Metallized Polyester Film
A metal-coated polyester film with a cured urethane resin and crosslinking agent composition addresses adhesion issues under high temperature and humidity, ensuring strong bonding and conductivity for applications like electromagnetic shielding and mirrors.
Patent Information
- Application Number
- JP2023037989
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-03-10
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2039-06-03
AI Technical Summary
Existing metal-coated polyester films face issues with adhesion between the metal coating layer and the film, particularly under high temperature and high humidity conditions, due to insufficient bonding.
A metal-coated polyester film with a coating layer containing a urethane resin having a polycarbonate structure, a crosslinking agent, and a polyester resin, which is cured to enhance adhesion, is developed. The composition includes specific ratios and components to improve bonding under adverse conditions.
The film exhibits excellent adhesion of the metal coating layer under high temperature and high humidity, making it suitable for applications requiring conductivity and aesthetic properties.
Smart Images

Figure 0007559858000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a metal-coated polyester film, and more particularly to a metal-coated polyester film obtained by coating a metal on a coating layer of a laminated polyester film having an easily adhesive coating layer. [Background technology]
[0002] There is a technique for providing a metal coating layer by plating the surface of a thermoplastic resin film. However, since these materials lack transparency and post-processability, their applications are limited (see, for example, Patent Documents 1 to 3).
[0003] There is a technique for providing a metal coating layer by plating the surface of the polyester film, but these techniques have a problem with the adhesion between the metal layer and the film, especially under high temperature and high humidity conditions (see, for example, Patent Documents 4 and 5). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 2-149666 [Patent Document 2] JP 2013-184425 A [Patent Document 3] JP 2015-061763 A [Patent Document 4] JP 2009-194071 A [Patent Document 5] JP 2014-160129 A Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention has been made in view of the above problems in the prior art. That is, an object of the present invention is to provide a metal-coated polyester film having excellent adhesion between a metal coating layer and the film under high temperature and high humidity conditions. [Means for solving the problem]
[0006] In the course of investigating the causes of the above problems in order to solve the above problems, the present inventors discovered that the problems of the present invention can be solved by having a coating layer on at least one side of a polyester film substrate, the coating layer being formed by curing a composition containing a crosslinking agent, a polyester resin, and a urethane resin having a polycarbonate structure, and further providing a metal coating layer by plating on the coating layer, which led to the completion of the present invention.
[0007] That is, the present invention comprises the following: 1. A metal-coated polyester film having a coating layer and a metal coating layer formed by plating on at least one surface of a polyester film substrate, in that order, the coating layer being formed by curing a composition containing a urethane resin having a polycarbonate structure, a crosslinking agent, and a polyester resin. The polyester resin is a 5-sodium sulfoisophthalic acid copolymer polyester. Metallized polyester film. 2. The metal-coated polyester film according to claim 1, wherein the urethane resin having a polycarbonate structure has a branched structure. 3. The metal-coated polyester film according to the above item 1 or 2, wherein the crosslinking agent is a compound having a tri- or higher functional blocked isocyanate group. 4. A metal-coated polyester film according to any one of claims 1 to 3, wherein the urethane resin having a polycarbonate structure is obtained by synthesizing and polymerizing a polycarbonate polyol component and a polyisocyanate component, and the mass ratio of the polycarbonate polyol component to the polyisocyanate component during the synthesis and polymerization (mass of the polycarbonate polyol component / mass of the polyisocyanate component) is 0.5 to 3. 5. The metal-coated polyester film according to any one of claims 1 to 4, wherein the content of the crosslinking agent is 5% by mass or more and 50% by mass or less when the total solid content of the polyester resin, the urethane resin having a polycarbonate structure, and the crosslinking agent is 100% by mass. 6. A metal-coated polyester film according to any one of claims 1 to 5, wherein the content of the urethane resin having a polycarbonate structure is 5% by mass or more and 50% by mass or less when the total solid content of the polyester resin, the urethane resin having a polycarbonate structure, and the crosslinking agent is 100% by mass. 7. 7. The metal-coated polyester film according to any one of claims 1 to 6, wherein the polyester resin content is 10% by mass or more and 70% by mass or less when the total solid content of the polyester resin, the urethane resin having a polycarbonate structure, and the crosslinking agent is 100% by mass. 8. The metal-coated polyester film according to any one of the above items 1 to 7, which is used for electromagnetic wave shielding, circuits, or mirrors. Effect of the Invention
[0008] The metal-coated polyester film of the present invention contains a conductive metal, and the metal coating layer has excellent adhesion even under high temperature and high humidity conditions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] (Polyester film base) In the present invention, the polyester resin constituting the polyester film substrate is polyethylene terephthalate, polybutylene terephthalate, polyethylene-2,6-naphthalate, polytrimethylene terephthalate, etc., as well as copolymerized polyester resins in which a portion of the diol component or dicarboxylic acid component of the above-mentioned polyester resins is replaced with a copolymerization component such as the following. For example, the copolymerization component may include diol components such as diethylene glycol, neopentyl glycol, 1,4-cyclohexanedimethanol, and polyalkylene glycol, and dicarboxylic acid components such as adipic acid, sebacic acid, phthalic acid, isophthalic acid, 5-sodium isophthalic acid, and 2,6-naphthalenedicarboxylic acid.
[0010] In the present invention, the polyester resin preferably used for the polyester film substrate is mainly selected from polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, and polyethylene-2,6-naphthalate. Among these polyester resins, polyethylene terephthalate is most preferable in terms of the balance between physical properties and cost. In addition, the polyester film substrate made of these polyester resins is preferably a biaxially oriented polyester film, which can improve chemical resistance, heat resistance, mechanical strength, etc.
[0011] The catalyst for polycondensation used in the production of polyester resin is not particularly limited, but antimony trioxide is suitable because it is inexpensive and has excellent catalytic activity. It is also preferable to use a germanium compound or a titanium compound. More preferable polycondensation catalysts include a catalyst containing aluminum and / or a compound thereof and a phenolic compound, a catalyst containing aluminum and / or a compound thereof and a phosphorus compound, and a catalyst containing an aluminum salt of a phosphorus compound.
[0012] In addition, the polyester film base material in the present invention is not particularly limited in terms of its layer structure, and may be a single-layer polyester film, a two-layer structure having different components, or a polyester film base material consisting of at least three layers having an outer layer and an inner layer.
[0013] (Coating layer) In the present invention, in order to improve the adhesion with the metal coating layer formed by plating, it is preferable that the coating layer on the polyester film has a coating layer formed by curing a composition containing a urethane resin having a polycarbonate structure, a crosslinking agent, and a polyester resin on at least one side of the polyester film. The coating layer is considered to be formed by curing a urethane resin or polyester resin having a polycarbonate structure crosslinked by a crosslinking agent, but since it is difficult to express the crosslinked chemical structure itself, it is expressed as being formed by curing a composition containing a urethane resin having a polycarbonate structure, a crosslinking agent, and a polyester resin. The coating layer may be provided on both sides of the polyester film, or may be provided on only one side of the polyester film, and a different resin coating layer may be provided on the other side. It is more preferable that the urethane resin having a polycarbonate structure has a branched structure in the molecular chain.
[0014] The composition of each coating layer will be described in detail below. (Urethane resin with polycarbonate structure) The urethane resin having a polycarbonate structure in the present invention preferably has a urethane bond portion derived from at least a polycarbonate polyol component and a polyisocyanate component, and more preferably has a branched structure. The urethane resin having a polycarbonate structure in the present invention contains a chain extender as necessary. The branched structure referred to here is preferably introduced by forming a branched molecular chain structure after synthesis and polymerization due to the presence of three or more terminal functional groups in any of the raw material components constituting the molecular chain.
