MASK BLANK, PHASE SHIFT MASK AND METHOD FOR MANUFACTURING SEMICONDUCTOR DEVICE
A two-layer phase shift film structure with hafnium and oxygen in the upper layer and silicon and oxygen in the lower layer addresses the resistance issues, enabling accurate pattern transfer with enhanced cleaning and chemical resistance for semiconductor devices.
Patent Information
- Application Number
- JP2021048833
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-23
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-03-23
AI Technical Summary
Phase shift films containing hafnium, silicon, and oxygen lack sufficient cleaning resistance and chemical resistance to acids and alkalis, which is a challenge in achieving high-resolution pattern transfer for semiconductor devices.
A mask blank and phase shift mask configuration with a two-layer structure, where the upper layer contains hafnium and oxygen, and the lower layer contains silicon and oxygen, with specific thickness and composition ratios to enhance cleaning and chemical resistance, while maintaining optical performance.
The configuration ensures high cleaning and chemical resistance, allowing for accurate pattern transfer onto semiconductor devices with good optical performance and phase difference, thereby improving the manufacturing process.
Smart Images

Figure 0007558861000001 
Figure 0007558861000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a mask blank for a phase shift mask, a method for manufacturing a phase shift mask and a semiconductor device. [Background technology]
[0002] In the manufacturing process of semiconductor devices, fine patterns are formed using photolithography. In addition, many transfer masks are usually used to form these fine patterns. In order to miniaturize the patterns of semiconductor devices, it is necessary to not only miniaturize the mask patterns formed on the transfer masks, but also to shorten the wavelength of the exposure light source used in photolithography.
[0003] As such a photomask, Patent Document 1 discloses a dielectric mask including a light-transmitting substrate 1 capable of transmitting laser light, a metal film 17 laminated on the surface of the light-transmitting substrate 1 and having a high reflectivity for laser light, a dielectric multilayer thin film 4 formed by alternately laminating first and second dielectric members 2 and 3, each having a different refractive index, on this metal film 17, and a plurality of openings 18 formed to penetrate this dielectric multilayer thin film 4 and the metal film 17 and arranged in a predetermined pattern. Patent Document 2 discloses an excimer laser processing mask having a structure in which a combination of two layers is repeatedly formed on a surface of a glass substrate 3 transparent to ultraviolet light, opposite the ultraviolet light incident side, of a first dielectric layer 1 having a film thickness whose optical path length is ¼ wavelength of the ultraviolet light being used, and a second dielectric layer 2 having an optical path length similarly ¼ wavelength and smaller than the refractive index of the first dielectric layer being laminated on the first dielectric layer, to form a dielectric multilayer film having a third dielectric layer 1' as the top layer, which has a refractive index larger than that of the glass substrate and whose optical path length is ¼ wavelength of the ultraviolet light being used, and a metal film 4 as the top layer.
[0004] In these Patent Documents 1 and 2, a KrF excimer laser (wavelength 248 nm) is mainly used as an exposure light source when manufacturing semiconductor devices. However, in recent years, ArF excimer lasers (wavelength 193 nm) have increasingly been used as exposure light sources when manufacturing semiconductor devices.
[0005] One type of transfer mask is a halftone phase shift mask. As a mask blank for a halftone phase shift mask, a mask blank having a structure in which a phase shift film made of a material containing silicon and nitrogen, a light-shielding film made of a chromium-based material, and an etching mask film (hard mask film) made of an inorganic material are laminated on a light-transmitting substrate has been known for some time. When manufacturing a halftone phase shift mask using this mask blank, first, the etching mask film is patterned by dry etching with a fluorine-based gas using a resist pattern formed on the surface of the mask blank as a mask, then the light-shielding film is patterned by dry etching with a mixed gas of chlorine and oxygen using the etching mask film as a mask, and further the phase shift film is patterned by dry etching with a fluorine-based gas using the pattern of the light-shielding film as a mask. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 7-325384 [Patent Document 2] Japanese Patent Application Publication No. 8-171197 Summary of the Invention [Problem to be solved by the invention]
[0007] In recent years, with the miniaturization and complexity of patterns, there is a demand for higher resolution pattern transfer. In order to realize such high resolution pattern transfer, it is effective to increase the transmittance of the phase shift film. As such a phase shift film, a composition containing hafnium, silicon, and oxygen has been considered. When a transfer pattern is formed on a phase shift film, a cleaning process using an acid or alkali is performed. However, it has been found that a phase shift film containing hafnium, silicon, or oxygen may not have sufficient cleaning resistance (chemical resistance) against acids or alkalis.
[0008] The present invention has been made to solve the problems of the related art, and aims to provide a mask blank capable of manufacturing a phase shift mask that fully satisfies the required cleaning resistance and chemical resistance and has good optical performance. Another aim of the present invention is to provide a phase shift mask that fully satisfies the required cleaning resistance and chemical resistance and has good optical performance. And the present invention provides a method for manufacturing a semiconductor device using such a phase shift mask. [Means for solving the problem]
[0009] The present invention has the following configuration as a means for solving the above problems.
[0010] (Configuration 1) A mask blank having a phase shift film on a light-transmitting substrate, the phase shift film includes a lower layer and an upper layer, the upper layer is provided in contact with a surface of the lower layer opposite to the light-transmitting substrate, the underlayer contains silicon and oxygen; the overlayer contains hafnium and oxygen; The thickness of the upper layer is 5 nm or more, The thickness of the phase shift film is 90 nm or less. A mask blank comprising:
[0011] (Configuration 2) 2. The mask blank according to claim 1, wherein the total content of hafnium and oxygen in the upper layer is 90 atomic % or more. (Configuration 3) 3. The mask blank according to claim 1, wherein the total content of silicon and oxygen in the lower layer is 90 atomic % or more.
[0012] (Configuration 4) 4. The mask blank according to any one of configurations 1 to 3, wherein the oxygen content in each of the lower layer and the upper layer is 50 atomic % or more. (Configuration 5) the phase shift film has a bottom layer between the light-transmitting substrate and the lower layer, the bottom layer is provided in contact with a surface of the lower layer facing the light-transmitting substrate, The bottom layer contains hafnium and oxygen. 5. The mask blank according to any one of configurations 1 to 4.
[0013] (Configuration 6) The mask blank according to configuration 5, wherein the thickness of the bottom layer is 5 nm or more. (Configuration 7) 7. The mask blank according to claim 5, wherein the total content of hafnium and oxygen in the lowermost layer is 90 atomic % or more.
[0014] (Configuration 8) 8. The mask blank according to any one of configurations 5 to 7, wherein the oxygen content in the lowermost layer is 50 atomic % or more. (Configuration 9) 9. The mask blank according to any one of configurations 1 to 8, wherein the thickness of the lower layer is 5 nm or more.
[0015] (Configuration 10) 10. A mask blank according to any one of structures 1 to 9, wherein the phase shift film has a function of transmitting ArF excimer laser exposure light with a transmittance of 20% or more and a function of generating a phase difference of 150 degrees or more and 210 degrees or less between the exposure light that has transmitted through the phase shift film and the exposure light that has passed through air a distance equal to the thickness of the phase shift film. (Configuration 11) 11. The mask blank according to any one of configurations 1 to 10, further comprising a light-shielding film on the phase shift film.
