Binder composition for secondary battery electrodes, conductive paste composition for secondary battery electrodes, slurry composition for secondary battery electrodes, secondary battery electrodes, and secondary batteries

A polymer-based binder composition with tailored monomer units and residual mercaptan levels improves dispersibility and stability, addressing the challenge of high internal resistance in secondary battery electrodes.

JP7559559B2Active Publication Date: 2024-10-02ZEON CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020563071
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-27
Filing Date
2019-12-12
Publication Date
2024-10-02
Estimated Expiration
2039-12-12

AI Technical Summary

Technical Problem

Conventional binder compositions for secondary battery electrodes face challenges in achieving high dispersibility and dispersion stability of conductive materials at elevated temperatures, leading to increased internal resistance in secondary batteries.

Method used

A binder composition containing a polymer with specific monomer units, including a nitrile group-containing monomer, aromatic vinyl monomer, and linear alkylene structural units, with controlled residual mercaptan amounts, is used to enhance dispersibility and stability, reducing internal resistance.

Benefits of technology

The composition enables the preparation of conductive material pastes with high dispersibility and stability at high temperatures, resulting in electrodes with reduced internal resistance and improved battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559559000001
    Figure 0007559559000001
Patent Text Reader

Abstract

The binder composition for a secondary battery electrode contains a polymer that contains a nitrile group-containing monomer unit, an aromatic vinyl monomer unit, and a linear alkylene structural unit, and has a residual mercaptan content of 1 ppm or more and 50 ppm or less by mass.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a binder composition for secondary battery electrodes, a conductive paste composition for secondary battery electrodes, a slurry composition for secondary battery electrodes, an electrode for a secondary battery, and a secondary battery. [Background technology]

[0002] Secondary batteries such as lithium-ion secondary batteries are small, lightweight, have high energy density, and can be repeatedly charged and discharged, and are used in a wide range of applications. Therefore, in recent years, improvements in battery components such as electrodes have been studied in order to further improve the performance of secondary batteries.

[0003] Here, an electrode used in a secondary battery such as a lithium ion secondary battery usually includes a current collector and an electrode mixture layer (positive electrode mixture layer or negative electrode mixture layer) formed on the current collector. This electrode mixture layer is formed, for example, by using a slurry composition in which an electrode active material and a binder composition containing a binding agent are dispersed in a dispersion medium.

[0004] Therefore, in recent years, attempts have been made to improve the binder composition used in forming the electrode mixture layer in order to achieve further improvements in the performance of secondary batteries. Specifically, for example, Patent Document 1 describes a method for producing a nitrile group-containing copolymer rubber having a predetermined structure and satisfying predetermined properties, characterized in that a nitrile group-containing copolymer rubber before metathesis reaction is subjected to a metathesis reaction in the presence of a chain transfer agent having a predetermined structure. In the production method according to Patent Document 1, it is preferable to carry out emulsion polymerization using an emulsifier during polymerization, and further describes that any polymerization initiator, molecular weight modifier, etc. can be used. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 6330801 Summary of the Invention [Problem to be solved by the invention]

[0006] Here, even if the conventional binder composition for a positive electrode is used, it is difficult to sufficiently improve the dispersibility of the conductive material in the conductive material paste or slurry composition and the dispersion stability at high temperatures. Furthermore, the positive electrode prepared using the conventional binder composition for a positive electrode has room for improvement in terms of further reducing the internal resistance of the secondary battery.

[0007] Therefore, an object of the present invention is to provide a binder composition for secondary battery electrodes, which is capable of preparing a conductive material paste having sufficiently high dispersibility of a conductive material and sufficiently high dispersion stability at high temperatures. Another object of the present invention is to provide a conductive material paste composition for secondary battery electrodes, which has sufficiently high dispersibility of conductive materials and dispersion stability at high temperatures, and can produce electrodes that reduce internal resistance when used to form a secondary battery. It is yet another object of the present invention to provide a slurry composition for a secondary battery electrode, which is capable of producing an electrode that reduces the internal resistance of the resulting secondary battery when formed into the battery. Another object of the present invention is to provide an electrode that reduces the internal resistance of a secondary battery obtained when the secondary battery is formed, and a secondary battery including such an electrode. [Means for solving the problem]

[0008] The present inventors have conducted extensive research with the aim of solving the above problems, and have found that a binder composition for secondary battery electrodes containing a polymer that contains a nitrile group-containing monomer unit, an aromatic vinyl monomer unit, and a linear alkylene structural unit and has a residual mercaptan content within a predetermined range makes it possible to prepare a conductive material paste having sufficiently high dispersibility of a conductive material and sufficiently high dispersion stability at high temperatures, and further makes it possible to prepare an electrode that reduces the internal resistance of the resulting secondary battery when the secondary battery is formed, thereby completing the present invention.

[0009] That is, the present invention aims to advantageously solve the above-mentioned problems, and the binder composition for secondary battery electrodes of the present invention is a binder composition for secondary battery electrodes containing a polymer, characterized in that the polymer contains a nitrile group-containing monomer unit, an aromatic vinyl monomer unit, and a linear alkylene structural unit, and the amount of residual mercaptan in the polymer is 1 ppm or more and 50 ppm or less based on the mass of the polymer. Thus, if the polymer contained in the binder composition contains a nitrile group-containing monomer unit, an aromatic vinyl monomer unit, and a linear alkylene structural unit, and does not contain a hydrophilic group-containing monomer unit, it is possible to prepare a conductive material paste having sufficiently high dispersibility of the conductive material and dispersion stability at high temperatures using such a binder composition, and further it is possible to prepare an electrode that reduces the internal resistance of a secondary battery. The "residual mercaptan content" in a polymer can be measured by the method described in the Examples. The polymer "contains a monomer unit" means that "a polymer obtained by using the monomer contains a structural unit derived from the monomer." The polymer "contains a linear alkylene structural unit" means that a polymer having a structural unit represented by the general formula: -C n H 2n - [where n is an integer]. Furthermore, the presence or absence of monomer units and structural units in the polymer and the content ratio thereof can be determined, for example, by the following formula: 1 It can be determined or measured by H-NMR.

[0010] In the binder composition for secondary battery electrodes of the present invention, the polymer preferably has an insoluble fraction of 1 mass% or less when dissolved in N-methylpyrrolidone. If the insoluble fraction of the polymer when dissolved in N-methylpyrrolidone (hereinafter, sometimes simply referred to as "insoluble fraction") is 1 mass% or less, the coatability of the resulting slurry composition can be improved. The "insoluble fraction" of the polymer can be measured by the method described in the examples.

[0011] In the binder composition for secondary battery electrodes of the present invention, the weight average molecular weight of the polymer is preferably 10,000 or more and 2,000,000 or less. If the weight average molecular weight of the polymer is 10,000 or more and 2,000,000 or less, the internal resistance of the obtained secondary battery can be further reduced, and the dispersibility of the conductive material in the obtained conductive material paste can be further increased. The weight average molecular weight of the polymer can be measured by gel permeation chromatography (GPC).

[0012] The present invention also aims to advantageously solve the above problems, and provides a conductive material paste composition for secondary battery electrodes, which is characterized by comprising a conductive material and any one of the binder compositions for secondary battery electrodes described above. If the paste composition contains any one of the binder compositions for secondary battery electrodes described above, the dispersibility of the conductive material and the dispersion stability at high temperatures are sufficiently high, and an electrode that reduces internal resistance when a secondary battery is formed can be produced.

[0013] In the conductive paste composition for secondary battery electrodes of the present invention, the conductive material may contain carbon nanotubes. If the paste composition contains the binder composition, the carbon nanotubes as the conductive material can be well dispersed in the paste composition.

[0014] The present invention also aims to advantageously solve the above problems, and provides a slurry composition for a secondary battery electrode, which is characterized by comprising an electrode active material, a solvent, and any one of the binder compositions for a secondary battery electrode described above. If the slurry composition contains any one of the binder compositions for a secondary battery electrode described above, it is possible to produce an electrode that has sufficiently high dispersion stability at high temperatures and reduces the internal resistance of the resulting secondary battery when the secondary battery is formed.

[0015] Furthermore, the present invention aims to advantageously solve the above problems, and the secondary battery electrode of the present invention is characterized in that it comprises an electrode mixture layer formed using the above-mentioned slurry composition for a secondary battery electrode. In this way, the electrode formed using the above-mentioned slurry composition for a secondary battery electrode can reduce the internal resistance of the secondary battery obtained when the secondary battery is formed.

[0016] The present invention aims to advantageously solve the above problems, and provides a secondary battery comprising a positive electrode, a negative electrode, an electrolyte, and a separator, the positive electrode or the negative electrode being the above-mentioned secondary battery electrode. In this way, the use of the above-mentioned secondary battery electrode provides a secondary battery with low internal resistance and excellent output characteristics. Effect of the Invention

[0017] According to the present invention, it is possible to provide a binder composition for a secondary battery electrode, which is capable of preparing a conductive material paste having sufficiently high dispersibility of a conductive material and sufficiently high dispersion stability at high temperatures. In addition, according to the present invention, it is possible to provide a conductive material paste composition for secondary battery electrodes, which has sufficiently high dispersibility of the conductive material and dispersion stability at high temperatures, and further, can produce an electrode that reduces internal resistance when a secondary battery is formed. Furthermore, according to the present invention, it is possible to provide a slurry composition for a secondary battery electrode, which is capable of producing an electrode that reduces the internal resistance of the secondary battery obtained when the secondary battery is formed. Furthermore, according to the present invention, it is possible to provide an electrode that reduces the internal resistance of a secondary battery obtained when the secondary battery is formed, and a secondary battery including such an electrode. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present invention will be described in detail. Here, the binder composition for secondary battery electrodes of the present invention can be suitably used when preparing a conductive material paste composition for secondary battery electrodes (hereinafter, sometimes simply referred to as "conductive material paste") and a slurry composition for secondary battery electrodes (hereinafter, sometimes simply referred to as "slurry composition"). The slurry composition for secondary battery electrodes prepared using the binder composition for secondary battery electrodes of the present invention can be suitably used when forming a positive electrode of a secondary battery such as a lithium ion secondary battery. Furthermore, the secondary battery of the present invention is characterized in that it uses a secondary battery electrode formed using the slurry composition for secondary battery electrodes of the present invention.

