Laminated Glazing and Processes

By balancing optical distortions using hidden layers with varying infrared reflectance on each glass ply, the invention addresses the issue of optical distortions in laminated glazing, improving ADAS camera clarity and functionality.

JP7558964B2Active Publication Date: 2024-10-01PILKINGTON GRP LTD

Patent Information

Application Number
JP2021557222
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-26
Filing Date
2020-03-26
Publication Date
2024-10-01
Estimated Expiration
2040-03-26

AI Technical Summary

Technical Problem

Existing laminated glazing technologies suffer from optical distortions near hidden bands, particularly when Advanced Driver Assistance Systems (ADAS) cameras are integrated, which can limit their effectiveness due to unbalanced optical distortions between glass plies.

Method used

The solution involves balancing optical distortions by using hidden layers with different infrared reflectance properties on each glass ply, ensuring that the optical distortions of sensor windows on both plies compensate for each other, thereby reducing the overall optical distortion.

Benefits of technology

This approach significantly reduces optical distortions in laminated glazing, enhancing the clarity and functionality of ADAS cameras by ensuring balanced optical power across the sensor window, meeting regulatory light transmission requirements and improving ADAS performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558964000001
    Figure 0007558964000001
  • Figure 0007558964000002
    Figure 0007558964000002
  • Figure 0007558964000003
    Figure 0007558964000003
Patent Text Reader

Abstract

A process for manufacturing laminated glazing and molded laminated glazing is disclosed, the laminated glazing comprising a first glass ply having a first surface and a second surface, a second glass ply having a third surface and a fourth surface, at least one polymer ply positioned between the first glass ply and the second glass ply, and a concealing band around at least a portion of the periphery of the laminated glazing, the concealing band having at least one sensor window and including a first concealing layer and a second concealing layer, the first glass ply having the first concealing layer attached to at least a portion of the periphery of the first surface or the second surface, the first concealing layer having at least one first concealing layer having an optical distortion in the region of the first sensor window. a first ply of glass having a sensor window portion, the second ply of glass having the second concealing layer adhered to at least a portion of the periphery of the third surface or the fourth surface, the second concealing layer comprising at least one second sensor window portion having an optical distortion of a second sensor window portion, the optical distortion of the first sensor window portion and the optical distortion of the second sensor window portion being controlled, respectively, so that the absolute magnitude of the optical distortion of the sensor window is less than the absolute magnitude of the optical distortion of the first sensor window and the optical distortion of the second sensor window.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to laminated glazing, automotive glazing, and processes for making such glazing. [Background technology]

[0002] Laminated glazing, which comprises two sheets of glazing material, usually glass, laminated together with a plastic interlayer (eg, polyvinyl butyral, PVB), is useful in architectural and especially automotive glazing.

[0003] Windshields and other increasingly popular automotive glazing are typically laminated glazing and may have an obscuration band placed around its perimeter. The obscuration band is often black or very dark in color and is typically opaque to visible light (and often other wavelengths, e.g., UV). The obscuration band serves to hide components on the glazing, such as fasteners, and also serves to provide UV protection, for example, to adhesives used to secure the glazing in place.

[0004] The hidden band may be produced using enamel. Such enamel, once fired, is resistant to weathering and abrasion. The hidden band may be applied by screen printing an enamel ink onto the glass. The enamel ink typically contains a frit (flux), pigment, and a liquid component (such as oil) to enhance its screen printing properties. After screen printing, the enamel ink may be cured (such as by exposure to ultraviolet light) or dried (such as by heating to about 300°C), and then heated to a high temperature and fired to melt the flux and ensure adhesion to the glass surface.

[0005] It is common practice to number the surfaces of laminated glazing starting from the surface facing the exterior of the vehicle or building to which the glazing is attached. Thus, surface 1 is the surface facing the exterior, and is the exposed surface. In a laminate including two plies of glazing material, surface 1 is the exterior surface of the outward facing ply. Surface 2 is the inward facing surface of the exterior ply, i.e., the surface of the exterior ply that faces towards the interior of the vehicle or building. Surface 2 is not an exposed surface because it is in contact with and covered by a plastic interlayer. Surface 3 is the outward facing surface of the interior ply, i.e., the surface of the interior ply that faces towards the exterior of the vehicle or building. Like surface 2, surface 3 is not an exposed surface because it is in contact with and covered by a plastic interlayer. Thus, surfaces 2 and 3 are unexposed or covered surfaces. Surface 4 is the interior surface of the inward facing ply, i.e., the exposed surface that faces the interior of the vehicle or building.

[0006] In laminated glazing, such as windshields, the hidden band may be printed on surface 4 or on the inner surface of the laminate (e.g., surface 2, the glass / polymer interface inside the laminate). Glazing with a hidden band on one glass ply is typically formed by applying enamel to the glass substrates and then heating each glass substrate to high temperature. Printing the hidden band on the inner surface of the laminate (e.g., surface 2 or surface 3) may reduce perspective distortion that can sometimes occur. WO-A-2017 / 159452 discloses laminated glazing, in which in some embodiments printed on surfaces 2 and 4, the perspective distortion near the hidden band is reduced.

[0007] Often the enamel is fired by a heating step. After molding, optical distortions can occur associated with the boundaries between the printed and unprinted areas of the glass. These optical distortions, sometimes called "burnlines," tend to run parallel to the boundaries.

[0008] Attempts have been made to reduce or eliminate burn lines by modifying bending process parameters such as temperature profiles and / or by designing, constructing and installing shields on the glass bending tools / molds.

[0009] EP-A-0415020 discloses a method for preferentially heating a glass sheet having a decorative ceramic enamel boundary without adversely affecting the optical quality of the glass. The preferential heating is accomplished by using a heater that radiates thermal energy at a selected wavelength that is more readily absorbed by the enamel than the glass, such that the enamel heats faster than the glass. In one particular embodiment, the glass having the ceramic enamel boundary is preheated to a temperature above its strain point temperature. The coated glass is then exposed to a quartz heater to preferentially heat the enamel to a temperature high enough to bake the enamel to the glass. The ceramic enamel is then cooled to the temperature of the remainder of the glass.

[0010] US-B-5,443,669 discloses a process for producing laminated glass sheets with single or double curvature, in particular for automobiles, more particularly for producing glass sheets with a printed pattern, in particular for automobile windshields, where the printed pattern may be a boundary. The printed pattern is formed by means of an enamel ink.

