Conductive paste, electronic components, and multilayer ceramic capacitors

A conductive paste with controlled components and dispersants stabilizes viscosity for thin electrode patterns, addressing the need for improved stability in multilayer ceramic capacitors.

JP7559489B2Active Publication Date: 2024-10-02SUMITOMO METAL MINING CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020171330
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-10-16
Filing Date
2020-10-09
Publication Date
2024-10-02
Estimated Expiration
2040-10-09

AI Technical Summary

Technical Problem

As electrode patterns become thinner, there is a need for further improvement in viscosity characteristics and dynamic viscosity stability of conductive pastes used in multilayer ceramic capacitors to maintain consistency during printing.

Method used

A conductive paste formulation containing specific ratios of conductive powder, ceramic powder, binder resin, and an amine-based dispersant, such as a secondary or tertiary amine, with controlled particle sizes and dispersant amounts, to stabilize viscosity over time.

Benefits of technology

The conductive paste exhibits minimal changes in viscosity and dynamic viscosity, ensuring stable printing and preventing issues like mesh marks and electrical short circuits in multilayer ceramic capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559489000006
    Figure 0007559489000006
  • Figure 0007559489000001
    Figure 0007559489000001
  • Figure 0007559489000002
    Figure 0007559489000002
Patent Text Reader

Abstract

To provide a conductive paste that resists change in consistency with time and resists change in kinetic viscosity with time.SOLUTION: A conductive paste contains conductive powder, ceramic powder, a dispersant, a binder resin and an organic solvent. The dispersant includes an amine dispersant that is a secondary amine or tertiary amine and has a dielectric constant of 10 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a conductive paste, an electronic component, and a multilayer ceramic capacitor. [Background technology]

[0002] As electronic devices such as mobile phones and digital devices become smaller and more powerful, there is a demand for smaller electronic components, including multilayer ceramic capacitors, with higher capacitance. Multilayer ceramic capacitors have a structure in which multiple dielectric layers and multiple internal electrode layers are alternately stacked, and by thinning these dielectric layers and internal electrode layers, it is possible to achieve smaller size and higher capacitance.

[0003] For example, a multilayer ceramic capacitor is manufactured as follows. First, a conductive paste for internal electrodes is printed in a predetermined electrode pattern on the surface of a dielectric green sheet containing a dielectric powder such as barium titanate (BaTiO3) and a binder resin, and then dried to form a dry film. Next, the dry film and the green sheet are alternately stacked to obtain a laminate. Next, this laminate is heated and pressed to be integrated to form a pressed body. This pressed body is cut, and after a binder removal process is performed in an oxidizing atmosphere or an inert atmosphere, it is fired to obtain a fired chip. Next, a paste for external electrodes is applied to both ends of the fired chip, and after firing, nickel plating or the like is performed on the surface of the external electrodes to obtain a multilayer ceramic capacitor.

[0004] Generally, the conductive paste used to form the internal electrode layer contains a conductive powder, a ceramic powder, a binder resin, and an organic solvent. The conductive paste may also contain a dispersant to improve the dispersibility of the conductive powder and the like. In recent years, the thickness of the internal electrode layer has become thinner, and the conductive powder also tends to become smaller in particle size. When the particle size of the conductive powder is small, the specific surface area of ​​the particle surface becomes large, and the surface activity of the conductive powder (metal powder) becomes high, which may result in a decrease in dispersibility and a decrease in viscosity characteristics.

[0005] Therefore, attempts have been made to improve the viscosity characteristics of conductive pastes over time. For example, Patent Document 1 describes a conductive paste that contains at least a metal component, an oxide, a dispersant, and a binder resin, in which the metal component is Ni powder having a specific surface composition, the dispersant has an acid site number of 500 to 2000 μmol / g, and the binder resin has an acid site number of 15 to 100 μmol / g. According to Patent Document 1, this conductive paste is said to have good dispersibility and viscosity stability.

[0006] Also, Patent Document 2 describes a conductive paste for internal electrodes that is made of conductive powder, resin, organic solvent, common material of ceramic powder mainly composed of TiBaO3, and coagulation inhibitor, in which the content of the coagulation inhibitor is 0.1% by weight or more and 5% by weight or less, and the coagulation inhibitor is a tertiary amine or secondary amine represented by a specific structural formula. According to Patent Document 2, this conductive paste for internal electrodes is said to suppress coagulation of the common material components, to have excellent long-term storage properties, and to enable the thinning of multilayer ceramic capacitors.

[0007] On the other hand, when the internal electrode layer is thinned, it is required that the density of the dry film obtained by printing the conductive paste for the internal electrode on the surface of the dielectric green sheet and drying it is high. For example, Patent Document 3 proposes a metal ultrafine powder slurry containing an organic solvent, a surfactant, and ultrafine metal particles, the surfactant being oleoyl sarcosine, the metal ultrafine powder slurry containing 70 mass% or more and 95 mass% or less of the metal ultrafine powder, and the surfactant containing more than 0.05 mass parts and less than 2.0 mass parts per 100 mass parts of the metal ultrafine powder. According to Patent Document 3, it is said that by preventing the aggregation of ultrafine particles, a metal ultrafine powder slurry without aggregated particles is obtained, which has excellent dispersibility and dry film density. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2015-216244 A [Patent Document 2] JP 2013-149457 A [Patent Document 3] JP 2006-063441 A Summary of the Invention [Problem to be solved by the invention]

[0009] However, as electrode patterns have become thinner in recent years, further improvement in viscosity characteristics over time is required. In particular, when forming a thinner electrode pattern, the dynamic viscosity stability of the conductive paste during printing is also required.