[0016] (Configuration 12) A phase shift mask comprising a phase shift film having a transfer pattern formed on a light-transmitting substrate, the phase shift film includes a lower layer and an upper layer, the upper layer is provided in contact with a surface of the lower layer opposite to the light-transmitting substrate, the underlayer contains silicon and oxygen; the overlayer contains hafnium and oxygen; The thickness of the upper layer is 5 nm or more, The thickness of the phase shift film is 90 nm or less. 1. A phase shift mask comprising:
[0017] (Configuration 13) 13. The phase shift mask of claim 12, wherein the total content of hafnium and oxygen in the upper layer is 90 atomic % or more.
[0018] (Configuration 14) 14. The phase shift mask of claim 12, wherein the total content of silicon and oxygen in the lower layer is 90 atomic % or more. (Configuration 15) 15. The phase shift mask of any one of structures 12 to 14, wherein the oxygen content in each of the lower layer and the upper layer is 50 atomic % or more.
[0019] (Configuration 16) the phase shift film has a bottom layer between the light-transmitting substrate and the lower layer, the bottom layer is provided in contact with a surface of the lower layer facing the light-transmitting substrate, The bottom layer contains hafnium and oxygen. 16. The phase shift mask according to any one of structures 12 to 15. (Configuration 17) 17. The phase shift mask of claim 16, wherein the thickness of the bottom layer is 5 nm or more.
[0020] (Configuration 18) 18. The phase shift mask of claim 16, wherein the total content of hafnium and oxygen in the lowermost layer is 90 atomic % or more. (Configuration 19) 19. The phase shift mask of any one of structures 16 to 18, wherein the oxygen content in the lowermost layer is 50 atomic % or more.
[0021] (Configuration 20) 20. A phase shift mask as recited in any one of claims 12 to 19, wherein the thickness of the lower layer is 5 nm or more. (Configuration 21) 21. A phase shift mask according to any one of structures 12 to 20, wherein the phase shift film has a function of transmitting ArF excimer laser exposure light with a transmittance of 20% or more and a function of generating a phase difference of 150 degrees or more and 210 degrees or less between the exposure light that has passed through the phase shift film and the exposure light that has passed through air a distance equal to the thickness of the phase shift film.
[0022] (Configuration 22) 22. The phase shift mask according to any one of Structures 12 to 21, further comprising a light-shielding film having a light-shielding pattern formed on the phase shift film. (Configuration 23) 23. A method for manufacturing a semiconductor device, comprising the step of exposing and transferring a transfer pattern onto a resist film on a semiconductor substrate using the phase shift mask according to any one of claims 12 to 22. Effect of the Invention
[0023] The mask blank of the present invention having the above configuration is a mask blank having a phase shift film on a light-transmitting substrate, the phase shift film includes a lower layer and an upper layer, the upper layer is provided in contact with the surface of the lower layer opposite to the light-transmitting substrate, the lower layer contains silicon and oxygen, the upper layer contains hafnium and oxygen, the upper layer has a thickness of 5 nm or more, and the phase shift film has a thickness of 90 nm or less. Therefore, it is possible to manufacture a phase shift mask that fully meets the required cleaning resistance and chemical resistance and has good optical performance. Furthermore, in the manufacture of a semiconductor device using this phase shift mask, it is possible to transfer a pattern to a resist film or the like on the semiconductor device with good accuracy. [Brief description of the drawings]
[0024] [Figure 1] 1 is a schematic cross-sectional view of a mask blank according to a first embodiment. [Diagram 2] 2A to 2C are schematic cross-sectional views illustrating a manufacturing process of the phase shift mask according to the first embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] The present inventors have conducted extensive research into a phase shift film containing hafnium, silicon, and oxygen that can enhance the phase shift effect by increasing the transmittance of the ArF excimer laser exposure light (hereinafter, sometimes simply referred to as exposure light) to a certain level (e.g., 20% or more) and can suppress the film thickness of the phase shift film to a certain level (e.g., 90 nm or less), thereby achieving good optical performance. A phase shift film must have both the function of transmitting the exposure light at a predetermined transmittance and the function of generating a predetermined phase difference between the exposure light that passes through the phase shift film and the exposure light that passes through the air a distance equal to the thickness of the phase shift film. If the thickness of the phase shift film is to be kept below a certain level, it becomes difficult to ensure a desired phase difference. A single-layer phase shift film has a problem of low design freedom.
[0026] Therefore, the inventors of the present application have considered forming the phase shift film into at least a two-layer structure. In addition, when the phase shift film is configured to include a lower layer and an upper layer from the light-transmitting substrate side, the upper layer contains hafnium and oxygen, and the lower layer contains silicon and oxygen, and it has been found that the desired phase difference can be ensured and the film thickness can be suppressed. A thin film containing hafnium and oxygen has an optical characteristic in which the refractive index n for the exposure light is significantly large but the extinction coefficient k is relatively small. In addition, a thin film containing silicon and oxygen has an optical characteristic in which the refractive index n for the exposure light is relatively small but the extinction coefficient k is significantly small. However, it has been found that cleaning resistance and chemical resistance against acids and alkalis may not be sufficient under this condition alone. The material containing hafnium and oxygen itself is considered to be a material with high cleaning resistance and chemical resistance, and it was initially thought that sufficient cleaning resistance and chemical resistance could be obtained by forming the upper layer from this material containing hafnium and oxygen.
[0027] As a result of further investigation, the present inventors have found that the thickness of the above-mentioned upper layer is important in order to fully satisfy the required cleaning resistance and chemical resistance, that is, the thickness of the above-mentioned upper layer needs to be 5 nm or more in order to fully satisfy the required cleaning resistance and chemical resistance.
[0028] The present inventors speculate that the reason for this is as follows. In manufacturing a phase shift mask blank, a phase shift film is formed on a light-transmitting substrate by a sputtering method. When using a sputtering method, it is difficult to form a thin film with a stoichiometrically stable metal oxide. That is, even if a SiO2 target is used as the target for the lower layer and a HfO2 target is used as the target for the upper layer, it is difficult to form each layer formed by a sputtering method with stoichiometrically stable SiO2 or HfO2. For this reason, both the lower layer and the upper layer are likely to have a state in which the oxygen content is less than the stoichiometrically stable oxygen content, that is, a state in which oxygen deficiency occurs. And, due to these oxygen deficiencies, some atoms in the upper layer and the lower layer are likely to move, and mutual diffusion occurs near the interface between the upper layer and the lower layer, and it is presumed that silicon partially penetrates into the upper layer containing hafnium and oxygen.
[0029] In addition, a certain degree of internal stress occurs in a thin film formed by sputtering. If the internal stress of a thin film is high, it may cause misalignment when a pattern is formed on the thin film. For this reason, an annealing treatment is often performed on the thin film after the film formation. While this annealing treatment can reduce the internal stress, it is thought that it promotes the interdiffusion between the upper and lower layers described above. From these facts, if the thickness of the upper layer containing hafnium and oxygen is less than 5 nm, silicon will penetrate into the surface region of the upper layer, and the entire upper layer will contain hafnium, oxygen, and silicon. This is presumed to significantly reduce cleaning resistance and chemical resistance. In other words, in order to prevent such a state, it is presumed that the thickness of the upper layer needs to be 5 nm or more. The present invention has been made based on the above findings. Note that this speculation is based on the present inventors' current findings and does not limit the scope of the present invention in any way.
[0030] Hereinafter, the detailed configuration of the present invention will be described with reference to the drawings. Note that the same components in each drawing are denoted by the same reference numerals.
