Coating solution containing cellulose nanocrystals containing anionic functional groups

The coating liquid with anionic functional cellulose nanocrystals and additives forms self-organized structures for quick drying and superior gas barrier properties, addressing viscosity and dispersibility issues in cellulose nanofiber coatings.

JP7559456B2Active Publication Date: 2024-10-02TOYO SEIKAN GRP HLDG LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020156229
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-17
Publication Date
2024-10-02
Estimated Expiration
2040-09-17

AI Technical Summary

Technical Problem

Existing cellulose nanofiber and nanocrystal coatings face issues with high viscosity, poor additive dispersibility, long drying times, and inadequate gas barrier properties, leading to coating defects and low economic efficiency.

Method used

A coating liquid containing anionic functional group-containing cellulose nanocrystals, mixed with a water-alcohol solvent, layered inorganic compounds, hydroxyl group-containing polymers, and polyhydric carboxylic acids, forming nematic liquid crystals for self-organized structures with enhanced gas barrier properties.

Benefits of technology

The coating liquid achieves low viscosity, quick drying times, excellent gas barrier properties, and improved economic efficiency with no coating defects, maintaining self-organized structures even under high humidity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559456000001
    Figure 0007559456000001
  • Figure 0007559456000002
    Figure 0007559456000002
  • Figure 0007559456000003
    Figure 0007559456000003
Patent Text Reader

Abstract

To provide a cellulose nanocrystal-containing coating liquid that uses a cellulose nanocrystal dispersion with excellent gas barrier and handling properties, and enables a crosslinked structure with uniformly dispersed cellulose nanocrystals to be formed by short-term drying.SOLUTION: A coating liquid contains anionic functional group-containing cellulose nanocrystals and an additive, with a solvent mixture composed of water and an alcohol to be used as a dispersion medium.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coating liquid containing cellulose nanocrystals containing anionic functional groups, and more specifically, to a coating liquid containing cellulose nanocrystals containing anionic functional groups, which has excellent handleability during coating, dispersibility of additives, coated surface condition and drying properties, and is capable of exhibiting excellent gas barrier properties. [Background technology]

[0002] Nanocellulose has been proposed for use in a variety of applications as an advanced biomass raw material, functional additive, film composite material, etc. In particular, materials such as membranes made of cellulose nanofibers (CNF) and laminates containing cellulose nanofibers are known to have excellent gas barrier properties, such as oxygen barrier properties, because they suppress the dissolution and diffusion of gases due to the strong hydrogen bonds and cross-linking interactions between the cellulose fibers, and barrier materials using cellulose nanofibers have been proposed. In order to reduce the size of cellulose fibers, in addition to mechanical treatment, chemical treatment is carried out to introduce hydrophilic functional groups, such as carboxyl groups or phosphate groups, into the hydroxyl groups of cellulose. This not only reduces the energy required for the reduction process, but also improves the barrier properties and dispersibility in aqueous solvents.

[0003] Dispersions using such cellulose nanofibers are also known. For example, Patent Document 1 listed below proposes a dispersion in which cellulose nanofibers having a crystallinity of 70% or more, a degree of polymerization of 160 or less as measured by a viscosimetry using a copper ethylenediamine solution, and a fiber diameter of 50 nm or less are dispersed in a dispersion medium. Furthermore, Patent Document 2 below proposes a coating agent that contains a water-soluble polymer and modified fine cellulose obtained by oxidizing and finely pulverizing cellulose, the modified fine cellulose having carboxyl groups on the surface, 70% or more of the total number of counter ions of the carboxyl groups being ammonium ions, the concentration of the water-soluble polymer being 1% by mass or more and 90% by mass or less, and the water-soluble polymer being at least one of polyvinyl alcohol, ethylene vinyl alcohol, and carboxymethyl cellulose. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-256546 A [Patent Document 2] JP 2020-37696 A Summary of the Invention [Problem to be solved by the invention]

[0005] In the cellulose nanofiber dispersion described in Patent Document 1, carboxyl groups are added to cellulose nanofibers with long fiber length by chemical treatment using a TEMPO catalyst, and the cellulose nanofiber dispersion has a very high viscosity due to the fiber length and the amount of carboxyl groups. In addition, since water is a good dispersion medium for nanocellulose, an aqueous dispersion is generally used for a nanocellulose-containing coating liquid, and it is difficult to mix with alcohol and to prepare a dispersion with a high solid content. In addition, the dispersion of additives is poor and coating defects occur on the coating surface due to the high viscosity described above. In addition, it takes a long time to dry, so it is not satisfactory in terms of handleability, productivity, and economic efficiency. In addition, cellulose nanofibers are not satisfactory in terms of gas barrier properties because of their long fiber length. It is possible to obtain high gas barrier properties by shortening the fiber length, but further processing is required for that, which is poor in economic efficiency. The coating agent described in Patent Document 2 is capable of exhibiting good gas barrier properties under high humidity conditions, but has an oxygen permeability of 2.3 to 3.4 cc / m 2 1 day·Pa (40% RH), which is not a satisfactory level of gas barrier properties. In addition, because it uses cellulose nanofibers that have been chemically treated with a TEMPO catalyst, it is not fully satisfactory in terms of coatability, productivity, and economy, just like Reference 1.

[0006] Cellulose nanocrystals (CNCs), which are made by hydrolyzing cellulose fibers with strong acids, are known as nanocelluloses with shorter fiber lengths than cellulose nanofibers. Because cellulose nanocrystals have short fiber lengths, they have low viscosity, are easy to handle when applied, and have excellent smoothness when applied. However, cellulose nanocrystals generally have inferior gas barrier properties compared to cellulose nanofibers with carboxyl groups introduced as described above. The inventors have proposed a cellulose nanocrystal-containing coating liquid that uses a cellulose nanocrystal dispersion liquid with excellent gas barrier properties and ease of handling, and by adding a water-soluble polymer, an inorganic layered compound, and a polycarboxylic acid to it, can efficiently form a crosslinked structure in which cellulose nanocrystals are uniformly dispersed (Patent Application No. 2020-5116). However, even in the case of the above-mentioned cellulose nanocrystal-containing coating liquid, it is difficult to efficiently dry a coating liquid having a high solid content in a short period of time, and further improvements in productivity and economic efficiency are desired.

[0007] Therefore, the object of the present invention is to provide a cellulose nanocrystal-containing coating liquid that has excellent gas barrier properties and handleability, good dispersion of additives, a high solids concentration, an excellent coating surface, and excellent productivity and economy, as well as the ability to shorten the drying time until the paint solidifies. Another object of the present invention is to provide a molded article having a cellulose nanocrystal-containing layer that has excellent gas barrier properties and interlayer adhesion. [Means for solving the problem]

[0008] According to the present invention, there is provided a coating solution containing an anionic functional group-containing cellulose nanocrystal and an additive, comprising: The additives include at least a layered inorganic compound, a hydroxyl group-containing polymer, and a polycarboxylic acid, There is provided a coating liquid characterized in that a mixed solvent of water and alcohol is used as a dispersion medium.