[0010] In view of the above circumstances, an object of the present invention is to provide a conductive paste that has little change in viscosity over time and little change in dynamic viscosity over time. [Means for solving the problem]

[0011] In a first aspect of the present invention, there is provided a conductive paste comprising a conductive powder, a ceramic powder, a dispersant, a binder resin and an organic solvent, wherein the dispersant is a secondary amine or a tertiary amine and comprises an amine-based dispersant having a dielectric constant of 10 or less.

[0012] The amine dispersant is preferably contained in an amount of 0.01 to 2 parts by mass relative to 100 parts by mass of the conductive powder, and the conductive powder is preferably contained in an amount of 40 to 60% by mass relative to the entire conductive paste.The dispersant preferably contains an amino acid dispersant represented by the following general formula (1) in an amount of 0.01 to 2 parts by mass relative to 100 parts by mass of the conductive powder.

[0013] [ka]

[0014] (In the formula (1), R1 represents a chain hydrocarbon group having 10 to 20 carbon atoms.)

[0015] The amine-based dispersant is preferably contained in an amount at least one time the amino acid-based dispersant in terms of mass ratio. The dispersant is preferably contained in an amount of 0.01% by mass or more and 3% by mass or less with respect to the entire conductive paste. The conductive powder preferably contains at least one metal powder selected from Ni, Pd, Pt, Au, Ag, Cu, and alloys thereof. The conductive powder preferably has an average particle size of 0.05 μm or more and 1.0 μm or less. The ceramic powder preferably contains a perovskite-type oxide. The conductive paste is preferably for use in internal electrodes of a multilayer ceramic component.

[0016] In a second aspect of the present invention, there is provided an electronic component formed using the above-mentioned conductive paste.

[0017] In a third aspect of the present invention, there is provided a multilayer ceramic capacitor having at least a laminate in which dielectric layers and internal electrodes are laminated, the internal electrodes being formed using the above-mentioned conductive paste. Effect of the Invention

[0018] According to the present invention, it is possible to provide a conductive paste that has little change in viscosity over time and little change in dynamic viscosity over time. [Brief description of the drawings]

[0019] [Figure 1] FIG. 1 is a perspective view and a cross-sectional view showing a multilayer ceramic capacitor according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The conductive paste of the present embodiment is a conductive paste including a conductive powder, a ceramic powder, a dispersant, a binder resin, and an organic solvent, and the dispersant includes an amine-based dispersant which is a secondary amine or a tertiary amine and has a dielectric constant of 10 or less. Hereinafter, the conductive powder, ceramic powder, dispersant, binder resin, and organic solvent of the present embodiment are included. Each component will be described in detail below.

[0021] (conductive powder) The conductive powder is not particularly limited, and a metal powder can be used, for example, one or more metal powders selected from Ni, Pd, Pt, Au, Ag, Cu, and alloys thereof. Among these, from the viewpoints of conductivity, corrosion resistance, and cost, Ni or its alloy powder is preferable. As the Ni alloy, for example, an alloy of Ni and at least one element selected from the group consisting of Mn, Cr, Co, Al, Fe, Cu, Zn, Ag, Au, Pt, and Pd (Ni alloy) can be used. The Ni content in the Ni alloy is, for example, 50 mass% or more, preferably 80 mass% or more. In addition, the Ni powder may contain about several hundred ppm of S in order to suppress rapid gas generation due to partial thermal decomposition of the binder resin during the binder removal process.

[0022] The average particle size of the conductive powder is preferably 0.05 μm or more and 1.0 μm or less, more preferably 0.1 μm or more and 0.5 μm or less. When the average particle size of the conductive powder is within the above range, it can be suitably used as a conductive paste for an internal electrode of a thin-film multilayer ceramic capacitor, and for example, the smoothness and density of the dry film are improved. The average particle size is a value determined by observation with a scanning electron microscope (SEM), and is the average value obtained by measuring the particle size of each of a plurality of particles from an image observed with an SEM at a magnification of 10,000 times.

[0023] The content of the conductive powder is preferably 30% by mass or more and less than 70% by mass, more preferably 40% by mass or more and 60% by mass or less, based on the total amount of the conductive paste. When the content of the conductive powder is within the above range, the conductive paste has excellent conductivity and dispersibility.

[0024] (ceramic powder) The ceramic powder is not particularly limited, and for example, in the case of a conductive paste for an internal electrode of a multilayer ceramic capacitor, a known ceramic powder is appropriately selected depending on the type of multilayer ceramic capacitor to be applied. Examples of the ceramic powder include perovskite oxides containing Ba and Ti, and preferably barium titanate (BaTiO3).

[0025] The ceramic powder may be a ceramic powder containing barium titanate as a main component and oxides as sub-components. Examples of oxides include oxides of Mn, Cr, Si, Ca, Ba, Mg, V, W, Ta, Nb, and one or more rare earth elements. The ceramic powder may be a perovskite-type oxide ferroelectric ceramic powder in which the Ba and Ti atoms of barium titanate (BaTiO3) are replaced with other atoms, such as Sn, Pb, and Zr.