[0031] <First embodiment> Fig. 1 shows a schematic configuration of a mask blank of the first embodiment. The mask blank 100 shown in Fig. 1 has a configuration in which a phase shift film 2, a light-shielding film 3, and a hard mask film 4 are laminated in this order on one main surface of a light-transmitting substrate 1. The mask blank 100 may have a configuration in which the hard mask film 4 is not provided, if necessary. Moreover, the mask blank 100 may have a configuration in which a resist film is laminated on the hard mask film 4, if necessary. The main components of the mask blank 100 will be described in detail below.
[0032] [Transparent substrate] The light-transmitting substrate 1 is made of a material that has good transparency to the exposure light used in the exposure step in lithography. Examples of such materials that can be used include synthetic quartz glass, aluminosilicate glass, soda-lime glass, low-thermal expansion glass (SiO2-TiO2 glass, etc.), and various other glass substrates. In particular, a substrate made of synthetic quartz glass has high transparency to ArF excimer laser light (wavelength: about 193 nm), and can therefore be suitably used as the light-transmitting substrate 1 of the mask blank 100. It should be noted that the exposure process in lithography referred to here is the exposure process in lithography using a phase shift mask fabricated using this mask blank 100, and the exposure light refers to ArF excimer laser light (wavelength: 193 nm) unless otherwise specified. The refractive index of the material forming the light-transmitting substrate 1 in the exposure light is preferably 1.5 or more and 1.6 or less, more preferably 1.52 or more and 1.59 or less, and even more preferably 1.54 or more and 1.58 or less.
[0033] [Phase shift film] In order to obtain an appropriate phase shift effect, the phase shift film 2 is preferably adjusted to have a function of generating a phase difference of 150 degrees or more and 210 degrees or less between the exposure light that has passed through the phase shift film 2 and the exposure light that has passed through air a distance equal to the thickness of the phase shift film 2. The phase difference in the phase shift film 2 is more preferably 155 degrees or more, and even more preferably 160 degrees or more. On the other hand, the phase difference in the phase shift film 2 is more preferably 195 degrees or less, and even more preferably 190 degrees or less.
[0034] In order to generate a sufficient phase shift effect between the exposure light transmitted through the phase shift film 2 and the exposure light transmitted through the air, it is preferable that the phase shift film 2 has a relatively high transmittance. Specifically, it is preferable that the phase shift film 2 has a function of transmitting the exposure light with a transmittance of 20% or more, and more preferably 30% or more. This is to generate a sufficient phase shift effect between the exposure light transmitted through the phase shift film 2 and the exposure light transmitted through the air. In addition, the transmittance of the phase shift film 2 to the exposure light is preferably 60% or less, and more preferably 50% or less. This is to keep the film thickness of the phase shift film 2 within an appropriate range that ensures optical performance.
[0035] The phase shift film 2 in this embodiment has a structure in which a bottom layer 21, a lower layer 22, and an upper layer 23 are laminated from the light-transmitting substrate 1 side.
[0036] In order to ensure optical performance, the thickness of the phase shift film 2 is preferably 90 nm or less, more preferably 80 nm or less, and more preferably 70 nm or less. In order to ensure the function of generating a desired phase difference, the thickness of the phase shift film 2 is preferably 45 nm or more, and more preferably 50 nm or more.
[0037] The upper layer 23 preferably contains hafnium and oxygen, and more preferably consists of hafnium and oxygen. Here, "consisting of hafnium and oxygen" refers to a material that contains only elements that are unavoidably contained in the upper layer 23 when the layer is formed by sputtering, in addition to these constituent elements (noble gases such as helium (He), neon (Ne), argon (Ar), krypton (Kr) and xenon (Xe), hydrogen (H), carbon (C), etc.) (the same applies to the description of the lower layer 22, described later, that consists of silicon and oxygen). By minimizing the presence of other elements that bond with hafnium in the upper layer 23, the ratio of bonds between hafnium and oxygen in the upper layer 23 can be significantly increased. For this reason, the total content of hafnium and oxygen in upper layer 23 is preferably 90 atomic % or more, more preferably 95 atomic % or more, even more preferably 98 atomic % or more, and even more preferably 99 atomic % or more. The oxygen content in upper layer 23 is preferably 50 atomic % or more, more preferably 55 atomic % or more, and even more preferably 60 atomic % or more. From the viewpoint of etching rate, the oxygen content in upper layer 23 is preferably 66 atomic % or less, at which oxygen deficiency occurs, and more preferably 65 atomic % or less. Furthermore, the total content of the above elements (noble gases, hydrogen, carbon, etc.) that are unavoidably contained in the upper layer 23 is preferably 3 atomic % or less.
[0038] The upper layer 23 preferably has a refractive index n of 3.1 or less for the exposure light, and more preferably has a refractive index n of 3.0 or less. The upper layer 23 preferably has a refractive index n of 2.5 or more, and more preferably has a refractive index n of 2.6 or more. On the other hand, the upper layer 23 preferably has an extinction coefficient k of 0.4 or less for the exposure light, in order to increase the transmittance of the phase shift film 2 for the exposure light. The upper layer 23 preferably has an extinction coefficient k of 0.05 or more, and more preferably has a refractive index k of 0.1 or more, and even more preferably has a refractive index k of 0.2 or more.
[0039] The thickness of the upper layer 23 is preferably 5 nm or more, more preferably 6 nm or more, from the viewpoint of chemical resistance and cleaning resistance. And, from the viewpoint of optical properties, it is preferably 30 nm or less, more preferably 20 nm or less, and even more preferably 15 nm or less. As described above, when the thickness of the upper layer 23 containing hafnium and oxygen is less than 5 nm, the interdiffusion occurring at the interface with the lower layer containing silicon and oxygen is likely to spread to the entire upper layer 23. A thin film containing hafnium, silicon, and oxygen has low chemical resistance and cleaning resistance. The upper layer 23 in which the entire layer is interdiffused has low chemical resistance and cleaning resistance. If the thickness of the upper layer 23 is 5 nm or more, the entire upper layer 23 can be prevented from interdiffusing, and the deterioration of the chemical resistance and cleaning resistance of the upper layer 23 can be prevented.
[0040] Preferably, underlayer 22 contains silicon and oxygen, and more preferably consists of silicon and oxygen. The proportion of silicon and oxygen bonds in underlayer 22 can be significantly increased by minimizing the presence of other elements that bond with silicon in underlayer 22. For this reason, the total content of silicon and oxygen in lower layer 22 is preferably 90 atomic % or more, more preferably 95 atomic % or more, and even more preferably 98 atomic % or more. From the viewpoint of being able to suppress diffusion of silicon into upper layer 23, the oxygen content in lower layer 22 is preferably 50 atomic % or more, more preferably 55 atomic % or more, and even more preferably 60 atomic % or more. Furthermore, the total content of the above elements (noble gases, hydrogen, carbon, etc.) that are unavoidably contained in lower layer 22 is preferably 3 atomic % or less.
[0041] The lower layer 22 preferably has a refractive index n of 2.0 or less to the exposure light, and more preferably has a refractive index n of 1.8 or less. The lower layer 22 preferably has a refractive index n of 1.5 or more, and more preferably has a refractive index n of 1.52 or more. On the other hand, the lower layer 22 is required to have an extinction coefficient k to the exposure light smaller than those of the lowermost layer 21 and the upper layer 23, and is preferably less than 0.05, and more preferably 0.02 or less. This is to increase the transmittance of the phase shift film 2 to the exposure light.
[0042] The thickness of the underlayer 22 is preferably 5 nm or more, more preferably 7 nm or more, from the viewpoint of chemical resistance and cleaning resistance of the sidewall of the pattern to be formed, and is preferably 30 nm or less, more preferably 20 nm or less, in order to suppress the film thickness of the phase shift film 2.
