Nonwoven fabric for electromagnetic wave shielding
A nonwoven fabric with a balanced blend of stretched and unstretched polyester fibers addresses the challenge of strength and metal coating suitability in electromagnetic shielding materials, ensuring thinness, lightness, and uniformity.
Patent Information
- Application Number
- JP2020194455
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-24
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-11-24
Smart Images

Figure 0007559301000001 
Figure 0007559301000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a nonwoven fabric for use as a substrate for an electromagnetic shielding material. [Background technology]
[0002] In recent years, with the miniaturization and high density of electronic component materials, there is a demand for electromagnetic shielding materials that are thin and lightweight, yet exhibit excellent electromagnetic shielding properties. For example, Patent Document 1 proposes an electromagnetic shielding material made of a nonwoven fabric treated with a metal coating. To make such an electromagnetic shielding material thin and lightweight, it is necessary to make the nonwoven fabric, which is the base material, thin and lightweight. However, since such nonwoven fabrics have poor strength, the strength is improved by making the fibers denser.
[0003] In electromagnetic shielding materials made of metal-coated nonwoven fabric, the nonwoven fabric base material is required to be thin and lightweight in order to reduce the thickness and weight. However, such nonwoven fabrics have poor strength, so their strength is maintained by making the fibers dense. On the other hand, dense nonwoven fabrics have a problem in that they are poorly suited for metal coating treatment. For example, when plating is used as the metal coating treatment, a plating solution is unlikely to penetrate into a dense nonwoven fabric, and a metal coating may not be formed inside the nonwoven fabric. When vapor deposition treatment is used, a uniform metal coating may not be formed because many areas are shaded by the fibers. To ensure suitability for metal coating treatment while remaining thin and lightweight, it is necessary to incorporate fibers that are relatively thick and provide gaps between the fibers (to increase breathability). However, nonwoven fabrics that incorporate thick fibers have a smaller number of fibers, which reduces their strength and makes them more susceptible to defects such as tearing during plating or adhesive processing. As described above, it has been difficult to simultaneously satisfy all the requirements required for a nonwoven fabric for use as an electromagnetic wave shielding material. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-75485 A Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a nonwoven fabric for an electromagnetic wave shielding material, which is thin and lightweight, yet has excellent suitability for metal coating treatment and strength, and from which an excellent electromagnetic wave shielding material can be obtained. [Means for solving the problem]
[0006] The means for solving the problems of the present invention are as follows. 1. At least, the fiber contains oriented polyester staple fibers and unoriented polyester staple fibers, The fiber contains 25% by mass or more and 65% by mass or less of drawn polyester staple fibers having a fineness of 0.15 dtex (fiber diameter 4.3 μm) to 3.3 dtex (fiber diameter 20.0 μm) based on the total amount of fibers, A nonwoven fabric for use as an electromagnetic shielding material, comprising 35% by mass or more and 65% by mass or less of unstretched polyester staple fibers having a melting point of 220°C or more and 240°C or less relative to the total amount of fibers. 2. The nonwoven fabric for electromagnetic shielding material according to 1., wherein the unstretched polyester staple fiber having a melting point of 220°C or more and 240°C or less has a fineness of 0.8 dtex (fiber diameter 9.8 μm) or more and 1.7 dtex (fiber diameter 14.3 μm) or less. 3. The nonwoven fabric for electromagnetic shielding material according to 2., characterized in that it contains from 1% by mass to 30% by mass of unstretched polyester staple fibers having a fineness of 0.3 dtex (fiber diameter 5.3 μm) or less relative to the total amount of fibers. 4.Basic weight 15g / m 2 4. The nonwoven fabric for use as an electromagnetic shielding material according to any one of 1. to 3., characterized in that: 5. Air permeability: 200cm 3 / (cm 2 ·s) over 510cm 3 / (cm2 5. The nonwoven fabric for use as an electromagnetic shielding material according to any one of 1. to 4., wherein the average value of the nonwoven fabric is less than 1.·s. Effect of the Invention
[0007] The nonwoven fabric for an electromagnetic shielding material of the present invention is thin and lightweight, yet has excellent suitability for metal coating treatment, uniformity, and sufficient processability. Since the nonwoven fabric for an electromagnetic shielding material of the present invention can form a uniform metal coating, an electromagnetic shielding material with excellent electromagnetic shielding properties can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The nonwoven fabric for electromagnetic wave shielding material (hereinafter also referred to as nonwoven fabric) of the present invention contains stretched polyester staple fibers and unstretched polyester staple fibers, The fiber contains 25% by mass or more and 65% by mass or less of drawn polyester staple fibers having a fineness of 0.15 dtex (fiber diameter 4.3 μm) to 3.3 dtex (fiber diameter 20.0 μm) based on the total amount of fibers, The fiber contains 35% by mass or more and 65% by mass or less of unstretched polyester staple fibers having a melting point of 220° C. or more and 240° C. or less based on the total amount of fibers.