[0026] In the conductive paste for the internal electrodes, a powder having the same composition as the dielectric ceramic powder constituting the green sheet of the multilayer ceramic capacitor may be used as the ceramic powder. This suppresses the occurrence of cracks due to a mismatch in shrinkage at the interface between the dielectric layer and the internal electrode layer during the sintering process. In addition to the above, examples of such ceramic powders include oxides such as ZnO, ferrite, PZT, BaO, Al2O3, Bi2O3, R (rare earth element)2O3, and TiO2. Note that one type of ceramic powder may be used, or two or more types may be used.

[0027] The average particle size of the ceramic powder is, for example, 0.01 μm to 0.5 μm, preferably 0.01 μm to 0.3 μm. When the average particle size of the ceramic powder is in the above range, it is possible to form a sufficiently fine, thin, and uniform internal electrode when used as a conductive paste for an internal electrode. The average particle size is a value determined by observation with a scanning electron microscope (SEM), and is the average value obtained by measuring the particle size of each of a plurality of particles from an image observed with an SEM at a magnification of 50,000 times.

[0028] The content of the ceramic powder is preferably 1 part by mass or more and 30 parts by mass or less, and more preferably 3 parts by mass or more and 30 parts by mass or less, relative to 100 parts by mass of the conductive powder.

[0029] The content of the ceramic powder is preferably 1% by mass or more and 20% by mass or less, more preferably 3% by mass or more and 20% by mass or less, based on the total amount of the conductive paste. When the content of the conductive powder is within the above range, the conductive paste has excellent conductivity and dispersibility.

[0030] (binder resin) The binder resin is not particularly limited, and known resins can be used. Examples of the binder resin include cellulose-based resins such as methyl cellulose, ethyl cellulose, ethyl hydroxyethyl cellulose, and nitrocellulose, acrylic resins, and butyral resins such as polyvinyl butyral. Among them, it is preferable to include ethyl cellulose from the viewpoint of solubility in a solvent and combustion decomposition. In addition, when used as a conductive paste for an internal electrode, a butyral resin may be included from the viewpoint of improving the adhesive strength with the green sheet, or a butyral resin may be used alone. One type of binder resin may be used, or two or more types may be used. For example, a cellulose-based resin and a butyral resin may be used as the binder resin. In addition, the molecular weight of the binder resin is, for example, about 20,000 to 200,000.

[0031] The content of the binder resin is preferably 1 part by mass or more and 10 parts by mass or less, and more preferably 1 part by mass or more and 8 parts by mass or less, relative to 100 parts by mass of the conductive powder.

[0032] The content of the binder resin is preferably 0.5% by mass to 10% by mass, more preferably 1% by mass to 6% by mass, based on the entire conductive paste. When the content of the binder resin is within the above range, the conductive paste has excellent conductivity and dispersibility.

[0033] (Organic solvent) The organic solvent is not particularly limited, and any known organic solvent capable of dissolving the binder resin can be used. Examples of the organic solvent include acetate-based solvents such as dihydroterpineyl acetate, isobornyl acetate, isobornyl propionate, isobornyl butyrate, isobornyl isobutyrate, ethylene glycol monobutyl ether acetate, and dipropylene glycol methyl ether acetate, terpene-based solvents such as terpineol and dihydroterpineol, and hydrocarbon-based solvents such as tridecane, nonane, and cyclohexane. The organic solvent may be used alone or in combination of two or more.

[0034] The content of the organic solvent is preferably 40 parts by mass or more and 100 parts by mass or less, more preferably 65 parts by mass or more and 95 parts by mass or less, relative to 100 parts by mass of the conductive powder. When the content of the organic solvent is within the above range, the conductive powder has excellent conductivity and dispersibility.

[0035] The content of the organic solvent is preferably 20% by mass to 60% by mass, more preferably 35% by mass to 55% by mass, based on the entire conductive paste. When the content of the organic solvent is within the above range, the conductive paste has excellent conductivity and dispersibility.

[0036] (Dispersant) The conductive paste of the present embodiment contains an amine-based dispersant which is a secondary amine or a tertiary amine and has a dielectric constant of not more than 10. By containing such an amine-based dispersant, the dispersed state of the conductive powder in the conductive paste can be maintained, and the change in viscosity of the conductive paste over time and the change in dynamic viscosity over time can be reduced.

[0037] The amine dispersant is preferably not a polymer dispersant. The amine dispersant may have a molecular weight of, for example, 1500 or less, or 1000 or less. The lower limit of the molecular weight of the amine dispersant may be, for example, 150 or more, 200 or more, or 500 or more.

[0038] The amine-based dispersant is preferably a tertiary amine or a secondary amine represented by the following general formula (2).

[0039] [ka]

[0040] (In the formula (2), R2 represents an alkyl group, an alkenyl group, or an alkynyl group having 8 to 18 carbon atoms, R3 represents an oxyethylene group, an oxypropylene group, or a methylene group, R4 represents an oxyethylene group, an oxypropylene group, or a methylene group, and R3 and R4 may be the same or different. In addition, the N atom in the formula (2) is not directly bonded to the O atom in R3 and R4, Y is a number from 0 to 7, and Z is a number from 1 to 7.)

[0041] In the above formula (2), R2 represents an alkyl group, an alkenyl group, or an alkynyl group having 8 to 18 carbon atoms. When the carbon number of R2 is within the above range, the powder in the conductive paste has sufficient dispersibility and excellent solubility in the solvent. R2 is preferably a linear hydrocarbon group.