[0009] In the coating solution of the present invention, 1. Contains nematic liquid crystal and / or chiral nematic liquid crystal; 2. Exhibits birefringence; 3. The anionic functional group-containing cellulose nanocrystal is contained in an amount of 0.5% by mass or more as a solid content; 4. The mixed solvent contains 10 to 50 parts by mass of alcohol per 90 to 50 parts by mass of water; 5. The alcohol is at least one of ethanol, methanol, and isopropyl alcohol; 6. The foregoing The layered inorganic compound is mica, the hydroxyl group-containing polymer is polyvinyl alcohol, and the polycarboxylic acid is citric acid. That is, 7. The anionic functional group is a sulfo group and / or a sulfate group derived from sulfuric acid decomposition; 8. The viscosity of the anionic functional group-containing cellulose nanocrystal measured with a rotational viscometer (rotation speed: 60 rpm, rotation time: 60 seconds) when the solid content is 0.5 to 3 mass% is 1 to 10,000 mPa s; 9. When the solid content of the anionic functional group-containing cellulose nanocrystal is 0.5 to 3 mass %, the time until the coated surface is solidified when the coated surface is dried at 150°C on a substrate is 60 seconds or less. is preferred.

[0010] According to the present invention, there is also provided a molded article comprising a layer containing a polyvalent cationic resin and cellulose nanocrystals formed on a substrate, the layer containing the anionic functional group-containing cellulose nanocrystals (solid content) being 1.0 g / cm 2 When the amount is 1.0cc / m2, the oxygen permeability (23℃ 50%RH) is 1.0cc / m2 2The molded article is characterized in that its viscosity is less than 1000 psi.day·atm. In the molded article of the present invention, it is preferable that the polyvalent cationic resin is polyethyleneimine. Effect of the Invention

[0011] In the coating solution of the present invention, since anionic functional group-containing cellulose nanocrystals having a short fiber length are used, the coating solution can be made low in viscosity despite the high solid content concentration, and is excellent in handling, additive mixing processing, and dispersibility. Moreover, since a mixed solvent of volatile alcohol and water can be used as a dispersion medium, the time until solidification can be shortened, and the coating solution is excellent in productivity and economy. This is also clear from the results of the examples described below, and in the coating film when a coating solution containing anionic functional group-containing cellulose nanocrystals at a solid content concentration of 0.5 to 3 wt % is applied to a substrate, no coating defects such as surface streaks, unevenness, coating voids, gels, bumps, orange peel, or voids in the coating film occur, and the coating surface can be dried at 150° C. in a short time of 60 seconds or less until solidification. In addition, the anionic functional group-containing cellulose nanocrystal has good dispersibility in a mixed solvent of water and alcohol, forms nematic liquid crystals and / or chiral nematic liquid crystals by self-alignment, and is solidified by drying treatment while maintaining the liquid crystal self-alignment, so that it is possible to form a sufficient self-organized structure in the coating film and to exhibit excellent gas barrier properties. The coating solution of the present invention exhibits birefringence due to the presence of the nematic liquid crystals and / or chiral nematic liquid crystals, which is evident from the results of the examples described below.

[0012] Furthermore, the coating liquid of the present invention preferably contains at least one of a layered inorganic compound, a hydroxyl group-containing polymer, and a polycarboxylic acid as an additive. This allows the hydroxyl groups of the cellulose nanocrystals and the polycarboxylic acid to form a dense crosslinked film, resulting in excellent gas barrier properties and water resistance. Contains acid groupsCombined with the improvement in gas barrier properties due to the inclusion of a polymer and a layered inorganic compound, it becomes possible to exhibit excellent gas barrier properties even under high humidity conditions. Furthermore, in a molded article formed by forming a layer containing the polyvalent cationic resin and cellulose nanocrystals of the present invention, the polyvalent cationic resin naturally diffuses between the cellulose nanocrystals, while maintaining the dense self-organized structure between the cellulose nanocrystals, creating a mixed state in which the polyvalent cationic resin is naturally diffused and interposed between the cellulose nanocrystals, and since the self-organized structure of the cellulose nanocrystals is further strengthened by the polyvalent cations, the article has gas barrier properties that are superior to those exhibited by cellulose nanocrystals alone. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] (Coating solution) In the present invention, by using cellulose nanocrystals containing anionic functional groups, it becomes possible to use a mixed solvent consisting of water and alcohol as a dispersion medium, and this has good additive mixing and dispersibility, an excellent coating surface without coating defects, and exhibits excellent gas barrier properties, while making it possible to shorten the drying time as described above. That is, the anionic functional group-containing cellulose nanocrystal used in the present invention forms an electric double layer between adjacent fibers due to the charge (anion) of the anionic functional group such as sulfate group and / or sulfo group or carboxyl group present on the nanocellulose surface, and a repulsive force (repulsion) occurs between the fibers. In addition, since the fiber length of cellulose nanocrystals is short, the fibers are characterized in that they are easier to separate from each other than cellulose nanofibers. Therefore, this cellulose nanocrystal can easily attract protic solvents such as water and alcohol between the fibers, and the solvent osmotic pressure of the mixed solvent consisting of water and alcohol attracted between the fibers and the above-mentioned repulsive force of the cellulose nanocrystals combine to enhance the isolated dispersibility of the cellulose nanocrystals, making it possible to obtain good dispersibility of the cellulose nanocrystals in the above-mentioned mixed solvent. In addition, the mixed solvent used in the present invention has polarity, which can reduce the effect of van der Waals forces, and effectively prevents the good dispersibility of the cellulose nanocrystals in the above-mentioned mixed solvent from being impaired.

[0014] As described above, the dispersion containing the anionic functional group-containing cellulose nanocrystal has a lower viscosity than the dispersion containing the cellulose nanofiber chemically treated with the TEMPO catalyst having a carboxyl group, which is an anionic functional group, and the coating solution of the present invention has a characteristic that the viscosity measured with a rotational viscometer (rotation speed 60 rpm, rotation time 60 seconds) when the solid content of the anionic functional group-containing cellulose nanocrystal is 0.5 to 3 wt % is 1 to 10,000 mPa·s. As a result, it is possible to prepare a coating solution with a low viscosity even if the solid content concentration is high, and the coating film has excellent dispersibility of additives, handleability such as coatability and film-forming property, and gas barrier properties, and in combination with the use of the above-mentioned water and alcohol mixed solvent, it is possible to further shorten the drying time of the coating film.

[0015] In addition, the anionic functional group-containing cellulose nanocrystal used in the present invention has many hydrogen bonds within or between molecules, and therefore has a large cohesive energy density. In addition, since it contains an anionic functional group that can contribute to the formation of a self-organized structure, the cellulose nanocrystal forms nematic liquid crystals and / or chiral nematic liquid crystals by self-alignment in a mixed solvent of water and alcohol, as described above. Since solidification by drying treatment is carried out while maintaining such liquid crystalline self-alignment, it is possible to form a sufficient self-organized structure in the coating film, and it is possible to exhibit excellent gas barrier properties.

[0016] In the coating solution of the present invention, water is used as an additive together with the anionic functional group-containing cellulose nanocrystals. Contains acid groups polymer, Layered Inorganic By containing compounds, polyvalent carboxylic acids, etc., the additives have excellent dispersibility, and as mentioned above, excellent gas barrier properties can be exhibited even under high humidity conditions. That is, the hydroxyl group-containing polymer can form a dense crosslinked structure together with the cellulose nanocrystals and can also impart flexibility, significantly improving the gas barrier properties of the resulting coating film. In addition, the layered inorganic compound has swelling and cleavage properties, so that the cellulose nanocrystals can be easily dispersible. Layered Inorganic The compound penetrates and expands the gap between the layers, and the layered inorganic compound provides a bypass effect for the permeating gas, and the crosslinked structure of the cellulose nanocrystals combine to provide excellent gas barrier properties even under high humidity conditions. In addition, the addition of a polycarboxylic acid as a reactive crosslinking agent makes it possible to more efficiently form the dense self-organized structure described above.