[0015] In the present invention, the urethane resin having a polycarbonate structure preferably has 3 to 6 terminal functional groups in the molecular chain due to its branched structure, since the resin can be stably dispersed in an aqueous solution and blocking resistance can be improved.
[0016] The lower limit of the mass ratio of the polycarbonate polyol component to the polyisocyanate component (mass of the polycarbonate polyol component / mass of the polyisocyanate component) when synthesizing and polymerizing the urethane resin having a polycarbonate structure in the present invention is preferably 0.5, more preferably 0.6, even more preferably 0.7, particularly preferably 0.8, and most preferably 1.0. If it is 0.5 or more, adhesion to UV ink can be improved, which is preferable. The upper limit of the mass ratio of the polycarbonate polyol component to the polyisocyanate component when synthesizing and polymerizing the urethane resin having a polycarbonate structure in the present invention is preferably 3.0, more preferably 2.2, even more preferably 2.0, particularly preferably 1.7, and most preferably 1.5. If it is 3.0 or less, blocking resistance can be improved, which is preferable.
[0017] The polycarbonate polyol component used for synthesizing and polymerizing the urethane resin having a polycarbonate structure in the present invention preferably contains an aliphatic polycarbonate polyol having excellent heat resistance and hydrolysis resistance. Examples of the aliphatic polycarbonate polyol include an aliphatic polycarbonate diol and an aliphatic polycarbonate triol, and the aliphatic polycarbonate diol is preferably used. Examples of the aliphatic polycarbonate diol used for synthesizing and polymerizing the urethane resin having a polycarbonate structure in the present invention include aliphatic polycarbonate diols obtained by reacting one or more diols such as ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, 1,8-nonanediol, neopentyl glycol, diethylene glycol, and dipropylene glycol with carbonates such as dimethyl carbonate, ethylene carbonate, and phosgene.
[0018] The number average molecular weight of the polycarbonate polyol in the present invention is preferably 1000 to 3000, more preferably 1200 to 2900, and most preferably 1500 to 2800. When it is 1000 or more, the adhesion to the metal coating layer can be improved, which is preferable. When it is 3000 or less, the blocking resistance can be improved, which is preferable.
[0019] Examples of polyisocyanates used in the synthesis and polymerization of the urethane resin having a polycarbonate structure in the present invention include aromatic aliphatic diisocyanates such as xylylene diisocyanate, alicyclic diisocyanates such as isophorone diisocyanate, 4,4-dicyclohexylmethane diisocyanate, and 1,3-bis(isocyanatomethyl)cyclohexane, aliphatic diisocyanates such as hexamethylene diisocyanate and 2,2,4-trimethylhexamethylene diisocyanate, and polyisocyanates in which one or more of these compounds are added to trimethylolpropane or the like in advance. When the aromatic aliphatic diisocyanates, alicyclic diisocyanates, or aliphatic diisocyanates are used, there is no problem of yellowing, which is preferable. In addition, the coating film does not become too hard, and the stress caused by the heat shrinkage of the polyester film substrate can be alleviated, and the adhesion becomes good, which is preferable.
[0020] Examples of chain extenders include glycols such as ethylene glycol, diethylene glycol, 1,4-butanediol, neopentyl glycol, and 1,6-hexanediol; polyhydric alcohols such as glycerin, trimethylolpropane, and pentaerythritol; diamines such as ethylenediamine, hexamethylenediamine, and piperazine; amino alcohols such as monoethanolamine and diethanolamine; thiodiglycols such as thiodiethylene glycol; and water.
[0021] In order to form a branched structure in the urethane resin, for example, a method can be preferably adopted in which the polycarbonate polyol component, polyisocyanate, and chain extender are reacted at an appropriate temperature for an appropriate time, and then a compound having a tri- or higher functional hydroxyl group or isocyanate group is added and the reaction is allowed to proceed further.
[0022] Specific examples of compounds having three or more functional hydroxyl groups include caprolactone triol, glycerol, trimethylolpropane, butane triol, hexane triol, 1,2,3-hexane triol, 1,2,3-pentane triol, 1,3,4-hexane triol, 1,3,4-pentane triol, 1,3,5-hexane triol, 1,3,5-pentane triol, polyether triol, etc. Examples of the polyether triol include compounds obtained by addition polymerization of one or more monomers such as ethylene oxide, propylene oxide, butylene oxide, amylene oxide, glycidyl ether, methyl glycidyl ether, t-butyl glycidyl ether, and phenyl glycidyl ether, using one or more compounds having three active hydrogens, such as alcohols such as glycerin and trimethylolpropane, and diethylenetriamine, as initiators.
[0023] A specific example of a compound having a trifunctional or higher isocyanate group may be a polyisocyanate compound having at least three isocyanate (NCO) groups in one molecule. In the present invention, the trifunctional or higher isocyanate compound may be a biuret, a nurate, an adduct, or the like, which is a modified isocyanate monomer having two isocyanate groups, such as an aromatic diisocyanate, an aliphatic diisocyanate, an araliphatic diisocyanate, or an alicyclic diisocyanate. Examples of aromatic diisocyanates include 1,3-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,4-phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-toluidine diisocyanate, dianisidine diisocyanate, and 4,4'-diphenyl ether diisocyanate. Examples of the aliphatic diisocyanate include trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1,2-propylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, dodecamethylene diisocyanate, and 2,4,4-trimethylhexamethylene diisocyanate. Examples of the aralkyl diisocyanate include xylylene diisocyanate, ω,ω'-diisocyanate-1,4-diethylbenzene, 1,4-tetramethylxylylene diisocyanate, and 1,3-tetramethylxylylene diisocyanate. Examples of alicyclic diisocyanates include 3-isocyanatemethyl-3,5,5-trimethylcyclohexyl isocyanate (also known as IPDI, isophorone diisocyanate), 1,3-cyclopentane diisocyanate, 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, methyl-2,4-cyclohexane diisocyanate, methyl-2,6-cyclohexane diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), and 1,4-bis(isocyanatemethyl)cyclohexane. The biuret form is a self-condensation product having a biuret bond formed by the self-condensation of an isocyanate monomer, and an example of such a product is a biuret form of hexamethylene diisocyanate. The nurate form is a trimer of an isocyanate monomer, and examples thereof include a trimer of hexamethylene diisocyanate, a trimer of isophorone diisocyanate, and a trimer of tolylene diisocyanate. The adduct refers to a tri- or higher functional isocyanate compound obtained by reacting the above-mentioned isocyanate monomer with a tri- or higher functional low-molecular-weight active hydrogen-containing compound. Examples of the adduct include a compound obtained by reacting trimethylolpropane with hexamethylene diisocyanate, a compound obtained by reacting trimethylolpropane with tolylene diisocyanate, a compound obtained by reacting trimethylolpropane with xylylene diisocyanate, and a compound obtained by reacting trimethylolpropane with isophorone diisocyanate.
[0024] Examples of chain extenders having three or more functional groups include trimethylolpropane and alcohols having three or more hydroxyl groups such as pentaerythritol, which are described above as chain extenders.
[0025] The coating layer in the present invention is preferably provided by an in-line coating method described below using a water-based coating liquid. Therefore, it is desirable that the urethane resin of the present invention is water-soluble or water-dispersible. The above-mentioned "water-soluble or water-dispersible" means that it is dispersible in water or an aqueous solution containing less than 50 mass% of a water-soluble organic solvent.
[0026] To impart water dispersibility to urethane resins, sulfonic acid (salt) groups or carboxylic acid (salt) groups can be introduced (copolymerized) into the urethane molecular structure. To maintain moisture resistance, it is preferable to introduce a weakly acidic carboxylic acid (salt) group. It is also possible to introduce a nonionic group such as a polyoxyalkylene group.