[0042] In the above formula (2), R3 represents an oxyethylene group, an oxypropylene group, or a methylene group, R4 represents an oxyethylene group, an oxypropylene group, or a methylene group, and R3 and R4 may be the same or different. In addition, the N atom in formula (2) is not directly bonded to the O atoms in R3 and R4, Y is a number from 0 to 7, and Z is a number from 1 to 7.

[0043] For example, R3 is -(AO) Y When R3 is an oxyalkylene group represented by - (Y is 1 or more), the most terminal O atom in the oxyalkylene group is bonded to the H atom adjacent to R3. When R3 is a methylene group, R3 is -(CH2) Y When Y is 1 or 2, it forms a methyl group (-CH3) or an ethyl group (-CH2-CH3) together with the adjacent H element. Also, when R4 is -(AO) Z In the case of an oxyalkylene group represented by - (Z is 1 or more), the most terminal O atom in the oxyalkylene group bonds to the H atom adjacent to R4.

[0044] In the above formula (2), when Y is 0, the above amine-based dispersant is an alkyl group, an alkenyl group, or an alkynyl group having 8 to 18 carbon atoms, one hydrogen group, and -(R4) Z H and a secondary amine having

[0045] In addition, in the above formula (2), when Y is 1 or more, the above amine-based dispersant is a compound represented by the formula (2) consisting of an alkyl group, an alkenyl group, or an alkynyl group having 8 to 17 carbon atoms and -(R3) Y H and -(R4) Z H and a tertiary amine.

[0046] The dielectric constant of the amine-based dispersant is 10 or less, more preferably 1 to 10, and even more preferably 2 to 10. If the dielectric constant of an amine-based dispersant that is not a polymer dispersant exceeds 10, the lipophilicity decreases and the dispersion of the conductive particles in the conductive paste cannot be maintained. The dielectric constant of the amine-based dispersant can be measured with an impedance meter.

[0047] The dielectric constant of an organic material is an index indicating the ease of polarization of the organic material, and depends on its molecular structure and functional groups. For example, in the above formula (2), when one of R3 and R4 of the amine-based dispersant is an oxyethylene group or an oxypropylene group, the dielectric constant is high. Furthermore, when both R3 and R4 are oxyethylene groups and / or oxypropylene groups, the dielectric constant is further increased. From the viewpoint of further improving the viscosity stability after long-term storage, it is desirable that at least one of R3 and R4 of the amine-based dispersant is an oxyethylene group or an oxypropylene group.

[0048] In the above formula (2), when at least one of R3 and R4 is an oxyethylene group or an oxypropylene group, the conductive powder can be easily maintained in a dispersed state in the conductive paste by increasing the dielectric constant of the amine dispersant up to an upper limit of 10, and the viscosity change over time and the dynamic viscosity change over time can be reduced. The dielectric constant of the amine dispersant may be, for example, 5 or more, or 6 or more.

[0049] In the above formula (2), when R3 is an oxyethylene group or an oxypropylene group, the dielectric constant tends to decrease as the value of Y increases. Similarly, when R4 is an oxyethylene group or an oxypropylene group, the dielectric constant tends to decrease as the value of Z increases.

[0050] When at least one of R3 and R4 is an oxyethylene group or an oxypropylene group, it is desirable that the sum of the values ​​of Y and Z is 3 or more. When the value of Z is 3 or more, the dynamic viscosity change over time of the obtained conductive paste can be reduced. Furthermore, each of the values ​​of Y and Z may be 3 or more, or 5 or more.

[0051] Furthermore, when R3 and R4 are methylene groups, the value of Y can be appropriately selected from the range of 0 to 7, and the value of Z can be appropriately selected from the range of 1 to 7. When R3 and R4 are methylene groups, the value of Y may be 5 or less, or may be 3 or less. When Z is 5 or less, or may be 3 or less. When R3 and R4 are methylene groups, the dielectric constant may be 5 or less, or may be 3 or less.

[0052] The conductive paste contains an amine-based dispersant in an amount of 0.01 to 2 parts by mass, preferably 0.02 to 1 part by mass, per 100 parts by mass of the conductive powder. When the amine-based dispersant is contained in the above range, the viscosity change over time can be suppressed and the viscosity stability can be improved. Note that, when the content of the amine-based dispersant exceeds 2 parts by mass, mesh marks may be generated on the printed surface or the viscosity of the paste may be significantly reduced when the conductive paste is printed on a green sheet.

[0053] The amine-based dispersant may be selected from commercially available products that satisfy the above-mentioned characteristics. The amine-based dispersant may be produced by a conventionally known production method so as to satisfy the above-mentioned characteristics.

[0054] The dispersant may also contain an amino acid-based dispersant. As shown in the following general formula (1), the amino acid-based dispersant preferably has an N-acylamino acid skeleton and a chain hydrocarbon group having 10 to 20 carbon atoms.

[0055] [ka]

[0056] (In the formula (1), R1 represents a chain hydrocarbon having 10 to 20 carbon atoms.)

[0057] In the above formula (1), R1 represents a chain hydrocarbon group having 10 to 20 carbon atoms. The number of carbon atoms in R1 is preferably 15 to 20. The chain hydrocarbon group may be a straight-chain hydrocarbon group or a branched hydrocarbon group. The chain hydrocarbon group may be an alkyl group, an alkenyl group, or an alkynyl group. R1 is preferably a straight-chain hydrocarbon group, more preferably a straight-chain alkenyl group, and has a double bond.