[0017] [Cellulose nanocrystal dispersion] The cellulose nanocrystals contained in the coating liquid of the present invention are prepared as a dispersion in which cellulose nanocrystals formed by acid hydrolysis of cellulose raw material with hydrochloric acid, sulfuric acid, or the like are used as a dispersoid, and a mixed solvent of water and alcohol is used as a dispersion medium. As described below, such a dispersion is preferably a cellulose nanocrystal dispersion that has not been solidified (never-dried) during preparation of the dispersion, i.e., a dispersion that is not one that has been solidified into a powder form by spray drying or the like and then redispersed. In other words, cellulose nanocrystals that have been solidified by drying are unlikely to orient the fibers in the dispersion, making it difficult to form a dense self-organized structure, and have inferior gas barrier properties compared to dispersions that have not been solidified.

[0018] In addition, in the cellulose nanocrystal dispersion liquid contained in the coating liquid of the present invention, all cellulose nanocrystals including those hydrolyzed by hydrochloric acid treatment can be used, but cellulose nanocrystals hydrolyzed by sulfuric acid treatment are preferred. That is, cellulose nanocrystals include those obtained by acid hydrolysis of cellulose fibers by sulfuric acid treatment or hydrochloric acid treatment, but cellulose nanocrystals obtained by sulfuric acid treatment are advantageously used because they already have sulfate groups and / or sulfo groups that can contribute to the formation of a self-organized structure. It is particularly preferable that the cellulose nanocrystal contains a total amount of sulfate groups and / or sulfo groups in the range of more than 0.01 mmol / g and not more than 4.0 mmol / g. By having the total amount of sulfate groups and / or sulfo groups in the above range, it is possible to form a sufficient self-organized structure while maintaining the crystal structure of the cellulose nanocrystal, and it is possible to express excellent gas barrier properties. In this specification, the sulfate group is a concept that includes sulfate ester groups. Furthermore, cellulose nanocrystals having a fiber diameter of 50 nm or less, particularly in the range of 2 to 50 nm, a fiber length of 100 to 500 nm, an aspect ratio of 5 to 50, and a crystallinity of 60% or more, particularly 70% or more, can be suitably used.

[0019] Alcohol, which serves as the dispersion medium in the anionic functional group-containing cellulose nanocrystal dispersion used in the present invention, has a higher relative evaporation rate than water, and by using a water / alcohol mixed solvent in an appropriate ratio, the drying time can be shortened while maintaining the dispersibility of the cellulose nanocrystals and the expressed birefringence, or achieving high gas barrier properties. In the present invention, the mixed solvent of water and alcohol serving as the dispersion medium is preferably a mixed solvent containing 10 to 50 parts by mass of alcohol per 90 to 50 parts by mass of water. If the amount of alcohol is less than the above range, the effect of shortening the drying time by blending alcohol cannot be fully obtained, whereas if the amount of alcohol is more than the above range, the dispersibility of cellulose nanocrystals and the expression of birefringence may be impaired, and the gas barrier properties that are expressed may be reduced. As the alcohol contained in the mixed solvent, from the viewpoints of compatibility with water, viscosity, etc., it is preferable to use a lower alcohol having 3 or less carbon atoms. Specific examples include methanol, ethanol, isopropyl alcohol, N-propyl alcohol, N-butanol, isobutanol, tertiary butanol, butanol, etc., and in particular, methanol, ethanol, and isopropyl alcohol can be preferably used. These alcohols can be used alone or in combination of two or more.

[0020] [Preparation of cellulose nanocrystal dispersion] The cellulose nanocrystal dispersion used in the present invention is prepared by dispersing sulfate and / or sulfo group-containing cellulose nanocrystals obtained by treating a cellulose raw material with sulfuric acid. The dispersion can also be prepared by further hydrophilizing the cellulose nanocrystals to prepare anionic functional groups containing sulfate and / or sulfo groups, and then dispersing the cellulose nanocrystals. Before or after the sulfuric acid treatment of the cellulose raw material or before or after the hydrophilizing treatment of the cellulose nanocrystals, the cellulose nanocrystals can be subjected to defibration treatment or solvent replacement treatment, if necessary.

[0021] [Cellulose nanocrystals] The cellulose nanocrystals contained in the coating solution of the present invention are rod-shaped cellulose crystalline fibers obtained by acid hydrolysis of cellulose fibers such as pulp with sulfuric acid or hydrochloric acid. In the present invention, it is preferable to use cellulose nanocrystals obtained by sulfuric acid treatment, which have sulfate groups and / or sulfo groups that can contribute to the formation of a self-organized structure. The cellulose nanocrystal preferably contains sulfate groups and / or sulfo groups in an amount of 0.01 to 2.0 mmol / g, particularly 0.01 to 0.2 mmol / g. The cellulose nanocrystal preferably has an average fiber diameter of 50 nm or less, particularly 2 to 50 nm, an average fiber length of 100 to 500 nm, an aspect ratio of 5 to 50, and a crystallinity of 60% or more, particularly 70% or more. Anionic functional group-containing cellulose nanocrystals can be obtained by subjecting cellulose nanocrystals having sulfate groups and / or sulfo groups, or by further subjecting the cellulose nanocrystals to the hydrophilization treatment described below. As described above, cellulose nanofibers having a fiber width of 50 nm or less and an aspect ratio of 10 or more produced by conventional oxidation methods may be contained within a range that does not impair the excellent barrier properties and handleability of nanocellulose containing anionic functional groups (including sulfate groups and / or sulfo groups); specifically, they can be used in an amount less than 50% of the cellulose nanocrystals.

[0022] [Hydrophilic treatment] In the present invention, the cellulose nanocrystal having the above-mentioned sulfate group and / or sulfo group, or the cellulose nanocrystal is further subjected to a hydrophilization treatment to adjust the amount of sulfate group and / or sulfo group, or to introduce an anionic functional group such as a carboxyl group or a phosphate group into the hydroxyl group at the 6-position of cellulose, thereby preparing a cellulose nanocrystal having a total amount of anionic functional groups such as sulfate group and / or sulfo group, carboxyl group, phosphate group, etc., of more than 0.01 mmol / g and 4.0 mmol / g or less, particularly in the range of 0.2 to 1.5 mmol / g. The sulfate group and the phosphate group are concepts that also include sulfate ester group and phosphate ester group, respectively. The hydrophilization treatment is performed by a never-dry treatment, or a combination of the never-dry treatment and any of a water-soluble carbodiimide, sulfuric acid, sulfur trioxide-pyridine complex, phosphoric acid-urea, TEMPO catalyst, or oxidizing agent. The treatment using any of carbodiimide, sulfuric acid, or sulfur trioxide-pyridine complex adjusts the amount of sulfate groups and / or sulfo groups in the cellulose nanocrystals, and further shortens the cellulose nanocrystals. The treatment using any of phosphoric acid-urea, TEMPO catalyst, or oxidizing agent introduces anionic functional groups such as phosphoric acid groups or carboxyl groups, and adjusts the total amount of anionic functional groups in the cellulose nanocrystals to the above range. As for the hydrophilization treatment, any one of the treatments may be carried out so long as the total amount of anionic functional groups falls within the above-mentioned range, but the same treatment may be carried out multiple times, or may be carried out multiple times in combination with other treatments.

