyte.
[0009] [Aprotic Solvents] Examples of aprotic solvents include cyclic carbonates such as ethylene carbonate (ethylene carbonate, EC), propylene carbonate (PC), butylene carbonate (BC), and vinylene carbonate (VC); chain carbonates such as diethyl carbonate (diethyl carbonate, DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and dipropyl carbonate (DPC); aliphatic carboxylic acid esters such as methyl formate, methyl acetate, and ethyl propionate; γ-lactones such as γ-butyrolactone; chain ethers such as 1,2-diethoxyethane (DEE) and ethoxymethoxyethane (EME); and tetrahydrofuran ( Examples of the organic solvent include cyclic ethers such as tetrahydrofuran (THF) and 2-methyltetrahydrofuran; fluorine derivatives thereof; dimethyl sulfoxide (DMSO), 1,3-dioxolane, formamide, acetamide, dimethylformamide (DMF), acetonitrile, propylnitrile, nitromethane, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, 3-methyl-2-oxazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethyl ether, 1,3-propane sultone, anisole, N-methylpyrrolidone, and fluorinated carboxylate esters. These aprotic organic solvents may be used alone or in combination of two or more.
[0010] The aprotic solvent preferably contains at least one solvent selected from the group consisting of cyclic carbonates, chain carbonates, aliphatic carboxylic acid esters, γ-lactones, cyclic ethers, and chain ethers, and more preferably contains at least one solvent selected from the group consisting of cyclic carbonates and chain carbonates.
[0011] [Supporting salt] The supporting salt is a substance that enhances the conductivity of an aprotic solvent, and examples thereof include lithium salts such as LiPF6, LiBF4, LiAsF6, LiSbF6, LiN(SO2F)2 (i.e., lithium bis(fluorosulfonyl)imide: LiFSI), LiAlCl4, LiClO4, LiCF3SO3, LiC4F9SO3, LiC(CF3SO2)3, LiN(CF3SO2)2, LiN(C2F5SO2)2, lithium carboxylate, lithium chloroborane, lithium tetraphenylborate, LiBr, LiI, LiSCN, LiCl, and LiF. These supporting salts may be used alone or in combination of two or more.
[0012] The supporting salt preferably contains a fluorine-containing lithium salt, and more preferably contains at least one substance selected from the group consisting of LiPF6, LiBF4, LIAsF6, LiSbF6, and LiN(SO2F)2.
[0013] The concentration of the supporting salt in the electrolytic solution is not particularly limited, but is preferably 0.5 to 2.0 mol / L, more preferably 0.6 to 1.8 mol / L, and may be 0.8 to 1.6 mol / L.
[0014] [Methacrylic acid ester polymer] The methacrylic acid ester polymer used in this embodiment is a copolymer of methyl methacrylate (MMA) and (3-ethyloxetan-3-yl)methyl methacrylate (OXMA).
[0015] In this embodiment, the methacrylic acid ester polymer has a weight average molecular weight (Mw) of 100,000 or more and 300,000 or less. When the weight average molecular weight is 100,000 or more, gelation occurs easily, and a polymer gel electrolyte is easily obtained. When the weight average molecular weight is 300,000 or less, the viscosity of the electrolyte can be reduced, and the impregnation of the electrode during injection can be improved. The weight average molecular weight of the methacrylic acid ester polymer is preferably 120,000 or more, more preferably 150,000 or more, and may be 200,000 or more. The weight average molecular weight is preferably 280,000 or less, more preferably 260,000 or less.
[0016] In this embodiment, the methacrylic acid ester polymer has a molecular weight distribution (Mw / Mn) of less than 2. When the molecular weight distribution is less than 2, gelation occurs easily. More specifically, the methacrylic acid ester polymer can be gelled without a high concentration, which is advantageous in obtaining good output characteristics and cycle characteristics. The molecular weight distribution of the methacrylic acid ester polymer is preferably 1.8 or less, more preferably 1.6 or less. Since the smaller the molecular weight distribution, the better, the lower limit is not particularly limited, and may be, for example, about 1.1.