[0019] (Binder composition for secondary battery electrodes) The binder composition for secondary battery electrodes of the present invention is a binder composition for secondary battery electrodes containing a polymer, the polymer containing a nitrile group-containing monomer unit, an aromatic vinyl monomer unit, and a linear alkylene structural unit as repeating units, and the amount of residual mercaptan in the polymer is 1 ppm or more and 50 ppm or less based on the mass of the polymer. According to the binder composition containing a polymer of such composition, it is possible to prepare a conductive material paste having sufficiently high dispersibility of the conductive material and dispersion stability at high temperatures. Furthermore, according to the slurry composition containing the above polymer, it is possible to form an electrode having low internal resistance when a secondary battery is formed. These advantages can be achieved due to the specific composition and properties of the above-mentioned polymer. In particular, when the amount of residual mercaptan in the polymer is within the above range, the dispersibility of the conductive material can be effectively increased when the polymer is contained in the conductive material paste, and the thickening of the conductive material paste under high temperature conditions can be effectively suppressed. Furthermore, by preparing a slurry composition using a polymer having a residual mercaptan content within the above range, the dispersibility of the conductive material in the obtained slurry composition and the dispersion stability at high temperatures can be improved, and the coatability of the slurry composition can be improved. Furthermore, by the polymer containing a nitrile group-containing monomer unit, the solubility of the polymer in an organic solvent such as N-methylpyrrolidone can be appropriately increased, and the viscosity of the conductive material paste or slurry composition can be adjusted within an appropriate range. As a result, the dispersibility of the solid content of the conductive material, etc. in the conductive material paste or slurry composition can be improved. Furthermore, by the polymer containing an aromatic vinyl monomer unit, the dispersibility of the solid content of the conductive material, etc. can be improved when the conductive material paste or slurry composition is prepared. And, by the polymer containing a linear alkylene structural unit, the viscosity increase of the conductive material paste and slurry composition containing such a polymer under high temperature conditions can be effectively suppressed.

[0020] <Polymer> The polymer is a component that functions as a binder, and in an electrode manufactured by forming an electrode mixture layer on a current collector using a slurry composition for secondary battery electrodes prepared using the binder composition, the polymer holds the components contained in the electrode mixture layer so that they do not detach from the electrode mixture layer. The polymer is required to contain a nitrile group-containing monomer unit, an aromatic vinyl monomer unit, and a linear alkylene structural unit. Furthermore, the polymer is required to have a residual mercaptan amount measured by a predetermined method of 1 ppm or more and 50 ppm or less based on the mass of the polymer. The polymer may contain other monomer units as long as the effect of the present invention is not impaired. In addition, the polymer is preferably a hydrogenated polymer obtained by polymerizing a monomer composition containing a nitrile group-containing monomer, an aromatic vinyl monomer, and a conjugated diene monomer, and hydrogenating the polymer obtained by a known method.

[0021] [Nitrile group-containing monomer unit] The nitrile group-containing monomer unit is a repeating unit derived from a nitrile group-containing monomer. Since the polymer contains the nitrile group-containing monomer unit, it has high solubility in an organic solvent such as N-methylpyrrolidone, and can effectively increase the viscosity of the obtained slurry composition. In addition, the viscosity change over time can be suppressed, and therefore the viscosity stability of the slurry composition can be effectively increased.

[0022] Here, examples of the nitrile group-containing monomer capable of forming the nitrile group-containing monomer unit include α,β-ethylenically unsaturated nitrile monomers. Specifically, the α,β-ethylenically unsaturated nitrile monomer is not particularly limited as long as it is an α,β-ethylenically unsaturated compound having a nitrile group, and examples thereof include acrylonitrile; α-halogenoacrylonitrile such as α-chloroacrylonitrile and α-bromoacrylonitrile; α-alkylacrylonitrile such as methacrylonitrile and α-ethylacrylonitrile; and the like. Among these, from the viewpoint of increasing the binding strength of the polymer, acrylonitrile and methacrylonitrile are preferred as the nitrile group-containing monomer, and acrylonitrile is more preferred. These may be used alone or in combination of two or more.

[0023] The content ratio of the nitrile group-containing monomer unit in the polymer is preferably 5% by mass or more, more preferably 10% by mass or more, more preferably 70% by mass or less, and more preferably 60% by mass or less, when the total repeating units in the polymer are taken as 100% by mass. If the content ratio of the nitrile group-containing monomer unit in the polymer is set to the above lower limit or more, the solubility of the polymer in an organic solvent such as N-methylpyrrolidone is appropriately increased, and it becomes possible to adjust the viscosity of a conductive material paste or slurry composition to an appropriate range when the conductive material paste or slurry composition is prepared. As a result, the dispersibility of solids such as conductive material in the conductive material paste or slurry composition can be improved. Furthermore, when an electrode is formed using such a slurry composition, the polymer can exhibit good binding force, and the peel strength of the electrode can be increased. Furthermore, if the content ratio of the nitrile group-containing monomer unit in the polymer is set to the above upper limit or less, the output characteristics of the secondary battery can be further improved. This is presumably because, when the content ratio of the nitrile group-containing monomer unit in the polymer is equal to or less than the above upper limit, the degree of swelling of the polymer in the electrolyte can be effectively prevented from increasing excessively, and the internal resistance of the secondary battery can be reduced.

[0024] [Aromatic vinyl monomer unit] The aromatic vinyl monomer unit is a repeating unit derived from an aromatic vinyl monomer. A polymer containing the aromatic vinyl monomer unit can enhance the dispersibility of solids such as a conductive material in a conductive material paste or slurry composition.

[0025] Here, examples of the monomer capable of forming an aromatic vinyl polymerization unit include aromatic vinyl monomers such as styrene, α-methylstyrene, vinyltoluene, etc. Among these, styrene is preferred because it has good copolymerizability with other monomers and relatively little side reactions such as branching, chain formation, and intermolecular crosslinking of the polymer.

[0026] The content of the aromatic vinyl monomer unit in the polymer is preferably 1% by mass or more, more preferably 5% by mass or more, and preferably 50% by mass or less, and more preferably 45% by mass or less, when the total repeating units in the polymer are taken as 100% by mass. By setting the content of the aromatic vinyl monomer unit in the polymer to the above lower limit or more, the dispersibility of the solid content of the conductive material, etc. can be effectively increased when a conductive material paste or slurry composition is prepared. Furthermore, by setting the content of the aromatic vinyl monomer unit in the polymer to the above upper limit or less, the dispersibility of the solid content of the conductive material, etc. can be effectively increased when a conductive material paste or slurry composition is prepared.

[0027] [Straight-chain alkylene structural unit] The linear alkylene structural unit (hereinafter, sometimes simply referred to as an "alkylene structural unit") is represented by the general formula: -C n H 2n - [where n is an integer] is a repeating unit composed only of a linear alkylene structure. Since the polymer has a linear alkylene structural unit, it is possible to suppress the solid content such as the conductive material from flocculating in the slurry composition after a period of time has elapsed since the preparation of the slurry composition, and to enhance the dispersion stability of the slurry composition. In order to achieve this effect even more effectively, the linear alkylene structural unit is preferably a linear alkylene structural unit having 4 or more carbon atoms, and in the above general formula, n is preferably an integer of 4 or more.

[0028] The method for introducing the linear alkylene structural unit into the polymer is not particularly limited, but may be, for example, the following method (1) or (2): (1) A method in which a polymer is prepared from a monomer composition containing a conjugated diene monomer, and the polymer is hydrogenated to convert the conjugated diene monomer unit into a linear alkylene structural unit. (2) A method for preparing a polymer from a monomer composition containing a 1-olefin monomer such as 1-butene or 1-hexene. These conjugated diene monomers and 1-olefin monomers can be used alone or in combination of two or more kinds. Among these, method (1) is preferred since the polymer can be easily produced.

[0029] Examples of the conjugated diene monomer that can be used in the above method (1) include conjugated diene compounds such as 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, and 1,3-pentadiene. Among them, 1,3-butadiene is preferred. That is, the linear alkylene structural unit is preferably a structural unit (conjugated diene hydrogenated unit) obtained by hydrogenating a conjugated diene monomer unit, and more preferably a structural unit (1,3-butadiene hydrogenated unit) obtained by hydrogenating a 1,3-butadiene unit. The hydrogenation can be carried out using a known method as described below.

