Process for producing nanocellulose materials comprising at least two stages of defibrillation of a cellulose feedstock and at least one intermediate fractionation stage

By integrating fractionation steps during defibrillation and other treatment stages, the method addresses the inconsistency in nanocellulose production, achieving higher quality and energy efficiency.

JP7558936B2Active Publication Date: 2024-10-01SUZANO SA
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2021525338
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-07-17
Filing Date
2019-07-17
Publication Date
2024-10-01
Estimated Expiration
2039-07-17

AI Technical Summary

Technical Problem

Existing nanocellulose production methods lack a comprehensive approach that incorporates fractionation steps between pre-treatment, defibrillation, and post-treatment, resulting in inconsistent quality and energy inefficiency.

Method used

Incorporating fractionation units during defibrillation and/or pre- or post-treatment stages to achieve a more homogeneous particle size distribution, optimizing morphology and rheology of nanocellulose production.

Benefits of technology

The proposed method enhances the homogeneity and quality of nanocellulose production by improving particle size distribution and thixotropic properties, reducing energy consumption in the mechanical process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558936000004
    Figure 0007558936000004
  • Figure 0007558936000005
    Figure 0007558936000005
  • Figure 0007558936000006
    Figure 0007558936000006
Patent Text Reader

Abstract

The present invention relates to a process for producing nanocellulose material based on the use of fractionation of a cellulose pulp stream from pretreatment or mechanical defibrillation (partially purified / defibrillated pulp) in combination with a mechanical defibrillation step, in which both the pass and fail fractions can be sent to a consistency adjustment step prior to another distinct defibrillation step, for example, where the pass material is sent to a consistency adjustment step prior to a second defibrillation step, while the fail material is sent to another independent step of consistency adjustment and returned to the first stage of mechanical defibrillation. [Selected Figure] Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001]

[0001] The present invention generally relates to a process for producing nanocellulose based on the use of fractionation of a cellulose pulp stream from a refining process (partially refined / defibrillated pulp) in combination with mechanical defibrillation stages. [Background technology]

[0002]

[0002] Nanocellulose is defined as a cellulose sample that contains cellulose particles with at least nanoscale dimensions (1-100 nm). Its shape and composition are highly dependent on the conditions and production method. Based on composition and dimensional properties, nanocellulose can be classified as: (1) cellulose nanocrystals (CNC), also known as cellulose whiskers, (2) cellulose nanofibrils (CNF), and (3) bacterial cellulose (BC).

[0003]

[0003] Methods for the production of nanocellulose can involve mechanical defibrillation, which can be carried out as a single step of the procedure or in combination with biological and / or chemical methods, such as pre- or post-treatment steps. Thus, the nanocellulose samples produced are generally mixtures of CNF, CNC, and microfibrillated cellulose (MFC), the portion of such fractions depending on the process technology and application conditions, factors that define the final quality of the product. In addition, the type of raw material used to produce nanocellulose is also a determining factor in the final quality of the product.

[0004]

[0004] Nanocellulose production methods can be based on pretreatment (chemical, mechanical or biological) followed by mechanical purification or by a single stage (usually mechanical defibrillation). Enzyme pretreatment or chemical oxidation, such as the TEMPO method (2,2,6,6-tetramethylpiperidine-1-oxyl radical-mediated oxidation) (Habibi Y, Chanzy H, Vignon MR: TEMPO-mediated surface oxidation of cellulose whiskers. Cellulose 2006, 13: 679-687), is widely used to facilitate the defibrillation of cellulose pulp and as a form of nanocellulose production using different samples of lignocellulose. A more comprehensive description can be found in Janardhnan S., Sain MM, Isolation of cellulose microfibrils - an enzymatic approach, BioResources, 2006, 2: 176-188 and Habibi Y, Chanzy H, Vignon MR: TEMPO-mediated surface oxidation of cellulose whiskers. Cellulose 2006, 13: 679-687.