[0058] The conductive paste may contain the amino acid-based dispersant represented by the above formula (1) in an amount of 0.01 to 2 parts by mass, preferably 0.02 to 1 part by mass, more preferably 0.03 to 0.6 parts by mass, and more preferably 0.1 to 0.6 parts by mass, relative to 100 parts by mass of the conductive powder. When the amino acid-based dispersant is contained in the above range, the dry film density can be improved. In addition, the upper limit of the content of the amino acid-based dispersant may be 0.5 parts by mass or less, or may be 0.3 parts by mass or less. By combining with the above amine-based dispersant, the above-mentioned effect can be obtained even if the content of the amino acid-based dispersant is reduced within the above range. Note that when the content of the amino acid-based dispersant exceeds 2 parts by mass, when the conductive paste is printed on a green sheet, mesh marks may be generated on the printed surface, or the viscosity of the paste may be significantly reduced.

[0059] The amino acid-based dispersant represented by the formula (1) can be selected from commercially available products that satisfy the above-mentioned properties. The amino acid-based dispersant may be produced by a conventionally known production method so as to satisfy the above-mentioned properties.

[0060] The dispersant (including the amino acid-based dispersant and amine-based dispersant) is preferably contained in an amount of 0.02 parts by mass or more and 4 parts by mass or less, more preferably 0.04 parts by mass or more and 2 parts by mass or less, relative to 100 parts by mass of the conductive powder. When the content of the dispersant is within the above range, the viscosity of the conductive paste can be adjusted to an appropriate range, and sheet attack and peeling failure of the green sheet can be suppressed.

[0061] The dispersant (including the amino acid-based dispersant and amine-based dispersant) is preferably contained in an amount of 3 mass% or less based on the entire conductive paste. The upper limit of the dispersant content is preferably 2.4 mass% or less, more preferably 2 mass% or less, and even more preferably 1 mass% or less. The lower limit of the dispersant content is not particularly limited, but is, for example, 0.01 mass% or more, preferably 0.05 mass% or more. When the dispersant content is within the above range, the viscosity of the conductive paste can be adjusted to an appropriate range, and sheet attack and peeling failure of the green sheet can be suppressed.

[0062] Furthermore, in the conductive paste of the present embodiment, the amine-based dispersant is preferably contained in an amount by mass of at least 1 time, more preferably at least 2 times, and even more preferably at least 3 times, the amino acid-based dispersant. By containing the amine-based dispersant in the above range, the change in viscosity of the conductive paste over time can be further suppressed.

[0063] The conductive paste may contain a dispersant other than the amino acid-based dispersant and the amine-based dispersant as long as the effect of the present invention is not impaired. Examples of dispersants other than the above include acid-based dispersants including higher fatty acids and polymeric surfactants, cationic dispersants other than acid-based dispersants, nonionic dispersants, amphoteric surfactants, and polymeric dispersants. These dispersants may be used alone or in combination of two or more.

[0064] (Conductive paste)

[0065] The conductive paste according to the present embodiment contains the above-mentioned components, thereby maintaining the dispersion state of the conductive powder in the conductive paste, and reducing the change in viscosity and the change in dynamic viscosity over time of the conductive paste. The change in dynamic viscosity over time of the conductive paste can be evaluated by the TI value, which is an index of dynamic viscosity.

[0066] Here, the TI value is the thixotropic index, which is a value expressed as the ratio of viscosity values ​​at two rotational speeds (also called shear speed or rotational speed) in a rotational viscometer or rheometer. The TI value is, for example, the ratio of viscosity values ​​at a rotational speed of 4 sec -1 The viscosity of -1 When using a rotational viscometer or rheometer, the viscosity of a conductive paste is high when the rotation speed (rotation speed or shear rate) is low, and low when the rotation speed is high.

[0067] Conductive paste TI value (4sec -1 / 40sec -1 ) is preferably 5 or less. A high TI value means that the viscosity increases at a low shear rate, and if the TI value is too high, it is likely to lead to defects such as mesh marks on the printed surface when the conductive paste is printed on a green sheet. -1 Viscosity / rotation speed 4sec -1 If the viscosity of the resin exceeds 5, the above problems may occur.

[0068] TI value (4sec -1 / 40sec -1 ) is not particularly limited, but may be, for example, 2 or more, and may be 3 or more. A low TI value means that the viscosity decreases at a low shear rate, and if the TI value is too low, for example, when a conductive paste is printed, the conductive paste may flow on the printed surface, causing problems such as the printed surface expanding. In particular, even if the amount of conductive paste applied during printing is controlled by making the electrode pattern thinner, if the TI value is low, the conductive paste may flow and the printed surface may expand, making it difficult to obtain a desired electrode pattern.

[0069] The TI value may decrease if the conductive paste is stored for a long period of time. If the TI value decreases due to changes in the conductive paste over time, it is expected that the conductive paste after the changes over time will have problems such as the conductive paste on the printed surface flowing and the printed surface expanding. For example, if the change in the TI value of the conductive paste is calculated by subtracting the "TI value after leaving the paste for 1 day from the reference time point" from the "viscosity TI value after leaving the paste for 22 days from the reference time point," the change in the TI value is preferably 1.0 or less. The lower limit of the change in the TI value is preferably -1.0 or more. The reference time point refers to 24 hours after the conductive paste is manufactured.