[0011] Unfortunately, such attempted solutions are insufficient and have disadvantages such as high additional costs and time to design, build, install and optimize the shielding of the tool. Also, because the shielding affects the forming of the rest of the glass, the general optical quality may be adversely affected by the additionally introduced shielding in terms of the glass forming in other areas. Moreover, the attempted solutions may lead to further aesthetic problems caused by the enamel ink of the hidden band under firing.

[0012] A more successful solution to the burn line problem may involve modifying the properties of the enamel to increase the spectral reflectance in the NIR (near infrared) and IR (infrared) wavelength ranges (which may be equivalent to reducing the emissivity difference between printed and unprinted glass surfaces, especially at medium and high temperatures), as described in WO-A-2017 / 068368.

[0013] Advanced driver assistance systems (ADAS) systems (such as those produced by Mobileye and other manufacturers) are becoming common in vehicles and may be used for lane departure warning, automatic emergency braking, high beam assist, speed limit identification, and other applications. Most of these systems rely on one or more cameras that are typically mounted on the inside surface of the windshield (i.e., surface 4). The preferred location for mounting the camera is toward the top edge of the windshield, typically centrally or symmetrically about the centerline of the windshield, i.e., near the rearview mirror, which is usually located in the same part of the windshield. The camera is often located behind a concealment band (as viewed from the outside of the vehicle), and therefore needs to provide an area free of the enamel, ink, etc. that make up the concealment band, through which the camera can view the area in front of the vehicle.

[0014] The area without the hidden band can take the form of, for example, an opening or recess in the hidden band, and is generally referred to as a "camera window." Thus, for example, the camera window may or may not be surrounded by the hidden band. The same considerations regarding providing forward visibility also apply to sensors, such as rain or light sensors, located on the surface 4 of the windshield, often in the same portion of the windshield, and thus the term may be generalized to "sensor window."

[0015] Optical distortions from the camera window can limit the effectiveness of camera and ADAS applications. US-A-2018 / 118116 discloses a vehicle camera system including a blackout layer disposed in the upper central region of the windshield. EP-A-1605729 discloses a vehicle windshield with an imaging device for viewing through a viewing zone including a resistive heating element that heats the viewing zone and thereby reduces the effect of icing or condensation on visibility through the viewing zone. DE202018105625U1 discloses a vehicle window glass having two printed areas, where the optical effect of the first printed area can be compensated by the optical effect of the second printed area. Summary of the Invention [Problem to be solved by the invention]

[0016] There is a need to further reduce optical distortion in laminated glazing, including ADAS camera windows in or near hidden bands printed on the laminated glazing. This is especially true because as ADAS performance demands increase, less and less optical distortion is tolerated in ADAS camera windows.

[0017] It is an object of the present invention to address the above needs. [Means for solving the problem]

[0018] Thus, the present invention provides in a first aspect a method for producing a composition comprising: A laminated glazing, comprising: a first ply of glass having a first surface and a second surface; a second ply of glass having a third surface and a fourth surface; at least one polymer ply positioned between the first and second glass plies; a concealment band around at least a portion of a periphery of the laminated glazing, the concealment band having at least one sensor window and including a first concealment layer and a second concealment layer; the first ply of glass having the first concealing layer attached to at least a portion of the perimeter of the first surface or the second surface, the first concealing layer comprising at least one first sensor window portion having an optical distortion of a first sensor window portion; the second ply of glass having the second concealing layer attached to at least a portion of the perimeter of the third surface or the fourth surface, the second concealing layer comprising at least one second sensor window portion having an optical distortion of a second sensor window portion; The optical distortion of the first sensor window portion and the optical distortion of the second sensor window portion are each controlled to provide a laminated glazing in which the absolute magnitude of the optical distortion of the sensor window is smaller than the absolute magnitude of the optical distortion of the first sensor window and the optical distortion of the second sensor window.

[0019] This is highly advantageous because by controlling the optical distortion at the sensor window of each ply ("sensor window optical distortion"), the overall optical distortion within the sensor window can be balanced, resulting in significantly less distortion across the sensor window of the laminated glazing, which can lead to a clearer view for, for example, an ADAS camera system.

[0020] In glazing, optical distortion is usually considered to be a property of the image seen by an observer (or a camera or other optical sensor) that can lead to pixel shifts. Optical power is usually considered to be a property of the glazing (such as glass) that can cause optical distortion. Optical power is usually measured in dioptres (equivalent to 1 / m; the inverse of the focal length of the lens P=1 / f), or more commonly in millidioptres (mdpts: 1mdpt=0.001 diopters). In this specification, optical distortion and optical power are used interchangeably unless the context requires otherwise.

[0021] Surprisingly, the inventors of the present invention have found that, in general, the optical distortion of the sensor window portion of each ply is not always high, but when laminated to the other ply, it may cause surface mismatches that may result in higher overall optical power and therefore optical distortion. By balancing the optical distortion of the two plies, and in particular the sensor window portion of each ply, the present invention can achieve a reduction in the overall optical power / distortion. By balancing the optical distortion of the sensor window portion of each ply, the overall optical distortion is reduced. The optical distortion of the sensor window of each ply is controlled so that they balance or compensate each other, resulting in a smaller net distortion. This has the effect of significantly reducing the overall magnitude of the optical distortion / optical power, as well as reducing the abrupt changes in optical power / optical distortion across the glazing. In an ideal situation, the optical distortions of the two plies are equal and opposite so that they cancel each other out.

[0022] The present invention also provides a first ply of glass having a first surface and a second surface; a second ply of glass having a third surface and a fourth surface; at least one polymer intermediate ply extending between the first and second glass plies; a concealment band around at least a portion of the periphery of the glazing; at least one sensor window provided in the concealment band, the concealment band comprising first and second concealment layers provided in the first and second plies of glass, the first ply of glass having a first concealing layer disposed about at least a portion of the perimeter of the first surface or the second surface, the first concealing layer comprising at least one first sensor window portion having an associated optical distortion; the second ply of glass having the second concealing layer disposed about at least a portion of the perimeter of the third surface or the fourth surface, the second concealing layer comprising at least one second sensor window portion having an associated optical distortion; the first hidden layer and the second hidden layer are formed of enamel; and A laminated glazing is provided in which the configuration of the sensor window portions and at least one property of the enamel are selected such that the optical distortions associated with each of the sensor window portions compensate each other to reduce net optical distortion in the glazing.