[0023] <Hydrophilic treatment using Never Dry treatment> Cellulose nanocrystals are solidified into powders or the like by drying treatments such as spray drying, heating, and reduced pressure, but during solidification by drying treatment, some of the anionic functional groups contained in the cellulose nanocrystals are eliminated, resulting in a decrease in hydrophilicity. In other words, a never-dry treatment that does not solidify cellulose nanocrystals into powders or the like that contains anionic functional groups is an example of a hydrophilization treatment. Examples of anionic functional groups include sulfate groups and / or sulfo groups, phosphate groups, and carboxyl groups.

[0024] <Hydrophilic treatment using carbodiimide> In the treatment using carbodiimide, cellulose nanocrystals and carbodiimide are stirred in a solvent such as dimethylformamide, sulfuric acid is added thereto, and the mixture is reacted for 5 to 300 minutes at a temperature of 0 to 80° C. to form a sulfate ester. The carbodiimide and sulfuric acid are preferably used in amounts of 5 to 30 mmol and 5 to 30 mmol per gram (solid content) of cellulose nanocrystals. Next, an alkaline compound such as sodium hydroxide is added to convert the sulfate and / or sulfo groups introduced into the cellulose nanocrystals from H type to Na type, which is preferable in terms of improving the yield. Then, impurities are removed by filtration using a dialysis membrane or the like to prepare sulfate and / or sulfo modified cellulose nanocrystals. Examples of carbodiimides include 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide, which is a water-soluble compound having a carbodiimide group (-N=C=N-) in the molecule. Dicyclohexylcarbodiimide, which is soluble in organic solvents, can also be used.

[0025] <Hydrophilic treatment using sulfuric acid> The cellulose nanocrystals used in the present invention are obtained by hydrolyzing cellulose fibers with sulfuric acid, but these cellulose nanocrystals can also be further hydrophilized using sulfuric acid. Sulfuric acid is preferably used at 40 to 60% by mass per 1 g (solid content) of cellulose nanocrystals. The reaction is carried out at a temperature of 40 to 60°C for 5 to 300 minutes, and then the mixture is subjected to a filtration process using a dialysis membrane or the like to remove impurities, thereby preparing sulfate and / or sulfo group-modified cellulose nanocrystals.

[0026] <Hydrophilic treatment using sulfur trioxide-pyridine complex> In the treatment using a sulfur trioxide-pyridine complex, cellulose nanocrystals are reacted with the sulfur trioxide-pyridine complex in dimethyl sulfoxide at a temperature of 0 to 60°C for 5 to 240 minutes to introduce a sulfate group and / or a sulfo group into the hydroxyl group at the 6-position of the cellulose glycol unit. The sulfur trioxide-pyridine complex is preferably mixed in an amount of 0.5 to 4 g by mass per 1 g (solid content) of cellulose nanocrystal. After the reaction, it is preferable to add an alkaline compound such as sodium hydroxide to convert the sulfate and / or sulfo groups introduced into the cellulose nanocrystals from H type to Na type in order to improve the yield. Then, dimethylformamide or isopropyl alcohol is added, and the mixture is washed by centrifugation or the like, after which impurities are removed by filtration using a dialysis membrane or the like, and the resulting concentrated liquid is dispersed in water to prepare sulfate and / or sulfo group-modified cellulose nanocrystals.

[0027] <Hydrophilic treatment using phosphoric acid-urea> The hydrophilization treatment using phosphoric acid-urea can be carried out in the same manner as the conventionally known treatment of introducing a phosphate group using phosphoric acid-urea. Specifically, in the presence of a urea-containing compound, cellulose nanocrystals are reacted with a phosphate group-containing compound at a temperature of 135 to 180°C for 5 to 120 minutes to introduce a phosphate group into the hydroxyl group of the cellulose glucose unit. Examples of the phosphate group-containing compound include phosphoric acid, lithium salts of phosphoric acid, sodium salts of phosphoric acid, potassium salts of phosphoric acid, and ammonium salts of phosphoric acid. Among them, sodium dihydrogen phosphate, ammonium dihydrogen phosphate, phosphoric acid, and the like can be preferably used alone or in combination. The phosphate group-containing compound is preferably added in an amount of 10 to 100 mmol per 10 g (solid content) of cellulose nanocrystals. Examples of the urea-containing compound include urea, thiourea, biuret, phenylurea, benzylurea, and dimethylurea. Among them, urea is preferably used. The urea-containing compound is preferably used in an amount of 150 to 200 mmol per 10 g (solid content) of cellulose nanocrystals.

[0028] <Hydrophilic treatment using TEMPO catalyst> The hydrophilic treatment using TEMPO catalyst (2,2,6,6 - tetramethylpiperidine - 1 - oxyl) can be carried out in the same manner as the conventionally known oxidation method using TEMPO catalyst. Specifically, cellulose nanocrystal having a sulfate group is subjected to a hydrophilic reaction that oxidizes the hydroxyl group at the 6 - position of the cellulose glucose unit to a carboxyl group under the conditions of an aqueous system, normal temperature, and normal pressure via TEMPO catalyst (2,2,6,6 - tetramethylpiperidine 1 - oxyl). As the TEMPO catalyst, in addition to the above - mentioned 2,2,6,6 - tetramethylpiperidine 1 - oxyl, derivatives of TEMPO such as 4 - acetamido - TEMPO, 4 - carboxy - TEMPO, and 4 - phosphonoxy - TEMPO can also be used. The usage amount of the TEMPO catalyst is 0.01 - 100 mmol, preferably 0.01 - 5 mmol, per 1 g of cellulose nanocrystal (solid content).

[0029] Also, during the hydrophilic oxidation treatment, it is preferable to use a co - oxidizing agent such as an oxidizing agent, bromide, or iodide alone or together with the TEMPO catalyst. Examples of the oxidizing agent include known oxidizing agents such as halogen, hypohalous acid, halous acid, perhalic acid or their salts, halogen oxides, and peroxides. In particular, sodium hypochlorite and sodium hypobromite can be preferably used. The oxidizing agent is in an amount of 0.5 - 500 mmol, preferably 5 - 50 mmol, per 1 g of cellulose nanocrystal (solid content). After adding the oxidizing agent and allowing a certain time to pass, post - oxidation treatment can also be carried out by adding the oxidizing agent again. Also, as the co - oxidizing agent, alkali metal bromides such as sodium bromide and alkali metal iodides such as sodium iodide can be preferably used. The co - oxidizing agent is in an amount of 0.1 - 100 mmol, preferably 0.5 - 5 mmol, per 1 g of cellulose nanocrystal (solid content). Also, the reaction solution preferably uses water or an alcohol solvent as the reaction medium.

[0030] The reaction temperature for the hydrophilization treatment is in the range of 1 to 50° C., particularly 10 to 50° C., and may be room temperature. The reaction time is preferably 1 to 360 minutes, particularly 60 to 240 minutes. As the reaction proceeds, carboxyl groups are produced in the cellulose, causing a decrease in the pH of the slurry. However, in order to ensure efficient oxidation reaction, it is desirable to maintain the pH in the range of 9 to 12 using a pH adjuster such as sodium hydroxide. After the oxidation treatment, the acid and catalyst used in the hydrophilization treatment are removed by washing with water, or by centrifugal separation or filtration and washing while adding water.