[0027] In order to introduce a carboxylic acid (salt) group into a urethane resin, for example, a polyol compound having a carboxylic acid group, such as dimethylolpropanoic acid or dimethylolbutanoic acid, is introduced as a copolymerization component as a polyol component, and neutralized with a salt-forming agent. Specific examples of salt-forming agents include ammonia, trialkylamines such as trimethylamine, triethylamine, triisopropylamine, tri-n-propylamine, and tri-n-butylamine, N-alkylmorpholines such as N-methylmorpholine and N-ethylmorpholine, and N-dialkylalkanolamines such as N-dimethylethanolamine and N-diethylethanolamine. These can be used alone or in combination of two or more kinds.
[0028] When a polyol compound having a carboxylic acid (salt) group is used as a copolymerization component to impart water dispersibility, the molar ratio of the polyol compound having a carboxylic acid (salt) group in the urethane resin is preferably 3 to 60 mol%, and more preferably 5 to 40 mol%, when the total polyisocyanate components of the urethane resin are taken as 100 mol%. When the molar ratio is 3 mol% or more, water dispersibility is obtained, which is preferable. Also, when the molar ratio is 60 mol% or less, water resistance is maintained and moist heat resistance is obtained, which is preferable.
[0029] The urethane resin of the present invention may have a blocked isocyanate structure at the end to improve hardness.
[0030] (Crosslinking agent) In the present invention, the crosslinking agent contained in the coating layer forming composition is preferably a blocked isocyanate, more preferably a trifunctional or higher blocked isocyanate, and particularly preferably a tetrafunctional or higher blocked isocyanate. These improve blocking resistance and adhesion to the hard coat layer. The number of isocyanate functional groups is preferably 8 or less, more preferably 6 or less.
[0031] The lower limit of the NCO equivalent of the blocked isocyanate is preferably 100, more preferably 120, even more preferably 130, particularly preferably 140, and most preferably 150. If the NCO equivalent is 100 or more, there is no risk of the coating cracking occurring, which is preferable. The upper limit of the NCO equivalent is preferably 500, more preferably 400, even more preferably 380, particularly preferably 350, and most preferably 300. If the NCO equivalent is 500 or less, blocking resistance is maintained, which is preferable.
[0032] The lower limit of the boiling point of the blocking agent of the blocked isocyanate is preferably 150°C, more preferably 160°C, even more preferably 180°C, particularly preferably 200°C, and most preferably 210°C. The higher the boiling point of the blocking agent, the more the volatilization of the blocking agent is suppressed even by the drying process after coating of the coating liquid or by heat addition in the film forming process in the case of the in-line coating method, the occurrence of minute unevenness on the coated surface is suppressed, and the transparency of the film is improved. The upper limit of the boiling point of the blocking agent is not particularly limited, but it is thought that the upper limit is about 300°C from the viewpoint of productivity. Since the boiling point is related to the molecular weight, in order to increase the boiling point of the blocking agent, it is preferable to use a blocking agent with a large molecular weight, and the molecular weight of the blocking agent is preferably 50 or more, more preferably 60 or more, and even more preferably 80 or more.
[0033] The upper limit of the dissociation temperature of the blocking agent is preferably 200°C, more preferably 180°C, even more preferably 160°C, particularly preferably 150°C, and most preferably 120°C. The blocking agent dissociates from the functional group by heat addition in the drying process after application of the coating liquid or in the case of the in-line coating method in the film formation process, and a regenerated isocyanate group is generated. Therefore, the crosslinking reaction with urethane resin etc. progresses, and the adhesiveness is improved. When the dissociation temperature of the blocked isocyanate is the above temperature or lower, the dissociation of the blocking agent progresses sufficiently, and the adhesiveness, especially the wet heat resistance, is good.
[0034] Examples of blocking agents having a dissociation temperature of 120° C. or less and a boiling point of 150° C. or more for use in the blocked isocyanate of the present invention include bisulfite compounds such as sodium bisulfite, pyrazole compounds such as 3,5-dimethylpyrazole, 3-methylpyrazole, 4-bromo-3,5-dimethylpyrazole, 4-nitro-3,5-dimethylpyrazole, active methylene compounds such as malonic acid diesters (dimethyl malonate, diethyl malonate, di-n-butyl malonate, di-2-ethylhexyl malonate), methyl ethyl ketone, etc., and triazole compounds such as 1,2,4-triazole. Among these, pyrazole compounds are preferred from the viewpoints of wet heat resistance and yellowing.
[0035] The trifunctional or higher polyisocyanate, which is a precursor of the blocked isocyanate of the present invention, can be suitably obtained by introducing an isocyanate monomer, for example, a biuret, a nurate, an adduct, etc., which are modified from an isocyanate monomer such as an aromatic diisocyanate, an aliphatic diisocyanate, an araliphatic diisocyanate, or an alicyclic diisocyanate having two isocyanate groups. The biuret form is a self-condensation product having a biuret bond formed by the self-condensation of an isocyanate monomer, and an example of such a product is a biuret form of hexamethylene diisocyanate. The nurate form is a trimer of an isocyanate monomer, and examples thereof include a trimer of hexamethylene diisocyanate, a trimer of isophorone diisocyanate, and a trimer of tolylene diisocyanate. The adduct refers to a tri- or higher functional isocyanate compound obtained by reacting an isocyanate monomer with a tri- or higher functional low-molecular-weight active hydrogen-containing compound, and examples thereof include a compound obtained by reacting trimethylolpropane with hexamethylene diisocyanate, a compound obtained by reacting trimethylolpropane with tolylene diisocyanate, a compound obtained by reacting trimethylolpropane with xylylene diisocyanate, and a compound obtained by reacting trimethylolpropane with isophorone diisocyanate.
[0036] The isocyanate monomers include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 1,5-naphthylene diisocyanate, 1,4-naphthylene diisocyanate, phenylene diisocyanate, tetramethylxylylene diisocyanate, 4,4'-diphenylether diisocyanate, 2-nitrodiphenyl-4,4'-diisocyanate, 2,2'-diphenylpropane-4,4'-diisocyanate, 3,3' Examples of the diisocyanates include aromatic diisocyanates such as 4,4'-dimethyldiphenylmethane-4,4'-diisocyanate, 4,4'-diphenylpropane diisocyanate, and 3,3'-dimethoxydiphenyl-4,4'-diisocyanate, aromatic aliphatic diisocyanates such as xylylene diisocyanate, alicyclic diisocyanates such as isophorone diisocyanate, 4,4-dicyclohexylmethane diisocyanate, and 1,3-bis(isocyanatemethyl)cyclohexane, and aliphatic diisocyanates such as hexamethylene diisocyanate and 2,2,4-trimethylhexamethylene diisocyanate. From the viewpoints of transparency, adhesion, and resistance to moist heat, aliphatic and alicyclic isocyanates and their modified products are preferred, and are preferred for optical applications that require no yellowing and high transparency.
[0037] The blocked isocyanate of the present invention can introduce a hydrophilic group into the precursor polyisocyanate in order to impart water solubility or water dispersibility. Examples of hydrophilic groups include (1) quaternary ammonium salts of dialkylamino alcohols and quaternary ammonium salts of dialkylaminoalkylamines, (2) sulfonates, carboxylates, phosphates, and (3) polyethylene glycols and polypropylene glycols one-end-blocked with an alkyl group. When a hydrophilic moiety is introduced, the isocyanate becomes (1) cationic, (2) anionic, or (3) nonionic. Among them, since many other water-soluble resins are anionic, anionic or nonionic is preferred because they are easily compatible. In addition, anionic is highly compatible with other resins, and nonionic is preferred because it does not have an ionic hydrophilic group, in order to improve resistance to moist heat.