[0017] Here, the weight-average molecular weight of the methacrylic acid ester polymer is measured in terms of polystyrene by gel permeation chromatography (GPC), and the molecular weight distribution is obtained by calculating the ratio (Mw / Mn) of the weight-average molecular weight (Mw) and the number-average molecular weight (Mn) obtained by the measurement.
[0018] The methacrylic acid ester polymer is a copolymer containing a structural unit represented by the following formula (1) (hereinafter referred to as MMA unit) and a structural unit represented by the following formula (2) (hereinafter referred to as OXMA unit). As the structural units derived from monomers, it is preferably composed substantially only of MMA units and OXMA units, but may contain structural units derived from other monomers as long as the effects are not impaired. Although not particularly limited, the total content of MMA units and OXMA units is preferably 90 mol% or more, more preferably 95 mol% or more, and still more preferably 99 mol% or more based on 100 mol% of all the structural units derived from monomers.
[0019] [Chemical formula]
[0020] In the methacrylic acid ester polymer, the ratio (m / n) of the number (degree of polymerization) m of OXMA units to the number (degree of polymerization) n of MMA units preferably satisfies 0.3 < m / n < 3.0. When m / n is greater than 0.3, gelation is likely to occur. When m / n is less than 3.0, the inclusion (retention) of the electrolyte becomes good. m / n is preferably 0.35 or more, more preferably 1.8 or more. Also, m / n is preferably 2.5 or less, more preferably 2.3 or less.
[0021] The number n of MMA units is not particularly limited, but preferably satisfies 190 < n < 1500, more preferably 200 < n < 1000. Also, the number m of OXMA units is not particularly limited, but preferably satisfies 340 < m < 1200, more preferably 400 < m < 1150.
[0022] Here, m / n of the methacrylic acid ester polymer is 1The content is the molar ratio (m / n) of OXMA and MMA determined by 1H-NMR measurement, and it is only required to satisfy 0.3 < m / n < 3.0 with the value rounded to the second decimal place. Also, the values of m and n are values calculated from the m / n value obtained in this way and the measured value of the number average molecular weight Mn, and each represents an average value.
[0023] In one embodiment, the methacrylate polymer is represented by the following general formula (3).
Chemical formula
[0024] The methacrylate polymer according to this embodiment can be obtained by radical copolymerization of methyl methacrylate (MMA) and (3-ethyloxetan-3-yl)methyl methacrylate (OXMA). As the radical polymerization method, free radical polymerization may be used, but since complicated processes such as fractionation operations are required, living radical polymerization is preferably used, and it is easy to obtain the methacrylate polymer with a small molecular weight distribution as described above.
[0025] The living radical polymerization is not particularly limited. For example, the RAFT (Reversible Addition / Fragmentation Chain Transfer Polymerization) method (Reversible Addition / Fragmentation Chain Transfer Polymerization), ATRP (Atom Transfer Radical Polymerization) method (Atom Transfer Radical Polymerization), NMP (Nitroxide-mediated Polymerization) method (Nitroxide-mediated Polymerization), etc. can be mentioned. For example, as the RAFT agent in the RAFT method, dithiobenzoate, trithiocarbonate, dithiocarbamate, xanthate, etc. can be mentioned, but it is not limited to these.
[0026] The content of the methacrylic acid ester polymer in the electrolytic solution is not particularly limited, but is preferably 0.5 to 10 mass% of the entire electrolytic solution (i.e., relative to 100 mass% of the electrolytic solution), more preferably 1 to 5 mass%, and even more preferably 1.5 to 2.5 mass%. By making the content of the methacrylic acid ester polymer 0.5 mass% or more, gelation is likely to occur, and by making it 10 mass% or less, deterioration of the battery characteristics can be suppressed.
[0027] In addition to the above components, additives such as acid anhydride, sulfonic acid ester, diphenyl disulfide, cyclohexylbenzene, biphenyl, fluorobenzene, and t-butylbenzene may be appropriately added to the electrolyte solution according to this embodiment.