[0030] The content of the linear alkylene structural unit in the polymer is preferably 10% by mass or more, more preferably 15% by mass or more, and preferably 60% by mass or less, and more preferably 50% by mass or less, when the total repeating units (the sum of the structural units and the monomer units) in the polymer is taken as 100% by mass. By making the content of the linear alkylene structural unit equal to or more than the above lower limit, the increase in viscosity of the conductive material paste and slurry composition under high temperature conditions can be effectively suppressed. In addition, by making the content of the linear alkylene structural unit equal to or less than the above upper limit, the solubility of the polymer in an organic solvent such as N-methylpyrrolidone can be appropriately increased, and the viscosity of the conductive material paste or slurry composition can be more effectively adjusted within an appropriate range. As a result, the dispersibility of solids such as the conductive material in the conductive material paste or slurry composition can be more effectively increased.

[0031] As described above, when the polymer is a hydrogenated polymer obtained by hydrogenating a polymer obtained by polymerizing a monomer composition containing a conjugated diene, the hydrogenated polymer may contain a linear alkylene structural unit and other units derived from conjugated dienes (for example, including unhydrogenated conjugated diene units). In this case, the total content ratio of the linear alkylene structural unit and other units derived from conjugated dienes in the hydrogenated polymer (hereinafter also referred to as the "content ratio of units derived from conjugated dienes") is preferably within the suitable content ratio range described above for the "content ratio of linear alkylene structural units". By setting the total ratio with the content ratio of units derived from conjugated dienes within the above range, the effects described for the upper and lower limits of the content ratio of linear alkylene structural units can be achieved.

[0032] [Other monomer units] Furthermore, the other monomer capable of forming the other monomer unit is not particularly limited, and examples thereof include known monomers copolymerizable with the above-mentioned monomers, such as hydrophilic group-containing monomers, (meth)acrylic acid ester monomers, fluorine-containing monomers, (meth)acrylamide compounds, and epoxy group-containing unsaturated compounds. These monomers can be used alone or in combination of two or more. In the present specification, "(meth)acrylic" means acrylic and / or methacrylic.

[0033] The content of the other monomer units in the polymer is preferably 20% by mass or less, more preferably 10% by mass or less, and may be 0% by mass. In particular, when the polymer contains an acidic group-containing monomer unit as the other monomer unit, the content of the acidic group-containing monomer unit in the polymer is preferably 10% by mass or less.

[0034] The "hydrophilic group-containing monomer" listed as an example of a monomer that can constitute the "other monomer unit" is a monomer that contains a hydrophilic group such as an acidic group and a hydroxyl group. Examples of the acidic group include a carboxylic acid group, a sulfonic acid group, and a phosphoric acid group.

[0035] Examples of the monomer having a carboxylic acid group include monocarboxylic acids and their derivatives, dicarboxylic acids and their acid anhydrides, and their derivatives. Examples of the monocarboxylic acid include acrylic acid, methacrylic acid, and crotonic acid. Examples of the monocarboxylic acid derivatives include 2-ethylacrylic acid, isocrotonic acid, α-acetoxyacrylic acid, β-trans-aryloxyacrylic acid, α-chloro-β-E-methoxyacrylic acid, and β-diaminoacrylic acid. The dicarboxylic acids include maleic acid, fumaric acid, and itaconic acid. Examples of dicarboxylic acid derivatives include methylmaleic acid, dimethylmaleic acid, phenylmaleic acid, chloromaleic acid, dichloromaleic acid, fluoromaleic acid, and maleic acid esters such as methylallyl maleate, diphenyl maleate, nonyl maleate, decyl maleate, dodecyl maleate, octadecyl maleate, and fluoroalkyl maleate. Examples of the acid anhydrides of dicarboxylic acids include maleic anhydride, acrylic anhydride, methylmaleic anhydride, and dimethylmaleic anhydride. Furthermore, as the compound having a carboxylic acid group, an acid anhydride which generates a carboxyl group upon hydrolysis can also be used. Other examples include monoesters and diesters of α,β-ethylenically unsaturated polycarboxylic acids such as monoethyl maleate, diethyl maleate, monobutyl maleate, dibutyl maleate, monoethyl fumarate, diethyl fumarate, monobutyl fumarate, dibutyl fumarate, monocyclohexyl fumarate, dicyclohexyl fumarate, monoethyl itaconate, diethyl itaconate, monobutyl itaconate, and dibutyl itaconate.

[0036] Examples of monomers having a sulfonic acid group include vinyl sulfonic acid, methyl vinyl sulfonic acid, (meth)allyl sulfonic acid, styrene sulfonic acid, (meth)acrylic acid-2-ethyl sulfonate, 2-acrylamido-2-methylpropanesulfonic acid, and 3-allyloxy-2-hydroxypropanesulfonic acid. In the present invention, "(meth)allyl" means allyl and / or methallyl.

[0037] Examples of the monomer having a phosphate group include 2-(meth)acryloyloxyethyl phosphate, methyl-2-(meth)acryloyloxyethyl phosphate, and ethyl-(meth)acryloyloxyethyl phosphate. In the present invention, "(meth)acryloyl" means acryloyl and / or methacryloyl.

[0038] Examples of monomers having a hydroxyl group include ethylenically unsaturated alcohols such as (meth)allyl alcohol, 3-butene-1-ol, and 5-hexene-1-ol; alkanol esters of ethylenically unsaturated carboxylic acids such as 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxyethyl methacrylate, and 2-hydroxypropyl methacrylate; and monomers having the general formula CH2=CR 1 -COO-(C n H 2n O) m -H (wherein m is an integer of 2 to 9, n is an integer of 2 to 4, R 1represents hydrogen or a methyl group) and (meth)acrylic acid esters; mono(meth)acrylic acid esters of dihydroxy esters of dicarboxylic acids such as 2-hydroxyethyl-2'-(meth)acryloyloxyphthalate and 2-hydroxyethyl-2'-(meth)acryloyloxysuccinate; vinyl ethers such as 2-hydroxyethyl vinyl ether and 2-hydroxypropyl vinyl ether; mono(meth)allyl ethers of alkylene glycols such as (meth)allyl-2-hydroxyethyl ether and (meth)allyl-2-hydroxypropyl ether; diethylene glycol mono(meth)allyl ether and polyoxyalkylene glycol (meth)monoallyl ethers such as dipropylene glycol mono(meth)allyl ether; mono(meth)allyl ethers of halogen- and hydroxy-substituted (poly)alkylene glycols such as glycerin mono(meth)allyl ether and (meth)allyl-2-chloro-3-hydroxypropyl ether; mono(meth)allyl ethers of polyhydric phenols such as eugenol and isoeugenol and halogen-substituted products thereof; and (meth)allyl thioethers of alkylene glycols such as (meth)allyl-2-hydroxyethyl thioether and (meth)allyl-2-hydroxypropyl thioether.

[0039] The above-mentioned nitrile group-containing monomer unit, aromatic vinyl monomer unit, and linear alkylene structural unit may not necessarily contain a hydrophilic group such as a carboxylic acid group, a sulfonic acid group, a phosphoric acid group, or a hydroxyl group.

[0040] [Iodine value] The polymer preferably has an iodine value of 80 mg / 100 mg or less, more preferably 70 mg / 100 mg or less, and even more preferably 50 mg / 100 mg or less. A polymer having an iodine value of the above upper limit or less can prepare a conductive material paste with higher dispersibility of the conductive material, and can also improve the dispersibility of the conductive material in a slurry composition prepared by the polymer. Here, the iodine value of the polymer can be, for example, 2 mg / 100 mg or more. In addition, when the polymer is a hydrogenated polymer, the iodine value of the polymer can be adjusted by changing the hydrogenation conditions. The "iodine value" of the polymer can be measured in accordance with JIS K6235 (2006).

[0041] [Weight average molecular weight] Furthermore, the polymer preferably has a weight-average molecular weight of 10,000 or more, more preferably 20,000 or more, preferably 2,000,000 or less, more preferably 1,500,000 or less, and even more preferably 1,000,000 or less. If the weight-average molecular weight of the polymer is equal to or greater than the lower limit, a conductive material paste having higher dispersibility of the conductive material can be prepared. If the weight-average molecular weight of the polymer is equal to or greater than the lower limit, the polymer can be prevented from excessively swelling in the electrolyte, and the internal resistance of the resulting secondary battery can be effectively prevented from increasing. If the weight-average molecular weight of the polymer is equal to or less than the upper limit, the viscosity of the conductive material paste can be effectively prevented from increasing and the dispersibility of the conductive material can be effectively prevented from decreasing when the conductive material paste is prepared. This makes it possible to form a good conductive path in the electrode, and the internal resistance of the resulting secondary battery can be effectively prevented from increasing.

[0042] [NMP insoluble fraction] Furthermore, the insoluble fraction of the polymer when dissolved in N-methylpyrrolidone is preferably 1% by mass or less, more preferably 0.5% by mass or less, and more preferably 0.2% by mass or less. If the insoluble fraction of the polymer is equal to or less than the upper limit, a conductive material paste having a higher dispersibility of the conductive material can be prepared. Furthermore, if the insoluble fraction of the polymer is equal to or less than the upper limit, a slurry composition having a higher coatability can be prepared, and the internal resistance of the obtained secondary battery can be further reduced.