[0009] The fibers that form the backbone of the nonwoven fabric without melting much due to heat applied in the manufacturing process of the nonwoven fabric (drying process, heat calendaring process, etc.) are called main fibers, and those that exhibit a binder effect by melting are called binder fibers. In the nonwoven fabric of the present invention, the drawn polyester staple fibers are the main fibers, and the undrawn polyester staple fibers having a melting point of 220°C or higher and 240°C or lower are the binder fibers.
[0010] Since oriented polyester staple fibers are crystallized, they do not melt until their melting point (approximately 260°C for PET). On the other hand, unoriented polyester staple fibers have a low softening point because they are unoriented and not crystallized, and they exhibit an adhesive effect at temperatures lower than their melting point. Furthermore, by heat treating them at around 200°C, they crystallize, improving their adhesive strength. The nonwoven fabric of the present invention contains unstretched polyester staple fibers with a low melting point of 220°C or more and 240°C or less, and therefore exerts a binder effect at low temperatures. Therefore, even when the nonwoven fabric of the present invention has gaps between the fibers (high breathability), it has excellent strength and is not easily cut during processing. In addition, the nonwoven fabric of the present invention can be uniformly metal-coated by having gaps between the fibers.
[0011] The binder fiber used in the present invention can be mainly a single component type, but is not limited to the use of composite fibers of the core-sheath type, eccentric type, side-by-side type, etc. The undrawn polyester fiber of the present invention can more preferably be mainly composed of a copolymer type polyester, and various polyesters such as polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, polyethylene isophthalate, polyphenylene terephthalate, and polyethylene naphthalate can be used, but an undrawn yarn in which 85 mol % or more of the main repeating units are polyesters consisting of ethylene terephthalate units obtained by reacting terephthalic acid with ethylene glycol is preferred. Components other than terephthalic acid and ethylene glycol, such as 2,6-naphthalenedicarboxylic acid, sodium 5-sulfoisophthalate, tetrabutylammonium 5-sulfoisophthalate, tetrabutylphosphonium 5-sulfoisophthalate, adipic acid, sebacic acid, azelaic acid, dodecanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, polycaprolactone, diethylene glycol, trimethylene glycol, pentamethylene glycol, hexamethylene glycol, cyclohexanediol, cyclohexanedimethanol, polyethylene glycol, etc. may be randomly or block copolymerized in small amounts (usually 15 mol % or less based on the terephthalic acid component, etc.). Among these, polyethylene terephthalate copolymerized with 0.5 mol % or more of sodium 5-sulfoisophthalate is preferably used for the undrawn polyester fiber of the present invention.
[0012] ·Stretched polyester staple fiber The nonwoven fabric of the present invention contains 25% by mass or more and 65% by mass or less of stretched polyester staple fibers having a fineness of 0.15 dtex (fiber diameter 4.3 μm) to 3.3 dtex (fiber diameter 20.0 μm) based on the total amount of fibers. If the blending amount of the stretched polyester staple fibers is less than 25% by mass, the suitability for metal coating treatment may decrease. On the other hand, if the blending amount of the stretched polyester staple fibers exceeds 65% by mass, the strength may decrease and the nonwoven fabric may be easily cut or torn. The blending amount of the stretched polyester staple fibers is preferably 27% by mass or more, more preferably 30% by mass or more. Moreover, the blending amount is preferably 60% by mass or less, more preferably 55% by mass or less, and even more preferably 50% by mass or less.
[0013] The fineness of the drawn polyester staple fiber is preferably 0.2 dtex (fiber diameter 4.6 μm) or more, more preferably 0.3 dtex (fiber diameter 5.3 μm) or more, and more preferably 1.7 dtex (fiber diameter 14.3 μm) or less, and even more preferably 0.8 dtex (fiber diameter 9.8 μm) or less. The fiber length of the stretched polyester staple fiber is preferably 1.5 mm or more, more preferably 2 mm or more, and even more preferably 2.5 mm or more. The fiber length is preferably 15 mm or less, more preferably 9 mm or less, and even more preferably 6 mm or less. When the fineness and / or fiber length of the stretched polyester staple fiber is within the above-mentioned range, appropriate gaps are formed between the fibers, and a nonwoven fabric with excellent metal film forming properties can be obtained.