[0028] [Lithium-ion secondary battery] The lithium ion secondary battery according to the embodiment includes a positive electrode, a negative electrode, and a polymer gel electrolyte obtained by crosslinking a methacrylic acid ester polymer using the above-mentioned electrolytic solution.
[0029] The polymer gel electrolyte contains an aprotic solvent, a supporting salt, and a crosslinked body obtained by crosslinking a methacrylic acid ester polymer. The crosslinked body is obtained by ring-opening polymerization of an oxetanyl group of the methacrylic acid ester polymer with a cationic polymerization initiator. As the cationic polymerization initiator, a generally known polymerization initiator can be used, but it is preferable to use a small amount of an acidic substance obtained by hydrolysis of a lithium salt and an anion component of the lithium salt contained in the electrolyte solution, as this has little effect on the battery.
[0030] The polymer gel electrolyte is the above-mentioned electrolytic solution in a gel state due to crosslinking of the methacrylic acid ester polymer. The gel state mentioned here includes not only a normal gel but also a state similar to an electrolyte called a gel electrolyte in the battery industry, and also includes a state where the liquid has little fluidity or no longer flows, even if it is not a gel in the strict sense.
[0031] The concentration of the supporting salt in the polymer gel electrolyte is the same as that in the above-mentioned electrolytic solution, and the content of the crosslinked methacrylic acid ester polymer in the polymer gel electrolyte is the same as that in the above-mentioned electrolytic solution.
[0032] The positive electrode contains at least a positive electrode active material, and for example, a positive electrode mixture layer containing a positive electrode active material can be formed on one or both sides of a current collector made of a metal such as aluminum foil. The positive electrode mixture layer can be formed by applying a paste containing a positive electrode mixture to a current collector, drying it, and compressing and molding it. The paste containing a positive electrode mixture can be obtained by dispersing and kneading a positive electrode active material together with a conductive assistant such as carbon black or graphite and a binder such as polyvinylidene fluoride (PVDF) in a dispersion medium such as N-methyl-2-pyrrolidone (NMP).
[0033] The positive electrode active material is not particularly limited, and for example, lithium-containing composite oxides such as LiCoO2, LiNiO2, and LiMn2O4 can be used. In addition, lithium-containing composite oxides in which the transition metal part of these lithium-containing composite oxides is replaced with other elements can also be used. These may be used alone or in combination of two or more.
[0034] The negative electrode contains at least a negative electrode active material, and for example, a negative electrode mixture layer containing a negative electrode active material can be formed on one or both sides of a current collector made of a metal such as copper foil. The negative electrode mixture layer can be formed, for example, by applying a negative electrode mixture-containing paste to a current collector, drying it, and compressing and molding it. The negative electrode mixture-containing paste can be obtained by dispersing and kneading the negative electrode active material together with a binder such as styrene butadiene rubber in a dispersion medium such as water. The negative electrode mixture-containing paste may further contain a thickener such as carboxymethyl cellulose salt or a conductive assistant such as carbon black. The negative electrode mixture layer may also be formed by a method such as a vapor deposition method, a CVD method, or a sputtering method.
[0035] The negative electrode active material is not particularly limited, and may be one or more materials selected from materials capable of absorbing and releasing lithium, including lithium metal or a lithium alloy. Specific examples of materials capable of absorbing and releasing lithium include carbon materials and oxides.
[0036] The lithium alloy is composed of lithium and a metal capable of forming an alloy with lithium, specifically, a binary or ternary or more alloy of lithium and a metal such as Al, Si, Pb, Sn, In, Bi, Ag, Ba, Ca, Hg, Pd, Pt, Te, Zn, or La.
[0037] Examples of carbon materials include graphite, amorphous carbon, diamond-like carbon, carbon nanotubes, and composite oxides thereof. Among these, graphite and amorphous carbon are preferred.
[0038] Examples of oxides that can be used include silicon oxide, tin oxide, indium oxide, zinc oxide, lithium oxide, and composites of these. Among these, silicon oxide is preferred because it is stable and does not react with other compounds.