[0043] [Residual mercaptan content] The polymer must have a residual mercaptan content of 1 ppm or more, preferably 2 ppm or more, and 50 ppm or less, preferably 30 ppm or less, and more preferably 23 ppm or less, based on the mass of the polymer, as measured according to a predetermined method. If the residual mercaptan content of the polymer is equal to or greater than the lower limit, a conductive material paste having sufficiently high dispersibility of the conductive material can be prepared. If the residual mercaptan content of the polymer is equal to or less than the upper limit, thickening of the conductive material paste under high temperature conditions can be effectively suppressed when the polymer is contained in the conductive material paste. Furthermore, by blending a polymer having a residual mercaptan content of equal to or less than the upper limit, the coatability of the resulting slurry composition can be improved.

[0044] Here, as a method for incorporating mercaptan into a polymer, a mercaptan compound may be blended as a molecular weight regulator when polymerizing the polymer according to an arbitrary method. The mercaptan compound that can be used as a molecular weight regulator is not particularly limited, and a compound having a mercapto group can be preferably used, for example, octyl mercaptan, 2,2,4,6,6-pentamethyl-4-heptanethiol, 2,4,4,6,6-pentamethyl-2-heptanethiol, 2,3,4,6,6-pentamethyl-2-heptanethiol, 2,3,4,6,6-pentamethyl-3-heptanethiol, t-dodecyl mercaptan, n-dodecyl mercaptan, and other compounds having a mercapto group with a carbon number of 8 to 12; 2,2,4,6,6-pentamethyl-4-octanethiol, 2,2,4,6,6,8,8-heptamethyl-4-nonanethiol, and other compounds having a mercapto group with a carbon number of 13 to 16. These can be used alone or in combination of two or more kinds. When multiple types of mercaptan compounds are used as the molecular weight regulator, the above "residual mercaptan amount" corresponds to the total amount of the multiple types of mercaptan compounds.

[0045] [Method of preparing polymer] The method for preparing the above-mentioned polymer is not particularly limited. For example, the polymer can be prepared by polymerizing a monomer composition containing the above-mentioned monomer in the presence of a molecular weight regulator containing the above-mentioned mercaptan compound and any additives to obtain a polymer, and then hydrogenating (adding hydrogen) the obtained polymer.

[0046] Here, the content of each monomer in the monomer composition used for preparing the polymer can be determined based on the content of each repeating unit in the polymer. The polymerization method is not particularly limited, and any method such as solution polymerization, suspension polymerization, bulk polymerization, emulsion polymerization, etc. Among them, it is preferable to prepare the polymer according to the emulsion polymerization method using an emulsifier (for example, see Japanese Patent No. 633801). Furthermore, the method for hydrogenating the polymer is not particularly limited, and general methods using a catalyst, such as an oil phase hydrogenation method, an aqueous phase direct hydrogenation method, and an aqueous phase indirect hydrogenation method (see, for example, International Publication No. 2013 / 080989, etc.), can be used.

[0047] Furthermore, when the above-mentioned method (1) (i.e., a method of converting a conjugated diene monomer unit into a linear alkylene structural unit by hydrogenating it) is adopted when introducing a linear alkylene structural unit into a polymer, it is preferable to carry out a metathesis reaction of the polymer, i.e., a metathesis reaction, followed by hydrogenation. The metathesis reaction of the polymer is not particularly limited, and can be carried out, for example, using the method and catalyst described in Japanese Patent No. 4509792 and International Publication No. 2016 / 103730. Specifically, the metathesis reaction of the polymer can be carried out in the presence of a catalyst and a co-olefin. Here, a known ruthenium-based catalyst can be used as the catalyst for the metathesis reaction. Among them, it is preferable to use a Grubbs catalyst such as bis(tricyclohexylphosphine)benzylidene ruthenium dichloride or 1,3-bis(2,4,6-trimethylphenyl)-2-(imidazolidinylidene)(dichlorophenylmethylene)(tricyclohexylphosphine)ruthenium as the catalyst for the metathesis reaction. As the coolefin, an olefin having 2 to 16 carbon atoms, such as ethylene, isobutane, or 1-hexane, can be used. As the hydrogenation catalyst for hydrogenation after the metathesis reaction, a known homogeneous hydrogenation catalyst, such as Wilkinson's catalyst ((PPh3)3RhCl), can be used.

[0048] [solvent] The binder composition may contain a solvent. The solvent is not particularly limited, and an organic solvent can be used. Examples of the organic solvent include alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, t-butanol, pentanol, hexanol, heptanol, octanol, nonanol, decanol, and amyl alcohol, ketones such as acetone, ethyl methyl ketone, and cyclohexanone, esters such as ethyl acetate and butyl acetate, ethers such as diethyl ether, dioxane, and tetrahydrofuran, amide polar organic solvents such as N,N-dimethylformamide and N-methylpyrrolidone (NMP), and aromatic hydrocarbons such as toluene, xylene, chlorobenzene, orthodichlorobenzene, and paradichlorobenzene. These may be used alone or in combination of two or more. Among them, NMP is preferable as the solvent.

[0049] [Other ingredients] In addition to the above components, the binder composition of the present invention may contain a polymer having a different composition from the above polymer, and known additives such as those described in JP-A-2013-179040. These components may be used alone or in combination of two or more at any ratio.

[0050] For example, polymers having a different composition from the above-mentioned polymers include polymers containing hydrophilic group-containing monomer units, fluorine-containing polymers such as polyvinylidene fluoride (PVdF), polyacrylonitrile, polymethyl methacrylate, etc. These polymers differ from the above-mentioned polymers in that they contain hydrophilic group-containing monomer units or do not contain at least one of nitrile group-containing monomer units, aromatic vinyl monomer units, and linear alkylene structural units.

[0051] <Method of preparing binder composition> The binder composition of the present invention can be prepared by mixing the above-mentioned components with a solvent. The mixing method is not particularly limited, and examples thereof include a mixing method using a mixer such as a ball mill, a sand mill, a bead mill, a pigment disperser, a crusher, an ultrasonic disperser, a homogenizer, a planetary mixer, or a Filmix.

[0052] (Conductive paste composition for secondary battery electrodes) The conductive material paste composition for secondary battery electrodes of the present invention (hereinafter, sometimes simply referred to as "conductive material paste composition") is characterized by containing the above-mentioned binder composition of the present invention and a conductive material. Since the conductive material paste composition of the present invention contains the binder composition of the present invention, the dispersibility of the conductive material is sufficiently high and the dispersion stability at high temperatures is excellent, and further, when a secondary battery is formed, an electrode that reduces internal resistance can be produced.

[0053] <Conductive material> The conductive material is a component that can be blended to promote electrical contact between electrode active materials in the electrode mixture layer. As the conductive material, conductive carbon materials such as carbon black (e.g., acetylene black, Ketjen Black (registered trademark), furnace black, etc.), graphite, carbon fiber, carbon flakes, etc.; fibers and foils of various metals, etc. can be used. Among them, the conductive material preferably contains carbon fiber, more preferably contains ultrashort carbon fibers such as carbon nanotubes and vapor-grown carbon fibers, and more preferably contains carbon nanotubes. These may be used alone or in combination of two or more.

[0054] The BET specific surface area of ​​the conductive material is preferably 100 m 2 / g or more, more preferably 150m 2 / g or more, usually 2500m 2 / g or less. If the BET specific surface area of ​​the conductive material is equal to or greater than the lower limit, a good conductive path is formed in the electrode mixture layer, and the output characteristics of the secondary battery can be further improved. If the BET specific surface area of ​​the conductive material is equal to or less than the upper limit, aggregation of the conductive material can be suppressed, and the dispersibility of the conductive material can be ensured.

[0055] Generally, conductive materials with a large BET specific surface area and fibrous conductive materials such as carbon nanotubes tend to aggregate and are difficult to disperse. However, the slurry composition for secondary battery electrodes of the present invention uses a binder composition containing a polymer that satisfies the above-mentioned specific composition and properties, so that even conductive materials with a large BET specific surface area can be dispersed well and stably.

[0056] <Other ingredients> Other components that can be blended in the conductive paste are not particularly limited, and include the same components as those that can be blended in the binder composition of the present invention. In addition, the other components may be used alone or in combination of two or more kinds in any ratio.

[0057] <Method of manufacturing conductive paste> The conductive material paste can be prepared by mixing the binder composition of the present invention described above, the conductive material, and any other components such as a solvent. The mixing method is not particularly limited, and may be the mixing method described above in the section <Preparation method of binder composition>. Here, the content ratio of the conductive material and the polymer of the specific composition in the conductive material paste is preferably 1 part by mass or more of the polymer (i.e., 1 / 100 or more of the conductive material content), more preferably 2 parts by mass or more (i.e., 1 / 50 or more of the conductive material content), even more preferably 5 parts by mass or more (i.e., 1 / 20 or more of the conductive material content), preferably 100 parts by mass or less (i.e., equal to or less than the conductive material content), more preferably 50 parts by mass or less (i.e., half or less of the conductive material content), and even more preferably 25 parts by mass or less (i.e., 1 / 4 or less of the conductive material content). The solid content of the conductive paste is, for example, 1% by mass or more, preferably 2% by mass or more, more preferably 3% by mass or more, and 30% by mass or less, preferably 25% by mass or less, and more preferably 20% by mass or less. The viscosity of the conductive paste is measured with a rheometer (MCR302 manufactured by Anton Paar) at a temperature of 25° C. and a shear rate of 0.1 s -1 When the viscosity is measured under the above conditions, it is usually 10,000 Pa·s or less, preferably 5,000 Pa·s or less, more preferably 1,000 Pa·s or less, even more preferably less than 500 Pa·s, particularly preferably less than 250 Pa·s, and is usually 50 Pa·s or more.