[0031] [Fiber defibration processing] In the present invention, since cellulose nanocrystals having short fiber length are used as the raw material, it is possible to carry out a defibration treatment after the hydrophilization treatment, although this is not necessarily required. The defibration treatment can be carried out by a conventionally known method. Specifically, the fiber can be pulverized using an ultra-high pressure homogenizer, an ultrasonic homogenizer, a grinder, a high-speed blender, a bead mill, a ball mill, a jet mill, a disintegrator, a beater, a twin-screw extruder, or the like. The defibration treatment can be performed by either a dry method or a wet method depending on the state of the cellulose nanocrystals after the hydrophilization treatment. Since the cellulose nanocrystals are preferably used in the form of a dispersion liquid, it is preferable to defibrate them using a water and alcohol mixed solvent as a dispersion medium with an ultra-high pressure homogenizer or the like.

[0032] [Distributed processing] The anionic functional group-containing cellulose nanocrystals are then subjected to a dispersion treatment to prepare a dispersion liquid. It is preferable to carry out the dispersion treatment using a mixed solvent of water and alcohol as the dispersion medium, but it is also possible to replace a part of the water in a previously prepared aqueous dispersion with alcohol by a solvent replacement step described below. For the dispersion treatment, a dispersing machine such as an ultrasonic dispersing machine, a homogenizer, or a mixer can be suitably used, and a stirring method using a stirring rod, stirring stone, or the like may also be used.

[0033] [Solvent replacement treatment] As described above, when a cellulose nanocrystal-containing aqueous dispersion is prepared in advance, a part of the water in the cellulose nanocrystal aqueous dispersion can be substituted with the above-mentioned alcohol as a solvent. The solvent replacement can be carried out by mixing the cellulose nanocrystal aqueous dispersion with alcohol while or after removing water from the aqueous dispersion using a dehydration method such as a centrifuge or filtration using a filter. After the solvent replacement treatment, the cellulose nanocrystals are dispersed in a mixed solvent of water and alcohol using the same method as the dispersion treatment described above to prepare a cellulose nanocrystal dispersion free of precipitation.

[0034] (Preparation of Coating Solution) The coating liquid of the present invention is obtained by further containing additives in addition to the above-mentioned anionic functional group-containing cellulose nanocrystal dispersion liquid. As mentioned above, examples of such additives include layered inorganic compounds, hydroxyl group-containing polymers, reactive crosslinking agents, acid catalysts, pH adjusters, etc. The coating solution of the present invention preferably contains anionic functional group-containing cellulose nanocrystals in an amount of 0.01 to 10 mass %, particularly 0.5 to 3.0 mass %, based on the solids content. If the amount is less than the above range, the gas barrier properties will be inferior compared to when the amount is within the above range, while if the amount is more than the above range, the coatability and film-forming properties will be inferior compared to when the amount is within the above range. Furthermore, the layered inorganic compound, hydroxyl group-containing polymer, and reactive crosslinking agent can be blended into the coating solution based on the content of cellulose nanocrystals (solids), and it is preferable to contain 1 to 50 parts by mass, particularly 20 to 40 parts by mass, of the layered inorganic compound, 1 to 50 parts by mass, particularly 20 to 40 parts by mass, of the hydroxyl group-containing polymer, and 1 to 50 parts by mass, particularly 5 to 20 parts by mass, of the reactive crosslinking agent, per 100 parts by mass of cellulose nanocrystals.As a result, a dense crosslinked structure is formed by the cellulose nanocrystals and the reactive crosslinking agent, as well as a flexible crosslinked structure by the hydroxyl group-containing polymer, and further, the uniformly dispersed layered inorganic compound provides a bypass effect for permeating gas, making it possible to exhibit excellent gas barrier properties even under high humidity conditions.

[0035] The pH of the coating liquid is preferably adjusted to 6 to 10, particularly 6.5 to 9.0, so that the layered inorganic compound is uniformly dispersed without aggregation, which contributes to the improvement of gas barrier properties due to the above-mentioned bypass effect. In the present invention, since it is preferable to use a polyvalent carboxylic acid having excellent crosslinking efficiency as the reactive crosslinking agent, the dispersion liquid is in the acidic range. On the other hand, since the layered inorganic compound is easily aggregated in the acidic range, it is desirable to adjust the pH of the dispersion liquid to the above range using a pH adjuster.

[0036] [Layered inorganic compounds] As the layered inorganic compound, a natural or synthetic compound, a conventionally known compound that exhibits hydrophilicity or hydrophobicity and swells in a solvent to exhibit cleavage can be used, including, but not limited to, kaolinite, dickite, nacrite, halloysite, antigorite, chrysotile, pyrophyllite, montmorillonite, hectorite, mica, tetracylic mica, sodium taeniolite, muscovite, margarite, talc, vermiculite, phlogopite, xanthophyllite, chlorite, etc., with synthetic mica (hydrophilic and swellable) being preferred.

[0037] [Hydroxyl group-containing polymer] Examples of the hydroxyl group-containing polymer include polyvinyl alcohol, vinyl acetate alcohol copolymer, ethylene vinyl alcohol copolymer, polyacrylic acid, polymethacrylic acid, carboxymethyl cellulose, hydroxypropyl cellulose, methyl cellulose, starch, modified starch, etc., and polyvinyl alcohol is preferably used. The polyvinyl alcohol is preferably a partially saponified or fully saponified type having a degree of polymerization of 100 to 10,000.

[0038] [Reactive crosslinking agent] As the reactive crosslinking agent, a polycarboxylic acid having good reaction efficiency is used. Examples of the polycarboxylic acid include alkyl dicarboxylic acids such as citric acid, oxalic acid, and malonic acid, aromatic dicarboxylic acids such as terephthalic acid and maleic acid, and anhydrides thereof, and in particular, anhydrous citric acid can be preferably used. In the coating liquid of the present invention, since the cellulose nanocrystals contain anionic functional groups, they can be stably dispersed without aggregation even under acidic conditions, and therefore the above-mentioned polyvalent carboxylic acids can be suitably used. The reactive crosslinking agent is preferably used together with an acid catalyst. Examples of such an acid catalyst include sulfuric acid, acetic acid, and hydrochloric acid, and sulfuric acid is particularly preferred. The acid catalyst is preferably blended in the range of 0.5 to 10 parts by mass per 100 parts by mass (solid content) of cellulose nanocrystals.

[0039] [pH adjuster] Examples of the pH adjuster include conventionally known bases such as sodium nitrate, ammonium hydroxide, sodium hydroxide, and ammonia. In particular, ammonia, which volatilizes during drying, is preferably used.

[0040] [others] The coating liquid of the present invention may contain known additives such as fillers, colorants, ultraviolet absorbers, antistatic agents, water-resistant agents, metal salts, colloidal silica, alumina sol, and titanium oxide, if necessary.

[0041] [Additive mixing and dispersion processing] As mentioned above, cellulose nanofibers have long fiber length and high viscosity, but anionic functional group-containing cellulose nanofibers have even higher affinity for dispersion media such as water and alcohol, and coating solutions using the cellulose nanofibers have low solid concentrations and high viscosity. Due to the high viscosity, the dispersion force due to the dispersion treatment and the fluidity of the coating solution are unevenly distributed, making it difficult to mix additives and disperse the additives in terms of the method, amount, time, and distribution and uniformity of the additives. In contrast, the coating solution of the present invention uses anionic functional group-containing cellulose nanocrystals having a short fiber length, so that a coating solution with a high solid content concentration and low viscosity can be prepared, and the dispersion force and fluidity of the coating solution due to the dispersion treatment become uniform, and the dispersion method, amount, time, and distribution and uniformity of additives are excellent. Furthermore, the coating solution using the anionic functional group-containing cellulose nanocrystals has excellent coatability and film-forming properties, and the coating film shows high gas barrier properties.