[0023] Preferably, the selected property of the enamel is its infrared reflectance.

[0024] The first sensor window portion and the second sensor window portion preferably have a sufficiently high light transmittance in the visible spectrum region to allow the ADAS camera to see through the laminated glazing. Currently, ADAS cameras and other sensors are generally mounted on windshields, which in most countries are required to have at least 70% visible light transmittance. Apart from regulatory requirements, the visible light transmittance (e.g., according to ISO 9050) is preferably greater than 55%, 60%, more preferably greater than 70%, and most preferably greater than 75%. As the sensitivity of ADAS cameras becomes even higher and the minimum light transmittance required for the ADAS cameras to function adequately decreases, they may be mounted on other glazing, such as backlights (i.e., rear windows), which may have a visible light transmittance of less than 20% (for privacy glazing), or less than 30%, or less than 40%, or less than 50%.

[0025] In general, the obscuring layer, and therefore the obscuring band, may be configured to be substantially opaque to visible light such that the ISO 9050 visible light transmission of the obscuring layer of the glazing is 1% or less, preferably 0.5% or less, and more preferably 0.1% or less.

[0026] The glass substrate of each ply of glass may be unshaped (e.g. it may be flat glass) but is preferably a shaped glass substrate and may have a thickness of, for example, 1 mm to 5 mm etc. Typically the cover layer is applied to a flat glass substrate which is then shaped to form, for example, an automobile windshield.

[0027] The polymer ply may comprise PVB (typically less than 1 mm thick, e.g. 0.76 mm thick). If greater performance or functionality (e.g. solar control) is required, there may be two PVB plies (e.g. 0.3-0.4 mm thick each) sandwiching a further plastic ply. For example, the further plastic ply may be made of PET and may have a solar control coating (e.g. having at least one silver layer and two or more dielectric layers) to provide such solar control.

[0028] The concealing layer may be pigmented to provide sufficient concealment, preferably being very dark, more preferably being substantially black in visible color. The concealing layer, and hence the concealment band, typically forms a band around at least a portion of the periphery of the glazing.

[0029] Typically, the first sensor window portion and the second sensor window portion are substantially enamel-free.

[0030] In one embodiment, the shape of the first sensor window portion may be different from the shape of the second sensor window portion, thereby controlling the optical distortion of the first sensor window portion and the optical distortion of the second sensor window portion.

[0031] Thus, the shape of the first sensor window portion and / or the shape of the second sensor window portion may independently be square, rectangular, trapezoidal, oval, or circular.

[0032] Typically, the first sensor window portion and / or the second sensor window portion are partially or fully surrounded by a first hidden layer and / or a second hidden layer, respectively, which may be on one side, two sides, three sides or four sides of the first sensor window portion and / or the second sensor window portion.

[0033] To improve control of optical distortion of the window portion, at least a portion of the periphery of the first sensor window portion or the second sensor window portion may be patterned, optionally including dots, lines, fade-outs, feathered edges, or sawtooth fade-outs.

[0034] In another embodiment of the invention, the first hidden layer and the second hidden layer may be formed of materials having different infrared reflectivities, thereby allowing control of the optical distortion of the first sensor window portion and the optical distortion of the second sensor window portion.

[0035] For example, the first hidden layer and / or the second hidden layer may have a relatively high infrared reflectance, such that at least a portion of the first hidden layer and / or the second hidden layer has an infrared reflectance of 21% or more over the region of the wavelength range of 800 nm to 2250 nm. The infrared reflectance of the portion may be 24% or more, preferably 27% or more, more preferably 30% or more, even more preferably 32% or more, even more preferably 35% or more, and most preferably 37% or more over the region of the wavelength range of 800 nm to 2250 nm. The region of the wavelength range of 800 nm to 2250 nm may extend to 400 nm or more, preferably 450 nm or more, more preferably 550 nm or more, and most preferably 610 nm or more.

[0036] Infrared reflectance can be measured in the above wavelength range using a spectrophotometer (such as a Perkin Elmer Lambda 9500).

[0037] An important characteristic is the difference in infrared reflectance between the first and second hidden layers. This difference may be the result of one hidden layer having a typical infrared reflectance, for example in the range of 17% to 20%, while the other hidden layer may have a high infrared reflectance, for example 21% or more, as described above, or a low infrared reflectance, for example 16% or less. Alternatively, one hidden layer may have a high infrared reflectance and the other hidden layer a low infrared reflectance. Preferably, the difference in infrared reflectance between the first and second hidden layers is at least 5%, 7%, 9%, 12%, 15%, 18% or 21%.

[0038] Thus, a generally high infrared reflectance concealing layer may have an average infrared reflectance of 30-50%, depending on process conditions. A concealing layer that does not provide particularly high infrared reflectance may have an infrared reflectance of about 17% or less, or 20% or less, in the infrared (800-2000 nm), while a highly reflective enamel may have a reflectance of 30% or more over much of that range.

[0039] The second hidden layer and / or the first hidden layer may have a relatively low infrared reflectance such that at least a portion of the first hidden layer and / or the second hidden layer has an infrared reflectance of 20% or 16% or less over the region of the wavelength range from 800 nm to 2250 nm.

[0040] The first hidden layer and / or the second hidden layer may comprise an enamel. Typically, the enamel comprises a frit and an inorganic pigment. The inorganic pigment may be selected from iron chrome pigments, ferrite pigments, chromite pigments, or ferrite / chromite (also known as iron chromite) pigments.

[0041] The enamel may be configured to provide suitable (e.g., high or low) emissivity characteristics by selecting appropriate infrared and / or near infrared reflective pigments and including an appropriate amount of infrared reflective pigment in the enamel. The enamel may include 10% to 50% by weight, preferably 10% to 40% by weight, more preferably 12% to 32% by weight of inorganic pigment. The enamel may include 20% to 80% by weight of frit.

[0042] The oxide frit may include particles of at least one compound selected from silica, titania, alumina, zirconia, compounds having fluoride ions (e.g., fluorite, fluorapatite, cryolite, etc.), bismuth oxide, zinc oxide, boron oxide, potassium oxide, sodium oxide, calcium oxide, barium oxide, lead oxide, lithium oxide, phosphorus oxide, molybdenum oxide, strontium oxide, and magnesium oxide.

[0043] Suitable inorganic pigments may include pigments selected from Fe / Cr pigments, Co / Al pigments, Co / Al / Cr pigments, Co / Ti pigments, Co / Cr pigments, Ni / Fe / Cr pigments, Ti / Cr / Sb pigments, Fe pigments, Cr pigments, and / or mixtures of two or more of these pigments.