[0014] The nonwoven fabric of the present invention may contain 25% by mass or more and 65% by mass or less of stretched polyester staple fibers having a fineness of 0.15 dtex (fiber diameter 4.3 μm) to 3.3 dtex (fiber diameter 20.0 μm) based on the total amount of fibers, and may also contain stretched polyester staple fibers having a fineness outside the range of 0.15 dtex (fiber diameter 4.3 μm) to 3.3 dtex (fiber diameter 20.0 μm). In addition, two or more types of staple fibers having different fiber lengths or finenesses, or both, may be used in combination as these stretched polyester staple fibers.
[0015] ·Unstretched polyester staple fiber The nonwoven fabric of the present invention contains 35% by mass to 65% by mass of unstretched polyester staple fibers having a melting point of 220°C to 240°C relative to the total amount of fibers. By containing unstretched polyester staple fibers having a melting point of 220°C to 240°C within this range, a nonwoven fabric that is easily melted during heat treatment and has excellent strength can be obtained. If the blending amount of unstretched polyester staple fibers having a melting point of 220°C to 240°C is less than 35% by mass, the binder effect is insufficient, and the strength is insufficient, making the nonwoven fabric prone to breakage and tearing. On the other hand, if the blending amount of unstretched polyester staple fibers having a melting point of 220°C to 240°C exceeds 65% by mass, the fibers melted during heat treatment cannot maintain a perfect circular shape and have a distorted cross section, and the proportion of deformed fibers becomes too high, resulting in a decrease in suitability for metal coating treatment. The blend amount of unstretched polyester staple fibers having a melting point of 220° C. or more and 240° C. or less is preferably 38% by mass or more, and more preferably 40% by mass or more, and preferably 60% by mass or less, more preferably 55% by mass or less, and even more preferably 50% by mass or less.
[0016] The fiber length of the unstretched polyester staple fiber having a melting point of 220° C. or more and 240° C. or less is preferably 1.5 mm or more, more preferably 2 mm or more, and even more preferably 2.5 mm or more, and preferably 15 mm or less, more preferably 9 mm or less, and even more preferably 6 mm or less. The fineness of the undrawn polyester staple fiber having a melting point of 220° C. to 240° C. is preferably 0.03 dtex (fiber diameter 1.9 μm) or more, more preferably 0.1 dtex (fiber diameter 3.9 μm) or more, and even more preferably 0.8 dtex (fiber diameter 9.8 μm) or more. The fineness is preferably 3.3 dtex (fiber diameter 20.0 μm) or less, more preferably 1.7 dtex (fiber diameter 14.3 μm) or less, and even more preferably 1.7 dtex (fiber diameter 14.3 μm) or less.
[0017] The nonwoven fabric of the present invention may contain 35% by mass to 65% by mass of unstretched polyester staple fibers having a melting point of 220° C. to 240° C., based on the total amount of fibers, and may also contain unstretched polyester staple fibers having a melting point exceeding 240° C. In addition, two or more types of staple fibers having different fiber lengths, finenesses, or both may be used in combination as unstretched polyester staple fibers having a melting point of 220° C. to 240° C., or a melting point exceeding 240° C. In addition, two or more types of staple fibers having different fiber lengths, finenesses, or both may be used in combination. By using two or more types of staple fibers having different fiber lengths, finenesses, or both, the impregnation and uniformity in the plating solution can be controlled.