[0042] (Molded body) The molded article of the present invention is a molded article in which a layer containing the cellulose nanocrystals and polyvalent cationic resin contained in the coating liquid of the present invention is formed on a substrate, and the cellulose nanocrystals are present in an amount of 1 m 2 When the oxygen permeability is 1.0 (cc / m2) at 23°C and 50% RH, 2 The molded article is capable of exhibiting excellent oxygen barrier properties, with a vapor barrier strength of less than 1000 psi (days atm), and when a layer containing cellulose nanocrystals and a polyvalent cation resin is formed on a substrate, the molded article can remarkably improve the adhesion between the layer and the substrate layer. Furthermore, in the molded body of the present invention, the presence of the polyvalent cationic resin improves the interfacial peel strength with the layer made of a hydrophobic resin, so that the interfacial peel strength between the substrate, particularly the substrate made of a thermoplastic resin, and the layer containing cellulose nanocrystals and polyvalent cationic resin is 2.3 (N / 15 mm) or more, effectively preventing the occurrence of interlayer delamination.

[0043] In the molded article of the present invention, a layer having a mixed state capable of exhibiting excellent gas barrier properties and adhesion to a substrate can be formed by forming a layer of the cellulose nanocrystal-containing coating liquid on a layer of a polyvalent cationic resin. In contrast, a coating liquid in which a polyvalent cationic resin and a cellulose nanocrystal are mixed will lose its self-organized structure due to aggregation, and the gas barrier properties of the coating layer will not be exhibited. Therefore, it is important to form a layer having a mixed state by forming a layer of a cellulose nanocrystal-containing coating liquid on a layer of a polyvalent cationic resin as described above. That is, it is difficult to quantitatively express the mixed state of a layer formed by the coating liquid and polyvalent cationic resin of the present invention, but it is formed only when the polyvalent cationic resin and the cellulose nanocrystal are mixed in a state in which the self-organized structure of the cellulose nanocrystals described above is maintained. The inside of the layer formed by the coating liquid and polyvalent cationic resin of the present invention has the characteristic that the cellulose nanocrystals and the polyvalent cationic resin are present from near the outermost surface to the substrate.

[0044] [Polycationic resin] The polyvalent cationic resin used in the molded article of the present invention is a resin containing a water-soluble or water-dispersible polyvalent cationic functional group. Examples of such polyvalent cationic resins include water-soluble amine polymers such as polyethyleneimine, polyallylamine, polyamine polyamide epichlorohydrin, polyamine epichlorohydrin, polyacrylamide, poly(diallyldimethylammonium salt), dicyandiamide formalin, poly(meth)acrylate, cationic starch, cationic gum, gelatin, chitin, chitosan, etc., and among them, water-soluble amine polymers, particularly polyethyleneimine, can be preferably used.

[0045] [Base material] Examples of the substrate include films, sheets, and molded articles in the form of bottles, cups, trays, pouches, packaging containers, etc., produced by means of extrusion molding, injection molding, blow molding, stretch blow molding, lamination molding, press molding, or the like using thermoplastic resins. The thickness of the substrate cannot be generally defined depending on the shape and application of the laminate, but in the case of a film, it is preferably in the range of 5 to 50 μm.

[0046] Examples of thermoplastic resins include olefin copolymers such as low-, medium-, or high-density polyethylene, linear low-density polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-butene copolymer, ionomer, ethylene-vinyl acetate copolymer, and ethylene-vinyl alcohol copolymer; aromatic polyesters such as polyethylene terephthalate, polybutylene terephthalate, polyethylene terephthalate / isophthalate, and polyethylene naphthalate; aliphatic polyesters such as polylactic acid, polycaprolactone, and polybutylene succinate; and polyarylsulfones such as nylon 6, nylon 6,6, nylon 6,10, and metaxylylene adipamide. Examples of suitable polymers include styrene-based copolymers such as polystyrene, styrene-butadiene block copolymer, styrene-acrylonitrile copolymer, and styrene-butadiene-acrylonitrile copolymer (ABS resin); vinyl chloride-based copolymers such as polyvinyl chloride and vinyl chloride-vinyl acetate copolymer; acrylic copolymers such as polymethyl methacrylate and methyl methacrylate-ethyl acrylate copolymer; polycarbonate, cellulose-based resins; and regenerated celluloses such as acetyl cellulose, cellulose acetyl propionate, cellulose acetate butyrate, and cellophane, with polyethylene terephthalate being preferred. The thermoplastic resin may contain one or more additives such as pigments, antioxidants, antistatic agents, ultraviolet absorbers, lubricants, etc., as desired.

[0047] In the laminate containing the molded article of the present invention, other layers may be formed as necessary in addition to the layer consisting of the substrate and the molded article. Although a layer made of a mixture of cellulose nanocrystals and a polyvalent cationic resin suppresses deterioration of gas barrier properties under high humidity conditions, it is desirable to further form a layer made of a conventional moisture-resistant resin such as an olefin resin, a polyester resin, or a cured reaction product of an epoxy resin and a polyamine resin.

[0048] (Method of Manufacturing Molded Product) The molded article of the present invention can be produced by a process of coating and drying a polyvalent cationic resin-containing solution on a substrate to form a layer made of a polyvalent cationic resin, and then coating and drying the coating liquid of the present invention on the layer made of a polyvalent cationic resin, thereby producing a molded article having a layer made of a mixture in which a polyvalent cationic resin and cellulose nanocrystals are mixed in a specific mixed state.

[0049] [Coating and drying of polycation resin-containing solution] The polycation resin-containing solution preferably contains the polycation resin in an amount of 0.01 to 30 mass %, particularly 0.1 to 10 mass %, based on the solid content. If the amount of the polycation resin is less than the above range, the gas barrier property and the interfacial peel strength cannot be improved as compared with the case where the amount is within the above range, while if the amount of the polycation resin is more than the above range, the gas barrier property and the interfacial peel strength cannot be further improved, resulting in poor economic efficiency and possibly poor coatability and film-forming property. The solvent used for the polyvalent cation resin-containing solution may be water, alcohols such as methanol, ethanol, and isopropanol, ketones such as 2-butanone and acetone, aromatic solvents such as toluene, and mixed solvents of these with water. Furthermore, the polyvalent cation resin-containing solution may contain known additives, such as fillers, colorants, ultraviolet absorbers, antistatic agents, water-resistant agents, clay minerals, crosslinking agents, metal salts, colloidal silica, alumina sol, and titanium oxide, as necessary.