[0043] In the present embodiment, bottom layer 21 preferably contains hafnium and oxygen, and more preferably consists of hafnium and oxygen, like upper layer 23. When bottom layer 21 is configured to contain hafnium and oxygen, specific matters regarding the preferred total content of hafnium and oxygen, the preferred oxygen content, the refractive index n for the exposure light, and the extinction coefficient k for the exposure light are the same as those for upper layer 23. From the viewpoint of chemical resistance and cleaning resistance of the sidewall of the pattern to be formed, the thickness of the bottom layer 21 is preferably 5 nm or more, and more preferably 6 nm or more, and is preferably 50 nm or less, and more preferably 40 nm or less. The material of the bottom layer 21 is not limited to the above-mentioned materials, and may be composed of other materials (e.g., transition metal silicide-based materials, SiN-based materials, chromium-based materials, tantalum-based materials, etc.) in addition to or instead of hafnium and oxygen.
[0044] It is more preferable that the thickness of the bottom layer 21 of the phase shift film 2 is thicker than that of the top layer 23. When the phase shift film 2 is patterned, in order to increase the verticality of the pattern sidewalls formed, the dry etching is continued even after the etching of the phase shift film 2 reaches the surface of the transparent substrate 1, that is, so-called overetching is performed. In the overetching, the transparent substrate 1 side of the pattern sidewalls formed in the phase shift film 2 is mainly etched. The lower layer 22 contains silicon and oxygen, and has a slower etching rate in dry etching than the bottom layer 21. When the bottom layer 21 is thick, the ratio of the bottom layer 21 to the transparent substrate 1 side of the pattern sidewalls of the phase shift film 2 is relatively high. In this case, the verticality of the pattern sidewalls of the phase shift film 2 can be easily controlled by overetching.
[0045] The refractive index n and extinction coefficient k of a thin film including the phase shift film 2 are not determined only by the composition of the thin film. The film density and crystalline state of the thin film also affect the refractive index n and extinction coefficient k. For this reason, the conditions for forming the thin film by reactive sputtering are adjusted so that the thin film has the desired refractive index n and extinction coefficient k. In order to set the refractive index n and extinction coefficient k of the phase shift film 2 within the above range, it is not limited to only adjusting the ratio of the mixed gas of the noble gas and the reactive gas (oxygen gas, nitrogen gas, etc.) when forming the film by reactive sputtering. There are many factors, such as the pressure in the film formation chamber when forming the film by reactive sputtering, the power applied to the sputtering target, and the positional relationship such as the distance between the target and the light-transmitting substrate 1. These film formation conditions are specific to the film formation device and are appropriately adjusted so that the thin film formed has the desired refractive index n and extinction coefficient k.
[0046] [Light-shielding film] The mask blank 100 includes a light-shielding film 3 on a phase shift film 2. In general, in a phase shift mask, the peripheral region of the region where a transfer pattern is formed (transfer pattern forming region) is required to have an optical density (OD) of a predetermined value or more so that the resist film is not affected by the exposure light transmitted through the peripheral region when the resist film on the semiconductor wafer is exposed and transferred using an exposure device. The peripheral region of the phase shift mask preferably has an OD of 2.8 or more, more preferably 3.0 or more. As described above, the phase shift film 2 has a function of transmitting the exposure light at a predetermined transmittance, and it is difficult to ensure a predetermined optical density with the phase shift film 2 alone. For this reason, it is necessary to laminate a light-shielding film 3 on the phase shift film 2 at the stage of manufacturing the mask blank 100 in order to ensure the insufficient optical density. By configuring the mask blank 100 in this way, if the light-shielding film 3 is removed from the region where the phase shift effect is used (basically the transfer pattern forming region) during the manufacturing process of the phase shift mask 200 (see FIG. 2), a phase shift mask 200 with a predetermined optical density in the peripheral region can be manufactured.
[0047] Either a single-layer structure or a laminated structure of two or more layers can be applied to the light-shielding film 3. In addition, each layer of the light-shielding film 3 having a single-layer structure and a laminated structure of two or more layers may have substantially the same composition in the thickness direction of the film or layer, or may have a composition gradient in the thickness direction of the layer.
[0048] The mask blank 100 in the embodiment shown in FIG. 1 has a configuration in which a light-shielding film 3 is laminated on a phase shift film 2 without any other film therebetween. In this configuration, the light-shielding film 3 needs to be made of a material having sufficient etching selectivity with respect to an etching gas used when forming a pattern in the phase shift film 2. In this case, the light-shielding film 3 is preferably made of a material containing chromium. Examples of the chromium-containing material for forming the light-shielding film 3 include chromium metal and materials containing chromium and one or more elements selected from oxygen, nitrogen, carbon, boron, and fluorine.
[0049] Generally, chromium-based materials are etched with a mixed gas of chlorine-based gas and oxygen gas, but the etching rate of chromium metal with respect to this etching gas is not very high. In consideration of increasing the etching rate with the mixed gas of chlorine-based gas and oxygen gas, the material for forming the light-shielding film 3 is preferably a material containing chromium and one or more elements selected from oxygen, nitrogen, carbon, boron, and fluorine. In addition, the chromium-containing material for forming the light-shielding film 3 may contain one or more elements of molybdenum, indium, and tin. By containing one or more elements of molybdenum, indium, and tin, the etching rate with respect to the mixed gas of chlorine-based gas and oxygen gas can be made faster.
[0050] Moreover, if the hard mask film 4 described later is formed on the light-shielding film 3 from a material containing chromium, the light-shielding film 3 may be formed from a material containing silicon. In particular, materials containing transition metals and silicon have high light-shielding performance, and the thickness of the light-shielding film 3 can be reduced. Examples of transition metals contained in the light-shielding film 3 include any one of molybdenum (Mo), tantalum (Ta), tungsten (W), titanium (Ti), chromium (Cr), nickel (Ni), vanadium (V), zirconium (Zr), ruthenium (Ru), rhodium (Rh), zinc (Zn), niobium (Nb), palladium (Pd), and alloys of these metals. Examples of metal elements other than the transition metal elements contained in the light-shielding film 3 include aluminum (Al), indium (In), tin (Sn), and gallium (Ga).
[0051] On the other hand, the light-shielding film 3 may have a structure in which a layer containing chromium and a layer containing a transition metal and silicon are laminated in this order from the side of the phase shift film 2. In this case, specific matters regarding the materials of the layer containing chromium and the layer containing a transition metal and silicon are the same as those in the light-shielding film 3 described above.
[0052] [Hard mask film] The hard mask film 4 is provided in contact with the surface of the light-shielding film 3. The hard mask film 4 is a film formed of a material having etching resistance against the etching gas used when etching the light-shielding film 3. This hard mask film 4 only needs to have a thickness that allows it to function as an etching mask until the dry etching for forming a pattern in the light-shielding film 3 is completed, and is basically not limited by its optical properties. Therefore, the thickness of the hard mask film 4 can be significantly thinner than the thickness of the light-shielding film 3.
[0053] When the light-shielding film 3 is made of a material containing chromium, the hard mask film 4 is preferably made of a material containing silicon. In this case, the hard mask film 4 tends to have low adhesion to a resist film made of an organic material, so it is preferable to treat the surface of the hard mask film 4 with HMDS (Hexamethyldisilazane) to improve the adhesion of the surface. In this case, the hard mask film 4 is more preferably made of SiO2, SiN, SiON, or the like.