[0039] The method for producing the lithium ion secondary battery is not particularly limited, and the battery can be produced by a known method. For example, a positive electrode and a negative electrode are stacked with a separator between them to form a laminate. Alternatively, the positive electrode and the negative electrode are rolled flat with a separator between them, and then molded into a wound body. The laminate or wound body is then inserted into an exterior body such as a can or a laminate material, and an electrolyte is injected into the exterior body and cured (gelled) to obtain a lithium ion secondary battery.
[0040] As a curing treatment, for example, after the injection of the electrolyte solution, charging and heating are performed, whereby the methacrylic acid ester polymer can be crosslinked by utilizing a trace amount of acidic substance formed by hydrolysis of the lithium salt and the anion component of the lithium salt contained in the electrolyte solution, thereby forming a polymer gel electrolyte.
[0041] As the separator, a material generally used in lithium ion secondary batteries can be used, such as a nonwoven fabric, a polyolefin microporous membrane, etc. Note that a separator is not essential, and the polymer gel electrolyte can also have the function of a separator.
[0042] According to the present embodiment, an electrolyte solution having low viscosity and good gelling properties can be obtained, so that when the electrolyte solution is injected into the battery before injection, a lithium ion secondary battery having excellent impregnation properties into the electrodes and good output characteristics and cycle characteristics can be obtained. Therefore, it is possible to achieve both good battery characteristics and improved injection properties of the electrolyte solution in the lithium ion secondary battery. EXAMPLES
[0043] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0044] <Measurement and evaluation method> [Weight average molecular weight, number average molecular weight, and molecular weight distribution of polymer] The methacrylic acid ester polymer was dissolved in tetrahydrofuran, and the weight average molecular weight (Mw), number average molecular weight (Mn), and molecular weight distribution (Mw / Mn) in terms of polystyrene were measured by gel permeation chromatography (GPC) (Prominence, Shimadzu Corporation) using four columns (Shodex GPC columns KF-601, KF-602, KF-603, KF-604, Showa Denko) packed with polystyrene gel. The column oven temperature was 40°C, the THF flow rate was 0.6 mL / min, and a differential refractive index detector (Shodex RI-504, Showa Denko Corporation) was used.
[0045] [m / n of polymer] The methacrylic acid ester polymer was dissolved in deuterated chloroform and analyzed by a nuclear magnetic resonance spectrometer (JEOL). 1 H-NMR measurement was performed to determine the molar ratio (m / n) of OXMA and MMA.
[0046] [Gelling property of electrolyte] The electrolyte was placed in a screw bottle, sealed, and heated for 20 hours in a thermostatic oven at 60° C. After that, the screw bottle was turned upside down, and those in which the formation of a gel-like substance was visually confirmed were marked with an ◯, and those in which it was not (remained liquid) were marked with an ×.
[0047] [Electrolyte viscosity] The vibration viscosity of the electrolyte at 25° C. was measured using a vibration viscometer (VISCOMATE MODEL VM-10A-L, manufactured by CBC Materials).
[0048] [Output characteristics] To evaluate the output characteristics, the cells were charged at a constant current (CC) of 0.5C in an atmosphere of 25°C, and then CC discharged at a predetermined current value (1, 2, 3C) to calculate the capacity retention rate (ratio to 0.2C discharge capacity). The charge / discharge voltage range was set to 2.7V to 4.2V. The 0.5C current value refers to a current value that is half the 1C current value at which the cell capacity can be discharged in 1 hour.
[0049] [Cycle characteristics] To evaluate cycle characteristics, the capacity retention (retention rate relative to the discharge capacity at the first cycle) (%) was calculated after 200 cycles of CC-CV (Constant Voltage) charging at a current value of 0.5 C and CC discharging at a current value of 1 C in an atmosphere of 25° C. The voltage range for charging and discharging was set to 2.7 V to 4.4 V.
[0050] According to the following Production Examples 1 to 5, methacrylic acid ester polymers 1 to 5, which are random copolymers of MMA and OXMA, were synthesized.