[0005]

[0005] In a paper published by Tanaka et al. (Tanaka A., Hoouni, J., Seppanen V., Pirkonem P. Nanocellulose characterization with mechanical fractionation, Nordic pulp and paper research journal, 2012, 27:689-694), the authors proposed the use of a membrane filter fractionation step as a method to characterize the already produced nano / microcellulose in terms of particle size (Figure 1A) and demonstrated that the device used was able to fractionate CNF samples in terms of particle size.

[0006]

[0006] Additionally, Osong and coworkers (Osong, SH, Norgren, S., Engstrand, P., An approach to produce nano-ligno-cellulose from mechanical pulp fine materials, Nordic Pulp and Paper Research Journal, 2013, 28: 472-479) demonstrated the production of nano-ligno-cellulose materials by homogenization of fractionated thermomechanical pulp (TMP) (1% consistency), as shown in Figure 1B. On the other hand, the same authors demonstrated that a similar process on a sample of bleached kraft pulp (BKP) consisting of 75 / 25 pine / spruce (softwood) did not give similar results and that a lower consistency had to be adopted for mechanical defibrillation by homogenization at high pressure, probably due to the higher cellulose content in the BKP fines fraction compared to that obtained with TMP.

[0007]

[0007] BR112014000862 A2 discloses a process for producing nanocellulose materials comprising fractionating a cellulose feedstock in the presence of an acid and mechanically treating the cellulose-rich solid to form cellulose fibrils and / or cellulose crystals. It therefore does not disclose a process of distributed comminution after the steps of fiber size selection / fractionation or continuous comminution (defibrillation).

[0008]

[0008] US Patent Application US6024834 A discloses a process for fractionating cellulose fibers by subjecting a first mixture of cellulose fibers to an effective fractionation medium to separate the first mixture of cellulose fibers into a second mixture of cellulose fibers and a third mixture of cellulose fibers, the second mixture of cellulose fibers having a fiber dispersion value of more than about 20 milligrams per 100 meters and a population average fiber length value of more than about 0.9 millimeters. This document also does not disclose a milling process in which dispersion is performed after a stage of fiber size selection / fractionation or continuous milling.

[0009]

[0009] To date, no process approach has been proposed for the production of nanocellulose that takes into account the use of fractionation steps between pre-treatment, defibrillation and post-treatment.

[0010]

[0010] The present invention provides for the incorporation of at least one fractionation unitary operation after at least one defibrillation stage in order to provide a homogenous stream for defibrillation pre- or post-treatment, which results in higher quality nanocellulose in terms of morphology and rheology. Summary of the Invention

[0011]

[0011] The present invention provides a method that, unlike the prior art, involves the use of a fractionation unit (unit operation) between the defibrillation and / or pre- or post-treatment unit operations. Hence, for all forms of embodiment, such unit operations are optimized in terms of the quality (morphology and rheology) of the nanocellulose produced, as well as offering gains related to the energy consumption in the mechanical process. By using a fractionation step in the nanocellulose production process, the defibrillation step is carried out on a sample stream that is more homogeneous in terms of particle size, which results in the nanocellulose produced having a higher homogeneity in terms of nanofibril size distribution. [Brief description of the drawings]

[0012] [Figure 1A]

[0012] Schematic diagram of the application of fractionation to nanocellulose characterization. [Figure 1B]

[0013] FIG. 1 is a schematic diagram of the production of nanolignocellulose using samples with low fiber content. [Figure 2A]

[0014] FIG. 1 is a schematic diagram of one embodiment of a fractionation application method in the production of nanofibrillated cellulose (CNF) and / or microfibrillated cellulose (MFC). [Figure 2B]

[0015] FIG. 1 is a schematic diagram of one embodiment of a fractionation application process in the production of nanofibrillated cellulose (CNF) and / or microfibrillated cellulose (MFC) by different types of purification. [Diagram 3]

[0016] FIG. 1 is an embodiment of the invention with a screening / sorting stage and fiber feedback between two grinding stages. [Figure 4]