[0070] In addition, the conductive paste of the present embodiment has a viscosity (4 sec -1 The change in viscosity (4sec) after long-term storage is preferably 100 Pa.S or less, may be 90 Pa.S or less, or may be 80 Pa.S or less. -1 The change in viscosity (4sec) after leaving the material for one day from the reference point -1 ) is the standard viscosity, the viscosity after standing for 92 days from the standard time (4sec -1 )" minus the "Standard Viscosity."

[0071] On the other hand, the viscosity of the conductive paste after long-term storage (4sec -1 It is not desirable for the change in viscosity (4sec) of the conductive paste to be significantly negative, i.e., for the viscosity to decrease. Conductive paste with a decreased viscosity after long-term storage may cause problems such as the conductive paste flowing out of the printed pattern, and in the worst case, it may connect with adjacent patterns, causing problems such as electrical short circuits in the electronic components obtained after firing. Therefore, the viscosity (4sec) of the conductive paste after long-term storage is -1 The lower limit of the change in viscosity is preferably -10 Pa.S or more, and more preferably -5 Pa.S or more.

[0072] The method for producing the conductive paste of the present embodiment is not particularly limited, and a conventionally known method can be used. The conductive paste can be produced, for example, by preparing the above-mentioned components and stirring and kneading them with a three-roll mill, a ball mill, a mixer, or the like. In this case, if a dispersant is applied to the surface of the conductive powder in advance, the conductive powder is sufficiently loosened without agglomeration, and the dispersant is distributed over the surface, making it easy to obtain a uniform conductive paste. Alternatively, the binder resin may be dissolved in an organic solvent for a vehicle to produce an organic vehicle, and the conductive powder, ceramic powder, organic vehicle, and dispersant may be added to the organic solvent for the paste, and the mixture may be stirred and kneaded with a mixer to produce the conductive paste.

[0073] The conductive paste can be suitably used in electronic components such as multilayer ceramic capacitors. A multilayer ceramic capacitor has dielectric layers formed using dielectric green sheets and internal electrode layers formed using the conductive paste.

[0074] In the multilayer ceramic capacitor, the dielectric ceramic powder contained in the dielectric green sheet and the ceramic powder contained in the conductive paste are preferably powders of the same composition. In the multilayer ceramic capacitor manufactured using the conductive paste of this embodiment, even if the thickness of the dielectric green sheet is, for example, 3 μm or less, sheet attack and peeling failure of the green sheet are suppressed.

[0075] [Electronic components] Hereinafter, embodiments of electronic components and the like of the present invention will be described with reference to the drawings. In the drawings, the components may be shown diagrammatically or at a different scale as appropriate. The positions and directions of components will be described with reference to an XYZ orthogonal coordinate system shown in FIG. 1 as appropriate. In this XYZ orthogonal coordinate system, the X and Y directions are horizontal directions, and the Z direction is vertical (up-down direction).

[0076] 1A and 1B are diagrams showing a multilayer ceramic capacitor 1, which is an example of an electronic component according to an embodiment. The multilayer ceramic capacitor 1 includes a ceramic laminate 10 in which dielectric layers 12 and internal electrode layers 11 are alternately laminated, and an external electrode 20.

[0077] A method for manufacturing a multilayer ceramic capacitor using the conductive paste will be described below. First, the conductive paste is printed on a dielectric layer made of a ceramic green sheet, and dried to form a dry film. A plurality of dielectric layers having this dry film on the upper surface are laminated by pressure bonding to obtain a laminate, and then the laminate is fired and integrated to produce a ceramic laminate 10 in which internal electrode layers 11 and dielectric layers 12 are alternately laminated. Then, a pair of external electrodes 20 is formed on both ends of the ceramic laminate 10 to manufacture a multilayer ceramic capacitor 1. A more detailed description will be given below.

[0078] First, a ceramic green sheet, which is an unfired ceramic sheet, is prepared. For example, the ceramic green sheet is prepared by adding an organic binder such as polyvinyl butyral and a solvent such as terpineol to a raw powder of a specific ceramic such as barium titanate, applying the dielectric layer paste to a support film such as a PET film in a sheet form, and drying to remove the solvent. The thickness of the dielectric layer made of the ceramic green sheet is not particularly limited, but is preferably 0.05 μm or more and 3 μm or less from the viewpoint of the demand for miniaturization of the multilayer ceramic capacitor.

[0079] Next, the above-mentioned conductive paste is printed (applied) on one side of the ceramic green sheet by a known method such as screen printing, and then dried to form a dry film, to prepare a plurality of sheets. Note that, from the viewpoint of the requirement for thinning of the internal electrode layer 11, it is preferable that the thickness of the printed conductive paste (dried film) is 1 μm or less after drying.

[0080] Next, the ceramic green sheet is peeled off from the support film, and the dielectric layer made of the ceramic green sheet and the dry film formed on one side thereof are alternately laminated, and then a laminate is obtained by a heat and pressure treatment. Note that a configuration in which protective ceramic green sheets not coated with the conductive paste are further arranged on both sides of the laminate may be adopted.