[0058] (Slurry composition for secondary battery electrodes) The slurry composition for secondary battery electrodes of the present invention contains an electrode active material, a solvent, and the above-mentioned binder composition, and optionally contains a conductive material and other components. That is, the slurry composition for secondary battery electrodes of the present invention contains an electrode active material, a solvent, and the above-mentioned polymer, and optionally contains a conductive material and other components. And, since the slurry composition for secondary battery electrodes of the present invention contains the above-mentioned binder composition, it is possible to prepare an electrode that reduces the internal resistance of the secondary battery obtained when the secondary battery is formed. In the following, as an example, the case where the slurry composition for a secondary battery electrode is a slurry composition for a positive electrode of a lithium ion secondary battery will be described, but the present invention is not limited to the following example.

[0059] <Electrode active material> An electrode active material is a substance that transfers electrons in the electrode of a secondary battery. And, as a positive electrode active material for a lithium ion secondary battery, a substance that can occlude and release lithium is usually used.

[0060] Specifically, the positive electrode active material for a lithium ion secondary battery is not particularly limited, and includes lithium-containing cobalt oxide (LiCoO2), lithium manganate (LiMn2O4), lithium-containing nickel oxide (LiNiO2), lithium-containing composite oxides of Co-Ni-Mn, lithium-containing composite oxides of Ni-Mn-Al, lithium-containing composite oxides of Ni-Co-Al, olivine-type lithium iron phosphate (LiFePO4), olivine-type lithium manganese phosphate (LiMnPO4), Li 1+x Mn 2-x O4 (0 < X < 2) lithium-excess spinel compounds represented by, Li[Ni 0.17 Li 0.2 Co 0.07 Mn 0.56 O2, LiNi 0.5 Mn 1.5 O4 and other known positive electrode active materials. Incidentally, as the lithium-containing composite oxides of Co-Ni-Mn, Li(Ni 0.5 Co 0.2 Mn 0.3 )O2, Li(Ni 1 / 3 Co 1 / 3 Mn 1 / 3 )O2 and the like can be mentioned. Among the above, from the viewpoint of improving the battery capacity and the like of the secondary battery, as the positive electrode active material, lithium-containing cobalt oxide (LiCoO2), lithium-containing nickel oxide (LiNiO2), lithium-containing composite oxides of Co-Ni-Mn, Li[Ni 0.17 Li 0.2 Co 0.07 Mn 0.56 O2 or LiNi0.5 Mn 1.5 It is preferable to use O4, and it is more preferable to use a lithium-containing composite oxide of Co-Ni-Mn. The amount and particle size of the positive electrode active material are not particularly limited, and may be the same as those of conventionally used positive electrode active materials.

[0061] <Conductive material> As the conductive material, those mentioned above in the section (Conductive material paste composition for secondary battery electrode) can be suitably used.

[0062] <Binder composition> As the binder composition, the above-mentioned binder composition for a secondary battery electrode of the present invention is used.

[0063] <Solvent> As the solvent, the same solvents as those listed as the solvents that can be contained in the binder composition for secondary battery electrodes of the present invention can be used.

[0064] <Content ratio> The content ratio of the conductive material in the slurry composition is preferably 0.01 parts by mass or more and 20 parts by mass or less, based on 100 parts by mass of the electrode active material. If the ratio of the conductive material is equal to or more than the lower limit, the electrical contact between the positive electrode active materials can be promoted. Also, if the blending amount of the conductive material is equal to or less than the upper limit, the coating property of the slurry composition can be improved. In addition, a suitable content ratio of the polymer in the slurry composition may be within the suitable range that can be derived from the suitable range of the polymer relative to the conductive material described above in the section <Method for producing conductive material paste> and the content ratio between the electrode active material and the conductive material described at the beginning of this paragraph.

[0065] <Other ingredients> Other components that can be blended in the slurry composition are not particularly limited, and include the same as the other components that can be blended in the binder composition of the present invention. In addition, the other components may be used alone or in combination of two or more at any ratio. In particular, when the slurry composition for secondary battery electrodes is a slurry composition for lithium ion secondary battery positive electrodes, it is preferable to use a fluorine-containing polymer such as polyvinylidene fluoride (PVdF) as a second polymer in addition to the above-mentioned polymer (hereinafter, sometimes referred to as a "predetermined polymer"). When a second polymer is used in combination as another component, the amount of the predetermined polymer used is preferably 10% by mass or less, more preferably 5% by mass or less, with the total content of the predetermined polymer and the second polymer being 100% by mass.

[0066] <Method for producing slurry composition> The above-mentioned slurry composition can be prepared by dissolving or dispersing each of the above components in a solvent such as an organic solvent. For example, as described in the section <Preparation method of binder composition>, the above-mentioned components and a solvent can be mixed to prepare the slurry composition by a known dispersion or mixing method. In addition, for example, the electrode active material and the above-mentioned optional components can be added to the conductive material paste of the present invention and subjected to the above-mentioned known dispersion or mixing method to prepare the slurry composition. The solvent contained in the binder composition may be used as the solvent used to prepare the slurry composition. Here, the order of addition of each component during preparation is not particularly limited, and the above-mentioned components may be mixed together or in stages. From the viewpoint of increasing the dispersibility of the conductive material, it is preferable to perform a process of adding and mixing the positive electrode active material, as well as optional components such as a solvent and a second polymer, to the conductive material paste after obtaining the above-mentioned conductive material paste. The viscosity of the slurry composition (measured with a single cylindrical rotational viscometer in accordance with JIS Z8803:1991 at 25°C and 60 rpm) is preferably 1500 mPa·s or more, more preferably 4000 mPa·s or more, and is preferably 20000 mPa·s or less, and more preferably 5000 mPa·s or less.

[0067] (Electrode for secondary batteries) The secondary battery electrode of the present invention comprises a current collector and an electrode mixture layer formed on the current collector, the electrode mixture layer being formed using the above-mentioned slurry composition for secondary battery electrodes. That is, the electrode mixture layer contains at least an electrode active material and a polymer. Note that each component contained in the electrode mixture layer is the same as that contained in the above-mentioned slurry composition for secondary battery electrodes, and the preferred ratio of each component is the same as the preferred ratio of each component in the slurry composition. The secondary battery electrode of the present invention is produced using a slurry composition containing the binder composition for a secondary battery electrode of the present invention, and therefore, by using the electrode, a secondary battery having low internal resistance can be formed.

[0068] <Electrode manufacturing method> The electrode for a secondary battery of the present invention is manufactured, for example, through a step of applying the above-mentioned slurry composition onto a current collector (application step) and a step of drying the slurry composition applied onto the current collector to form an electrode composite layer on the current collector (drying step).

[0069] [Coating process] The method of applying the above-mentioned slurry composition onto the current collector is not particularly limited, and any known method can be used. Specifically, the application method can be a doctor blade method, a dip method, a reverse roll method, a direct roll method, a gravure method, an extrusion method, a brush coating method, or the like. In this case, the slurry composition may be applied to only one side of the current collector, or may be applied to both sides. The thickness of the slurry film on the current collector after application and before drying can be appropriately set according to the thickness of the electrode mixture layer obtained by drying.

[0070] Here, as the current collector to which the slurry composition is applied, a material having electrical conductivity and electrochemical durability is used. Specifically, as the current collector, for example, a current collector made of iron, copper, aluminum, nickel, stainless steel, titanium, tantalum, gold, platinum, etc. can be used. Among them, as the current collector used for the positive electrode, aluminum foil is particularly preferable, and as the current collector used for the negative electrode, copper foil is particularly preferable. Note that the above-mentioned materials may be used alone or in combination of two or more kinds at any ratio.

[0071] [Drying process] The method for drying the slurry composition on the current collector is not particularly limited and may be a known method, for example, a drying method using warm air, hot air, or low-humidity air, a vacuum drying method, or a drying method using irradiation with infrared rays or electron beams, etc. By drying the slurry composition on the current collector in this manner, an electrode mixture layer can be formed on the current collector, and a secondary battery electrode including the current collector and the electrode mixture layer can be obtained.

[0072] After the drying step, the electrode mixture layer may be subjected to a pressure treatment using a mold press or a roll press. The pressure treatment can effectively increase the density of the electrode mixture layer and improve the adhesion between the electrode mixture layer and the current collector. Furthermore, when the electrode mixture layer contains a curable polymer, it is preferable to cure the polymer after the electrode mixture layer is formed.

[0073] (Secondary battery) The secondary battery of the present invention comprises a positive electrode, a negative electrode, an electrolyte, and a separator, and at least one of the positive electrode and the negative electrode is the electrode for the secondary battery of the present invention. Since the secondary battery of the present invention comprises the electrode for the secondary battery of the present invention, the secondary battery of the present invention has excellent battery characteristics (particularly, output characteristics). In the following, as an example, a case will be described in which the secondary battery is a lithium ion secondary battery and the positive electrode is made of the secondary battery electrode of the present invention, but the present invention is not limited to the following example.

[0074] <Negative electrode> As the negative electrode, a known negative electrode can be used. Specifically, as the negative electrode, for example, a negative electrode made of a thin plate of metallic lithium or a negative electrode formed by forming a negative electrode mixture layer on a current collector can be used. The current collector may be made of a metal material such as iron, copper, aluminum, nickel, stainless steel, titanium, tantalum, gold, or platinum. The negative electrode mixture layer may be a layer containing a negative electrode active material and a binder. The binder is not particularly limited, and any known material may be used.