[0017] FIG. 1 is an embodiment of the invention with a screening / sorting step and fiber feedback between two grinding steps for multiple processes. [Diagram 5]

[0018] FIG. 1 is an embodiment of the invention with two stages of crushing followed by screening / sorting and fiber feedback for multiple processes. [Figure 6]

[0019] Both are embodiments of the invention with two successive stages of screening / sorting and fiber feedback between the two grinding stages for multiple processes. [Figure 7]

[0020] FIG. 1 is an embodiment of the invention with a screening / sorting step and fiber feedback between two grinding steps for multiple processes. [Figure 8]

[0021] FIG. 13 is an embodiment of the invention with a screening / sorting step and fiber feedback between two consistency adjustment steps for multiple processes. [Figure 9]

[0022] 1 is an embodiment of the invention with two successive stages of grinding for multiple processes. [Figure 10]

[0023] 1 is an embodiment of the invention with two successive stages of grinding for multiple processes. [Figure 11]

[0024] FIG. 13 is an embodiment of the invention with two defibrillation conditioning stages followed by a sorting / fractionation stage and fiber feedback. [Figure 12]

[0025] 1 is an embodiment of the invention comprising various defibrillation conditioning steps followed by various sorting / fractionation and fiber feedback steps. [Figure 13]

[0026] The length distribution of fines per fine range (%) is shown. [Figure 14]

[0027] The length distribution of fines per fine range (%) is shown. [Figure 15]

[0028] The fiber size distribution (%) per range of fines (μm) is shown. [Figure 16]

[0029] 1 shows the change in viscosity versus shear rate (RPM) with the curve for Sample A overlaying the curve for Sample B. [Figure 17]

[0030] Illustrated are scanning electron microscope images of unsorted samples (A and D), rejects (B and E), and sorted accepts (C and F) after five grinding passes. [Figure 18]

[0031] 1 illustrates the dynamic viscosity profiles of fractionated and unfractionated samples after 5 milling passes (A) and 10 milling passes (B). [Figure 19]

[0032] 1 illustrates the dynamic viscosity profiles of fractionated and unfractionated samples. [Figure 20]

[0033] FIG. 1 illustrates the dynamic viscosity profiles of microfibrillated cellulose samples (fractionated and unfractionated) produced by disk refining. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013]

[0034] The present invention provides a method in which, unlike the literature, the authors suggest the use of a fractionation unit between the defibrillation and / or pre- or post-treatment unit operations. From this, for all embodiments, such unit operations are optimized in terms of homogeneity of the generated nanocellulose (in terms of morphology and with different rheological profiles). More specifically, they suggest the use of a fractionation step in the nanocellulose generation process, in this way the defibrillation step is carried out with a sample stream that is more homogeneous in terms of particle size, and thus the generated nanocellulose will have a higher quality and homogeneity in terms of particle size distribution (Figure 2A).

[0014]

[0035] In addition, the proposed embodiments allow for the production of different types of CNFs and / or MFCs, as demonstrated in the process embodiments shown in Figures 2B, 4, 5, 6, 7, 8, 9, 10, and 12.

[0015]

[0036] In particular, the present invention is directed to a process for producing nanocellulose material from a previously partially defibrillated cellulose feedstock. Preferably, the cellulose feedstock may be agro-industrial waste such as sugarcane bagasse and straw or rice straw or wheat straw, obtained by pulp from softwood or hardwood, more particularly eucalyptus, or pine, or birch or beech, bleached kraft pulp (BEKP) from eucalyptus, or kraft pulp; or sulfite pulping; or steam explosion; or fiber explosion with ammonia; or dilute acid hydrolysis; or alkaline hydrolysis; or oxidative alkali treatment; or enzymatic treatment; or organosolv treatment. However, there is no restriction on the cellulose material to be provided at the beginning of the process (step a).