[0081] Next, the laminate is cut to a predetermined size to form green chips, and the green chips are subjected to a binder removal process and fired under a reducing atmosphere to manufacture the ceramic laminate 10. The binder removal process is preferably performed in air or N2 gas. The temperature during the binder removal process is, for example, 200°C or higher and 400°C or lower. The temperature is preferably held for 0.5 hours or higher and 24 hours or lower during the binder removal process. The firing is performed in a reducing atmosphere to suppress oxidation of the metal used in the internal electrode layers, and the temperature during firing of the laminate is, for example, 1000°C or higher and 1350°C or lower, and the temperature is held for, for example, 0.5 hours or higher and 8 hours or lower.

[0082] By firing the green chip, the organic binder in the green sheet is completely removed, and the ceramic raw material powder is fired to form the ceramic dielectric layer 12. The organic vehicle in the dry film is also removed, and the nickel powder or the alloy powder mainly composed of nickel is sintered or melted and integrated to form the internal electrodes, forming a multilayer ceramic sintered body in which a plurality of dielectric layers 12 and internal electrode layers 11 are alternately stacked. Note that, from the viewpoint of taking oxygen into the dielectric layers to increase reliability and suppressing reoxidation of the internal electrodes, the sintered multilayer ceramic sintered body may be subjected to an annealing treatment.

[0083] Then, a pair of external electrodes 20 is provided on the produced fired laminated ceramic body to manufacture the laminated ceramic capacitor 1. For example, the external electrode 20 includes an external electrode layer 21 and a plating layer 22. The external electrode layer 21 is electrically connected to the internal electrode layer 11. Note that, for example, copper, nickel, or an alloy thereof can be suitably used as the material for the external electrode 20. Note that the electronic component is not limited to a laminated ceramic capacitor, and may be an electronic component other than a laminated ceramic capacitor. EXAMPLES

[0084] The present invention will be described in detail below based on examples and comparative examples, but the present invention is not limited to these examples.

[0085] [Evaluation method] (Evaluation of the viscosity and TI value of conductive paste) The viscosity of the conductive paste was measured 24 hours after the production of the conductive paste as the reference point, and was measured by flow curve measurement using a rheometer (Anton Paar Rheometer M501) at a rotation speed of 4 sec after leaving the paste at room temperature (25°C) for 1 day, 22 days, and 92 days from the reference point. -1 The viscosity after standing still for 1 day from the reference time point was taken as the reference viscosity, and the reference viscosity was subtracted from each of the viscosities after standing still for 22 days and 92 days to calculate the change in viscosity.

[0086] In addition, the TI value of the conductive paste (4sec -1 / 40sec -1 ) is the rotation speed of 4 sec after leaving it for 1 day and 22 days from the reference time. -1 The viscosity of -1 The viscosity was calculated by dividing it by the viscosity of the

[0087] (Dielectric constant of amine-based dispersants) Using an impedance meter, the amine-based dispersant was placed in a sample holder and the capacitance was measured using the four-terminal method at a frequency of 100 Hz, an applied voltage of 1 V, and an equivalent circuit resistance value of 100 MΩ, and the dielectric constant (relative dielectric constant) of the amine-based dispersant was calculated. [Materials used] (conductive powder) As the conductive powder, Ni powder (SEM average particle size: 0.2 μm) was used.

[0088] (ceramic powder) Barium titanate (BaTiO3; SEM average particle size 0.06 μm) was used as the ceramic powder.

[0089] (binder resin) The binder resins used were ethyl cellulose resin and polyvinyl butyral resin (PVB resin), which were prepared as a vehicle by dissolving them in terpineol.

[0090] (Dispersant) (1) As an amine-based dispersant, in the above general formula (2), R2=C 12 H 25 Dispersant a (dielectric constant 7.7) represented by R3 = C2H4O, R4 = C2H4O, Y = 7, and Z = 7; 12 H 25 , R3=CH2, R4=CH2, Y=1, Z=1; and a dispersant b (dielectric constant 2.2) represented by the above general formula (2), R2=C 12 H 25 , R3 A dispersant d (dielectric constant 9.1) with R4 = C2H4O, R4 = C2H4O, Y = 1, and Z = 1 was used.

[0091] (2) As an amino acid-based dispersant, in the above general formula (1), R1=C 17 H 33 Dispersant c represented by (straight-chain hydrocarbon group) was used. (Organic solvent) Terpineol was used as the organic solvent.

[0092] [Example 1] A conductive paste was prepared by mixing 50% by mass of Ni powder, 3.8% by mass of ceramic powder, 3% by mass of binder resin in a vehicle consisting of ethyl cellulose resin and polyvinyl butyral resin, 0.05% by mass of amino acid-based dispersant, 0.5% by mass of dispersant a as an amine-based dispersant, and 100% by mass of terpineol as a whole, and mixing these materials. The change in viscosity after leaving the conductive paste for 22 days and 92 days relative to the reference viscosity, and the TI after leaving the paste for 1 day and 22 days from the reference time were evaluated by the above method. The evaluation results are shown in Table 1. In Table 1, the change in TI value is the value obtained by subtracting the TI value after leaving the paste for 1 day from the TI value after leaving the paste for 22 days.