[0044] Thus, the inorganic pigment may be selected from iron chrome pigments, ferrite pigments, chromite pigments, or ferrite / chromite (also known as iron chromite) pigments.

[0045] Depending on the nature of the laminated glazing design, the enamel of the first ply of glass and the enamel of the second ply of glass may be independently selected from high infrared reflectance enamels or low infrared reflectance enamels.

[0046] The infrared reflectance of the first hidden layer or the second hidden layer may be controlled by using appropriate enamels of different infrared reflectance or different emissivity.

[0047] Thus, the enamel of the first hidden layer and / or the enamel of the second hidden layer may be selected from a low infrared reflectance enamel or a high infrared reflectance enamel, thereby allowing control of the optical distortion of the first sensor window portion and the optical distortion of the second sensor window portion.

[0048] Thus, the infrared reflectance of the high infrared reflectance enamel may be 21% or more over the wavelength range of 800 nm to 2250 nm. The infrared reflectance may be 24% or more over the wavelength range of 800 nm to 2250 nm, preferably 27% or more, more preferably 30% or more, even more preferably 32% or more, even more preferably 35% or more, and most preferably 37% or more.

[0049] The region of the wavelength range from 800 nm to 2250 nm can extend to 400 nm or more, preferably 450 nm or more, more preferably 550 nm or more, and most preferably 610 nm or more.

[0050] Further control of optical distortion may be achieved if the periphery of either the first sensor window portion or the second sensor window portion is provided with a hidden frame portion having a lower (or higher) infrared reflectance than the hidden layer on the remainder of the ply and / or a hidden frame portion having a lower (or higher) infrared reflectance than the hidden layer on the other ply of glass.

[0051] That is, the periphery of the second sensor window portion may include a hidden frame portion.

[0052] The use of ceramic / enamel for the concealing layer / concealing band is advantageous because it uses known processes and the durability and performance of enamel is proven. The enamel / ceramic layer is likely to be useful at the glazing edge to protect the bond (such as adhesive) to the vehicle, so the use of ceramic eliminates the need to color match other methods applied to the sensor window. The present invention offers a significant advantage because it allows the optical distortion / light power to be reduced close to that of formed glass without the ceramic layer. The use of a concealing layer formed of a ceramic layer (i.e. enamel) is advantageous in itself.

[0053] In another embodiment, the first and second sensor window portions may be of different sizes, i.e., one of the two sensor window portions may be larger than the other. For example, the first sensor window portion may be larger than the second sensor window portion. More specifically, the first sensor window portion may have an x-axis dimension and / or a y-axis dimension, and the second sensor window portion may have an x-axis dimension and / or a y-axis dimension, and the x-axis dimension and / or the y-axis dimension of the first sensor window portion are different from the x-axis dimension and / or the y-axis dimension of the second sensor window portion, respectively, thereby allowing control of the optical distortion of the first sensor window portion and the optical distortion of the second sensor window portion.

[0054] The x-axis dimension of the first sensor window portion may be greater than the x-axis dimension of the second sensor window portion, and / or the y-axis dimension of the first sensor window portion may be greater than the y-axis dimension of the second sensor window portion.

[0055] The smaller window portion may be positioned relative to the larger window portion such that there is an offset at each end of a dimension. Preferably, the smaller window portion is positioned relative to the larger window portion such that there is an offset at each end of a dimension. The offsets at each end of a dimension may be substantially the same or different.

[0056] The optical distortion of the first sensor window portion and / or the optical distortion of the second sensor window portion may contribute to the optical power / optical distortion of the sensor window. Therefore, it is preferred that the first sensor window portion and / or the second sensor window portion have a controlled optical distortion in the range of -405 to +405 millidiopters, optionally in the range of -310 to +310 millidiopters. More preferably, the first sensor window portion and / or the second sensor window portion have an optical distortion in the range of -205 to +205 millidiopters, optionally in the range of -185 to +185 millidiopters, preferably in the range of -155 to +155 millidiopters.

[0057] The present invention is highly advantageous in that the control (and balancing) of the optical distortion of the first sensor window portion and the optical distortion of the second sensor window portion results in significant improvements in the sensor window, particularly in the following: ±250mdpt (i.e., the absolute magnitude of the optical distortion of the sensor window is 250mdpt), ±245mdpt, ±205mdpt, ±200mdpt, ±195mdpt, ±190mdpt, ±175mdpt, ±165mdpt, ±160mdpt, ±157mdpt, ±152mdpt, This is because it can result in a sensor window having optical power / optical distortion in the ranges of ±147mdpt, ±145mdpt, ±142mdpt, ±137mdpt, ±132mdpt, ±127mdpt, ±122mdpt, ±117mdpt, ±112mdpt, ±107mdpt, ±102mdpt, ±97mdpt, ±92mdpt, ±87mdpt, ±82mdpt, ±77mdpt, ±72mdpt, ±67mdpt, ±65mdpt, ±62mdpt or ±60mdpt.

[0058] The optical distortion / optical power range may be wider or narrower and may depend on the glazing tilt angle, window size, window design, and bending process.

[0059] To reduce condensation and / or icing on the sensor window, the or each sensor window portion may include a heating device, for example comprising an electrical resistive heating wire or other conductor, and optionally an electrical heating grid.

[0060] It may be desirable to use laminated glazing with more than one sensor or camera, and thus in some cases the laminated glazing may include more than one sensor window.

[0061] The present invention provides in a second aspect a motor vehicle windshield comprising a laminated glazing according to the first aspect of the invention.

[0062] In a third aspect, the present invention provides a method for producing a pharmaceutical composition comprising the steps of: 1. A process for producing molded laminated glazing, comprising: providing a first glass substrate having a first surface and a second surface and a second glass substrate having a third surface and a fourth surface; applying a first hidden layer to at least a first portion of the first surface or the second surface of the first glass substrate, the first hidden layer comprising at least one first sensor window portion having a controlled first sensor window portion optical distortion; applying a second hidden layer to at least a first portion of the third surface or the fourth surface of the second glass substrate, the second hidden layer comprising at least one second sensor window portion having a controlled second sensor window portion optical distortion; Optionally, shaping the first and second glass substrates by heating the first and second glass substrates to a temperature greater than 570° C.; disposing at least one polymer ply between the first glass substrate and the second glass substrate; laminating the first glass substrate, the polymer ply, and the second glass substrate; A process is provided in which the optical distortion of the first sensor window portion and the optical distortion of the second sensor window portion are controlled so that the absolute magnitude of the optical distortion of the sensor window is made smaller than the absolute magnitude of the optical distortion of the first sensor window portion and the optical distortion of the second sensor window portion.