[0016]

[0037] The method of producing nanocellulose material that is the object of the present invention comprises at least two stages occurring between pre-treatment, defibrillation and post-treatment, one being fractionation of the cellulose feedstock and the other being defibrillation of the cellulose feedstock, and it is possible to have at least one additional stage of mechanical defibrillation or chemical pre-treatment / post-treatment with a consistency adjustment stage. The output of at least one of the defibrillation stages comprises returning the fibers either to itself or to the same stage. For example, if a first defibrillation stage outputs a first batch of fibers, they may be returned partially or completely to such stage. Similarly, such fibers may be sent together to a second defibrillation stage, which outputs a second batch of fibers, which may be returned partially to the second or first stage.

[0017]

[0038] Therefore, the process that is the object of the present invention comprises carrying out a first stage of defibrillation of said feedstock (stage b) followed by a first screening / sorting stage (stage c). Preferably, the screening / sorting is carried out by particles passing through a sieve varying between 50 and 350 mesh (for example up to 200 mesh), called the pass fraction. The particles that have not passed the screening in the sieve, called the reject fraction, follow the feedback of stage b (stage d), i.e. they are sent again to a grinding stage and later to screening / sorting (c). The particles of the pass fraction from stage (c) are sent to a second defibrillation stage (stage f) (stage e). After repeated iterations of defibrillation of the fibrils of the pass fraction, the result (stage g) is the nanocellulose material from stage f.

[0018]

[0039] The process that is the object of the present invention further comprises additional sorting / fractionation steps. At least one further sorting / fractionation step may be envisaged following the sorting / fractionation step (such as step c).

[0019]

[0040] In addition, the process may have an additional defibrillation step after defibrillation step (b).

[0020]

[0041] In addition, the process object of the present invention may comprise a step of consistency adjustment after at least one of the defibrillation steps or after at least one screening / fractionation step.

[0021]

[0042] Further variations of the process for producing nanocellulose material include: (a) providing a cellulosic feedstock; (b) carrying out a first stage of defibrillation of said feedstock; (c) performing at least a first sorting / fractionation step of the particles; (d) passing the flow of reject fraction particles from (c) to step (b); (e) passing the particles of the pass fraction from step (c) to step (f); (f) carrying out a second defibrillation step of said feedstock; (g) recovering the nanocellulose material from step (f); It can be provided with:

[0022]

[0043] Such a variant preferably partially routes the reject fraction from step (d) to step (b). Also preferably, the reject fraction from step (f) can be fed back to step (f) or routed to step (b). Furthermore, such a process may present an additional sorting / fractionation step after step (c) and an additional defibrillation step after step (b).

[0023]

[0044] Overall, the process object of the present invention may further comprise a step of consistency adjustment after at least one screening / sorting step.

[0024]

[0045] The nanocellulose material is preferably microfibrillated cellulose, nanofibrillated cellulose, or cellulose nanocrystals.

[0025]

[0046] The process is therefore a process of enrichment of nanocellulose material, in which the use of a fractionation step occurs between pre-treatment, defibrillation and post-treatment, and comprises at least one step of sorting / fractionation of the defibrillation product from a defibrillation step to the same or an earlier defibrillation step, or to an additional defibrillation step, to provide the nanocellulose material. Example 1

[0026]

[0047] According to the approach described in Figure 2A, the process of the present invention takes place between pretreatment, defibrillation and post-treatment. Eucalyptus bleached kraft pulp in suspension with 4% consistency (solid content) was subjected to a disk refining process for 6.0 hours until an L-fines content of 70.30% (length-based fines) or an A-fines content of 33.35% (area-based fines) was reached at 57.93 ± 1.43 °C. The resulting material was then subjected to a fractionation process in a Bauer McNETT unit using a screen / sieve with 200 mesh orifices. As a result of the fractionation step, a mass recovery of about 43% was obtained in the reject fraction (fraction collected in a separate stream that did not pass through the screen in the fractionation) and 56% in the pass fraction, resulting in 22% and 94% L-fines for the reject and pass fractions, respectively. Both fractions underwent thickening (consistency adjustment) on a silk screen (550 mesh), resulting in a consistency of 21.28% for the fail fraction and 17.73% for the pass fraction, as presented in the approach in FIG. 2A.