[0075] <Electrolyte> As the electrolyte, an organic electrolyte in which a supporting electrolyte is dissolved in an organic solvent is usually used. As the supporting electrolyte of the lithium ion secondary battery, for example, a lithium salt is used. As the lithium salt, for example, LiPF6, LiAsF6, LiBF4, LiSbF6, LiAlCl4, LiClO4, CF3SO3Li, C4F9SO3Li, CF3COOLi, (CF3CO)2NLi, (CF3SO2)2NLi, (C2F5SO2)NLi, etc. are listed. Among them, LiPF6, LiClO4, and CF3SO3Li are preferred, and LiPF6 is particularly preferred, since they are easily dissolved in the solvent and show a high degree of dissociation. Note that one type of electrolyte may be used alone, or two or more types may be used in combination at any ratio. Usually, the lithium ion conductivity tends to be higher as the supporting electrolyte with a higher degree of dissociation is used, so the lithium ion conductivity can be adjusted by the type of supporting electrolyte. The concentration of the supporting electrolyte in the electrolytic solution (25° C.) can be, for example, 0.5 mol / L or more and 2.0 mol / L or less.

[0076] The organic solvent used in the electrolytic solution is not particularly limited as long as it can dissolve the supporting electrolyte, but for example, carbonates such as dimethyl carbonate (DMC), ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), butylene carbonate (BC), and ethyl methyl carbonate (EMC); esters such as γ-butyrolactone and methyl formate; ethers such as 1,2-dimethoxyethane and tetrahydrofuran; sulfur-containing compounds such as sulfolane and dimethyl sulfoxide; and the like are preferably used. A mixture of these solvents may also be used. Among them, it is preferable to use carbonates because they have a high dielectric constant and a wide stable potential range, and it is preferable to use a mixture of ethylene carbonate and diethyl carbonate. In addition, additives such as vinylene carbonate (VC), fluoroethylene carbonate, and ethyl methyl sulfone can be added to the electrolytic solution.

[0077] <separator> The separator is not particularly limited, and may be one described in, for example, JP 2012-204303 A. Among these, a microporous film made of a polyolefin resin (polyethylene, polypropylene, polybutene, polyvinyl chloride) is preferred, since it can reduce the thickness of the entire separator, thereby increasing the ratio of the electrode active material in the secondary battery and increasing the capacity per volume.

[0078] <Secondary battery manufacturing method> The secondary battery of the present invention can be produced, for example, by stacking a positive electrode and a negative electrode with a separator therebetween, wrapping or folding the stack according to the shape of the battery as necessary, placing the stack in a battery container, injecting an electrolyte into the battery container, and sealing the container. In order to prevent the occurrence of an internal pressure rise in the secondary battery, overcharging and discharging, etc., a fuse, an overcurrent prevention element such as a PTC element, an expanded metal, a lead plate, etc. may be provided as necessary. The shape of the secondary battery may be, for example, a coin type, a button type, a sheet type, a cylindrical type, a square type, a flat type, or any other type. EXAMPLES

[0079] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples. In the following description, "%" and "parts" expressing amounts are based on mass unless otherwise specified. Pressure is gauge pressure. In the examples and comparative examples, the polymer composition, the amount of residual mercaptan, the insoluble fraction in NMP, the iodine value, the weight average molecular weight, the dispersibility of the conductive material in the conductive material paste, the dispersion stability of the conductive material paste at high temperatures, the coatability of the slurry composition, and the initial resistance of the secondary battery were measured and evaluated by the following methods.

[0080] <Polymer composition> In all examples and comparative examples, 1 H-NMR measurement confirmed the presence of linear alkylene structural units (1,3-butadiene hydride units) having 4 or more carbon atoms. <Residual mercaptan content> When measuring the amount of residual mercaptan contained in the polymer, for the polymers obtained in the examples and comparative examples, extraction with methanol was carried out in accordance with JIS K6229 to remove free mercaptan, and then dried to obtain the polymer to be measured. The generated gas when the polymer to be measured thus obtained was heated at 150 °C for 20 minutes was measured by gas chromatography-mass spectrometry. The standard substance was also measured, and from the retention time, MS spectrum, and peak area, the amount of mercaptan compound contained in the polymer was measured according to the calibration curve method. The amount of mercaptan compound measured in this way was shown in the column of "residual mercaptan amount" in Table 1 in ppm units based on the total mass of the polymer. The measurement conditions for the measurement by gas chromatography-mass spectrometry were as follows. <<Measurement conditions>> Separation column: HP-5ms (length 30 m, inner diameter 0.25 mm, film thickness 0.25 μm) Column oven temperature rise: Held at 40 °C for 3 minutes, then heated to 280 °C at 10 °C / min Injection temperature: 300 °C Detector temperature: 280 °C Measured ions: 29 - 550 <Insoluble fraction in NMP> 0.5 g of the polymers prepared in the examples and comparative examples was dissolved by heating at 80 °C with stirring in 100 g of NMP, and the insoluble fraction was recovered. After drying the recovered insoluble fraction, the mass was measured, and the mass of the insoluble fraction (g) / 0.5 (g) × 100% was calculated. <Iodine value of the polymer> 100 g of the aqueous dispersion of the polymers prepared in the examples and comparative examples was coagulated with 1 L of methanol and then vacuum dried at 60 °C for 12 hours. Then, the iodine value of the obtained dried polymer was measured in accordance with JIS K6235 (2006). <Weight average molecular weight of the polymer> The weight average molecular weight of the polymers prepared in the examples and comparative examples was measured by gel permeation chromatography (GPC). Specifically, a calibration curve was prepared using polystyrene as a standard substance, and the weight average molecular weight was calculated as a standard substance equivalent value. The measurement conditions were as follows. <<Measurement conditions>> Column: TSKgel α-M x 2 (inner diameter 7.8 mm x 30 cm x 2, Tosoh Corporation) Eluent: Dimethylformamide (50 mM lithium bromide, 10 mM phosphoric acid) Flow rate: 0.5mL / min. Sample concentration: Approximately 0.5g / L (solid concentration) Injection volume: 200μL Column temperature: 40℃ Detector: Differential refractive index detector RI (Tosoh HLC-8320 GPC RI detector) Detector conditions: RI: Pol(+), Res(1.0s) Molecular weight marker: Tosoh Corporation standard polystyrene kit PStQuick K

[0081] <Dispersibility of conductive material in conductive paste> The viscosity of the conductive paste prepared in the examples and comparative examples was measured using a rheometer (Anton Paar MCR302) at a temperature of 25°C and a shear rate of 0.1 s -1 The viscosity was measured under the following conditions. At the same solid content concentration, the lower the viscosity, the better the dispersibility of the conductive material. A: Viscosity less than 250 Pa s B: Viscosity is 250 Pa·s or more and less than 500 Pa·s C: Viscosity is 500 Pa·s or more

[0082] <Dispersion stability of conductive paste at high temperatures> Carbon nanotubes as conductive materials (specific surface area: 150 m 23.0 parts of the cellulose acetate hydrochloride (100% by mass / g), 0.6 parts of the binder composition (solid content equivalent), and 96.4 parts of NMP were stirred using a disper (3000 rpm, 10 minutes), and then mixed for 1 hour at a temperature of 20°C at a peripheral speed of 8 m / s using a bead mill using zirconia beads with a diameter of 1 mm, to produce a conductive paste with a solid content concentration of 3.6 mass%. The viscosity of the obtained conductive paste was measured using a rheometer (MCR302 manufactured by Anton Paar) at a shear rate of 0.1 s -1 The viscosity before heating was measured under the conditions of 0.1 s and 1.0 s, and the viscosity before heating η0 was obtained. Furthermore, a bead mill using zirconia beads with a diameter of 1 mm was used to mix the mixture for 1 hour at a peripheral speed of 8 m / s and a temperature of 40°C, thereby producing a conductive paste with a solid content concentration of 3.6 mass%. The viscosity of the obtained conductive paste was measured using a rheometer (MCR302 manufactured by Anton Paar) at a shear rate of 0.1 s and 1.0 s. -1 The viscosity was measured under the above conditions to obtain a post-heating viscosity η1. Based on the thus obtained pre-heating viscosity η0 and post-heating viscosity η1, the viscosity retention rate Δη=(η1 / η0)×100% was calculated. The closer the thus calculated viscosity retention rate of the conductive material paste is to 100%, the more excellent the dispersion stability of the conductive material paste at high temperatures, which in turn means that the electrode slurry composition containing the conductive material paste has excellent dispersion stability at high temperatures. A: Viscosity retention rate is less than 110% B: Viscosity retention rate is 110% or more and less than 150% C: Viscosity retention rate is 150% or more

[0083] <Coatability of Slurry Composition> In the examples and comparative examples, when preparing the positive electrode, coating was started, and the coating weight at time t when the target coating weight was achieved was designated as W0. Coating was continued for 10 minutes from time t, and the coating weight 10 minutes after time t was designated as W1. The coating weight maintenance rate ΔW=(W1 / W0)×100% was calculated from W0 and W1. The closer the coating weight maintenance rate is to 100%, the more evenly the slurry composition can be coated and the easier the leveling, and therefore the better the coating properties. A: Weight retention rate is less than 105% B: Weight retention rate is 105% or more but less than 110% C: Weight retention rate is 110% or more