[0063] The present invention is applicable to any forming process used for flat glass, whether in vehicles or buildings. For example, forming can be performed by press bending, i.e., pressing the heat-softened glass sheet between opposing bending moulds, or by sag (gravity) bending, i.e., allowing the heat-softened glass sheet to deform under its own weight while supported on a sag bending mould, typically in a rail furnace. Forming can also be performed by die-assisted sag bending, in which the heat-softened glass sheet is sag-bent, but a portion of the sheet is also pressed by a small pad or mould.

[0064] It has been found that different forming processes tend to produce different optical powers in the glass plies. For example, sag bends suffer from burn lines that are concentrated in intensity at surface 4, whereas burn lines developed at surface 2 tend to be more moderate in strength and more diffuse, i.e., spread over a larger area. This tendency can be controlled by using an infrared reflective ink on surface 4, thereby attenuating the optical power generated at surface 4 and achieving the desired balance between surfaces 2 and 4. In this way, a reduction in net optical distortion is achieved.

[0065] On the one hand, press bending tends to weaken the burn lines on surface 4, whereas the burn lines on surface 2 are variable and appear to be highly dependent on the properties of the part being manufactured. If the burn lines on surface 2 are stronger than on surface 4, then, counterintuitively, an ink with lower infrared reflectivity on surface 4 may be used, actually increasing the optical distortion on that surface. However, by better balancing the distortion on surface 2, a smaller net optical distortion is achieved. Alternatively, if the burn lines on surface 2 are weaker than on surface 4, then a more reflective ink may be used on surface 4, or a less reflective ink may be used on surface 2, depending on the absolute magnitude of the two distortions, and on the inks available.

[0066] It is therefore desirable to select an approach to reduce burn lines to the molding process being used, particularly properties such as infrared reflectance of the ink being used.

[0067] Applying the first and second hidden layers can include applying an enamel ink, the enamel ink including an inorganic pigment and a frit.

[0068] Other features of the third aspect are generally as described above in relation to the first aspect, with appropriate mutatis mutandis. [Brief description of the drawings]

[0069] The invention will now be described, by way of example only, with reference to the accompanying drawings in which: [Figure 1(a)] FIG. 1 is a schematic plan view of one embodiment of laminated glazing according to the present invention. [Figure 1(b)] FIG. 2 is a schematic cross-sectional view of a portion of the glazing of FIG. 1(a) taken along line AA. [Diagram 2] FIG. 2 is a schematic plan view of another embodiment of a laminated glazing according to the present invention. [Figure 3(a)]FIG. 1 is a schematic diagram of a sensor window used in the examples (second window portion on surface 4 is larger than the first window portion on surface 2 and has an offset at the top, bottom and sides). [Figure 3(b)] Schematic diagram of the sensor window used in the examples (the second window portion on surface 4 is larger again (compared to the first window portion on surface 2), with faded out top and bottom, and offsets on the top, bottom and sides). [Figure 3(c)] FIG. 1 is a schematic diagram of a sensor window used in the examples (a second window portion on a larger surface 4 with an offset all around it (compared to a first window portion on surface 2) and a high infrared reflectance / low emissivity hidden frame around the second window portion on surface 4). [Figure 4] 1 is a graph of optical power versus pixel position for Example 1. [Diagram 5] 11 is a graph of optical power versus pixel position for Example 2. [Figure 6] 13 is a graph of optical power versus pixel position for Example 3. [Figure 7] 13 is a graph of optical power versus pixel position for Example 4. [Figure 8] 13 is a graph of optical power versus pixel position for Example 5. [Figure 9] 1 shows alternative schematic diagrams of sensor windows of various designs illustrating the shapes of a first window portion on surface 2 (S2) and a second window portion on surface 4 (S4). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0070] Figure 1(a) shows a laminated glazing 2 according to the present invention. The laminated glazing 2 is a windshield for an automobile. The laminated glazing 2 comprises two plies of glass laminated together with an interlayer extending between the glass plies. The interlayer comprises a ply of polymer plastic material, for example a ply of polyvinyl butyral (PVB). The laminated glazing 2 has a peripheral concealment band 6 surrounding a transparent portion 4 of the laminated glazing 2. The concealment band 6 is optically opaque, concealing parts of the vehicle and also protecting the adhesive from UV light.

[0071] The hidden band 6 at the top edge of the windshield (if installed in the vehicle) has an optically transparent advanced driver assistance system (ADAS) camera sensor window 10, i.e., an enamel-free area of ​​the hidden band 6. When installed in the vehicle, the ADAS camera sensor window 10 allows a camera to form an image that is seen through the top of the windshield.

[0072] When the glass plies are heated to the high temperatures required for bending, differences are observed in the heating rate of the portion of the glazing with the black hidden band 6 compared to the transparent portion 4 of the glazing 2 and the transparent camera window 10. These differences in heating rates result in the development of local temperature differences in the glass, which in turn cause differences in the viscosity of the heat-softened glass. It is believed that these differences may result in optical distortions. Optical distortions have been found to occur after heating / forming of the glass plies in the portions of the glass plies at the periphery 8 of the transparent portion, near the edges of the hidden band 6, and at the sensor window 10. Heating / forming of the glass plies may be performed by sag bending or press bending methods, and as previously mentioned, the degree and type of optical distortions may differ between the methods. Optical distortions may also occur after cooling of the printed glass plies, which is also believed to be due to the development of temperature differences.

[0073] Figure 1(b) shows a cross section along line AA of figure 1(a). The laminated glazing 2 has an outer first ply of glass 12 (facing the exterior of the vehicle when installed), an inner second ply of glass 14, and a polymer interlayer of PVB 16 (typically 0.76 mm thick). The covert band 6 shown in figure 1(a) comprises two covert layers, one on surface 2 and one on surface 4 of the glazing. A covert layer 18 of black opaque enamel on surface 2 is printed on surface 2 of the outer first ply of glass 12 (i.e. the non-exposed surface of the first ply of glass 12 that is on the inside of the laminate and faces the interior of the vehicle) with an unprinted, i.e. transparent, area forming the first sensor window portion 15. A covert layer 20 of black opaque enamel on surface 4 is printed on surface 4 of the second ply of glass 14 (i.e. the surface of the inner ply of glass 14 that faces the interior of the vehicle when installed) with an unprinted area forming the second sensor window portion 17. The first sensor window portion 15 and the second sensor window portion 17 together form a sensor window 10 (eg for an ADAS camera) in the laminated glazing 2.