[0027]

[0048] The material obtained from fractionation (rejected and accepted fractions) and the MFC sample with 70.30% fine-L content were then subjected to dilution to 1% consistency and then defibrillation by grinding using 10 passes in a Masuko (Supermasscolloider-MKCA6) with an ultra-fine 120#MKGC (Silicon Carbide-SiC) grinding wheel. For the purpose of comparing the morphology of the samples, Figures 13, 14, and 15 present the distribution profiles (%) of L-fines, fiber length, and fiber width, respectively.

[0028]

[0049] As shown in Figure 13, the fractionated and processed samples in the sieving process present a gain in increasing the fraction of fines in the smaller size range (1-23 μm) for a stage where the other ranges are very similar. On the other hand, considering the fiber length distribution (Figure 14), the use of fractionation during the defibrillation process (refining and grinding) results in an increase in the percentage of the fraction in the smaller length range (200-289 μm), indicating that the use of fractionation according to the approach of Figure 2A results in a reduction in fiber size after defibrillation when compared to the distribution of the other samples. Furthermore, from the morphology point of view, the approach of Figure 2A provides a reduction in fiber width and a more homogenous sample (greater relationship between the height and width at the base of the curve) (Figure 15).

[0029]

[0050] A positive effect was also observed on the rheological behavior of the samples, as shown in Figure 16, indicating a significant gain in the thixotropic properties of nanofibrillated cellulose produced following the process approach demonstrated in Figure 2A.

[0030]

[0051] The benefits of the presented process approach can also be identified in the results in Table 1, where it is possible to appreciate the gain in fines content in area as well as in terms of energy expended in the final mechanical process.

[0031]

[0052] Table 1: Mean fines content based on area and energy expended in the final defibrillation of the samples. [Table 1] Example 2

[0032]

[0053] According to the approach described in Figure 2A, the process of the present invention takes place between pretreatment, defibrillation and post-treatment. Eucalyptus bleached kraft pulp in suspension with 4% consistency (solid content) was subjected to a disk refining process for 6.0 hours until an L-fines content of 70.30% (length-based fines) or an A-fines content of 33.35% (area-based fines) was reached at 57.93 ± 1.43 °C. The resulting material was then subjected to a fractionation process in a Bauer McNETT unit using a screen / sieve with 200 mesh orifices. As a result of the fractionation step, a mass recovery of about 43% was obtained in the reject fraction (fraction collected in a separate stream that did not pass through the screen in the fractionation) and 56% in the pass fraction, resulting in 22% and 94% L-fines for the reject and pass fractions, respectively. Both fractions were subjected to thickening (consistency adjustment) on a silk screen (550 mesh), resulting in a consistency of 21.28% for the fail fraction and 17.73% for the pass fraction, as presented in the approach in FIG. 2A.

[0033]

[0054] The material obtained from the fractionation (rejected and accepted fractions) was then diluted to a consistency of 1% and then diluted with ultrafine 120# MKGA (aluminum oxide-A l2O3 The samples were subjected to defibrillation by grinding using 10 passes in a Masuko (Supermasscolloider-MKCA6) grinding wheel. For the purpose of comparing the morphology of the samples after the grinding process, FIG. 17 shows images obtained by scanning electron microscopy. As shown in the MEV diagram, it is possible to identify the highest level of agglomeration after grinding of the fibrils in the unfractionated samples and in the rejects of the fractionation, when compared to the samples that passed the fractionation.