[0051] [Production Example 1 (Synthesis of Methacrylic Acid Ester Polymer 1)] 2-cyano-2-propylbenzodithioate 9.3 mg, 2,2'-azobis(isobutyronitrile) (AIBN) 3.4 mg, and diethyl carbonate 1.00 g were added to prepare a polymerization initiator solution. 188.9 mg of methyl methacrylate, 811.1 mg of (3-ethyloxetan-3-yl)methyl methacrylate were placed in a thoroughly dried polymerization tube, and 0.10 g of polymerization initiator solution and 1.40 g of diethyl carbonate were added. The tube was immediately connected to a vacuum line, and degassed by repeating the freeze degassing method three times. The tube was sealed under reduced pressure, and reacted for 72 hours in a 60 ° C oil bath. Immediately after the reaction, the polymerization tube was cooled on ice, and then diluted with 5.69 g of diethyl carbonate to obtain a 13.9 mass % solution of methacrylic acid ester polymer (concentration is an actual measured value. The same as in Production Examples 2 and 3). 2.348 g of ethylene carbonate and 0.604 g of diethyl carbonate were added to 4,000 g of this solution to dilute it, and the solution was dried over a molecular sieve to obtain methacrylic acid ester polymer 1 as an 8 mass % solution.
[0052] [Production Example 2 (Synthesis of Methacrylic Acid Ester Polymer 2)] A polymerization initiator solution was prepared by adding 1.00 g of diethyl carbonate to 18.3 mg of 2-cyano-2-propyl benzodithioate and 6.8 mg of 2,2'-azobis(isobutyronitrile) (AIBN). 930.0 mg of methyl methacrylate and 570.2 mg of (3-ethyloxetan-3-yl)methyl methacrylate were placed in a thoroughly dried polymerization tube, and 0.10 g of polymerization initiator solution and 1.40 g of diethyl carbonate were added. The tube was immediately connected to a vacuum line, and degassed by repeating the freeze degassing method three times. The tube was sealed under reduced pressure and reacted for 72 hours in a 60°C oil bath. Immediately after the reaction, the polymerization tube was cooled on ice, and then diluted with 9.53 g of diethyl carbonate to obtain a 13.6% by mass solution of methacrylic acid ester polymer. 2.296 g of ethylene carbonate and 0.504 g of diethyl carbonate were added to 4,000 g of this solution to dilute it, and the solution was dried with a molecular sieve to obtain methacrylic acid ester polymer 2 as an 8 mass % solution.
[0053] [Production Example 3 (Synthesis of Methacrylic Acid Ester Polymer 3)] A polymerization initiator solution was prepared by adding 1.00 g of diethyl carbonate to 18.6 mg of 2-cyano-2-propyl benzodithioate and 6.9 mg of 2,2'-azobis(isobutyronitrile) (AIBN). 188.9 mg of methyl methacrylate and 811.1 mg of (3-ethyloxetan-3-yl)methyl methacrylate were placed in a thoroughly dried polymerization tube, and 0.10 g of polymerization initiator solution and 1.40 g of diethyl carbonate were added. The tube was immediately connected to a vacuum line, and degassed by repeating the freeze degassing method three times. The tube was sealed under reduced pressure and reacted for 48 hours in an oil bath at 60 ° C. Immediately after the reaction, the polymerization tube was cooled on ice, and then diluted with 5.59 g of diethyl carbonate to obtain a 14.1 mass% solution of methacrylic acid ester polymer. 2.380 g of ethylene carbonate and 0.668 g of diethyl carbonate were added to 4.000 g of this solution to dilute it, and the solution was dried with a molecular sieve to obtain methacrylic acid ester polymer 3 as an 8 mass % solution.
[0054] [Production Example 4 (Synthesis of Methacrylic Acid Ester Polymer 4)] In a thoroughly dried 3000mL separable flask, 165.0g of methyl methacrylate, 55.2g of (3-ethyloxetan-3-yl)methyl methacrylate, and 880.8g of ethylene carbonate were added, and the mixture was stirred for 90 minutes at 70°C with nitrogen bubbling, after which a solution of 0.364g of 2,2'-azobis(isobutyronitrile) (AIBN) dissolved in 3.27g of diethyl carbonate was added to initiate the reaction. After 3 and 6 hours of reaction, a solution of 0.108g of AIBN dissolved in 0.972g of diethyl carbonate was added, and the mixture was heated and stirred for a total of 9 hours, after which it was diluted with 28.8g of ethylene carbonate and 1618.5g of diethyl carbonate. This solution was dried with a molecular sieve to obtain methacrylic acid ester polymer 4 as an 8% by mass solution.