[0093] [Example 2] A conductive paste was prepared and evaluated in the same manner as in Example 1, except that dispersant a was changed to dispersant b as the amine-based dispersant. The results are shown in Table 1. [Example 3] A conductive paste was prepared and evaluated in the same manner as in Example 1, except that dispersant a was replaced with dispersant d as the amine-based dispersant and the amount of amine-based dispersant d was 0.25 mass%. The results are shown in Table 1. [Example 4] A conductive paste was prepared and evaluated in the same manner as in Example 1, except that dispersant a was changed to dispersant d as the amine-based dispersant. The results are shown in Table 1. [Example 5] A conductive paste was prepared and evaluated in the same manner as in Example 1, except that dispersant a was changed to dispersant d as the amine-based dispersant and the amount of amine-based dispersant d was 1.0 mass %. The results are shown in Table 1.

[0094] [Example 6] A conductive paste was prepared and evaluated in the same manner as in Example 4, except that the content of the amino acid-based dispersant was 0.5 mass % and the content of the amine-based dispersant d was 0.05 mass %. The results are shown in Table 1.

[0095] [Comparative Example 1] Except for not using the amine-based dispersant, a conductive paste was prepared in the same manner as in Example 1. The results are shown in Table 1.

[0096] [Comparative Example 2] Except for not using the amino acid-based dispersant, a conductive paste was prepared in the same manner as in Example 4. The results are shown in Table 1.

[0097] [Table 1]

[0098] (Evaluation Results) The conductive pastes of Examples 1 to 6, in which an amine-based dispersant was added, showed smaller changes in viscosity after being left standing for 22 days and 92 days from the baseline than the conductive paste of Comparative Example 1, in which an amine-based dispersant was not added, and the change in TI value after being left standing for 1 day from the baseline to 22 days was also smaller.

[0099] It is also found that the conductive paste of Example 1 using dispersants a and d (in formula (2), R3 and R4 are oxyethylene groups), which are amine-based dispersants, shows a smaller change in viscosity after long-term storage (after leaving the paste stationary for 92 days from the reference time point) than the conductive paste of Example 2 using dispersant b (in formula (2), R3 and R4 are methylene groups), which is an amine-based dispersant. Furthermore, the conductive paste using the amine-based dispersant of Example 9, which has a higher dielectric constant than that of Example 1, showed a smaller change in viscosity and TI value after long-term storage compared to the conductive paste of Example 1.

[0100] Furthermore, the conductive paste of Example 4, in which the amine-based dispersant was contained in a larger amount than the amino acid-based dispersant, showed a smaller change in viscosity after long-term storage (especially after being left undisturbed for 92 days from the reference time point) compared to the conductive paste of Example 6, in which the amine-based dispersant was contained in a smaller amount than the amino acid-based dispersant, although the total amount of dispersant was the same.

[0101] On the other hand, in the conductive paste of Comparative Example 2, which contained an amine-based dispersant but no amino acid-based dispersant, the change in viscosity after long-term storage (after leaving it undisturbed for 92 days from the reference point) became a large negative value, and the viscosity was significantly reduced. [Explanation of symbols]

[0102] 1. Multilayer ceramic capacitor 10...Ceramic laminate 11...Internal electrode layer 12...Dielectric layer 20…External electrode 21...External electrode layer 22…Plating layer

Claims

1. A conductive paste comprising a conductive powder, a ceramic powder, a dispersant, a binder resin and an organic solvent, The dispersant includes an amine-based dispersant and an amino acid-based dispersant, The amine-based dispersant is a tertiary amine and has a dielectric constant of 10 or less; The amine-based dispersant is contained in an amount equal to or more than one time of the amino acid-based dispersant in terms of mass ratio. Conductive paste.

2. 2. The conductive paste according to claim 1, wherein the amine-based dispersant is contained in an amount of 0.01 parts by mass or more and 2 parts by mass or less relative to 100 parts by mass of the conductive powder, and the conductive powder is contained in an amount of 40% by mass or more and 60% by mass or less relative to the entire conductive paste.

3. A conductive paste as described in claim 1 or 2, wherein the amino acid-based dispersant is represented by the following general formula (1) and contains 0.01 parts by mass or more and 2 parts by mass or less per 100 parts by mass of the conductive powder. [Formula 1] (In the formula (1), R 1 represents a chain hydrocarbon group having 10 to 20 carbon atoms.

4. The conductive paste according to any one of claims 1 to 3, wherein the dispersant is contained in an amount of 0.01 mass % to 3 mass % based on the entire conductive paste.

5. The conductive paste according to any one of claims 1 to 4, wherein the conductive powder contains at least one metal powder selected from the group consisting of Ni, Pd, Pt, Au, Ag, Cu, and alloys thereof.

6. The conductive paste according to any one of claims 1 to 5, wherein the conductive powder has an average particle size of 0.05 µm or more and 1.0 µm or less.

7. The conductive paste according to any one of claims 1 to 6, wherein the ceramic powder contains a perovskite oxide.

8. The conductive paste according to any one of claims 1 to 7, which is for use in an internal electrode of a multilayer ceramic capacitor.

9. An electronic component formed using the conductive paste according to any one of claims 1 to 7.

10. The laminate has at least a dielectric layer and an internal electrode layer stacked thereon, 9. A multilayer ceramic capacitor, wherein the internal electrode layers are formed using the conductive paste according to claim 8.

Citation Information

Patent Citations

  • Ultrafine metal powder slurry

    JP2006063441A

  • Conductive paste for internal electrode

    JP2013149457A

  • Conductive paste and ceramic electronic part

    JP2015216244A

  • Conductive paste, electronic component, and multilayer ceramic capacitor

    JP2018198202A