[0084] <Initial resistance of secondary battery> The secondary batteries prepared in the examples and comparative examples were charged at a constant current of 0.2C until the battery voltage reached 4.2V under the condition of a temperature of 25°C, and then charged at a constant voltage of 4.2V until the charging current reached 0.02C. Subsequently, the batteries were discharged at a constant current of 0.2C until the battery voltage reached 3.87V (SOC50%), and then the voltage change after 30 seconds of discharge was measured at 0.2C, 0.5C, 1.0C, 2.0C, 2.5C, and 3.0C. Each discharge current and the measured voltage change were plotted, and the slope was taken as the initial resistance value (Ω). The calculated initial resistance value was evaluated according to the following criteria. A: Initial resistance is less than 4Ω B: Initial resistance is between 4Ω and 6Ω C: Initial resistance is 6Ω or more

[0085] Example 1 <Preparation of Polymer> [Preparation of polymer intermediate] Into a reactor, 180 parts of ion-exchanged water, 25 parts of an aqueous solution of sodium dodecylbenzenesulfonate (emulsifier for emulsion polymerization) having a concentration of 10% by mass, 60 parts of acrylonitrile as a nitrile group-containing monomer, 20 parts of styrene as an aromatic vinyl monomer, 5 parts of methacrylic acid as a hydrophilic group-containing monomer, and 0.6 parts of a mixture of compounds having a mercapto group including t-dodecyl mercaptan, which is a mercaptan compound as a molecular weight regulator (hereinafter, in the examples and comparative examples, abbreviated as "t-dodecyl mercaptan"), were charged in this order, and the gas inside was replaced with nitrogen three times, and then 15 parts of 1,3-butadiene as a conjugated diene monomer was charged. The reactor was kept at 10°C, 0.1 parts of cumene hydroperoxide (polymerization initiator) and 0.1 parts of ferrous sulfate were charged, and the polymerization reaction was continued while stirring. When the polymerization conversion rate reached 85%, 0.1 parts of a 10% by mass aqueous hydroquinone solution (polymerization terminator) was added to terminate the polymerization reaction. Next, the residual monomer was removed at a water temperature of 80°C to obtain an aqueous dispersion of the polymer precursor (particulate polymer), that is, a latex of nitrile rubber. Then, a part of the obtained latex was added to an aqueous solution of magnesium sulfate in an amount of 12% by mass relative to the nitrile rubber content, and the latex was coagulated by stirring. After that, it was filtered while being washed with water, and the obtained coagulated matter was vacuum dried at a temperature of 60°C for 12 hours to obtain nitrile rubber, which is an intermediate (polymer intermediate) of the target polymer. [Metathesis of polymer intermediates] Next, 9 parts of the obtained nitrile rubber was dissolved in 141 parts of monochlorobenzene and put into a reactor. Then, after heating the reactor to a temperature of 80°C, 2 L of a monochlorobenzene solution containing bis(tricyclohexylphosphine)benzylidene ruthenium dichloride as a Grubbs catalyst was added so that the amount of Grubbs catalyst per 100 parts of polymer was 0.25 parts. Then, the inside of the reactor was pressurized to 3.5 MPa with ethylene as a coolefin, and the metathesis reaction of the nitrile rubber was carried out at a stirring speed of 600 rpm. During the reaction, the temperature was kept constant using a cooling coil connected to a temperature control device and a heat sensor. [Hydrogenation of metathesis polymer intermediates] Then, the inside of the reactor was degassed three times with 0.7 MPa H2 while continuing stirring. Then, the temperature of the reactor was raised to 130°C, and 1 L of monochlorobenzene solution containing Wilkinson's catalyst and triphenylphosphine was added to the reactor. The amount of Wilkinson's catalyst and triphenylphosphine per 100 parts of metathesis-completed polymer intermediate was 0.075 parts, and the amount of triphenylphosphine was 1 part. Then, the temperature was raised to 138°C, and the polymer was hydrogenated for 6 hours under a hydrogen pressure of 8.4 MPa to obtain the target polymer, which is a hydrogenated polymer. After the reaction was completed, 0.2 parts of activated carbon with an average diameter of 15 μm was added to the reactor and stirred for 30 minutes. Then, the mixture was filtered through a filter with a pore size of 5 μm to obtain a filtrate. Then, steam was introduced into the filtrate, and monochlorobenzene was recovered and removed by steam distillation, and the target polymer (hydrogenated polymer) generated as a precipitate was separated, dried, and recovered. The amount of residual mercaptan in the hydrogenated polymer, as well as the iodine value, the insoluble fraction in NMP, and the weight average molecular weight of the hydrogenated polymer were measured. The results are shown in Table 1.

[0086] <Preparation of Binder Composition for Positive Electrode> 64 parts of the hydrogenated polymer obtained as described above was collected, and 800 parts of N-methylpyrrolidone (NMP) was added as a solvent. The mixture was heated and dissolved at a temperature of 80° C. to obtain a binder composition for a positive electrode (NMP solution) containing the hydrogenated polymer as a binder.

[0087] <Preparation of conductive paste for positive electrode> Carbon nanotubes as conductive materials (specific surface area: 150 m 2 3.0 parts of 1000g / g, 0.6 parts of the binder composition (solid content equivalent), and 96.4 parts of NMP were stirred using a disperser (3000 rpm, 10 minutes), and then mixed for 1 hour at a peripheral speed of 8 m / s using a bead mill using zirconia beads with a diameter of 1 mm to produce a conductive material paste with a solid content concentration of 3.6 mass %. The conductive material paste obtained was then evaluated for dispersibility of the conductive material in the conductive material paste according to the above. The results are shown in Table 1.

[0088] <Preparation of Positive Electrode Slurry Composition> The conductive paste for the positive electrode obtained as described above was mixed with 0.04 parts in terms of polymer solid content, and a ternary active material having a layered structure (Li(Ni 0.5 Co 0.2 Mn 0.3 100 parts of 1,2-dichloromethane (O2, average particle size: 10 μm), 0.96 parts (solid content equivalent) of polyvinylidene fluoride (PVdF) as a second polymer, and NMP as an organic solvent were added and stirred with a planetary mixer (60 rpm, 30 minutes) to prepare a positive electrode slurry composition. The amount of NMP added was adjusted so that the viscosity of the resulting positive electrode slurry composition (measured with a single cylindrical rotational viscometer in accordance with JIS Z8803:1991. Temperature: 25°C, rotation speed: 60 rpm) was within the range of 4000 to 5000 mPa·s.

[0089] <Preparation of positive electrode> An aluminum foil having a thickness of 20 μm was prepared as a current collector. The positive electrode slurry composition was applied to the aluminum foil with a comma coater so that the coating weight after drying was 20 mg / cm. 2 The slurry composition was applied at a rate of 1 m / min so that the thickness of the positive electrode blank was 1.0 mm, and the positive electrode blank was dried at 90° C. for 20 minutes and at 120° C. for 20 minutes, and then heated at 60° C. for 10 hours to obtain a positive electrode blank. The coating property of the slurry composition was evaluated according to the method described above. The obtained positive electrode blank was rolled with a roll press to obtain a density of 3.2 g / cm. 3 A sheet-shaped positive electrode was produced by combining the positive electrode mixture layer and aluminum foil. The thickness of the sheet-shaped positive electrode was 70 μm. This sheet-shaped positive electrode was cut to a width of 4.8 cm and a length of 50 cm to prepare a positive electrode for a lithium-ion secondary battery.

[0090] <Preparation of negative electrode> 90 parts of spherical artificial graphite (volume average particle size: 12 μm) as the negative electrode active material and SiO X A mixture of 10 parts of cellulose acetate (volume average particle diameter: 10 μm), 1 part of styrene-butadiene polymer as a binder, 1 part of carboxymethyl cellulose as a thickener, and an appropriate amount of water as a dispersion medium was stirred in a planetary mixer to prepare a slurry composition for a negative electrode. Next, a copper foil having a thickness of 15 μm was prepared as a current collector. The negative electrode slurry composition was applied to both sides of the copper foil in a coating amount of 10 mg / cm after drying. 2 The coating was applied so that the coating would become 1.8 g / cm 2 and then dried at 60° C. for 20 minutes and at 120° C. for 20 minutes. The coating was then heat-treated at 150° C. for 2 hours to obtain a negative electrode blank. The negative electrode blank was rolled with a roll press to obtain a negative electrode blank with a density of 1.8 g / cm 2 . 3 A sheet-shaped negative electrode was produced consisting of the negative electrode mixture layer (on both sides) and copper foil. The sheet-shaped negative electrode was then cut to a width of 5.0 cm and a length of 52 cm to prepare a negative electrode for a lithium ion secondary battery.

[0091] <Preparing the separator> A single-layer polypropylene separator (manufactured by Celgard, product name "Celgard 2500") was cut to a size of 120 cm x 5.5 cm.

[0092] <Manufacturing lithium-ion secondary batteries> The positive electrode and the negative electrode were wound with the separator interposed therebetween using a core having a diameter of 20 mm to obtain a wound body. The wound body obtained was then compressed in one direction at a speed of 10 mm / sec until the thickness became 4.5 mm. The wound body after compression had an elliptical shape in a plan view, and the ratio of the major axis to the minor axis (major axis / minor axis) was 7.7. In addition, an electrolyte solution (composition: LiPF6 solution with a concentration of 1.0 M (the solvent is a mixed solution of ethylene carbonate / ethyl methyl carbonate = 3 / 7 (mass ratio) mixed solvent to which 5 mass% of fluoroethylene carbonate was added, and 2 volume% of vinylene carbonate was added as an additive)) was prepared. The compressed wound body was then housed in an aluminum laminate case together with 3.2 g of non-aqueous electrolyte. A nickel lead wire was connected to a predetermined position of the negative electrode, and an aluminum lead wire was connected to a predetermined position of the positive electrode, and the opening of the case was sealed by heat to obtain a lithium ion secondary battery. This lithium ion secondary battery was a pouch-shaped battery with a width of 35 mm, a height of 48 mm, and a thickness of 5 mm, and the nominal capacity of the battery was 700 mAh. The initial resistance of the obtained lithium ion secondary battery was evaluated according to the above. The results are shown in Table 1.