[0055] [Production Example 5 (Synthesis of Methacrylic Acid Ester Polymer 5)] In a thoroughly dried 3000mL separable flask, 55.1g of methyl methacrylate, 165.2g of (3-ethyloxetan-3-yl)methyl methacrylate, 323.6g of ethylene carbonate, and 557.2g of diethyl carbonate were added, and the mixture was stirred for 90 minutes while bubbling with nitrogen at 70°C. Then, a solution of 0.5461g of 2,2'-azobis(isobutyronitrile) (AIBN) dissolved in a mixed solvent of 1.201g of ethylene carbonate and 2.069g of diethyl carbonate was added to start the reaction. After 3 and 6 hours of reaction, a solution of 0.1621g of AIBN dissolved in 0.357g of ethylene carbonate and 0.614g of diethyl carbonate was added, and the mixture was heated and stirred for a total of 9 hours, and then diluted with 604.4g of ethylene carbonate and 1041.0g of diethyl carbonate. This solution was dried with a molecular sieve to obtain methacrylic acid ester polymer 5 as an 8% by mass solution.
[0056] [Preparation Example 1 (Preparation of Electrolyte 1)] In a glove box filled with dry nitrogen gas, the 8 mass% solution of the methacrylic acid ester polymer 1 obtained in Production Example 1, lithium hexafluorophosphate (LiPF6), and ethylene carbonate / diethyl carbonate (volume ratio: 3 / 7) were mixed and dissolved in predetermined amounts to obtain an electrolyte solution 1 having a lithium hexafluorophosphate concentration of 1 mol / L and a methacrylic acid ester polymer concentration of 1.8 mass%.
[0057] [Preparation Example 2 (Preparation of Electrolyte Solution 2)] In a glove box filled with dry nitrogen gas, an 8 mass% solution of the methacrylic acid ester polymer 2 obtained in Production Example 2, lithium hexafluorophosphate (LiPF6), and ethylene carbonate / diethyl carbonate (volume ratio: 3 / 7) were mixed and dissolved in predetermined amounts to obtain an electrolyte solution 2 having a lithium hexafluorophosphate concentration of 1 mol / L and a methacrylic acid ester polymer concentration of 2.0 mass%.
[0058] [Preparation Example 3 (Preparation of Electrolyte 3)] In a glove box filled with dry nitrogen gas, an 8 mass% solution of the methacrylic acid ester polymer 3 obtained in Production Example 3, lithium hexafluorophosphate (LiPF6), and ethylene carbonate / diethyl carbonate (volume ratio: 3 / 7) were mixed and dissolved in predetermined amounts to obtain an electrolyte solution 3 having a lithium hexafluorophosphate concentration of 1 mol / L and a methacrylic acid ester polymer concentration of 2.3 mass%.
[0059] [Preparation Example 4 (Preparation of Electrolyte 4)] In a glove box filled with dry nitrogen gas, the 8 mass% solution of the methacrylic acid ester polymer 4 obtained in Production Example 4, lithium hexafluorophosphate (LiPF6), and ethylene carbonate / diethyl carbonate (volume ratio: 3 / 7) were mixed and dissolved in predetermined amounts, and the concentration of lithium hexafluorophosphate in the electrolyte was adjusted to 1 mol / L and the concentration of the methacrylic acid ester polymer to 2.0 mass%, to obtain electrolyte solution 4.
[0060] [Preparation Example 5 (Preparation of Electrolyte Solution 5)] Electrolyte solution 5 was obtained in the same manner as in Preparation Example 4, except that the concentration of the methacrylic acid ester polymer in the electrolyte solution was 1.8 mass %.