[0018] -Unstretched polyester staple fibers with a fineness of 0.3 dtex (fiber diameter 5.3 μm) or less In the nonwoven fabric of the present invention, when the unstretched polyester staple fiber having a melting point of 220°C to 240°C has a fineness of 0.8 dtex (fiber diameter 9.8 μm) or more, it is preferable to contain unstretched polyester staple fibers having a fineness of 0.3 dtex or less (fiber diameter 5.3 μm) in addition to the unstretched polyester staple fibers. The melting point of the unstretched polyester staple fibers having a fineness of 0.3 dtex or less (fiber diameter 5.3 μm) is not limited to 220°C to 240°C. Since unstretched polyester staple fibers having a fineness of 0.3 dtex (fiber diameter 5.3 μm) or less are thin and easily retain water, the inclusion of unstretched polyester staple fibers having a fineness of 0.3 dtex (fiber diameter 5.3 μm) or less improves the papermaking properties during wet papermaking. In addition, by blending unstretched polyester staple fibers having a fineness of 0.3 dtex (fiber diameter 5.3 μm) or less, the roughness of the nonwoven fabric can be adjusted, making it easy to adjust the air permeability to a desired value. Furthermore, by using unstretched polyester staple fibers having a fineness of 0.3 dtex (fiber diameter 5.3 μm) or less, the strength of the nonwoven fabric is increased, and the mechanical strength required for plating can be maintained. On the other hand, if unstretched polyester staple fibers having a fineness of 0.8 dtex (fiber diameter 9.8 μm) or more are not included, appropriate gaps are not formed between the fibers, and metal film formation may be poor. In the present invention, as the undrawn polyester staple fibers having a fineness of 0.3 dtex (fiber diameter 5.3 μm) or less, two or more kinds of staple fibers having different fiber lengths, finenesses, or both may be used in combination.
[0019] From the viewpoint of papermaking properties, the nonwoven fabric of the present invention preferably contains 1% by mass or more and 30% by mass or less of unstretched polyester staple fibers having a fineness of 0.3 dtex (fiber diameter 5.3 μm) or less with respect to the total amount of fibers. If the blending amount of unstretched polyester staple fibers having a fineness of 0.3 dtex (fiber diameter 5.3 μm) or less is less than 1% by mass, the papermaking property improvement effect is hardly expected. On the other hand, if it exceeds 30% by mass, the papermaking property improvement effect is hardly expected, and furthermore, the nonwoven fabric becomes dense and the metal coating treatment suitability may decrease. The blending amount of unstretched polyester staple fibers having a fineness of 0.3 dtex (fiber diameter 5.3 μm) or less is more preferably 5% by mass or more, and even more preferably 10% by mass or more. Moreover, this blending amount is more preferably 25% by mass or less, and even more preferably 20% by mass or less.
[0020] "Manufacturing method" The nonwoven fabric used in the present invention can be produced by a conventionally known papermaking method. Examples of the paper machine include a cylinder paper machine, an inclined short wire paper machine, a Fourdrinier paper machine, and a twin wire paper machine. In the present invention, the nonwoven fabric can be dried by a conventionally known drying method. Examples of the drying process in the papermaking method used in the present invention include a Yankee dryer type, a multi-cylinder type, a hot air type, and an infrared heating type. The heat treatment step may be performed by the drying step, or may be performed as a separate step. The heat treatment step is preferably a thermal calendaring step, because the thermally melted binder resin is entangled with the main fibers, improving the strength. The heat treatment temperature may be any temperature at which the unstretched polyester staple fibers, which have a melting point of 220°C to 240°C, are softened and can exert their binder effect, and is, for example, about 170°C to 220°C.
[0021] The basis weight of the nonwoven fabric of the present invention can be selected depending on the desired thinness, lightness, etc., but specifically, it is 20 g / m 2 It is preferable that the thickness is less than 15 g / m 2 More preferably, it is 10 g / m or less. 2 The thickness is preferably 30 μm or less, more preferably 25 μm or less, and even more preferably 20 μm or less. In order to prevent cutting or tearing during processing, the nonwoven fabric of the present invention has a tensile strength in the MD direction measured in accordance with JIS P8113 of preferably 5 N / 15 mm or more, more preferably 5.2 N / 15 mm or more, and even more preferably 5.5 N / 15 mm or more.
[0022] The nonwoven fabric of the present invention has an air permeability of 200 cm as measured in accordance with JIS L1096 8.26.1 Method A (Fragile method). 3 / (cm 2 ·s) over 510cm 3 / (cm 2 It is preferable that the air permeability is less than 200 cm 3 / (cm 2If the thickness is less than 510 cm, the nonwoven fabric may be too dense and may be poorly suited for metal coating treatment. 3 / (cm 2 If the air permeability is more than 210 cm, the nonwoven fabric becomes sparse, and the electromagnetic shielding properties of the resulting electromagnetic shielding material may be insufficient. 3 / (cm 2 s) or more is more preferable, and 220 cm 3 / (cm 2 It is more preferable that the thickness is 410 cm or more. 3 / (cm 2 s), and more preferably less than 320 cm 3 / (cm 2 It is even more preferable that the ratio is equal to or less than s.