[0074] The second sensor window portion 17 is larger than the first sensor window portion 15 in the embodiment of Figure 1. This results in an offset 19 between the bottom edges of the two sensor window portions, as well as an offset 21 at the top edges, and offsets 19, 21 are the difference in the vertical (i.e. y-axis) dimensions at the top and bottom edges of the outer window portion 15 and the inner window portion 17 (after the glazing is installed, as shown in Figure 1(a)). The offsets 19, 21 are substantially the same in the embodiment of Figure 1, but may be different in other embodiments.

[0075] In the embodiment shown in FIG. 1, both glass plies are shaped with sag bends, and surprisingly, the larger inner window portion 17 tends to balance the optical distortions from hidden layer 18 on surface 2 and hidden layer 20 on surface 4, reducing the overall or net optical distortion of the sensor window 10.

[0076] 2 shows a laminated glazing 22 according to another embodiment of the invention. The laminated glazing 22 is a windshield for an automobile. The laminated glazing 22 comprises two plies of glass laminated together with an interlayer polymer layer, for example polyvinyl butyral (PVB). The laminated glazing 22 has a peripheral concealment band 26 that surrounds the transparent portion 24 of the glazing. The concealment band 26 is optically opaque, concealing portions of the vehicle and also protecting the adhesive from UV light.

[0077] A hidden band 26 at the top edge of the windshield (if installed on the vehicle) has two optically transparent advanced driver assistance system (ADAS) camera sensor windows, including a left sensor window 30 and a right sensor window 32. The sensor windows are free of enamel in the hidden band 26. When installed on the vehicle, the sensor windows 30, 32 allow one or more cameras to form an image that is seen through the top of the windshield.

[0078] 1, due to differences in heating rates between the black covert band 26 and the clear portions of the glazing 24 and clear camera window 30, optical distortions may occur after heating / forming of the glass ply in the portions of the glass ply at the periphery 28 of the clear portions, near the edges of the covert band 26, and at the sensor windows 30, 32. Heating / forming of the glass ply may be performed by sag bending or press bending methods, and the degree and type of optical distortions may vary between methods.

[0079] The covert band in both embodiments comprises enamel formed by screen printing an enamel ink onto a surface, curing / drying, and then firing the ink. The enamel may include borosilicate glass frit and at least one inorganic pigment (e.g., containing iron and / or chromium).

[0080] FIG. 3 shows a schematic diagram of the camera / sensor window used in the examples. In each of FIGS. 3(a), 3(b) and 3(c), the hidden band 40 has a sensor window 42. In FIG. 3(a), the second sensor window portion 44 of surface 4, which is larger than the first sensor window portion of surface 2, has an offset at the top, 5 mm sides (i.e. the sensor window portion of surface 4 is 5 mm larger at the top and sides than the sensor window portion of surface 2) and an offset of 8 mm at the bottom. In FIG. 3(b), the second sensor window portion of the larger surface 4, which has an offset as in FIG. 3(a), also has a sawtooth fade-out 46 at the bottom and top of the window portion. The sawtooth fade-out 46 is added to the top and bottom edges (rather than subtracted from them), so that the black print may extend a little further towards the center of the sensor window than in the arrangement of FIG. 3(b). Other patterns such as dots, lines or feathered edges may be used instead of the sawtooth pattern. In FIG. 3( c ), a larger second sensor window portion 44 of Surface 4, having a circumferential offset of 5 mm, is positioned in a hidden frame 48 of Surface 4 within the hidden band 40, said hidden frame 48 comprising high infrared reflectance enamel (one with a higher infrared reflectance than that of the remainder of the hidden band on Surface 4, and that of the enamel on Surface 2).

[0081] Many variations in these camera / sensor window configurations are possible: for example, the sensor window portion of surface 4 may be smaller than the sensor window portion of surface 2. Furthermore, the offset need not be symmetrical but may be offset, i.e., the offset may differ top-bottom and / or left-right.

[0082] Figure 9 shows several other designs of sensor window portion showing designs for Surface 2 (S2) (i.e., first sensor window portion) and Surface 4 (S4) (i.e., second sensor window portion). Figure 9(a) is generally as shown in Figure 3(a) and Figure 9(b) shows a one-sided S4 sensor window portion with a single bottom bar on S4. Figures 9(c) and (e) are three-sided "hat" or "U" profiles for S4 and Figure 9(d) shows multiple bars / blocks on S4.

[0083] Laminated glazing as shown in FIG. 1 or FIG. 2 can generally be manufactured as follows: A flat glass substrate (for example, soda lime float glass with a thickness of 2.1 mm) is screen-printed by a doctor blade with silk screen and enamel ink (for example, using a screen with a polyester screen of 50 to 120 threads / cm, for example a polyester screen of 77 or 100 threads / cm) to form a screen-printed border, which is optionally dried by exposing the substrate to infrared radiation from an infrared heater at a temperature of less than 300° C. Then, the two printed glass substrates for forming the outer first ply of glass 12 and the inner second ply of glass 14 are stacked and the stacked substrates are bent. At this stage, a heat source is provided and the substrate is heated to a temperature of 570° C., usually for 8 minutes or more, and held at this temperature for 1 minute, before being bent at that temperature in a standard bending mould or frame by press bending or sag bending to perform the bending. The substrates are separated and, after cooling, laminated with a PVB interlayer (approximately 0.76 mm thick).

[0084] The glazing may be laminated, for example, by a method that first involves pre-nipping with nip rollers or using vacuum rings applied to the edges of the first and second plies of glass to degas the assembly of glass plies and PVB interlayer. The first and second plies of glass and the PVB interlayer are then laminated together in an autoclave at pressures ranging from 6 bar to 14 bar and temperatures ranging from 110°C to 150°C.

[0085] The present invention is further illustrated by, but not limited to, the following examples. EXAMPLES

[0086] In the examples, laminated windows were fabricated according to the methods described above using black enamels (e.g., Johnson Matthey 1L530, Prince DV174100 and Prince DV17450, high infrared reflectance enamels) and with sensor window portions of various sizes and shapes on surfaces 2 and 4 as shown in Figure 3. Another ink tested was Johnson Matthey 1L4755-WF789P, a medium performance ink.