[0038] The anionic hydrophilic group is preferably one having a hydroxyl group for introduction into polyisocyanate and a carboxylic acid group for imparting hydrophilicity. Examples include glycolic acid, lactic acid, tartaric acid, citric acid, oxybutyric acid, oxyvaleric acid, hydroxypivalic acid, dimethylolacetic acid, dimethylolpropanoic acid, dimethylolbutanoic acid, and polycaprolactone having a carboxylic acid group. To neutralize the carboxylic acid group, an organic amine compound is preferred. Examples of the amine include linear or branched primary, secondary or tertiary amines having 1 to 20 carbon atoms, such as ammonia, methylamine, ethylamine, propylamine, isopropylamine, butylamine, 2-ethylhexylamine, cyclohexylamine, dimethylamine, diethylamine, dipropylamine, diisopropylamine, dibutylamine, trimethylamine, triethylamine, triisopropylamine, tributylamine, and ethylenediamine; cyclic amines, such as morpholine, N-alkylmorpholine, and pyridine; and hydroxyl group-containing amines, such as monoisopropanolamine, methylethanolamine, methylisopropanolamine, dimethylethanolamine, diisopropanolamine, diethanolamine, triethanolamine, diethylethanolamine, and triethanolamine.
[0039] As the nonionic hydrophilic group, the repeating units of ethylene oxide and / or propylene oxide of polyethylene glycol or polypropylene glycol capped at one end with an alkyl group are preferably 3 to 50, more preferably 5 to 30. If the repeating units are small, the compatibility with the resin is poor and the haze increases, and if they are large, the adhesiveness under high temperature and high humidity may decrease. In order to improve the water dispersibility, the blocked isocyanate of the present invention may be added with a nonionic, anionic, cationic or amphoteric surfactant. For example, surfactants such as polyethylene glycol, polyhydric alcohol fatty acid ester, etc., anionic fatty acid salt, alkyl sulfate ester, alkylbenzene sulfonate, sulfosuccinate, alkyl phosphate, etc., cationic alkylamine salt, alkylbetaine, etc., carboxylate amine salt, sulfonate amine salt, sulfate ester salt, etc. may be mentioned.
[0040] In addition to water, a water-soluble organic solvent may be contained. For example, the organic solvent used in the reaction may be removed and another organic solvent may be added.
[0041] (polyester resin) The polyester resin used to form the coating layer in the present invention may be a straight-chain one, but is more preferably a polyester resin composed of a dicarboxylic acid and a diol having a branched structure. The dicarboxylic acid referred to here includes aliphatic dicarboxylic acids such as adipic acid and sebacic acid, and aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, and 2,6-naphthalenedicarboxylic acid, as well as terephthalic acid, isophthalic acid, phthalic acid, and 2,6-naphthalenedicarboxylic acid. The branched glycol is a diol having a branched alkyl group, and examples thereof include 2,2-dimethyl-1,3-propanediol, 2-methyl-2-ethyl-1,3-propanediol, 2-methyl-2-butyl-1,3-propanediol, 2-methyl-2-propyl-1,3-propanediol, 2-methyl-2-isopropyl-1,3-propanediol, 2-methyl-2-n-hexyl-1,3-propanediol, 2,2-diethyl-1,3-propanediol, 2-ethyl-2-n-butyl-1,3-propanediol, 2-ethyl-2-n-hexyl-1,3-propanediol, 2,2-di-n-butyl-1,3-propanediol, 2-n-butyl-2-propyl-1,3-propanediol, and 2,2-di-n-hexyl-1,3-propanediol.
[0042] It can be said that the polyester resin contains the branched glycol component, which is a more preferred embodiment of the above, in the total glycol components at a ratio of preferably 10 mol % or more, more preferably 20 mol % or more. If it is 10 mol % or more, the crystallinity is not too high, and the adhesiveness of the coating layer is good, which is preferable. The upper limit of the glycol component in the total glycol components is preferably 80 mol % or less, more preferably 70 mass %. If it is 80 mol % or less, the concentration of oligomers, which are by-products, is unlikely to increase, and the transparency of the coating layer is good, which is preferable. As the glycol component other than the above compounds, ethylene glycol is the most preferable. If it is a small amount, diethylene glycol, propylene glycol, butanediol, hexanediol, or 1,4-cyclohexanedimethanol may be used.
[0043] The dicarboxylic acid as a component of the polyester resin is most preferably terephthalic acid or isophthalic acid. In addition to the dicarboxylic acid, in order to impart water dispersibility to the copolymerized polyester resin, it is preferable to copolymerize 5-sulfoisophthalic acid or the like in the range of 1 to 10 mol%, for example, sulfoterephthalic acid, 5-sulfoisophthalic acid, 5-sodium sulfoisophthalic acid, etc. A polyester resin containing a dicarboxylic acid having a naphthalene skeleton may be used, but in order to suppress a decrease in adhesion to UV ink, the quantitative ratio is preferably 5 mol% or less in the total carboxylic acid components, and it may not be used.
[0044] When the total solid content of the polyester resin, the urethane resin having a polycarbonate structure, and the crosslinking agent in the coating liquid is 100% by mass, the lower limit of the content of the crosslinking agent is preferably 5% by mass, more preferably 7% by mass, even more preferably 10% by mass, and most preferably 12% by mass. If it is 5% by mass or more, blocking resistance can be improved, which is preferable. The upper limit of the content of the crosslinking agent is preferably 50% by mass, more preferably 40% by mass, even more preferably 35% by mass, and most preferably 30% by mass. If it is 50% by mass or less, transparency is high, which is preferable.
[0045] When the total solid content of the polyester resin, the urethane resin having a polycarbonate structure, and the crosslinking agent in the coating liquid is 100% by mass, the lower limit of the content of the urethane resin having a polycarbonate structure is preferably 5% by mass. If it is 5% by mass or more, adhesion to UV ink can be improved, which is preferable. The upper limit of the content of the urethane resin having a polycarbonate structure is preferably 50% by mass, more preferably 40% by mass, even more preferably 30% by mass, and most preferably 20% by mass. If the content of the urethane resin is 50% by mass or less, blocking resistance can be improved, which is preferable.
[0046] When the total solid content of the polyester resin, urethane resin and crosslinking agent in the coating solution is 100% by mass, the lower limit of the polyester resin content is preferably 10% by mass, more preferably 20% by mass, even more preferably 30% by mass, particularly preferably 35% by mass, and most preferably 40% by mass. If the polyester resin content is 10% by mass or more, the adhesion between the coating layer and the polyester film substrate becomes good, which is preferable. The upper limit of the polyester resin content is preferably 70% by mass, more preferably 67% by mass, even more preferably 65% by mass, particularly preferably 62% by mass, and most preferably 60% by mass. If the polyester resin content is 70% by mass or less, the moist heat resistance becomes good, which is preferable.
[0047] (Additives) In the coating layer of the present invention, known additives such as surfactants, antioxidants, heat stabilizers, weather stabilizers, ultraviolet absorbers, organic lubricants, pigments, dyes, organic or inorganic particles, antistatic agents, nucleating agents, etc. may be added within the range that does not impair the effects of the present invention.
[0048] In the present invention, in order to further improve the blocking resistance of the coating layer, it is also a preferred embodiment to add particles to the coating layer.The particles contained in the coating layer in the present invention include, for example, titanium oxide, barium sulfate, calcium carbonate, calcium sulfate, silica, alumina, talc, kaolin, clay, etc., or mixtures thereof, and further include inorganic particles such as calcium phosphate, mica, hectorite, zirconia, tungsten oxide, lithium fluoride, calcium fluoride, etc., used in combination, and organic polymer particles such as styrene-based, acrylic-based, melamine-based, benzoguanamine-based, silicone-based, etc.