[0054] In addition, when the light-shielding film 3 is formed of a material containing chromium, the material of the hard mask film 4 may be a material containing tantalum in addition to the above. In this case, the material containing tantalum may be tantalum metal, or a material containing tantalum and one or more elements selected from nitrogen, oxygen, boron, and carbon. For example, Ta, TaN, TaO, TaON, TaBN, TaBO, TaBON, TaCN, TaCO, TaCON, TaBCN, TaBOCN, etc. are included. In addition, when the light-shielding film 3 is formed of a material containing silicon, the hard mask film 4 is preferably formed of the material containing chromium.
[0055] In the mask blank 100, a resist film made of an organic material is preferably formed with a thickness of 100 nm or less in contact with the surface of the hard mask film 4. In the case of a fine pattern corresponding to the DRAM hp32 nm generation, a transfer pattern (phase shift pattern) to be formed in the hard mask film 4 may be provided with a SRAF (Sub-Resolution Assist Feature) with a line width of 40 nm. However, even in this case, the cross-sectional aspect ratio of the resist pattern can be made low at 1:2.5, so that the resist pattern can be prevented from collapsing or detaching during development, rinsing, etc. of the resist film. It is more preferable that the resist film has a thickness of 80 nm or less.
[0056] [Resist film] In the mask blank 100, a resist film made of an organic material is preferably formed with a thickness of 100 nm or less on the surface of the hard mask film 4. In the case of a fine pattern corresponding to the DRAM hp32 nm generation, a SRAF (Sub-Resolution Assist Feature) with a line width of 40 nm may be provided in the light-shielding pattern to be formed in the light-shielding film 3. However, even in this case, the thickness of the resist film can be suppressed by providing the hard mask film 4 as described above, and the cross-sectional aspect ratio of the resist pattern composed of this resist film can be reduced to 1:2.5. Therefore, the resist pattern can be prevented from collapsing or detaching during development, rinsing, etc. of the resist film. It is more preferable that the resist film has a thickness of 80 nm or less. The resist film is preferably a resist for electron beam lithography exposure, and more preferably the resist is a chemically amplified type.
[0057] The phase shift film 2 in the mask blank 100 of the first embodiment can be patterned by a multi-stage dry etching process using a chlorine-based gas and a fluorine-based gas. It is preferable to pattern the bottom layer 21 and the upper layer 23 by dry etching using a chlorine-based gas, and the lower layer 22 by dry etching using a fluorine-based gas. The etching selectivity is very high between the bottom layer 21 and the lower layer 22, and between the lower layer 22 and the upper layer 23. Although not particularly limited, by performing an etching process in multiple stages on the phase shift film 2 having the above characteristics, the effect of side etching can be suppressed and a good pattern cross-sectional shape can be obtained.
[0058] In general, when a pattern is formed on a thin film by dry etching, additional etching (so-called overetching) is performed to improve the verticality of the sidewalls of the pattern formed on the thin film. In addition, the overetching is often set based on the time when the etching reaches the bottom surface of the thin film, that is, the so-called just etching time. As described above, by applying an etching process divided into multiple stages to the patterning of the phase shift film 2, the time based on the overetching time can be set to the just etching time of the bottom layer 21 of the phase shift film 2. This makes it possible to shorten the overetching time and obtain good etching depth uniformity. Here, the chlorine-based gas is preferably a chlorine-based gas containing boron, more preferably BCl3 gas, and even more preferably a mixed gas of BCl3 gas and Cl2 gas.
[0059] Although the phase shift film 2 has a three-layer structure in the first embodiment, the present invention is not limited thereto. As long as it has the above-mentioned upper layer 23 and lower layer 22 and satisfies the desired transmittance, retardation, and film thickness as a phase shift film, it may have a two-layer structure or a four-layer or more structure. In addition, the mask blank 100 in the first embodiment forms the phase shift film 2 in contact with the surface of the light-transmitting substrate 1, but is not limited thereto. For example, when the phase shift film 2 is composed of two layers, an upper layer 23 and a lower layer 22, an etching stopper film may be provided between the light-transmitting substrate 1 and the phase shift film 2. In this case, the etching stopper film is preferably formed of a material containing aluminum, one or more elements selected from hafnium, chromium, and silicon, and oxygen. For example, the material of the etching stopper film may be a material containing aluminum, silicon, and oxygen, or a material containing aluminum, hafnium, and oxygen. In particular, the etching stopper film is preferably formed of a material containing aluminum, hafnium, and oxygen.
[0060] [Mask blank manufacturing procedure] The mask blank 100 having the above configuration is manufactured in the following procedure. First, a light-transmitting substrate 1 is prepared. The end faces and main surface of this light-transmitting substrate 1 are polished to a predetermined surface roughness (for example, a root-mean-square roughness Sq of 0.2 nm or less within an inner region of a rectangle with sides of 1 μm), and then the substrate is subjected to a predetermined cleaning process and drying process.
[0061] Next, the phase shift film 2 is formed on the transparent substrate 1 by sputtering, starting from the bottom layer 21, followed by the bottom layer 22 and the top layer 23, so that each layer has the desired thickness as described above. The bottom layer 21, the bottom layer 22 and the top layer 23 of the phase shift film 2 are formed by sputtering, and any sputtering such as DC sputtering, RF sputtering and ion beam sputtering can be applied. In consideration of the film formation rate, it is preferable to apply DC sputtering. In the case of using a target with low conductivity, it is preferable to apply RF sputtering or ion beam sputtering, but in consideration of the film formation rate, it is more preferable to apply RF sputtering.
[0062] For the bottom layer 21 and top layer 23 of the phase shift film 2, either a sputtering target containing hafnium or a sputtering target containing hafnium and oxygen can be used. For the lower layer 22 of the phase shift film 2, either a sputtering target containing silicon or a sputtering target containing silicon and oxygen can be used.
[0063] After the phase shift film 2 is formed, an annealing process is appropriately performed at a predetermined heating temperature. Next, the above-mentioned light-shielding film 3 is formed on the phase shift film 2 by a sputtering method. Then, the above-mentioned hard mask film 4 is formed on the light-shielding film 3 by a sputtering method. In the film formation by the sputtering method, a sputtering target and a sputtering gas containing the materials constituting each of the above-mentioned films at a predetermined composition ratio are used, and further, if necessary, a mixed gas of the above-mentioned noble gas and reactive gas is used as the sputtering gas for film formation. After this, if the mask blank 100 has a resist film, if necessary, HMDS (Hexamethyldisilazane) treatment is performed on the surface of the hard mask film 4. Then, a resist film is formed on the surface of the hard mask film 4 that has been subjected to the HMDS treatment by a coating method such as a spin coat method, and the mask blank 100 is completed. Thus, according to the mask blank 100 of the first embodiment, it is possible to manufacture a phase shift mask 200 that fully satisfies the required cleaning resistance and chemical resistance and has good optical performance.
[0064] Phase Shift Mask and Manufacturing Method Thereof 2 shows a phase shift mask 200 according to an embodiment of the present invention manufactured from the mask blank 100 of the above embodiment and its manufacturing process. As shown in FIG. 2(g), the phase shift mask 200 is characterized in that a phase shift pattern 2a, which is a transfer pattern, is formed on the phase shift film 2 of the mask blank 100, and a light-shielding pattern 3b having a pattern including a light-shielding band is formed on the light-shielding film 3. This phase shift mask 200 has the same technical features as the mask blank 100. Matters related to the light-transmitting substrate 1, the bottom layer 21, the lower layer 22, the upper layer 23 of the phase shift film 2, and the light-shielding film 3 in the phase shift mask 200 are the same as those in the mask blank 100. The hard mask film 4 is removed during the preparation of this phase shift mask 200.