[0061] [Preparation Example 6 (Preparation of Electrolyte 6)] In a glove box filled with dry nitrogen gas, the 8 mass% solution of the methacrylic acid ester polymer 5 obtained in Production Example 5, lithium hexafluorophosphate (LiPF6), and ethylene carbonate / diethyl carbonate (volume ratio: 3 / 7) were mixed and dissolved in predetermined amounts to prepare an electrolyte solution with a lithium hexafluorophosphate concentration of 1 mol / L and a methacrylic acid ester polymer concentration of 2.5 mass%, thereby obtaining electrolyte solution 6.
[0062] [Preparation Example 7 (Preparation of Electrolyte Solution 7)] Electrolyte solution 7 was obtained in the same manner as in Preparation Example 6, except that the concentration of the methacrylic acid ester polymer in the electrolyte solution was 2.0 mass %.
[0063] [Example 1 (Production and Evaluation of Lithium-Ion Secondary Battery)] (Preparation of positive electrode) LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 A positive electrode mixture-containing paste was prepared by adding N-methyl-2-pyrrolidone as a dispersion medium to 92 parts by mass of a positive electrode active material consisting of O2, 4 parts by mass of PVDF as a binder, 2 parts by mass of SuperP (manufactured by Timcal, carbon black) and 2 parts by mass of KS6 (manufactured by Timcal, graphite) as conductive assistants, and kneading them using a planetary mixer.
[0064] The paste containing the positive electrode mixture was applied to both sides of an aluminum foil (positive electrode current collector) having a thickness of 15 μm, and then vacuum dried at 130° C. for 8 hours to form a positive electrode mixture layer on both sides of the aluminum foil. Then, a press treatment was performed to adjust the thickness and density of the positive electrode mixture layer, and a belt-shaped positive electrode having a length of 60 mm and a width of 30 mm was produced. The positive electrode mixture layer in the obtained positive electrode had a thickness of 57 μm per side.
[0065] (Preparation of negative electrode) A paste containing a negative electrode mixture was prepared by adding water to and mixing 96 parts by mass of graphite having an average particle diameter D50 of approximately 10 μm as the negative electrode active material, 2.5 parts by mass of styrene butadiene rubber (SBR) as the binder, and 1.5 parts by mass of carboxymethylcellulose sodium salt (CMC) as the thickener.
[0066] The negative electrode mixture-containing paste was applied to both sides of a copper foil (negative electrode current collector) having a thickness of 10 μm, and then vacuum dried at 130 ° C for 8 hours to form a negative electrode mixture layer on both sides of the copper foil. Then, a press treatment was performed to adjust the thickness and density of the negative electrode mixture layer, and a strip-shaped negative electrode having a length of 62 mm and a width of 32 mm was produced. The negative electrode mixture layer in the obtained negative electrode had a thickness of 60 μm per side. The upper limit charging voltage of the battery at this time was set to 4.4 V, and the battery capacity was 0.5 Ah.
[0067] (Battery Assembly) The positive and negative electrodes obtained above were laminated with a polyolefin-based single-layer separator sandwiched between them, and the positive and negative electrodes were ultrasonically welded to the positive and negative terminals. The laminate was placed in an aluminum laminate packaging material and heat-sealed, leaving an opening for injection, to produce a positive electrode area of 18 cm. 2 , negative electrode area 19.8cm 2 A pre-injection battery was produced. Next, the electrolyte 1 obtained in Preparation Example 1 was injected from the opening for injection, and the opening was then sealed. Then, the battery was charged to 4.2 V at 0.2 C, and then heated in a thermostatic chamber at 60° C. for 20 hours to obtain a lithium ion secondary battery according to Example 1.
[0068] (Examples 2 to 3, Comparative Examples 1 to 4) Lithium ion secondary batteries according to Examples 2 to 3 and Comparative Examples 1 to 4 were produced in the same manner as in Example 1, except that the type of the electrolyte was changed as shown in Table 1 below.
[0069] For Examples 1 to 3 and Comparative Examples 1 to 4, the Mw, Mn, Mw / Mn, and m / n of the methacrylic acid ester polymer, the gelling property and viscosity of the electrolyte, and the measurement results of the output characteristics are shown in Table 1.