[0049] The average particle size of the particles in the coating layer (average particle size based on the number of particles as measured by a scanning electron microscope (SEM) (hereinafter the same)) is preferably 0.04 to 2.0 μm, and more preferably 0.1 to 1.0 μm. When the average particle size of the inactive particles is 0.04 μm or more, it is easy to form irregularities on the film surface, which improves the handling properties such as the slipperiness and winding properties of the film, and the processability during lamination is good, which is preferable. On the other hand, when the average particle size of the inactive particles is 2.0 μm or less, it is preferable that the particles are less likely to fall off. The particle concentration in the coating layer is preferably 1 to 20 mass % of the solid components.
[0050] The average particle size of the particles was measured by observing the particles on the cross section of the laminated polyester film with a scanning electron microscope, observing 30 particles, and taking the average value as the average particle size.
[0051] As long as the object of the present invention is satisfied, the shape of the particles is not particularly limited, and spherical particles and irregular non-spherical particles can be used. The particle size of irregular particles can be calculated as the circle equivalent diameter. The circle equivalent diameter is the value obtained by dividing the observed particle area by π, calculating the square root, and multiplying it by two.
[0052] (Manufacture of laminated polyester film) In the present invention, it is preferable to produce a laminated polyester film having a coating layer on a polyester film substrate, and then provide a metal coating layer on the coating layer by plating. Hereinafter, a film having a coating layer on a polyester film substrate may be referred to as a "laminated polyester film". The method for producing a laminated polyester film will be described using an example in which a polyethylene terephthalate (hereinafter sometimes abbreviated as PET) film substrate is used, but the method is not limited thereto.
[0053] After thoroughly drying the PET resin in a vacuum, it is fed to an extruder, and the molten PET resin at about 280°C is extruded from a T-die into a sheet shape onto a rotating cooling roll, and cooled and solidified by an electrostatic application method to obtain an unstretched PET sheet. The unstretched PET sheet may be a single layer structure or a multilayer structure formed by a coextrusion method.
[0054] The obtained unstretched PET sheet is uniaxially or biaxially stretched to obtain a uniaxially stretched PET film. For example, in the case of biaxial stretching, the film is stretched 2.5 to 5.0 times in the longitudinal direction with a roll heated to 80 to 120°C to obtain a uniaxially stretched PET film, and the ends of the film are held with clips and introduced into a hot air zone heated to 80 to 180°C, where it is stretched 2.5 to 5.0 times in the width direction. In the case of uniaxial stretching, the film is stretched 2.5 to 5.0 times in a tenter. After stretching, the film is introduced into a heat treatment zone and heat-treated to complete the crystal orientation.
[0055] The lower limit of the temperature of the heat treatment zone is preferably 170°C, more preferably 180°C. When the temperature of the heat treatment zone is 170°C or higher, curing is sufficient, blocking properties in the presence of liquid water are good, and it is preferable, and there is no need to extend the drying time. On the other hand, the upper limit of the temperature of the heat treatment zone is preferably 230°C, more preferably 200°C. When the temperature of the heat treatment zone is 230°C or lower, there is no risk of the physical properties of the film being deteriorated, which is preferable.
[0056] The coating layer can be provided after or during the film production process. In particular, from the viewpoint of productivity, it is preferable to form a coating layer by applying a coating liquid to at least one side of an unstretched or uniaxially stretched PET film at any stage of the film production process.
[0057] The coating solution can be applied to the PET film by any known method. For example, reverse roll coating, gravure coating, kiss coating, die coater, roll brush, spray coating, air knife coating, wire bar coating, pipe doctor, impregnation coating, curtain coating, etc. These methods can be used alone or in combination.
[0058] In the present invention, the thickness of the coating layer can be appropriately set in the range of 0.001 to 2.00 μm, but in order to achieve both processability and adhesiveness, the range is preferably 0.01 to 1.00 μm, more preferably 0.02 to 0.80 μm, and even more preferably 0.05 to 0.50 μm. If the thickness of the coating layer is 0.001 μm or more, the adhesiveness is good, which is preferable. If the thickness of the coating layer is 2.00 μm or less, blocking is less likely to occur, which is preferable.
[0059] The upper limit of the haze of the laminated polyester film in the present invention is preferably 1.5%, more preferably 1.3%, even more preferably 1.2%, and particularly preferably 1.0%. The lower the haze, the better, and ideally 0% is most preferable, but 0.1% or more is acceptable, and even 0.3% or more is practically no problem. It is preferable that the laminated polyester film before the metal coating layer is provided by plating has a haze of 1.5% or less, since this is related to the smoothness of the coating layer surface of the laminated polyester film, and it is possible to impart a beautiful luster to the metal-coated polyester film having the coating layer provided with the metal coating layer by plating.
[0060] (metallized polyester film) The metal coating layer in the present invention is obtained by plating. For the plating, known methods such as those described in Patent Documents 1 to 5 can be used. Metals that can be used in electrolytic plating to provide conductivity include gold, silver, copper, zinc, and iron. Copper is preferred from the standpoint of cost and functionality.
[0061] The laminated polyester film has a coating layer, which provides excellent adhesion between the metal coating layer and the laminated polyester film, particularly under high temperature and high humidity. After a metal coating layer is formed on the coating layer of the laminated polyester film by plating, the film is left at 85°C and 85% RH for 24 hours, and then at 23°C and 65% RH for 12 hours. When a Cellophane Tape (registered trademark) peel test is performed, the metal coating layer does not peel off and has sufficient adhesion strength.
[0062] Incidentally, the expression "metal coating layer formed by plating" may be considered as a so-called product-by-process expression, but this expression, like "coating layer," is considered to be a generally established concept for expressing structure and characteristics, and since there is no other concise way of expressing the structure and characteristics of the obtained product, this expression is used in the present invention.
[0063] The metal-coated polyester film of the present invention is used for electromagnetic wave shielding and circuits because the metal-coated layer has electrical conductivity, and can also be used for mirrors because of its beautiful luster. EXAMPLES
[0064] The present invention will now be described in detail with reference to examples and comparative examples, but the present invention is not limited to the following examples. First, the evaluation methods used in the present invention will be described below.
[0065] (1) Hayes The haze of the laminated polyester film having a coating layer on a polyester film substrate and before a metal coating layer was provided thereon was measured using a turbidity meter (NDH5000, manufactured by Nippon Denshoku Corporation) in accordance with JISK 7136:2000.
[0066] (2) Adhesion of metal coating layer under high temperature and humidity The metal-coated polyester film was used as a sample, and was left at 85°C and 85% RH for 24 hours, and then left at 23°C and 65% RH. Next, a cutter guide with a gap of 2 mm was used to make 100 grid-shaped cuts on the metal-coated layer surface, penetrating the metal-coated layer and reaching the coating layer. Next, cellophane adhesive tape (manufactured by Nichiban, No. 405; 24 mm wide) was attached to the grid-shaped cut surface, and rubbed with an eraser to completely adhere it. After that, the cellophane adhesive tape was peeled vertically from the metal-coated polyester film, and the number of squares peeled off from the metal-coated polyester film surface was counted visually, and the adhesion between the metal-coated layer and the coating layer of the laminated polyester film was calculated using the following formula. Note that the squares that were partially peeled off were also counted as peeled off squares. The adhesion of the metal-coated layer was considered to pass if it was 100(%). Adhesion of metal coating layer under high temperature and humidity (%) = 100 - (number of peeled squares)
[0067] (3) Method for measuring number average molecular weight of polycarbonate polyol When a urethane resin having a polycarbonate structure is measured by proton nuclear magnetic resonance spectroscopy (1H-NMR), a peak derived from a methylene group adjacent to an OCOO bond is observed at around 4.1 ppm. In addition, a peak derived from a methylene group adjacent to a urethane bond generated by the reaction of a polyisocyanate with a polycarbonate polyol is observed about 0.2 ppm higher than the peak. The number average molecular weight of the polycarbonate polyol was calculated from the integral value of these two peaks and the molecular weight of the monomer that constitutes the polycarbonate polyol.