[0050] The amount of the polyvalent cationic resin-containing solution to be applied is determined based on the amount of cellulose nanocrystals (solid content) in the layer formed from the coating solution of the present invention, depending on the concentration of the polyvalent cationic resin-containing solution. 2 When the polyvalent cation resin is contained in an amount of 1.0 g per m 2It is preferable to coat the polycation resin in an amount of 0.01 to 2.0 g per coating. If the amount of the polycation resin is less than the above range, the interfacial peel strength with respect to a hydrophobic substrate such as a polyester resin cannot be improved as compared with the case where the amount is within the above range, while if the amount of the polycation resin is more than the above range, the gas barrier property of the molded article may not be improved as compared with the case where the amount is within the above range. The coating method is not limited to the above, but can be, for example, spray coating, immersion, or coating with a bar coater, roll coater, gravure coater, etc. The coating is preferably dried at a temperature of 5 to 200° C. for 0.1 seconds to 24 hours. The drying process can be performed by hot air drying, oven drying, infrared heating, high frequency heating, etc., but natural drying is also possible.

[0051] [Coating and drying of coating solution containing cellulose nanocrystals] The coating solution of the present invention described above has a cellulose nanocrystal (solid content) of 1 m 2 It is preferable to coat the coating amount so that the coating amount is 0.1 to 3.0 g per coating amount. The coating and drying methods of the coating solution can be performed in the same manner as the coating and drying methods of the polyvalent cation-containing solution, and therefore drying may be performed at a temperature of 5°C to 200°C for 1 second to 24 hours. In particular, in order to prevent deterioration of the substrate or coating layer due to high temperatures and to shorten the drying time, the coating solution of the present invention can form a coating film without causing coating defects even when dried under conditions in which the time required for solidification is 60 seconds or less when dried at 150°C when the solid content concentration is 0.5 to 3 mass%. Examples of coating defects include streaks, unevenness, coating voids, gels, bumps, orange peel, and voids in the coating film on the coating surface.

[0052] As described above, the coating solution using the anionic functional group-containing cellulose nanofiber has high viscosity, which causes coating defects during coating processing. When alcohol is added to the anionic functional group-containing cellulose nanofiber, it may gel and further increase the viscosity. In addition, since the viscosity is high and the solidification concentration cannot be increased, the amount of volatile solvent is large and the coating solution is in a gel state, so the drying process time until the coating solution using the anionic functional group-containing cellulose nanofiber is solidified is long. In contrast, the coating solution containing the anionic functional group-containing cellulose nanocrystals of the present invention has low viscosity as described above, and does not cause coating defects during coating processing. In addition, since the viscosity is low and the solid content concentration can be increased, the amount of volatile solvent can be reduced, and since the coating solution using the anionic functional group-containing cellulose nanocrystals is in liquid form, the drying process time until solidification is shortened. The coating solution of the present invention is suitable in that it does not cause coating defects on the coated surface when applied to a PET film using a bar coater (No. 30), and that when the coated surface of the coating solution having a solids concentration of cellulose nanocrystals of 0.5 to 3 mass % is dried at 150°C in a hot air oven dryer, the time until solidification is 60 seconds or less. EXAMPLES

[0053] Examples of the present invention will be described below. Note that the following examples are merely examples of the present invention, and the present invention is not limited to these examples. The measurement methods for each item are as follows.

[0054] <Amount of anionic functional groups> The dispersion of CNC containing anionic functional groups was weighed and ion-exchanged water was added to prepare a total volume of 100 ml. 0.1 g of cation exchange resin was added to this dispersion of CNC containing anionic functional groups and stirred. Filtration was then performed to separate the cation exchange resin and the dispersion of CNC containing anionic functional groups. A 0.05 M sodium hydroxide solution was dropped onto the dispersion after cation exchange using an automatic potentiometric titrator (Kyoto Electronics Co., Ltd.), and the change in the electrical conductivity of the dispersion of CNC containing anionic functional groups was measured. The titration amount of sodium hydroxide consumed for neutralization of the anionic functional groups was determined from the obtained conductivity curve, and the amount of anionic functional groups (mmol / g) was calculated using the following formula (1). Amount of anionic functional group (mmol / g) = Titration amount of sodium hydroxide consumed for neutralizing anionic functional group (ml) × Concentration of sodium hydroxide (mmol / ml) ÷ Solid mass of CNC containing anionic functional group (g) (1)

[0055] <Birefringence> The coating liquid was observed by polarized light using a polarizing plate in a polarizing inspection device by a sensitive color method to confirm the presence or absence of birefringence due to the refraction image of the nematic liquid crystal and / or the chiral nematic liquid crystal. In the table, the case where birefringence was confirmed is indicated as "○".

[0056] <Viscosity measurement> The viscosity (mPa·S) of the coating liquid was measured using a rotational viscometer (VISCO, Atago) at a spindle speed of 60 rpm for 60 seconds.

[0057] <Evaluation of coated surface and drying time> The coating solution was applied to a corona-treated PET film using a bar coater (#30), and the coated surface was evaluated. The coated surface was also heated and dried at 150°C in an oven, and the time it took for the coating to solidify was measured.

[0058] <Oxygen permeability> Using an oxygen transmission rate measuring device (OX-TRAN2 / 22, Mocon), the oxygen transmission rate (cc / m 2·day·atm) was measured.

[0059] <Example 1> <Preparation of cellulose nanocrystal dispersion in water> Anionic functional group-containing cellulose nanocrystals were prepared by decomposing pulp with 64% by weight sulfuric acid, and ion-exchanged water was added to the cellulose nanocrystals and dispersed in a mixer to obtain a dispersion of anionic functional group-containing cellulose nanocrystals dispersed in water.

[0060] <Preparation of coating solution containing cellulose nanocrystals dispersed in water / alcohol> Polyvinyl alcohol (fully saponified type), synthetic mica (hydrophilic swelling mica), anhydrous citric acid, and sulfuric acid were added to the cellulose nanocrystal-containing dispersion liquid and stirred, and NH3 was further added and stirred until the pH reached 7, thereby preparing a cellulose nanocrystal dispersion liquid containing anionic functional groups and additives. Furthermore, a predetermined amount of 2-propanol was added to the anionic functional group-containing cellulose nanocrystal dispersion containing the additives and stirred to prepare a coating liquid containing cellulose nanocrystals dispersed in water / alcohol, in which the solid amount of the anionic functional group-containing cellulose nanocrystals was 0.5 parts by mass per 100 parts by mass of the total of the mass of the solvent in the coating liquid and the mass of the anionic functional group-containing cellulose nanocrystals, the amounts of polyvinyl alcohol, synthetic mica, anhydrous citric acid, and sulfuric acid were 30 parts by mass, 30 parts by mass, 10 parts by mass, and 2 parts by mass, respectively, per 100 parts by mass of the anionic functional group-containing cellulose nanocrystals, and the water / alcohol mixing ratio was 10 parts by mass of 2-propanol per 90 parts by mass of water.

[0061] <Molded product having a layer containing a polyvalent cationic resin and a cellulose nanocrystal> A corona-treated biaxially stretched PET film (Lumirror P60, 12 μm, Toray Industries, Inc.) was used as the substrate, and polyethyleneimine (PEI) was applied as a polyvalent cationic resin to this substrate using a bar coater at a solid weight of 0.06 g / m 2The coating was then applied so that the coating liquid would become 100% by weight, and the coating liquid was dried at 50°C for 10 minutes in a hot air dryer (MSO-TP, manufactured by ADVANTEC) to solidify the coating liquid. The cellulose nanocrystal-containing coating liquid was applied onto the solidified polycationic resin (PEI) using a bar coater, and the coating liquid was air-dried at room temperature overnight, followed by heat treatment at 150°C to prepare a molded product having a layer containing the polycationic resin (PEI) and the cellulose nanocrystals. The solid amount of the anionic functional group-containing cellulose nanocrystals in the molded product was 1.0 g / m 2 It was.