[0065] The method for manufacturing the phase shift mask 200 according to the embodiment of the present invention uses the above-mentioned mask blank 100, and is characterized by including a step of forming a transfer pattern in the light-shielding film 3 by dry etching, a step of forming a transfer pattern in the phase shift film 2 by dry etching using the light-shielding film 3 having the transfer pattern as a mask, and a step of forming a light-shielding pattern 3b in the light-shielding film 3 by dry etching using a resist film (resist pattern 6b) having the light-shielding pattern as a mask. Hereinafter, the method for manufacturing the phase shift mask 200 of the present invention will be described according to the manufacturing steps shown in FIG. 2. Hereinafter, the method for manufacturing the phase shift mask 200 using the mask blank 100 in which the hard mask film 4 is laminated on the light-shielding film 3 will be described. Also, the case where a material containing chromium is applied to the light-shielding film 3 and a material containing silicon is applied to the hard mask film 4 will be described.
[0066] First, a resist film is formed by spin coating in contact with the hard mask film 4 of the mask blank 100. Next, a first pattern, which is a transfer pattern (phase shift pattern) to be formed in the phase shift film 2, is exposed to the resist film by electron beam and then subjected to predetermined processes such as development to form a first resist pattern 5a having a phase shift pattern (see FIG. 2(a)). Next, using the first resist pattern 5a as a mask, dry etching is performed using a fluorine-based gas to form a first pattern (hard mask pattern 4a) in the hard mask film 4 (see FIG. 2(b)).
[0067] Next, after removing the resist pattern 5a, a predetermined process such as cleaning with an acid or alkali is performed, and then dry etching is performed with a mixed gas of chlorine-based gas and oxygen gas using the hard mask pattern 4a as a mask to form a first pattern (light-shielding pattern 3a) in the light-shielding film 3 (see FIG. 2(c)). Next, dry etching with a chlorine-based gas and dry etching with a fluorine-based gas are alternately performed three times using the light-shielding pattern 3a as a mask to form a first pattern (phase shift pattern 2a) in the phase shift film 2, and the hard mask pattern 4a is removed (see FIG. 2(d)). More specifically, dry etching with a chlorine-based gas is performed on the bottom layer 21 and the upper layer 23, and dry etching with a fluorine-based gas is performed on the lower layer 22.
[0068] Next, a resist film is formed on the mask blank 100 by spin coating. Next, a second pattern, which is a pattern (light-shielding pattern) to be formed on the light-shielding film 3, is exposed to and written on the resist film by electron beam exposure, and then a predetermined process such as development is performed to form a second resist pattern 6b having a light-shielding pattern (see FIG. 2(e)). Next, using the second resist pattern 6b as a mask, dry etching is performed using a mixed gas of chlorine gas and oxygen gas to form a second pattern (light-shielding pattern 3b) on the light-shielding film 3 (see FIG. 2(f)). Furthermore, the second resist pattern 6b is removed, and a predetermined process such as cleaning using an acid or alkali is performed to obtain a phase shift mask 200 (see FIG. 2(g)).
[0069] The chlorine-based gas used in the dry etching is not particularly limited as long as it contains Cl. Examples include Cl2, SiCl2, CHCl3, CH2Cl2, CCl4, and BCl3. The chlorine-based gas used in the dry etching of the bottom layer 21 and the top layer 23 is preferably one containing boron, and more preferably one containing BCl3. In particular, a mixed gas of BCl3 gas and Cl2 gas is preferable because it has a relatively high etching rate for hafnium.
[0070] Phase shift mask 200 manufactured by the manufacturing method shown in FIG. 2 is a phase shift mask comprising, on light-transmitting substrate 1, phase shift film 2 having a transfer pattern (phase shift pattern 2a).
[0071] By manufacturing phase shift mask 200 in this manner, it is possible to obtain phase shift mask 200 that fully satisfies the required cleaning resistance and chemical resistance and has good optical performance. Then, when phase shift mask 200 having this phase shift film is set in an exposure tool and exposed and transferred onto a transfer target (such as a resist film on a semiconductor substrate), an exposure margin can be ensured.
[0072] On the other hand, the etching process used in the above-mentioned phase shift mask manufacturing method is not only applicable to the mask blank of the present invention, but can be used in a wider range of applications. In a mask blank having a pattern-forming thin film including a structure in which a layer containing oxygen and silicon and a layer containing hafnium and oxygen are stacked in this order on a substrate, it can also be applied when forming a transfer pattern in the pattern-forming thin film. The transfer mask manufacturing method, which is an application of the above-mentioned phase shift mask manufacturing method, preferably has the following configuration.
[0073] That is, a method for producing a transfer mask using a mask blank having a pattern-forming thin film on a substrate, comprising the steps of: the pattern-forming thin film includes a structure in which a lower layer containing silicon and oxygen and an upper layer containing hafnium and oxygen are laminated in this order from the substrate side, performing dry etching using a boron-containing chlorine-based gas to form a transfer pattern on the upper layer; performing dry etching using a fluorine-based gas by using the upper layer on which the transfer pattern is formed as a mask to form a transfer pattern on the lower layer; The method for producing a transfer mask is characterized by comprising the steps of:
[0074] Furthermore, the method for manufacturing a semiconductor device of the present invention is characterized by comprising a step of exposing and transferring a transfer pattern onto a resist film on a semiconductor substrate using the phase shift mask 200 described above.
[0075] Since the phase shift mask 200 and mask blank 100 of the present invention have the above-mentioned effects, when the phase shift mask 200 is set on the mask stage of an exposure apparatus using an ArF excimer laser as exposure light and a transfer pattern is transferred by exposure to a resist film on a semiconductor device, the transfer pattern can be transferred to the resist film on the semiconductor device with high CD uniformity. Therefore, when a circuit pattern is formed by dry etching an underlying film using the resist film pattern as a mask, a highly accurate circuit pattern can be formed without wiring short circuits or breaks due to a decrease in CD uniformity. EXAMPLES
[0076] In the following, Example 1 and Comparative Example 1 will be described in more detail to explain the embodiment of the present invention.
[0077] Example 1 [Mask blank manufacturing] Referring to Fig. 1, a light-transmitting substrate 1 was prepared, which is made of synthetic quartz glass and has a main surface with dimensions of about 152 mm x about 152 mm and a thickness of about 6.35 mm. The end faces and main surface of this light-transmitting substrate 1 are polished to a predetermined surface roughness (0.2 nm or less in square), and then subjected to a predetermined cleaning and drying process. When the optical characteristics of the light-transmitting substrate 1 were measured using a spectroscopic ellipsometer (JA Woollam M-2000D), the refractive index for light with a wavelength of 193 nm was 1.556 and the extinction coefficient was 0.000.
[0078] Next, the transparent substrate 1 was placed in a single-wafer RF sputtering apparatus, and a phase shift film 2 was formed on the transparent substrate 1 by sputtering (RF sputtering) using an HfO2 target and an SiO2 target alternately and argon (Ar) gas as a sputtering gas, the phase shift film 2 being composed of a bottom layer 21 composed of hafnium and oxygen, a lower layer 22 composed of silicon and oxygen, and an upper layer 23 composed of hafnium and oxygen. The thickness D1 of the bottom layer 21 was 38 nm, the thickness of the lower layer 22 was 16 nm, and the thickness of the upper layer 23 was 5 nm, all of which were 5 nm or more. The thickness of the phase shift film 2 was 59 nm, which was 90 nm or less.