[0087] The horizontal and vertical optical power of a significant number of each laminated glazing sample was measured at an angle of 55° (converted to a test angle of 60° for comparison) using an optical power measurement system equivalent to the ISRAVision AG standard system with a filter to define the optical power integration length (e.g. 1 / 2 / 0 ISRA filter, equivalent to a 1mm / 1mm filter in the optical power measurement system).

[0088] The light transmission in the visible spectrum 380-780 nm was at least 54% measured at the installation angle.

[0089] The average vertical optical power along the centerline of each window was determined from top to bottom and the results are shown in the graphs in Figures 4 to 8. The x-axis shows the measurement position in mm relative to the center of the window, so that the top of the window is on the left (x=negative) and the bottom of the window is on the right (x=positive). The y-axis shows the optical power measured at each position in mdpt, but transformed to 60° as mentioned above.

[0090] [Example 1] In this example, inks that generate standard levels of optical power are used. The results are shown in FIG. 4 when standard sensor window areas are present on surfaces 2 and 4. There is a relative S2 / S4 offset of 5 mm all around and 8 mm at the bottom (the S4 window area is larger). Line D shows the optical power generated at surface 2, which is negative, and line E shows the optical power generated at surface 4, which is also negative in the center of the window but positive toward the top and bottom. Line F shows the net optical power, which is reduced in absolute magnitude toward the top and especially the bottom of the window, but with little improvement in the center. FIG. 4 shows how balancing the opposing optical powers at the printed surface adjacent to the hidden layer can reduce optical distortion compared to individual plies. However, the optical power generated at surface 2 is significantly weaker than that generated at surface 4, so optimal results have not yet been achieved.

[0091] [Example 2] In this example, a highly infrared reflective enamel was used for surface 4, and the results are shown in FIG. 5. The windshield and sensor window design is the same as in Example 1, but with an offset of 5 mm all around (S4 was about 5 mm larger than S2 all around). As mentioned before, the hidden layer on surface 4 uses a highly infrared reflective enamel (the enamel on surface 2 is a standard enamel as in Example 1). Line D is the same as in Example 1. Line G shows the optical power generated on surface 4 by the highly infrared reflective enamel. Line H shows the net optical power in the window; the proximity of this line to the x-axis shows how much the optical distortion has been reduced. The selection of a highly infrared reflective ink for surface 4 produced a distortion profile much closer to the opposite side of surface 2 (line D) than in Example 1. As a result, the optical distortion of the combined system is further significantly reduced. In comparison, line I shows the optical power of unprinted glass as a baseline. It can be seen that the net optical power towards the bottom of the window is actually better than the unprinted glass, and towards the top the optical power is close to that of the unprinted glass.

[0092] [Example 3] In this example, a different windshield is used than in examples 1 and 2. As in example 1, standard ink is used and the results are shown in FIG. 6. The design of the sensor window is the same as in example 1, offset by 5 mm overall and 8 mm at the bottom. Line J shows the optical power generated at surface 2 and line K shows the optical power generated at surface 4. Line L shows the combined optical power. Although a different design of windshield was used, the results show a similar effect to example 1. The optical power of surface 4 (line K) is higher in absolute magnitude than the optical power of surface 2 (line J), ​​so the compensation effect is only partially achieved, i.e. towards the bottom of the windshield.

[0093] [Example 4] This example uses the windshield of Example 3, with high infrared reflectance enamel on surface 4. The results are shown in FIG. 7. The windshield and sensor window design are the same as in Example 3, but with a 5mm offset all around (S4 was about 5mm more all around than S2), and the hidden layer on surface 4 uses high infrared reflectance enamel. Line J is the same as in Example 3, and line M shows the optical power achieved on surface 4 using high infrared reflectance enamel. Note that line M is almost a mirror image of line J, mirroring the x-axis. The net optical power is shown by line N, and is significantly reduced. Again, this shows that with proper selection of the sensor window design and the inks used, equal and opposite optical powers can be achieved in the individual plies, which can essentially cancel each other out after lamination. Line O shows the baseline optical power of unprinted glass as a comparison. The optical distortion is significantly reduced, approaching that of unprinted glass.

[0094] [Example 5] This example shows a number of approaches to balancing optical distortion / power as well as sensor window design and enamel combinations. The results are shown in Figure 8. The windshield and sensor window design used S4 "caps" around three sides of the window (as in Figure 9(c)), but offset S2 (as in the other examples) by 2-3 mm (S4 was about 5 mm larger overall than S2) around all four sides. The sensor window design was generally similar to Figure 9(c). Line P shows the optical power of surface 2 with standard enamel, line Q shows the optical power of surface 2 with high infrared reflectance enamel, and line T shows the optical power of surface 4 with high infrared reflectance enamel. Windshields were fabricated using two different configurations, one where the sensor window portion of surface 4 is larger than the sensor window portion of surface 2 (line R) and one where the sensor window portion of surface 2 is larger than the sensor window portion of surface 4 (line S). In both cases the enamel had high infrared reflectance. It can be seen that both Lines R and S show improvements over the individual plies (Lines Q and T), but Line R provides the best results overall.

[0095] In summary, the present invention demonstrates that balancing the optical power profiles of the first and second plies of glass significantly reduces the overall optical distortion and optical power for a sensor window. [Explanation of symbols]

[0096] [Reference Number] 2:Laminated glazing 4: Transparent part of glazing 6:Hidden band 8: Around the transparent part 10: Sensor (e.g. ADAS camera) window 12: First (e.g., outer) glass ply 14: Second (e.g., inner) glass ply 15: First sensor window part 16: Polymer intermediate layer 17: Second sensor window 18: Hidden layer of surface 2 19: Bottom offset 20: Hidden layer of surface 4 21: Top offset 22:Laminated glazing 24: Transparent part of glazing 26:Hidden Band 28: Transparent area 30: Left sensor (e.g. ADAS camera) window 32: Right sensor (e.g. ADAS camera) window 40:Hidden band 42: Sensor window 44: Window offset for surface 4 46: Sawtooth Fade Out 48: Hidden frame (e.g., high infrared reflectivity)