[0034]

[0055] In addition, a positive effect was also observed in the rheological behavior of the samples, as shown in Figure 18, indicating that there was a very significant gain in the thixotropic properties of nanofibrillated cellulose produced following the process approach demonstrated in Figure 2A for different numbers of passes in the grinding stage. Example 3

[0035]

[0056] According to the approach described in FIG. 2A, the process of the invention takes place between pretreatment, defibrillation and post-treatment. Bleached eucalyptus kraft pulp (BEKP) in a suspension of 4% consistency (solid content) was subjected to a disk refining process (18.66 km / rev) for 6.0 hours until an L-fines content of 69.89% (fine based on length) was reached at 57.93±1.43° C. The resulting material was then diluted to 3.5% solids and subjected to a fractionation process using a pressurized basket with a 75 mesh screen (200 μm). In this case, fractionation took place after dilution of the suspension to a consistency of 3.5%, with a volumetric rejection rate of 40% with a rotor speed of 12 m / s and an average passing speed of 0.07 m / s.

[0036]

[0057] As a main result of the fractionation, it can be seen that a separation of the particles occurs according to their respective size, reflected in the values ​​of the average length of the fibers in each fraction as well as in the respective fines content, as shown in Table 2. In addition, the consistency values ​​are also different, with the passing fraction being more dilute (2.81% consistency) than the fraction obtained in the rejects (3.91% consistency).

[0037]

[0058] Table 2: Fines content and average fiber length data for standard and fractionated samples. [Table 2]

[0038]

[0059] The efficiency of the fractionation process in improving the quality of the microfibrillated cellulose suspensions is also evident in their respective dynamic viscosity profiles (thixotropic properties), as shown in FIG.

[0039]

[0060] The suspension produced in the fractionation pass was subjected to disk refining using a 12" disk with a cut length of 95.5 km / s (3.82 km / rev). For comparison, a BEKP sample was subjected to disk refining using two 12" disk refining stages with cut lengths of 44.25 km / s (1.77 km / rev) and 95.5 km / s (3.82 km / rev) of the disks used in the two successive refining stages. In this case, the first stage resulted in a sample with 65% fines in length or 34.1% fines in area. The refined samples (standard BEKP and fractionation pass) were analyzed for fines content (fines defined as particles less than 80 μm, fibers defined as other particles) and are shown in Table 3, showing the gain obtained from the use of separation between defibrillation stages by refining disks and demonstrated for the mill defibrillation in Example 1.

[0040]

[0061] Table 3: Data on fines content and on standard and fractionated samples [Table 3]

[0041]

[0062] In addition to the morphological analysis results, there is also a gain in the thixotropic properties of the nanofibrillated cellulose produced according to the process approach demonstrated in FIG. The invention as originally claimed in the present application is set forth below. [1] A process for producing nanocellulose material from a cellulose feedstock, the process comprising at least two stages of defibrillation of the cellulose feedstock. [2] A process for producing nanocellulose material as described in [1], wherein a fractionation step occurs between pretreatment, defibrillation and post-treatment. [3] (a) providing a cellulosic feedstock; (b) carrying out a first stage of defibrillation of said feedstock; (c) performing at least a first sorting / fractionation step of the particles; (d) passing the flow of reject fraction particles from (c) to step (b); (e) passing the particles of the pass fraction from step (c) to step (f); (f) carrying out a second defibrillation step of said feedstock; (g) recovering the nanocellulose material from step (f); A process for producing the nanocellulose material described in [1] or [2], comprising: [4] The process described in [3], presenting an additional sorting / separation step after step (c). [5] The process according to [4], which presents an additional defibrillation step after step (b). [6] The process according to [5], further comprising a consistency adjustment step after at least one defibrillation step. [7] The process of [6], further comprising a consistency adjustment step after at least one screening / fractionation step. [8] The process of [3], wherein the nanocellulose material is microfibrillated cellulose and / or nanocellulose. [9] (a) providing a cellulosic feedstock; (b) carrying out a first stage of defibrillation of said feedstock; (c) performing at least one first stage of screening / fractionation of particles passing through a sieve ranging from 50 to 350 mesh; (d) passing the flow of reject fraction particles from (c) to step (b); (e) passing the particles of the pass fraction from step (c) to step (f); (f) carrying out a second defibrillation step of said feedstock; (g) recovering the nanocellulose material from step (f); A process for producing the nanocellulose material described in [1] or [2], comprising:

[10] The process of [9], wherein the sieve in step (c) is a 75 mesh sieve.