[0062] <Example 2> A cellulose nanocrystal-containing coating liquid and a molded product were prepared in the same manner as in Example 1, except that the solid amount of the anionic functional group-containing cellulose nanocrystal was changed to 1 part by mass.

[0063] <Example 3> A cellulose nanocrystal-containing coating liquid and a molded product were prepared in the same manner as in Example 1, except that the solid amount of the anionic functional group-containing cellulose nanocrystal was changed to 2 parts by mass.

[0064] <Example 4> A cellulose nanocrystal-containing coating liquid and a molded product were prepared in the same manner as in Example 1, except that the solid amount of the anionic functional group-containing cellulose nanocrystal was changed to 3 parts by mass.

[0065] <Example 5> A cellulose nanocrystal-containing coating liquid and a molded product were prepared in the same manner as in Example 2, except that the water / alcohol mixing ratio was changed to 80 parts by mass of water and 20 parts by mass of 2-propanol.

[0066] <Example 6> A cellulose nanocrystal-containing coating liquid and a molded product were prepared in the same manner as in Example 2, except that the water / alcohol mixing ratio was changed to 70 parts by mass of water and 30 parts by mass of 2-propanol.

[0067] <Example 7> A cellulose nanocrystal-containing coating liquid and a molded product were prepared in the same manner as in Example 2, except that the water / alcohol mixing ratio was changed to 60 parts by mass of water and 40 parts by mass of 2-propanol.

[0068] <Example 8> A cellulose nanocrystal-containing coating liquid and a molded product were prepared in the same manner as in Example 2, except that the water / alcohol mixing ratio was changed to 50 parts by mass of water and 50 parts by mass of 2-propanol.

[0069] <Example 9> A cellulose nanocrystal-containing coating liquid and a molded product were prepared in the same manner as in Example 3, except that the water / alcohol mixing ratio was changed to 80 parts by mass of water and 20 parts by mass of 2-propanol.

[0070] <Example 10> A cellulose nanocrystal-containing coating solution and a molded product were prepared in the same manner as in Example 3, except that the water / alcohol mixing ratio was changed to 70 parts by mass of water and 30 parts by mass of 2-propanol.

[0071] <Comparative Example 1> To an aqueous dispersion of 10 g (solids) of kraft pulp, 0.8 mmol of TEMPO catalyst (Sigma Aldrich) and 12.1 mmol of sodium bromide were added, and the mixture was made up to 1 L with ion-exchanged water and stirred until uniformly dispersed. The reaction system was added with 15 mmol of sodium hypochlorite per 1 g of cellulose to initiate the oxidation reaction. During the reaction, the pH of the system was maintained at 10.0 to 10.5 with 0.5N aqueous sodium hydroxide solution, and the oxidation reaction was carried out at 30°C for 4 hours. The oxidized cellulose was thoroughly washed until it became neutral using a high-speed refrigerated centrifuge (16,500 rpm, 10 min) while adding ion-exchanged water. Water was added to the washed oxidized cellulose, and the mixture was defibrated using a mixer (7011JBB, Osaka Chemical Co., Ltd.) to prepare a dispersion of anionic functional group-containing cellulose nanofibers containing carboxyl groups. A specified amount of 2-propanol was then added and stirred to prepare a coating liquid containing cellulose nanofibers dispersed in water / alcohol, in which the solid content of the anionic functional group-containing cellulose nanofibers was 1 part by mass and the water / alcohol mixing ratio was 90 parts by mass of water to 10 parts by mass of 2-propanol. Thereafter, the same procedure as in Example 2 was carried out, except that the cellulose nanocrystal-containing coating liquid was changed to the cellulose nanofiber-containing coating liquid, to prepare a molded product.

[0072] <Comparative Example 2> A cellulose nanofiber-containing coating liquid and a molded product were prepared in the same manner as in Comparative Example 1, except that 30 parts by mass of polyvinyl alcohol, 30 parts by mass of synthetic mica, 10 parts by mass of anhydrous citric acid, and 2 parts by mass of sulfuric acid were added per 100 parts by mass of cellulose nanofiber.

[0073] [Table 1]

[0074] [Table 2]

[0075] [Table 4]

[0076] [Table 4] [Industrial Applicability]

[0077] The coating liquid of the present invention can form a dense cross-linked structure in which anionic functional group-containing cellulose nanocrystals are uniformly dispersed, and has excellent gas barrier properties even under high humidity conditions, so it can be used as a coating liquid that can impart gas barrier performance.Moreover, despite its high solids concentration, it can be made into a coating liquid with low viscosity, has good dispersibility of additives, and is free of coating defects on the coated surface.Combined with the use of a mixed solvent of water and alcohol, it is possible to shorten the time until solidification, and is therefore excellent in productivity and economy. Furthermore, by forming a molded article having a layer consisting of a mixture of the cellulose nanocrystal-containing coating liquid of the present invention and a polyvalent cationic resin, it is possible to exhibit better gas barrier properties, and the interfacial peel strength with a hydrophobic substrate consisting of a thermoplastic resin or the like is also improved, making it suitable for use as a gas barrier laminate.

Claims

1. A coating liquid containing anionic functional group-containing cellulose nanocrystals and additives, the coating liquid containing at least a layered inorganic compound, a hydroxyl group-containing polymer, and a polycarboxylic acid as the additives, and using a mixed solvent of water and alcohol as a dispersion medium.

2. 2. The coating liquid according to claim 1, which contains a nematic liquid crystal and / or a chiral nematic liquid crystal.

3. 3. The coating solution according to claim 2, which exhibits birefringence.

4. The coating liquid according to any one of claims 1 to 3, wherein the anionic functional group-containing cellulose nanocrystal is contained in an amount of 0.5 mass% or more as a solid content.

5. 5. The coating liquid according to claim 1, wherein the mixed solvent contains 10 to 50 parts by mass of alcohol with respect to 90 to 50 parts by mass of water.

6. The coating liquid according to any one of claims 1 to 5, wherein the alcohol is at least one of ethanol, methanol, and isopropyl alcohol.

7. The coating solution according to claim 1, wherein the layered inorganic compound is mica, the hydroxyl group-containing polymer is polyvinyl alcohol, and the polycarboxylic acid is citric acid.

8. The coating liquid according to any one of claims 1 to 7, wherein the anionic functional group is a sulfo group and / or a sulfate group derived from decomposition of sulfuric acid.

9. The coating liquid according to any one of claims 1 to 8, wherein the viscosity of the anionic functional group-containing cellulose nanocrystal measured with a rotational viscometer (rotation speed: 60 rpm, rotation time: 60 seconds) when the solid content is 0.5 to 3 mass % is 1 to 10,000 mPa·s.

10. The coating solution according to any one of claims 1 to 9, wherein the coating surface of the coating solution applied to a substrate having a solid content of the anionic functional group-containing cellulose nanocrystal of 0.5 to 3 mass % is dried at 150°C in a time period of 60 seconds or less until solidification.

Citation Information

Patent Citations

  • Cellulose nanofiber

    JP2013256546A

  • Cosmetic

    JP2017048181A

  • Molding sheet, laminated sheet, and curable composition for molding

    JP2019081877A

  • Coating composition and coated film, and article

    JP2020033486A

  • Coating agent, barrier film, packaging film and method for producing coating agent

    JP2020037696A