Claims

1. 1. A laminated glazing comprising: a first ply of glass having a first surface and a second surface; a second ply of glass having a third surface and a fourth surface; at least one polymer ply positioned between the first and second glass plies; a concealment band around at least a portion of a periphery of the laminated glazing, the concealment band having at least one sensor window and including a first concealment layer and a second concealment layer; the first ply of glass having the first concealing layer attached to at least a portion of the perimeter of the first surface or the second surface, the first concealing layer comprising at least one first sensor window portion having an optical distortion of a first sensor window portion; the second ply of glass having the second concealing layer attached to at least a portion of the perimeter of the third surface or the fourth surface, the second concealing layer comprising at least one second sensor window portion having an optical distortion of a second sensor window portion; an optical distortion of the first sensor window portion and an optical distortion of the second sensor window portion are controlled, respectively, so that an absolute magnitude of the optical distortion of the sensor window is smaller than an absolute magnitude of the optical distortion of the first sensor window and an absolute magnitude of the optical distortion of the second sensor window; 1. A laminated glazing, wherein the first and second concealing layers are formed of materials having different emissivity or infrared reflectivity, thereby enabling control of optical distortion of the first sensor window portion and optical distortion of the second sensor window portion.

2. 2. The laminated glazing of claim 1, wherein a shape of the first sensor window portion differs from a shape of the second sensor window portion to control optical distortion of the first sensor window portion and optical distortion of the second sensor window portion.

3. 3. The laminated glazing of claim 1 or 2, wherein the shape of the first sensor window portion and / or the shape of the second sensor window portion is square, rectangular, trapezoidal, elliptical or circular.

4. 4. A laminated glazing as claimed in any one of the preceding claims, wherein the first sensor window portion and / or the second sensor window portion are partially or wholly surrounded by the first concealing layer and / or the second concealing layer, respectively.

5. 5. The laminated glazing of any one of claims 1 to 4, wherein at least a portion of the periphery of the first sensor window portion or the second sensor window portion is patterned, optionally including dots, lines, fade-outs, feathered edges, or sawtooth fade-outs.

6. 6. A laminated glazing according to any one of the preceding claims, wherein the first hidden layer and / or at least a portion of the second hidden layer has an infrared reflectance of 21% or greater over the region of the wavelength range from 800 nm to 2250 nm.

7. 7. A laminated glazing according to any one of the preceding claims, wherein the first hidden layer and / or the second hidden layer comprises an enamel, the enamel comprising a frit and an inorganic pigment, and the inorganic pigment is selected from iron-chrome pigments, ferrite pigments, chromite pigments, or ferrite / chromite (also known as iron-chromite) pigments.

8. 8. The laminated glazing of claim 7, wherein the enamel of the first concealing layer and / or the enamel of the second concealing layer are selected from low emissivity or low infrared reflectance enamels, or high emissivity or high infrared reflectance enamels, thereby enabling control of optical distortion of the first sensor window portion and optical distortion of the second sensor window portion.

9. 9. The laminated glazing of claim 1, wherein the periphery of either the first sensor window portion or the second sensor window portion comprises a concealing frame portion having a lower (or higher) infrared reflectance than the concealing layer on the remainder of the first or second glass ply and / or a concealing frame portion having a lower (or higher) infrared reflectance than the concealing layer on the other of the first and second glass plies.

10. 10. The laminated glazing of claim 9, wherein the periphery of the second sensor window portion comprises the hidden frame portion.

11. 11. A laminated glazing as claimed in any one of claims 1 to 10, wherein the first sensor window portion has an x-axis dimension and / or a y-axis dimension and the second sensor window portion has an x-axis dimension and / or a y-axis dimension, and the x-axis dimension and / or the y-axis dimension of the first sensor window portion differs from the x-axis dimension and / or the y-axis dimension of the second sensor window portion, respectively, thereby enabling control of the optical distortion of the first sensor window portion and the optical distortion of the second sensor window portion.

12. 12. The laminated glazing of claim 11, wherein the x-axis dimension of the first sensor window portion is greater than the x-axis dimension of the second sensor window portion and / or the y-axis dimension of the first sensor window portion is greater than the y-axis dimension of the second sensor window portion.

13. A laminated glazing as described in claim 12, wherein the smaller of the first sensor window portion and the second sensor window portion is positioned such that there is an offset at each end of a dimension relative to the larger of the first sensor window portion and the second sensor window portion.

14. 14. A laminated glazing according to any one of the preceding claims, wherein the first sensor window portion and / or the second sensor window portion have an optical distortion in the range of -405 to +405 millidiopters, optionally in the range of -310 to +310 millidiopters, optionally in the range of -205 to +205 millidiopters, optionally in the range of -185 to +185 millidiopters, preferably in the range of -155 to +155 millidiopters.

15. 15. A laminated glazing according to any one of the preceding claims, wherein the sensor window has an optical distortion in the range of -195 to +195 millidiopters, optionally in the range of -145 to +145 millidiopters.

16. 1. A process for producing molded laminated glazing, comprising: providing a first glass substrate having a first surface and a second surface and a second glass substrate having a third surface and a fourth surface; applying a first hidden layer to at least a first portion of the first surface or the second surface of the first glass substrate, the first hidden layer comprising at least one first sensor window portion having a controlled optical distortion of the first sensor window portion; applying a second hidden layer to at least a first portion of the third surface or the fourth surface of the second glass substrate, the second hidden layer comprising at least one second sensor window portion having a controlled optical distortion of the second sensor window portion; Optionally, shaping the first and second glass substrates by heating the first and second glass substrates to a temperature greater than 570° C.; disposing at least one polymer ply between the first glass substrate and the second glass substrate; laminating the first glass substrate, the polymer ply, and the second glass substrate; by controlling the optical distortion of the first sensor window portion and the optical distortion of the second sensor window portion, an absolute magnitude of the optical distortion of the sensor window is made smaller than an absolute magnitude of the optical distortion of the first sensor window portion and the optical distortion of the second sensor window portion; a process in which the first hidden layer and the second hidden layer are formed of materials having different emissivity or infrared reflectivity, thereby allowing control of the optical distortion of the first sensor window portion and the optical distortion of the second sensor window portion.

Citation Information

Patent Citations

  • Windshield and on-vehicle system

    JP2016107755A

  • Laminated glass

    JP2017122022A

  • Laminated glass

    JP2017165608A

  • Laminated glass for vehicle

    JP2019026248A

  • Glazing with a frame for an information acquisition system

    JP2021511275A

Cited By

  • Laminated glazing and process

    JP2025011094A