[11] The process of [9], wherein the sieve in step (c) is a 200 mesh sieve.

[12] The process according to any one of [9] to

[11] , wherein the stream of reject fractions from step (d) is partially sent to step (b).

[13] The process of

[12] , wherein the stream of the reject fraction from step (f) is fed back to step (f) or sent to step (b).

[14] The process described in

[13] , presenting an additional sorting / separation step after step (c).

[15] The process according to

[14] , presenting an additional defibrillation step after step (b).

[16] The process according to

[15] , comprising a consistency adjustment step after at least one defibrillation step.

[17] The process of

[16] , comprising a consistency adjustment step after at least one screening / fractionation step.

[18] A process for concentrating nanocellulose material, the process comprising at least one step of feedback of a defibrillation product from a defibrillation step to the same defibrillation step or to a previous defibrillation step to provide nanocellulose material.

Claims

1. A process for producing nanocellulose material from a cellulose feedstock, comprising at least two stages of defibrillation of the cellulose feedstock, the process comprising: (a) providing a cellulosic feedstock; (b) carrying out a first defibrillation step of said feedstock; (c) performing a consistency adjustment of the defibrillated feedstock of step (b); (d) performing at least a first screening / fractionation step of the feedstock of step (c); (e) passing the flow of reject fraction particles from (d) to step (b); (f) passing the particles of the pass fraction from step (d) to step (g); (g) carrying out a second defibrillation step of said feedstock; (h) recovering the nanocellulose material from step (g); A process comprising:

2. 2. The process for producing nanocellulose material as described in claim 1, wherein a fractionation step is further carried out between the pre-treatment step and the first defibrillation and / or between the second defibrillation and the post-treatment step.

3. 3. The process of claim 2, comprising an additional screening / sorting step after step (c).

4. 4. The process of claim 3, comprising an additional defibrillation step after step (b).

5. 5. The process of claim 4, comprising a consistency adjustment step after at least one screening / sorting step.

6. 3. The process of claim 2, wherein the nanocellulose material is microfibrillated cellulose and / or nanofibrillated cellulose.

7. A process for producing nanocellulose material as described in claim 1 or 2, wherein step (d) is a step of performing at least one first sorting / fractionation step of particles passing through a sieve ranging from 50 to 350 mesh.

8. 8. The process of claim 7, wherein the sieve in step (d) is a 75 mesh sieve.

9. 8. The process of claim 7, wherein the sieve in step (d) is a 200 mesh sieve.

10. The process according to any one of claims 7 to 9, wherein the stream of the reject fraction from step (e) is partially sent to step (b).

11. 11. The process of claim 10, further comprising the step of obtaining a rejects fraction after step (g), said rejects fraction stream from step (g) being fed back to step (g) or sent to step (b).

12. 12. The process of claim 11, comprising an additional screening / sorting step after step (d).

13. 13. The process of claim 12, comprising an additional defibrillation step after step (b).

14. 14. The process of claim 13, comprising a consistency adjustment step after at least one defibrillation step.

15. 15. The process of claim 14, comprising a consistency adjustment step after at least one screening / sorting step.

16. 13. A process for concentrating the nanocellulose material produced by the process of claim 1, comprising at least one step of feedback of the defibrillation product from a defibrillation step to the same defibrillation step or to a previous defibrillation step to provide the nanocellulose material.

Citation Information

Patent Citations

  • Method for producing nanofiber, and nanofiber

    JP2008169497A

  • Methods and systems for producing nanocellulose, and nanocellulose

    JP2013545904A