[0079] Next, the transparent substrate 1 on which the phase shift film 2 was formed was subjected to a heat treatment to reduce the film stress of the phase shift film 2. The transmittance and phase difference of the phase shift film 2 after the heat treatment for light with a wavelength of 193 nm were measured using a phase shift amount measuring device (MPM193 manufactured by Lasertec Corporation), and the transmittance was 40.9% and the phase difference was 177.2 degrees (deg.). In addition, the optical properties of the phase shift film 2 were measured using a spectroscopic ellipsometer (M-2000D manufactured by JA Woollam Co., Ltd.), and the refractive index n and extinction coefficient k of the bottom layer 21 and top layer 23 for light with a wavelength of 193 nm were 2.93 and 0.24, respectively, and the refractive index n and extinction coefficient k of the bottom layer 22 were 1.56 and 0.00, respectively. Moreover, the oxygen content in the upper layer 23 of this phase shift film 2 was 66 atomic % or less, and oxygen deficiency occurred.
[0080] Next, the light-transmitting substrate 1 on which the phase shift film 2 was formed was placed in a single-wafer RF sputtering apparatus, and reactive sputtering (RF sputtering) was performed in a mixed gas atmosphere of argon (Ar), carbon dioxide (CO2) and helium (He) using a chromium (Cr) target. As a result, a light-shielding film (CrOC film) 3 composed of chromium, oxygen and carbon was formed in contact with the phase shift film 2 with a thickness of 53 nm.
[0081] Next, the light-transmitting substrate 1 on which the light-shielding film (CrOC film) 3 was formed was subjected to a heat treatment. After the heat treatment, the optical density of the laminated structure of the phase shift film 2 and the light-shielding film 3 of the light-transmitting substrate 1 on which the phase shift film 2 and the light-shielding film 3 were laminated was measured at the wavelength (about 193 nm) of the light of an ArF excimer laser using a spectrophotometer (Cary4000 manufactured by Agilent Technologies). It was confirmed that the optical density was 3.0 or more.
[0082] Next, the light-transmitting substrate 1 on which the phase shift film 2 and the light-shielding film 3 were laminated was placed in a single-wafer RF sputtering apparatus, and a hard mask film 4 composed of silicon and oxygen was formed to a thickness of 12 nm on the light-shielding film 3 by RF sputtering using a silicon dioxide (SiO2) target and argon (Ar) gas as a sputtering gas. A predetermined cleaning process was then performed, and the mask blank 100 of Example 1 was manufactured.
[0083] [Cleaning test (chemical resistance test)] In addition, the phase shift film of Example 1 was formed on another light-transmitting substrate, and a cleaning test (chemical resistance test) was performed after performing a desired annealing treatment. Specifically, the phase shift film of Example 1 was formed on another light-transmitting substrate, and an annealing treatment was performed at 500 degrees for 30 minutes. Then, the entire surface (front and side surfaces) of the phase shift film of Example 1 was subjected to SC-1 cleaning (ammonia-hydrogen peroxide solution cleaning) and SPM cleaning (sulfuric acid / hydrogen peroxide cleaning) five times each for a predetermined period of time. A rinse treatment with pure water was performed between the SC-1 cleaning and the SPM cleaning. After carrying out this cleaning test, the surface and sides of the phase shift film in Example 1 were observed for the presence or absence of film loss, and almost no film loss was observed on either the surface or sides.
[0084] [Phase shift mask manufacturing] Next, the mask blank 100 of Example 1 was used to manufacture the halftone phase shift mask 200 of Example 1 in the following procedure. First, the surface of the hard mask film 4 was treated with HMDS. Then, a resist film made of a chemically amplified resist for electron beam lithography was formed with a thickness of 80 nm on the surface of the hard mask film 4 by spin coating. Next, a first pattern, which is a phase shift pattern to be formed in the phase shift film 2, was lithographed on the resist film with an electron beam, and a predetermined development process and a cleaning process using an acid or alkali were performed to form a resist pattern 5a having the first pattern (see FIG. 2(a)).
[0085] Next, using the resist pattern 5a as a mask, dry etching was performed using CF4 gas to form a first pattern (hard mask pattern 4a) in the hard mask film 4 (see FIG. 2(b)).
[0086] Next, the resist pattern 5a was removed. After a cleaning process using an acid or alkali, dry etching was performed using a mixture of chlorine gas (Cl2) and oxygen gas (O2) with the hard mask pattern 4a as a mask to form a first pattern (light-shielding pattern 3a) in the light-shielding film 3 (see FIG. 2(c)).
[0087] Next, using the light-shielding pattern 3a as a mask, dry etching was performed to form a first pattern (phase shift pattern 2a) in the phase shift film 2, and at the same time, the hard mask pattern 4a was removed (see FIG. 2(d)). At this time, the bottom layer 21 and the upper layer 23 were dry-etched with a mixed gas of BCl3 gas and Cl2 gas, and the lower layer 22 was dry-etched with a fluorine-based gas (mixed gas of SF6 and He).
[0088] Next, a resist film made of a chemically amplified resist for electron beam lithography was formed on the light-shielding pattern 3a with a thickness of 150 nm by spin coating. Next, a second pattern, which is a pattern to be formed on the light-shielding film (a pattern including a light-shielding band pattern), was exposed and written on the resist film, and a predetermined process such as a development process was performed to form a resist pattern 6b having a light-shielding pattern (see FIG. 2(e)). Next, using the resist pattern 6b as a mask, dry etching was performed using a mixed gas of chlorine gas (Cl2) and oxygen gas (O2), and a second pattern (light-shielding pattern 3b) was formed on the light-shielding film 3 (see FIG. 2(f)). Furthermore, the resist pattern 6b was removed, and a predetermined process such as washing with an acid or alkali was performed to obtain a phase shift mask 200 (see FIG. 2(g)). When the cross section of phase shift pattern 2a in phase shift mask 200 of Example 1 was observed, no film loss was observed on either the surface or the side of phase shift pattern 2a, and phase shift pattern 2a was in a good condition.
[0089] [Evaluation of pattern transfer performance] A simulation of a transferred image was performed by exposing the phase shift mask 200 produced by the above procedure to a resist film on a semiconductor device using an AIMS193 (manufactured by Carl Zeiss) with exposure light of a wavelength of 193 nm. When the exposure transfer image of this simulation was verified, it was found that the CD in-plane uniformity was high and the design specifications were fully satisfied. From this result, it can be said that even if the phase shift mask 200 of this Example 1 is set on the mask stage of an exposure tool and exposed and transferred to a resist film on a semiconductor device, the circuit pattern finally formed on the semiconductor device can be formed with high accuracy.
[0090] Comparative Example 1 [Mask blank manufacturing] The mask blank of Comparative Example 1 was manufactured in the same manner as in Example 1, except for the thickness of the phase shift film. The phase shift film of Comparative Example 1 had different film formation conditions from Phase Shift Film 2 of Example 1. Specifically, a light-transmitting substrate was placed in a single-wafer RF sputtering device, and a phase shift film was formed on the light-transmitting substrate by sputtering (RF sputtering) using an HfO2 target and an SiO2 target alternately and argon (Ar) gas as the sputtering gas, the bottom layer being composed of hafnium and oxygen, a lower layer being composed of silicon and oxygen, and an upper layer being composed of hafnium and oxygen. The bottom layer had a thickness of 42 nm, the lower layer had a thickness of 11 nm, and the upper layer had a thickness of 4 nm, resulting in a phase shift film thickness of 57 nm. Thus, the thickness of the upper layer of the phase shift film of Comparative Example 1 was less than 5 nm.