[0068] (Polymerization of urethane resin A-1 having a polycarbonate structure) Into a four-neck flask equipped with a stirrer, a Dimroth condenser, a nitrogen inlet tube, a silica gel drying tube, and a thermometer, 27.5 parts by mass of hydrogenated m-xylylene diisocyanate, 6.5 parts by mass of dimethylolpropanoic acid, 61 parts by mass of polyhexamethylene carbonate diol having a number average molecular weight of 1800, 5 parts by mass of neopentyl glycol, and 84.00 parts by mass of acetone as a solvent were added, and the mixture was stirred for 3 hours at 75°C under a nitrogen atmosphere, and it was confirmed that the reaction liquid reached a predetermined amine equivalent. Next, 2.2 parts by mass of trimethylolpropane were added, and the mixture was stirred for 1 hour at 75°C under a nitrogen atmosphere, and it was confirmed that the reaction liquid reached a predetermined amine equivalent. After lowering the temperature of this reaction liquid to 40°C, 5.17 parts by mass of triethylamine were added to obtain a polyurethane prepolymer solution. Next, 450g of water was added to a reaction vessel equipped with a homodisper capable of high-speed stirring, and the temperature was adjusted to 25°C, and the mixture was stirred for 2000min. -1 The polyurethane prepolymer solution was added while stirring and mixing at 40° C., and dispersed in water. Then, the acetone and a part of the water were removed under reduced pressure to prepare a water-dispersible urethane resin solution (A-1) with a solid content of 34% by mass.
[0069] (Polymerization of urethane resin A-2 having a polycarbonate structure) Into a four-neck flask equipped with a stirrer, a Dimroth condenser, a nitrogen inlet tube, a silica gel drying tube, and a thermometer, 25 parts by mass of 4,4-dicyclohexylmethane diisocyanate, 5 parts by mass of dimethylolpropanoic acid, 52 parts by mass of polyhexamethylene carbonate diol having a number average molecular weight of 2600, 6 parts by mass of neopentyl glycol, and 84.00 parts by mass of acetone as a solvent were added, and the mixture was stirred for 3 hours at 75°C under a nitrogen atmosphere, and it was confirmed that the reaction liquid reached a predetermined amine equivalent. Next, 10 parts by mass of a polyisocyanate compound having an isocyanurate structure made from hexamethylene diisocyanate (manufactured by Asahi Kasei Chemicals, Duranate TPA, trifunctional) was added, and the mixture was stirred for 1 hour at 75°C under a nitrogen atmosphere, and it was confirmed that the reaction liquid reached a predetermined amine equivalent. Thereafter, the reaction liquid temperature was lowered to 50°C, and 4 parts by mass of methyl ethyl ketoxime was added dropwise. After the temperature of this reaction liquid was lowered to 40°C, 5.17 parts by mass of triethylamine was added to obtain a polyurethane prepolymer solution. Next, 450g of water was added to a reaction vessel equipped with a homodisperser capable of high speed stirring, and the temperature was adjusted to 25°C. The polyurethane prepolymer solution was added while stirring and mixing at 2000 min-1 to disperse in water. Then, acetone and a part of the water were removed under reduced pressure to prepare a water-dispersible urethane resin solution (A-2) with a solid content of 35% by mass.
[0070] (Polymerization of urethane resin A-3 having a polycarbonate structure) Into a four-neck flask equipped with a stirrer, a Dimroth condenser, a nitrogen inlet tube, a silica gel drying tube, and a thermometer, 22 parts by mass of 4,4-dicyclohexylmethane diisocyanate, 20 parts by mass of polyethylene glycol monomethyl ether having a number average molecular weight of 700, 53 parts by mass of polyhexamethylene carbonate diol having a number average molecular weight of 2100, 5 parts by mass of neopentyl glycol, and 84.00 parts by mass of acetone as a solvent were added, and the mixture was stirred for 3 hours at 75°C under a nitrogen atmosphere, and it was confirmed that the reaction liquid reached a predetermined amine equivalent. Next, 9 parts by mass of a polyisocyanate compound having an isocyanurate structure made from hexamethylene diisocyanate as a raw material (Asahi Kasei Chemicals, Duranate TPA, trifunctional) were added, and the mixture was stirred for 1 hour at 75°C under a nitrogen atmosphere, and it was confirmed that the reaction liquid reached a predetermined amine equivalent. Thereafter, the reaction liquid temperature was lowered to 50°C, and 4 parts by mass of methyl ethyl ketoxime was added dropwise. After the reaction solution was cooled to 40° C., a polyurethane prepolymer solution was obtained. Next, 450 g of water was added to a reaction vessel equipped with a homodisperser capable of high speed stirring, and the temperature was adjusted to 25° C. and stirred for 2000 min. -1 The polyurethane prepolymer solution was added while stirring and mixing at 40° C. to disperse the mixture in water. Then, the acetone and a portion of the water were removed under reduced pressure to prepare a water-dispersible urethane resin solution (A-3) with a solid content of 35% by mass.
[0071] (Polymerization of urethane resin A-4 having a polycarbonate structure) 22 parts by mass of 4,4-dicyclohexylmethane diisocyanate, 3 parts by mass of dimethylol butanoic acid, 74 parts by mass of polyhexamethylene carbonate diol having a number average molecular weight of 2000, 1 part by mass of neopentyl glycol, and 84.00 parts by mass of acetone as a solvent were added to a four-neck flask equipped with a stirrer, a Dimroth condenser, a nitrogen inlet tube, a silica gel drying tube, and a thermometer, and the mixture was stirred for 3 hours at 75°C under a nitrogen atmosphere, and it was confirmed that the reaction liquid reached a predetermined amine equivalent. Next, 2 parts by mass of trimethylolpropane were added, and the mixture was stirred for 1 hour at 75°C under a nitrogen atmosphere, and it was confirmed that the reaction liquid reached a predetermined amine equivalent. Next, the reaction liquid was cooled to 40°C, and then 8.77 parts by mass of triethylamine was added to obtain a polyurethane prepolymer solution. Next, 450 g of water was added to a reaction vessel equipped with a homodisper capable of high-speed stirring, and the temperature was adjusted to 25°C, and the mixture was stirred for 2000 min. -1 The polyurethane prepolymer solution was added while stirring and mixing at 40° C. to disperse the mixture in water. Then, the acetone and part of the water were removed under reduced pressure to prepare a water-dispersible urethane resin solution (A-4) with a solid content of 34% by mass.
[0072] (Polymerization of urethane resin A-5 having a polycarbonate structure) Into a four-neck flask equipped with a stirrer, a Dimroth condenser, a nitrogen inlet tube, a silica gel drying tube, and a thermometer, 47 parts by mass of 4,4-dicyclohexylmethane diisocyanate, 21 parts by mass of polyethylene glycol monomethyl ether having a number average molecular weight of 700, 20 parts by mass of polyhexamethylene carbonate diol having a number average molecular weight of 1200, 12 parts by mass of neopentyl glycol, and 84.00 parts by mass of acetone as a solvent were added, and the mixture was stirred for 3 hours at 75°C under a nitrogen atmosphere, and it was confirmed that the reaction liquid reached a predetermined amine equivalent. Next, 2.5 parts by mass of trimethylolpropane were added, and the mixture was stirred for 1 hour at 75°C under a nitrogen atmosphere, and it was confirmed that the reaction liquid reached a predetermined amine equivalent. Next, after lowering the temperature of this reaction liquid to 40°C, 8.77 parts by mass of triethylamine were added to obtain a polyurethane prepolymer solution. Next, 450 g of water was added to a reaction vessel equipped with a homodisper capable of high-speed stirring, and the temperature was adjusted to 25°C, and the mixture was stirred for 2000 min.-1 The polyurethane prepolymer solution was added while stirring and mixing at 40° C. to disperse the mixture in water. Then, the acetone and part of the water were removed under reduced pressure to prepare a water-dispersible urethane resin solution (A-5) with a solid content of 34% by mass.