[0023] The method for metal coating treatment of the nonwoven fabric of the present invention is not particularly limited, and any conventionally known method can be used, such as electroless plating, electroplating, vapor deposition, sputtering, etc. Among these, electroless plating is preferred because a metal coating can be formed simply by contacting the nonwoven fabric with a plating solution. The metals include gold, silver, copper, zinc, nickel, tin, and alloys thereof, and the same or different metals may be used to form a coating of two or more layers. Among these, it is preferable to use copper from the viewpoints of electrical conductivity and manufacturing costs.
[0024] The processing step of the metal film treatment by electroless plating method can be carried out by a conventional method, for example, as follows. A refining process is carried out to remove the paste and oil adhering to the surface of the nonwoven fabric, and then the nonwoven fabric is immersed in an alkaline solution for weight reduction as necessary. The refined nonwoven fabric is preferably subjected to a catalyst process in which a treatment agent in which palladium, which is the core of electroless metal plating, is colloidized with tin is adsorbed on the fiber surface, and the fabric is washed with water, and then the colloid is activated in an acceleration process. After the activation process, the fabric is washed with water again and immersed in a plating bath to form a metal film on the surface of the nonwoven fabric. EXAMPLES
[0025] The present invention will be described in more detail below with reference to examples, but the configuration of the present invention is not limited thereto. The obtained nonwoven fabric was evaluated by the following measurement methods, and the results are shown in Tables 1 and 2.
[0026] Measurement method · Basis weight, thickness, density The basis weight was measured according to JIS P8124. The thickness of one sheet was measured at a pressure of 100 kPa between the pressure surfaces in accordance with JIS P8118. According to JIS P8118, the basis weight (g / m 2 The density was calculated by dividing the thickness (μm) by the thickness (μm).
[0027] Tensile strength Complies with JIS P8113. Air permeability [cm 3 / (cm 2 s)] Using an air permeability measuring device conforming to JIS L1096 8.26.1 A method (Fragile method), measure the air permeability of 1 cm of the sample at a differential pressure of 125 Pa. 2 The volume of air passing through the area in one second was measured.
[0028] (Processing suitability) The processability was evaluated according to the following criteria based on tensile strength (measured in accordance with JIS P8113) in order to determine the possibility of paper tearing during plating and adhesive processing. 〇: MD; 4.5N / 15mm or more and CD; 2.0N / 15mm or more ×: MD; less than 4.5N / 15mm, or CD; less than 2.0N / 15mm
[0029] (Metal coating suitability / uniformity) The suitability and uniformity of metal coating were evaluated based on the breathability of the nonwoven fabric (measured according to JIS L1096 8.26.1 Method A (Fragile method)) according to the following criteria. The higher the number, the better the evaluation. -Suitable for metal coating 5:410cm 3 / (cm 2 ·s) or more 4:240cm 3 / (cm 2 ·s) over 410cm 3 / (cm 2 Less than s) 3:200cm 3 / (cm 2 ·s) over 240cm 3 / (cm 2 Less than s) 2:100cm 3 / (cm 2 ·s) over 200cm 3 / (cm 2 Less than s) 1:100cm 3 / (cm 2 Less than s) ·Uniformity 5:100cm 3 / (cm 2 Less than s) 4:100cm 3 / (cm 2 ·s) more than 300cm 3 / (cm 2 Less than s) 3:300cm 3 / (cm 2 ·s) over 410cm 3 / (cm 2 Less than s) 2:410cm 3 / (cm 2 ·s) over 510cm 3 / (cm 2 Less than s) 1:510cm 3 / (cm 2 ·s) or more
[0030] (comprehensive evaluation) The overall evaluation was determined based on the following criteria, taking into account processability, metal coating processability and uniformity. When processing suitability is 〇, metal coating processing suitability + uniformity = 8, overall evaluation is ◎ Metal coating suitability + uniformity = 7 Overall rating: Good When metal coating suitability + uniformity is ≦6, overall evaluation is × If processing suitability is ×, overall evaluation is ×
[0031] "Example 1" 40% by mass of stretched polyester staple fiber (manufactured by Unitika Ltd., product number 521, melting point approximately 259°C, fiber length 5 mm, fineness 0.4 dtex (fiber diameter 7.0 μm)) and 60% by mass of unstretched polyester staple fiber (manufactured by Teijin Ltd., Tepyrus (registered trademark) TR07N, melting point approximately 233°C, fiber length 5 mm, fineness 1.2 dtex (fiber diameter 11.8 μm)) were mixed and paper-formed on a short-wire Yankee papermaking machine to obtain a paper with a basis weight of 8.0 g / m 2 The base paper was wet-made, and then heat-pressurized using a thermal calendar with a pair of heated rolls at a roll surface temperature of 200°C, a linear pressure of 50 N / mm, and a processing speed of 40 m / min to obtain a nonwoven fabric for electromagnetic wave shielding material.