[0070] [Table 1]
[0071] As shown in Table 1, in Comparative Example 1, the weight-average molecular weight of the methacrylic acid ester polymer was large, the gelling property of the electrolyte was good, and the output characteristics and cycle characteristics of the battery were also good, but the viscosity of the electrolyte was high, and there was a risk of impregnation failure during injection. Therefore, as in Comparative Example 2, the concentration of the methacrylic acid ester polymer was reduced to 1.8 mass% to reduce the viscosity, but the viscosity was not sufficiently reduced at a concentration that could maintain the gelling property. Therefore, the battery characteristics were not evaluated in Comparative Example 2.
[0072] On the other hand, in Comparative Examples 3 and 4, the weight-average molecular weight of the methacrylic acid ester polymer was small and the viscosity of the electrolyte was reduced, but the molecular weight distribution was large and the number-average molecular weight was small, so that at the same methacrylic acid ester polymer concentration as in Comparative Example 1, the gelling property was poor as shown in Comparative Example 4. As shown in Comparative Example 3, the gelling property was improved by increasing the polymer concentration, but the output characteristics, 2C discharge capacity / 0.2C discharge capacity, were less than 0.85 and 3C discharge capacity / 0.2C discharge capacity, were less than 0.60, so good output characteristics were not obtained and the cycle characteristics were also significantly deteriorated.
[0073] In contrast, in Examples 1 to 3, the methacrylic acid ester polymer synthesized by living radical polymerization had a small weight-average molecular weight and a narrow molecular weight distribution, so that the gelling property of the electrolyte was good and the viscosity was low, and therefore the impregnation into the electrode during injection was excellent. In addition, the battery characteristics were also good output characteristics and cycle characteristics equivalent to those of Comparative Example 1, which used a methacrylic acid ester polymer with a large weight-average molecular weight. Therefore, good battery characteristics and improved injection properties of the electrolyte were achieved at the same time in the lithium ion secondary battery.
[0074] Although several embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. These embodiments and their omissions, substitutions, modifications, etc. are included in the scope and gist of the invention as well as the invention and its equivalents described in the claims.
Claims
1. An electrolyte solution comprising an aprotic solvent, a supporting salt, and a methacrylic acid ester polymer which is a copolymer of methyl methacrylate and (3-ethyloxetan-3-yl)methyl methacrylate and has a weight average molecular weight of 100,000 or more and 300,000 or less and a molecular weight distribution of less than 2, The content of the methacrylic acid ester polymer is 1.5 to 2.5% by mass of the total amount of the electrolyte solution.
2. 2. The electrolyte solution according to claim 1, comprising, as the aprotic solvent, at least one solvent selected from the group consisting of cyclic carbonates, chain carbonates, aliphatic carboxylic acid esters, γ-lactones, cyclic ethers, and chain ethers.
3. The supporting salt is LiPF 6 , LiBF 4 , LiAsF 6 , LiSbF 6 and LiN(SO 2 F) 2 The electrolyte solution according to claim 1 or 2, comprising at least one substance selected from the group consisting of:
4. A lithium ion secondary battery comprising a positive electrode, a negative electrode, and a polymer gel electrolyte obtained by crosslinking the methacrylic acid ester polymer using the electrolytic solution according to any one of claims 1 to 3.
5. The lithium ion secondary battery according to claim 4 , wherein the positive electrode contains a lithium-containing composite oxide as a positive electrode active material.
6. 6. The lithium ion secondary battery according to claim 4, wherein the negative electrode contains, as a negative electrode active material, a material selected from the group consisting of materials capable of absorbing and releasing lithium.
7. 7. The lithium ion secondary battery according to claim 6, wherein the material capable of absorbing and desorbing lithium includes a carbon material.
Citation Information
Patent Citations
Reactive polymer supporting porous film for separator for battery and electrode / separator assembly obtained therefrom
JP2009193755A
Polymer gel electrolyte and polymer secondary battery using same
WO2011004483A1
Lithium secondary battery
WO2016125726A1