[0073] (Polymerization of urethane resin AX that does not contain polycarbonate polyol components) 75 parts by weight of polyester polyol having a molecular weight of 5000 and composed of terephthalic acid, isophthalic acid, ethylene glycol, and neopentyl glycol, 30 parts by weight of hydrogenated m-xylylene diisocyanate, 7 parts by weight of ethylene glycol, 6 parts by weight of dimethylolpropionic acid, and 84.00 parts by weight of acetone as a solvent were added, and the mixture was stirred for 3 hours at 75°C under a nitrogen atmosphere, and it was confirmed that the reaction liquid reached a predetermined amine equivalent. After lowering the temperature of this reaction liquid to 40°C, 5.17 parts by weight of triethylamine was added to obtain a polyurethane prepolymer solution. Next, 450g of water was added to a reaction vessel equipped with a homodisper capable of high-speed stirring, and the temperature was adjusted to 25°C. The mixture was stirred for 2000min. -1 While stirring and mixing at 40°C, the polyurethane prepolymer solution was added and dispersed in water. Then, the acetone and part of the water were removed under reduced pressure to prepare a water-dispersible urethane resin solution (AX) with a solid content of 34 mass %.
[0074] (Polymerization of blocked isocyanate crosslinking agent B-1) In a flask equipped with a stirrer, a thermometer, and a reflux condenser, 66.04 parts by mass of a polyisocyanate compound having an isocyanurate structure made from hexamethylene diisocyanate (Asahi Kasei Chemicals, Duranate TPA), 17.50 parts by mass of N-methylpyrrolidone, and 23.27 parts by mass of 3,5-dimethylpyrazole (dissociation temperature: 120 ° C, boiling point: 218 ° C) were dropped, and the mixture was kept at 70 ° C for 1 hour under a nitrogen atmosphere. Then, 8.3 parts by mass of dimethylolpropanoic acid were dropped. After measuring the infrared spectrum of the reaction solution and confirming that the absorption of the isocyanate group had disappeared, 5.59 parts by mass of N,N-dimethylethanolamine and 132.5 parts by mass of water were added to obtain a blocked polyisocyanate aqueous dispersion (B-1) with a solid content of 40% by mass. The functional group number of the blocked isocyanate crosslinking agent is 4, and the NCO equivalent is 280.
[0075] (Polymerization of blocked isocyanate crosslinking agent B-2) A flask equipped with a stirrer, a thermometer, and a reflux condenser was charged with 100 parts by mass of a polyisocyanate compound having an isocyanurate structure made from hexamethylene diisocyanate (Asahi Kasei Chemicals, Duranate TPA), 55 parts by mass of propylene glycol monomethyl ether acetate, and 30 parts by mass of polyethylene glycol monomethyl ether (average molecular weight 750), and the mixture was kept at 70°C for 4 hours under a nitrogen atmosphere. Thereafter, the reaction liquid temperature was lowered to 50°C, and 49 parts by mass of methyl ethyl ketoxime was added dropwise. The infrared spectrum of the reaction liquid was measured to confirm that the absorption of the isocyanate group had disappeared, and 210 parts by mass of water was added to obtain an oxime-blocked isocyanate crosslinking agent (B-2) with a solid content of 40% by mass. The number of functional groups of the blocked isocyanate crosslinking agent was 3, and the NCO equivalent was 170.
[0076] (Polymerization of carbodiimide B-3) A flask equipped with a stirrer, a thermometer, and a reflux condenser was charged with 168 parts by mass of hexamethylene diisocyanate and 220 parts by mass of polyethylene glycol monomethyl ether (M400, average molecular weight 400), and stirred at 120 ° C for 1 hour. Further, 26 parts by mass of 4,4'-dicyclohexylmethane diisocyanate and 3.8 parts by mass of 3-methyl-1-phenyl-2-phospholene-1-oxide (2% by mass relative to the total isocyanate) were added as a carbodiimide catalyst, and the mixture was stirred at 185 ° C for another 5 hours under a nitrogen stream. The infrared spectrum of the reaction solution was measured, and it was confirmed that the absorption at wavelengths of 220 to 2300 cm-1 had disappeared. The mixture was allowed to cool to 60 ° C, and 567 parts by mass of ion-exchanged water was added to obtain a carbodiimide aqueous resin solution (B-3) with a solid content of 40% by mass.
[0077] (Polymerization of polyester resin C-1) In a stainless steel autoclave equipped with a stirrer, a thermometer, and a partial reflux condenser, 194.2 parts by mass of dimethyl terephthalate, 184.5 parts by mass of dimethyl isophthalate, 14.8 parts by mass of dimethyl-5-sodium sulfoisophthalate, 233.5 parts by mass of diethylene glycol, 136.6 parts by mass of ethylene glycol, and 0.2 parts by mass of tetra-n-butyl titanate were charged, and an ester exchange reaction was carried out at a temperature of 160°C to 220°C for 4 hours. The temperature was then raised to 255°C, and the reaction system was gradually depressurized, and the reaction was carried out for 1 hour and 30 minutes under a reduced pressure of 30 Pa to obtain a copolymer polyester resin (C-1). The obtained copolymer polyester resin (C-1) was pale yellow and transparent. The reduced viscosity of the copolymer polyester resin (C-1) was measured and found to be 0.70 dl / g. The glass transition temperature measured by DSC was 40°C.
[0078] (Preparation of polyester water dispersion Cw-1) In a reactor equipped with a stirrer, a thermometer, and a reflux device, 15 parts by mass of polyester resin (C-1) and 15 parts by mass of ethylene glycol n-butyl ether were placed, and the resin was dissolved by heating and stirring at 110°C. After the resin was completely dissolved, 70 parts by mass of water was gradually added to the polyester solution while stirring. After the addition, the liquid was cooled to room temperature while stirring to produce a milky white polyester water dispersion (Cw-1) with a solid content of 15% by mass.
[0079] Example 1 (1) Preparation of coating solution The following coating agent was mixed into a mixed solvent of water and isopropanol to prepare a coating solution with a solids mass ratio of urethane resin solution (A-1) / crosslinking agent (B-1) / polyester water dispersion (Cw-1) of 25 / 26 / 49. Urethane resin solution (A-1) 3.55 parts by weight Crosslinking agent (B-1) 3.16 parts by mass Polyester water dispersion (Cw-1) 16.05 parts by mass Particles 0.47 parts by mass (Dry process silica with average particle size of 200 nm, solid content concentration 3.5% by mass) Particles 1.85 parts by mass (Silica sol with average particle size of 40 to 50 nm, solid content concentration of 30% by mass) Surfactant 0.30 parts by weight (Silicone-based, solids concentration 10% by weight)
[0080] (2) Manufacturing of laminated polyester film As the raw polymer for the film, PET resin pellets having an intrinsic viscosity of 0.62 dl / g (solvent: phenol / tetrachloroethane = 60 / 40) and substantially free of particles were dried at 135°C for 6 hours under a reduced pressure of 133 Pa. Then, the pellets were fed to an extruder, melt-extruded into a sheet at about 280°C, and rapidly cooled and solidified on a rotating cooling metal roll maintained at a surface temperature of 20°C to obtain an unstretched PET sheet.