[0093] Example 2 In preparing the polymer, the blending amounts of various monomers and mercaptan compounds were changed to 55 parts of acrylonitrile, 5 parts of styrene, 0.3 parts of t-dodecyl mercaptan, and 35 parts of 1,3-butadiene, respectively, in the same manner as in Example 1. A hydrogenated polymer, a conductive paste for a positive electrode, a binder composition for a positive electrode, a slurry composition for a positive electrode, a positive electrode for a secondary battery, a negative electrode for a secondary battery, and a secondary battery were produced. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0094] Example 3 In preparing the polymer, the blending amounts of various monomers and mercaptan compounds were changed to 15 parts of acrylonitrile, 45 parts of styrene, 0.8 parts of t-dodecyl mercaptan, and 35 parts of 1,3-butadiene, respectively, in the same manner as in Example 1. A hydrogenated polymer, a conductive paste for a positive electrode, a binder composition for a positive electrode, a slurry composition for a positive electrode, a positive electrode for a secondary battery, a negative electrode for a secondary battery, and a secondary battery were produced. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0095] Example 4 In preparing the polymer, the amounts of the various monomers were changed to 45 parts of acrylonitrile, 40 parts of styrene, 0 parts of methacrylic acid (no additives), and 15 parts of 1,3-butadiene, respectively, in the same manner as in Example 1. A hydrogenated polymer, a conductive paste for a positive electrode, a binder composition for a positive electrode, a slurry composition for a positive electrode, a positive electrode for a secondary battery, a negative electrode for a secondary battery, and a secondary battery were produced. Various measurements and evaluations were then carried out in the same manner as in Example 1. The results are shown in Table 1.

[0096] Example 5 During the preparation of the polymer, metathesis of the polymer intermediate was not carried out. Specifically, 9 parts of the polymer obtained in Example 1 was dissolved in 141 parts of monochlorobenzene and charged into a reactor. Without metathesis of the polymer, the polymer intermediate was hydrogenated to obtain a hydrogenated polymer by carrying out the same operation as in [hydrogenation of metathesis-completed polymer intermediate] in Example 1. Using the obtained hydrogenated polymer, a conductive paste for a positive electrode, a binder composition for a positive electrode, a slurry composition for a positive electrode, a positive electrode for a secondary battery, a negative electrode for a secondary battery, and a secondary battery were produced. Various measurements and evaluations were then carried out in the same manner as in Example 1. The results are shown in Table 1.

[0097] Comparative Example 1 When preparing the polymer, metathesis of the polymer intermediate was not performed. In addition, when preparing the polymer intermediate, the blending amount of t-dodecyl mercaptan, which is a mercaptan compound as a molecular weight regulator, was set to 2 parts. Except for these points, a polymer intermediate was obtained in the same manner as in Example 1. 9 parts of the obtained polymer intermediate was dissolved in 141 parts of monochlorobenzene and charged into a reactor. The polymer intermediate was hydrogenated by performing the same operation as in the [hydrogenation of metathesis-completed polymer intermediate] in Example 1 without metathesis of the polymer to obtain a hydrogenated polymer. Using the obtained hydrogenated polymer, a conductive material paste for a positive electrode, a binder composition for a positive electrode, a slurry composition for a positive electrode, a positive electrode for a secondary battery, a negative electrode for a secondary battery, and a secondary battery were produced. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0098] Comparative Example 2 A hydrogenated polymer, a conductive paste for a positive electrode, a binder composition for a positive electrode, a slurry composition for a positive electrode, a positive electrode for a secondary battery, a negative electrode for a secondary battery, and a secondary battery were produced in the same manner as in Example 1, except that the molecular weight modifier was changed to α-methylstyrene dimer during the preparation of the polymer. Various measurements and evaluations were then carried out in the same manner as in Example 1. The results are shown in Table 1.

[0099] Comparative Example 3 During the preparation of the polymer, styrene was not added, and the blending amounts of the various monomers were changed to 40 parts of acrylonitrile and 55 parts of 1,3-butadiene, respectively, and the blending amount of the mercaptan compound was changed to 0.5 parts. Except for this, a hydrogenated polymer, a conductive paste for a positive electrode, a binder composition for a positive electrode, a slurry composition for a positive electrode, a positive electrode for a secondary battery, a negative electrode for a secondary battery, and a secondary battery were produced in the same manner as in Example 1. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0100] In Table 1, "AN" stands for acrylonitrile unit. "ST" stands for styrene unit, "H-BD" is a structural unit represented by the general formula: -C2H4-, which is a 1,3-butadiene hydride unit. "BD" refers to units derived from 1,3-butadiene monomers other than H-BD. "TDM" is a mixture of compounds containing mercapto groups, including t-dodecyl mercaptan. "αMSD" is α-methylstyrene dimer, "NCM" stands for Li (Ni 0.5 Co 0.2 Mn 0.3 )O2, "PVdF" is an abbreviation for polyvinylidene fluoride. "ND" indicates not detected.

[0101] [Table 1]

[0102] From Table 1, it can be seen that the binder compositions of Examples 1 to 5 make it possible to prepare conductive material pastes having sufficiently high dispersibility of the conductive material and dispersion stability at high temperatures, and furthermore, make it possible to prepare electrodes that reduce internal resistance when used in secondary batteries. On the other hand, in Comparative Examples 1 and 2 in which the amount of residual mercaptan contained in the polymer was outside the specified range, and in Comparative Example 3 in which a polymer not containing an aromatic vinyl monomer unit was used, it was found that the excellent attributes achieved in Examples 1 to 5 could not be obtained. [Industrial Applicability]

[0103] According to the present invention, it is possible to provide a binder composition for a secondary battery electrode, which is capable of preparing a conductive material paste having sufficiently high dispersibility of a conductive material and sufficiently high dispersion stability at high temperatures. In addition, according to the present invention, it is possible to provide a conductive material paste composition for secondary battery electrodes, which has sufficiently high dispersibility of the conductive material and dispersion stability at high temperatures, and further, can produce an electrode that reduces internal resistance when a secondary battery is formed. Furthermore, according to the present invention, it is possible to provide a slurry composition for a secondary battery electrode, which is capable of producing an electrode that reduces the internal resistance of the secondary battery obtained when the secondary battery is formed. Furthermore, according to the present invention, it is possible to provide an electrode that reduces the internal resistance of a secondary battery obtained when the secondary battery is formed, and a secondary battery including such an electrode.

Claims

1. A binder composition for a secondary battery positive electrode, comprising a polymer, The polymer contains a nitrile group-containing monomer unit, an aromatic vinyl monomer unit, and a linear alkylene structural unit, In accordance with JIS K6229, the polymer is extracted with methanol and then dried to obtain a polymer to be measured, and the polymer to be measured is heated at a temperature of 150° C. for 20 minutes, the generated gas is measured by gas chromatography-mass spectrometry, and the amount of mercaptan is measured according to a calibration curve method, the obtained amount of mercaptan is 1 ppm or more and 50 ppm or less based on the mass of the polymer, In the polymer, the content ratio of the nitrile group-containing monomer unit is 5% by mass or more and 70% by mass or less, the content ratio of the aromatic vinyl monomer unit is 1% by mass or more and 50% by mass or less, and the content ratio of the linear alkylene structural unit is 10% by mass or more and 60% by mass or less. A binder composition for a secondary battery positive electrode.

2. 2. The binder composition for a secondary battery positive electrode according to claim 1, wherein the polymer has an insoluble fraction of 1 mass % or less when dissolved in N-methylpyrrolidone.

3. 3. The binder composition for a secondary battery positive electrode according to claim 1, wherein the weight average molecular weight of the polymer is 10,000 or more and 2,000,000 or less.

4. A conductive paste composition for a secondary battery positive electrode, comprising a conductive material and the binder composition for a secondary battery positive electrode according to any one of claims 1 to 3.

5. The conductive paste composition for secondary battery positive electrodes according to claim 4 , wherein the conductive material comprises carbon nanotubes.

6. A slurry composition for a secondary battery positive electrode, comprising a positive electrode active material, a solvent, and the binder composition for a secondary battery positive electrode according to any one of claims 1 to 3.

7. A positive electrode for a secondary battery, comprising a positive electrode mixture layer formed using the slurry composition for a secondary battery positive electrode according to claim 6.

8. A battery comprising a positive electrode, a negative electrode, an electrolyte, and a separator; A secondary battery, wherein the positive electrode is the positive electrode for a secondary battery according to claim 7.

Citation Information

Patent Citations

  • Solar light condensing and transmitting device

    JP1988030801A

  • Methacrylic resin composition

    JP1994228403A

  • Lithium secondary battery

    JP2004178879A

  • Acrylic syrup

    JP2010047767A

  • Binder for secondary-battery electrode

    JP2010146870A