[0091] The transmittance and phase difference of the phase shift film for light with a wavelength of 193 nm were measured using a phase shift amount measuring device (Lasertec MPM193), and the transmittance was 40.9% and the phase difference was 177.2 degrees (deg.). In addition, the optical properties of the phase shift film were measured using a spectroscopic ellipsometer (JA Woollam M-2000D), and the refractive index n of the bottom layer and the top layer for light with a wavelength of 193 nm was 2.93, the extinction coefficient k was 0.24, and the refractive index n of the bottom layer was 1.56, and the extinction coefficient k was 0.00. In addition, the oxygen content in the upper layer of this phase shift film was 66% or less, and oxygen deficiency occurred.
[0092] Next, a light-shielding film (CrOC film) composed of chromium, oxygen and carbon was formed to a thickness of 53 nm in contact with the phase shift film in the same manner as in Example 1. The optical density of the laminated structure of the phase shift film and the light-shielding film of Comparative Example 1 at the wavelength (about 193 nm) of the light of an ArF excimer laser was measured using a spectrophotometer (Cary4000 manufactured by Agilent Technologies) for the transparent substrate on which the phase shift film and the light-shielding film were laminated, and it was confirmed to be 3.0 or more.
[0093] [Cleaning test (chemical resistance test)] In addition, the phase shift film of Comparative Example 1 was formed on another light-transmitting substrate, and a cleaning test (chemical resistance test) was performed after performing a desired annealing treatment. Specifically, the phase shift film of Comparative Example 1 was formed on another light-transmitting substrate, and an annealing treatment was performed at 500 degrees for 30 minutes. Then, the entire surface (front and side surfaces) of the phase shift film of Comparative Example 1 was subjected to SC-1 cleaning (ammonia-hydrogen peroxide solution cleaning) and SPM cleaning (sulfuric acid / hydrogen peroxide cleaning) five times each for a predetermined period of time. A rinse treatment with pure water was performed between the SC-1 cleaning and the SPM cleaning. After carrying out this cleaning test, the surface and sides of the phase shift film in Comparative Example 1 were observed for the presence or absence of film loss. It was found that significant film loss had occurred on the surface and sides of the upper layer portion of the phase shift film. [Fabrication and evaluation of phase shift masks] Next, using this mask blank of Comparative Example 1, a manufacturing process for a phase shift mask of Comparative Example 1 was carried out in the same manner as in Example 1. However, significant film loss occurred in the phase shift film during the formation of the transfer pattern, and a phase shift mask having the desired characteristics could not be manufactured. [Explanation of symbols]
[0094] 1 Translucent substrate 2 Phase shift film 21 Bottom Floor 22 Lower layer 23 Upper layer 2a Phase shift pattern 3. Light-shielding film 3a, 3b Light-shielding pattern 4. Hard mask film 4a Hard mask pattern 5a Resist pattern 6b Resist pattern 100 mask blanks 200 Phase Shift Mask
Claims
1. A mask blank having a phase shift film on a light-transmitting substrate, the phase shift film includes a lower layer and an upper layer, the upper layer is provided in contact with a surface of the lower layer opposite to the light-transmitting substrate, the underlayer contains silicon and oxygen; the overlayer contains hafnium and oxygen; The thickness of the upper layer is 5 nm or more, The thickness of the phase shift film is 90 nm or less. A mask blank comprising:
2. 2. The mask blank according to claim 1, wherein the total content of hafnium and oxygen in said upper layer is 90 atomic % or more.
3. 3. The mask blank according to claim 1, wherein the total content of silicon and oxygen in the lower layer is 90 atomic % or more.
4. 4. The mask blank according to claim 1, wherein the oxygen content in each of the lower layer and the upper layer is 50 atomic % or more.
5. the phase shift film has a bottom layer between the light-transmitting substrate and the lower layer, the bottom layer is provided in contact with a surface of the lower layer facing the light-transmitting substrate, The bottom layer contains hafnium and oxygen. The mask blank according to claim 1 .
6. 6. The mask blank according to claim 5, wherein the thickness of the bottom layer is 5 nm or more.
7. 7. The mask blank according to claim 5, wherein the total content of hafnium and oxygen in the lowermost layer is 90 atomic % or more.
8. 8. The mask blank according to claim 5, wherein the oxygen content in the lowermost layer is 50 atomic % or more.
9. 9. The mask blank according to claim 1, wherein the lower layer has a thickness of 5 nm or more.
10. 10. A mask blank according to any one of claims 1 to 9, characterized in that the phase shift film has a function of transmitting ArF excimer laser exposure light with a transmittance of 20% or more, and a function of generating a phase difference of 150 degrees or more and 210 degrees or less between the exposure light that has passed through the phase shift film and the exposure light that has passed through air a distance equal to the thickness of the phase shift film.
11. The mask blank according to claim 1 , further comprising a light-shielding film on the phase shift film.
12. A phase shift mask comprising a phase shift film having a transfer pattern formed on a light-transmitting substrate, the phase shift film includes a lower layer and an upper layer, the upper layer is provided in contact with a surface of the lower layer opposite to the light-transmitting substrate, the underlayer contains silicon and oxygen; the overlayer contains hafnium and oxygen; The thickness of the upper layer is 5 nm or more, The thickness of the phase shift film is 90 nm or less.
1. A phase shift mask comprising:
13. 13. The phase shift mask according to claim 12, wherein the total content of hafnium and oxygen in said upper layer is 90 atomic % or more.
14. 14. The phase shift mask according to claim 12, wherein the total content of silicon and oxygen in said lower layer is 90 atomic % or more.
15. 15. The phase shift mask according to claim 12, wherein the oxygen content in each of said lower layer and said upper layer is 50 atomic % or more.
16. the phase shift film has a bottom layer between the light-transmitting substrate and the lower layer, the bottom layer is provided in contact with a surface of the lower layer facing the light-transmitting substrate, The bottom layer contains hafnium and oxygen.
16. The phase shift mask according to claim 12,
17. 17. The phase shift mask of claim 16, wherein the bottom layer has a thickness of 5 nm or more.
18. 18. The phase shift mask according to claim 16, wherein the total content of hafnium and oxygen in said lowermost layer is 90 atomic % or more.
19. 19. The phase shift mask according to claim 16, wherein the oxygen content in the lowermost layer is 50 atomic % or more.
20. 20. The phase shift mask according to claim 12, wherein the thickness of the lower layer is 5 nm or more.
21. 21. A phase shift mask as described in any one of claims 12 to 20, characterized in that the phase shift film has a function of transmitting ArF excimer laser exposure light with a transmittance of 20% or more, and a function of generating a phase difference of 150 degrees or more and 210 degrees or less between the exposure light that has passed through the phase shift film and the exposure light that has passed through air a distance equal to the thickness of the phase shift film.
22. 22. The phase shift mask according to claim 12, further comprising a light-shielding film having a light-shielding pattern formed on the phase shift film.
23. 23. A method for manufacturing a semiconductor device, comprising the step of exposing and transferring said transfer pattern onto a resist film on a semiconductor substrate by using a phase shift mask according to claim 12.
Citation Information
Patent Citations
Dielectric mask, method and device for producing the same
JP1995325384A
Mask for excimer laser beam machining andits production
JP1996171197A
Halftone phase shift mask blank and mask
JP2002258460A
Manufacturing method of halftone phase shift photomask
JP2012083521A
Mask blank, phase shift mask and method for producing semiconductor device
WO2021044917A1