[0032] "Example 2" A nonwoven fabric for an electromagnetic wave shielding material was obtained in the same manner as in Example 1, except that the amount of stretched polyester staple fibers was 50% by mass and the amount of unstretched polyester staple fibers was 50% by mass. "Example 3" A nonwoven fabric for an electromagnetic wave shielding material was obtained in the same manner as in Example 1, except that the amount of the stretched polyester staple fiber was 60 mass % and the amount of the unstretched polyester staple fiber was 40 mass %.
[0033] "Comparative Example 1" A nonwoven fabric for an electromagnetic wave shielding material was obtained in the same manner as in Example 1, except that the amount of the stretched polyester staple fiber was 30 mass % and the amount of the unstretched polyester staple fiber was 70 mass %. "Comparative Example 2" A nonwoven fabric for an electromagnetic wave shielding material was obtained in the same manner as in Example 1, except that the amount of stretched polyester staple fibers was 70 mass % and the amount of unstretched polyester staple fibers was 30 mass %.
[0034] "Comparative Example 3" A nonwoven fabric for electromagnetic wave shielding material was obtained in the same manner as in Example 1, except that the material used was 50 mass% of stretched polyester staple fibers (Teijin Limited, Tepyrus (registered trademark) TA04PN, melting point approximately 259°C, fiber length 3 mm, fineness 0.1 dtex (fiber diameter 3.9 μm)) and 50 mass% of unstretched polyester staple fibers (Teijin Limited, Tepyrus (registered trademark) TK08PN, melting point approximately 248°C, fiber length 3 mm, fineness 0.2 dtex (fiber diameter 4.6 μm)).
[0035] "Comparative Example 4" A nonwoven fabric for electromagnetic wave shielding material was obtained in the same manner as in Example 1, except that a paper material containing 50 mass% of drawn polyester staple fiber (Teijin Limited, Tepyrus (registered trademark) TA04PN, melting point approximately 259°C, fiber length 3 mm, fineness 0.1 dtex (fiber diameter 3.9 μm)) and 50 mass% of (Teijin Limited, Tepyrus (registered trademark) TR07N, melting point approximately 233°C, fiber length 5 mm, fineness 1.2 dtex (fiber diameter 11.8 μm)) was used.
[0036] [Table 1]
[0037] The nonwoven fabrics of the present invention obtained in Examples 1 to 3 were able to achieve a good balance between processability, suitability for metal coating treatment, and uniformity. In contrast, the nonwoven fabric obtained in Comparative Example 1 was inferior in uniformity, and the nonwoven fabric obtained in Comparative Example 2 was inferior in processability. Moreover, the nonwoven fabrics obtained in Comparative Examples 3 and 4 were too dense and inferior in metal coating treatment suitability.
[0038] "Example 4" A nonwoven fabric for electromagnetic wave shielding material was obtained in the same manner as in Example 1, except that a paper material containing 30 mass% of stretched polyester staple fibers, 60 mass% of unstretched polyester staple fibers, and 10 mass% of unstretched polyester staple fibers having a fineness of 0.2 dtex (fiber diameter 4.6 μm) (Teijin Limited, Tepyrus (registered trademark) TK08P, binder fiber, melting point approximately 248° C., fiber length 3 mm, fineness 0.2 dtex (fiber diameter 4.6 μm)) was used.
[0039] "Example 5" A nonwoven fabric for electromagnetic wave shielding material was obtained in the same manner as in Example 4, except that a paper material containing 40% by mass of stretched polyester staple fiber, 50% by mass of unstretched polyester staple fiber, and 10% by mass of unstretched polyester staple fiber having a fineness of 0.2 dtex (fiber diameter 4.6 μm) was used. "Example 6" A nonwoven fabric for electromagnetic wave shielding material was obtained in the same manner as in Example 4, except that a paper material containing 50% by mass of stretched polyester staple fiber, 40% by mass of unstretched polyester staple fiber, and 10% by mass of unstretched polyester staple fiber having a fineness of 0.2 dtex (fiber diameter 4.6 μm) was used. "Example 7" A nonwoven fabric for electromagnetic wave shielding material was obtained in the same manner as in Example 4, except that a paper material containing 40 mass% stretched polyester staple fiber, 45 mass% unstretched polyester staple fiber, and 15 mass% unstretched polyester staple fiber with a fineness of 0.2 dtex (fiber diameter 4.6 μm) was used. "Example 8" A nonwoven fabric for electromagnetic wave shielding material was obtained in the same manner as in Example 4, except that a paper material containing 30% by mass of stretched polyester staple fiber, 50% by mass of unstretched polyester staple fiber, and 20% by mass of unstretched polyester staple fiber having a fineness of 0.2 dtex (fiber diameter 4.6 μm) was used. "Example 9" A nonwoven fabric for electromagnetic wave shielding material was obtained in the same manner as in Example 4, except that a paper material containing 40% by mass of stretched polyester staple fiber, 40% by mass of unstretched polyester staple fiber, and 20% by mass of unstretched polyester staple fiber having a fineness of 0.2 dtex (fiber diameter 4.6 μm) was used.
[0040] "Comparative Example 5" A nonwoven fabric for electromagnetic wave shielding material was obtained in the same manner as in Example 4, except that a paper material containing 40% by mass of stretched polyester staple fiber, 30% by mass of unstretched polyester staple fiber, and 30% by mass of unstretched polyester staple fiber having a fineness of 0.2 dtex (fiber diameter 4.6 μm) was used. "Comparative Example 6" A nonwoven fabric for electromagnetic wave shielding material was obtained in the same manner as in Example 4, except that a paper material containing 40 mass% stretched polyester staple fibers, 45 mass% unstretched polyester staple fibers (Teijin Limited, Tepyrus (registered trademark) TA07N, melting point approximately 257°C, fiber length 5 mm, fineness 1.2 dtex (fiber diameter 11.3 μm)), and 15 mass% unstretched polyester staple fibers having a fineness of 0.2 dtex (fiber diameter 4.6 μm) was used.
[0041] [Table 2]
[0042] The nonwoven fabrics of the present invention obtained in Examples 4 to 9 were able to achieve a good balance of processability, metal coating suitability, and uniformity, and in particular, the nonwoven fabrics of the present invention obtained in Examples 6 to 8 were able to achieve an even higher level of balance among each property. In contrast, the nonwoven fabric obtained in Comparative Example 5 was poor in suitability for metal coating treatment, and the nonwoven fabric obtained in Comparative Example 6 was poor in suitability for processing.
Claims
1. At least, the fiber contains oriented polyester staple fibers and unoriented polyester staple fibers, The fiber contains 25% by mass or more and 65% by mass or less of drawn polyester staple fibers having a fineness of 0.3 dtex or more and 0.8 dtex or less based on the total amount of fibers, A nonwoven fabric for use as an electromagnetic shielding material, comprising 35% by mass to 65% by mass of unstretched polyester staple fibers having a melting point of 220° C. or more and 240° C. or less and a fineness of 0.8 dtex or more and 1.7 dtex or less, based on the total amount of fibers.
2. 2. The nonwoven fabric for electromagnetic shielding material according to claim 1, characterized in that it contains 1% by mass or more and 30% by mass or less of undrawn polyester staple fibers having a fineness of 0.3 dtex or less based on the total amount of fibers.
3. Basis weight 15g / m 2 3. The nonwoven fabric for electromagnetic wave shielding material according to claim 1, wherein the nonwoven fabric is:
4. Ventilation rate: 200 cm 3 / (cm 2 ・s) or more 510cm 3 / (cm 2 4. The nonwoven fabric for electromagnetic wave shielding material according to claim 1, wherein the thickness of said nonwoven fabric is less than 1 mm.
Citation Information
Patent Citations
Base material for tape, and method of manufacturing the same
JP2014019959A
Electromagnetic wave shielding material
JP2014075485A
Method for manufacturing nonwoven fabric substrate for electromagnetic wave-shielding material
JP2019049079A
Nonwoven fabric substrate for electromagnetic wave-shielding material
JP2019049080A
Biomass-derived polyester short fibers and wet nonwoven fabric formed from same
WO2012057105A1