[0081] This unstretched PET sheet was heated to 100° C. using a group of heated rolls and an infrared heater, and then stretched 3.5 times in the longitudinal direction using a group of rolls with different peripheral speeds to obtain a uniaxially stretched PET film.
[0082] Next, the coating solution, which had been left to stand at room temperature for 5 hours or more, was applied to both sides of a PET film by roll coating, and then dried at 80° C. for 20 seconds. The coating amount after the final drying (after biaxial stretching) was 0.15 g / m 2 The film was then stretched 4.0 times in the width direction at 120°C using a tenter, and while the length of the film in the width direction was fixed, it was heated at 230°C for 5 seconds, and further subjected to a 3% width direction relaxation treatment at 100°C for 10 seconds to obtain a 100μm laminated polyester film.
[0083] Next, the A4-sized laminated polyester film was immersed in an aqueous solution containing hydrazine, and catalyst was added using OPC-80 Catalyst M (Okuno Pharmaceutical Co., Ltd.). After thorough rinsing with water, acceleration treatment was performed using OPC-555 (Okuno Pharmaceutical Co., Ltd.). After the above pretreatment, electroless copper plating was performed at 65°C for 30 minutes in a solution containing copper sulfate hydrate and formaldehyde. After further rinsing with an aqueous solution containing ammonium persulfate and sulfuric acid, electrolytic copper plating was performed in a bath containing copper sulfate hydrate and sulfuric acid to provide a copper coating layer of about 20 μm thickness on the coating layer, thereby obtaining a metal-coated polyester film. The evaluation results are shown in Table 1.
[0084] Example 2 A metal-coated polyester film was obtained in the same manner as in Example 1, except that the urethane resin was changed to (A-2).
[0085] Example 3 A metal-coated polyester film was obtained in the same manner as in Example 1, except that the urethane resin was changed to (A-3).
[0086] Example 4 A metal-coated polyester film was obtained in the same manner as in Example 1, except that the crosslinking agent was changed to (B-2).
[0087] Example 5 A metal-coated polyester film was obtained in the same manner as in Example 1, except that the urethane resin was changed to (A-2) and the crosslinking agent was changed to (B-2).
[0088] Example 6 A metal-coated polyester film was obtained in the same manner as in Example 1, except that the urethane resin was changed to (A-3) and the crosslinking agent was changed to (B-2).
[0089] Example 7 A metal-coated polyester film was obtained in the same manner as in Example 1, except that the following coating agent was mixed into a mixed solvent of water and isopropanol, and the solid mass ratio of the urethane resin solution (A-2) / total of the crosslinking agents (B-1, B-2) / polyester water dispersion (Cw-1) was changed to 25 / 25 / 50. Urethane resin solution (A-1) 3.55 parts by weight Crosslinking agent (B-1) 2.10 parts by mass Crosslinking agent (B-2) 1.00 parts by mass Polyester water dispersion (Cw-1) 16.20 parts by mass Particles 0.47 parts by mass (Dry process silica with average particle size of 200 nm, solid content concentration 3.5% by mass) Particles 1.85 parts by mass (Silica sol with average particle size of 40 to 50 nm, solid content concentration of 30% by mass) Surfactant 0.30 parts by weight (Silicone-based, solids concentration 10% by weight)
[0090] Example 8 A metal-coated polyester film was obtained in the same manner as in Example 7, except that the urethane resin was changed to (A-2).
[0091] Example 9 A metal-coated polyester film was obtained in the same manner as in Example 1, except that the following coating agent was mixed into a mixed solvent of water and isopropanol, and the solid mass ratio of the urethane resin solution (A-1) / crosslinking agent (B-1) / polyester water dispersion (Cw-1) was changed to 22 / 10 / 68. Urethane resin solution (A-1) 2.71 parts by weight Crosslinking agent (B-1) 1.00 parts by mass Polyester water dispersion (Cw-1) 19.05 parts by mass Particles 0.47 parts by mass (Dry process silica with average particle size of 200 nm, solid content concentration 3.5% by mass) Particles 1.85 parts by mass (Silica sol with average particle size of 40 to 50 nm, solid content concentration of 30% by mass) Surfactant 0.30 parts by weight (Silicone-based, solids concentration 10% by weight)
[0092] Example 10 A metal-coated polyester film was obtained in the same manner as in Example 9, except that the urethane resin was changed to (A-2).
[0093] Example 11 A metal-coated polyester film was obtained in the same manner as in Example 9, except that the urethane resin was changed to (A-3).
[0094] Example 12 A metal-coated polyester film was obtained in the same manner as in Example 9, except that the crosslinking agent was changed to (B-3).
[0095] Example 13 A metal-coated polyester film was obtained in the same manner as in Example 9, except that the urethane resin was changed to (A-4).
[0096] Example 14 A metal-coated polyester film was obtained in the same manner as in Example 9, except that the urethane resin was changed to (A-5).
[0097] Comparative Example 1 A metal-coated polyester film was obtained in the same manner as in Example 1, except that the urethane resin was changed to (AX).
[0098] Example 15 A laminated polyester film was obtained in the same manner as in Example 1. Thereafter, a metal-coated polyester film was obtained in the same manner as in Example 1, except that the metal coating layer was obtained in the following manner. The laminated polyester film provided with the coating layer was immersed in a 1 wt% silver nitrate aqueous solution, then washed with pure water, and further air-dried to provide an electroless plating catalyst precursor (silver ion). Then, it was immersed for 1 minute in an alkaline aqueous solution (pH 12) containing 0.14 wt% NaOH and 0.25 wt% formalin, then washed with pure water, and the following electroplating treatment was performed. The electroplating solution used was Dyne Silver Bright PL50 (manufactured by Daiwa Kasei Co., Ltd.), adjusted to pH 7.8 with potassium hydroxide, and the film was immersed therein and plated for 15 seconds at 0.5 A / dm2, then washed with pure water, and further air-dried. The thickness of the silver coating layer was about 0.2 μm.
[0099] As shown in Table 1, in each Example, a metal-coated polyester film having excellent adhesion of the metal coating layer in a high-temperature individual room was obtained. Since the haze of the laminated polyester film before the metal coating layer was provided was low, the metal-coated polyester film after the metal coating layer was provided had a beautiful luster. On the other hand, in Comparative Example 1, the adhesion of the metal coating layer under high temperature and high humidity was not satisfactory, possibly because the composition forming the coating layer on the polyester film substrate did not contain a urethane resin having a polycarbonate structure.
[0100] Table 1 summarizes the evaluation results of each of the examples and comparative examples.
[0101] [Table 1] [Industrial Applicability]
[0102] According to the present invention, it is possible to provide a metal-coated polyester film which is electrically conductive, has excellent adhesion of the metal coating layer under high temperature and high humidity conditions, and has a beautiful luster, and which can be suitably used in fields such as electromagnetic wave shielding, circuits, and mirrors.
Claims
1. A metal-coated polyester film having a coating layer and a metal coating layer formed by plating in this order on at least one surface of a polyester film substrate, the coating layer being formed by curing a composition containing a urethane resin having a polycarbonate structure, a crosslinking agent, and a polyester resin, the polyester resin being 5-sodium sulfoisophthalic acid copolymerized polyester, The crosslinking agent is a compound having a tri- or higher functional blocked isocyanate group. Metallized polyester film.
2. 2. The metal-coated polyester film according to claim 1, wherein the urethane resin having a polycarbonate structure has a branched structure.
3. 3. The metal-coated polyester film according to claim 1, wherein the urethane resin having a polycarbonate structure is obtained by synthesizing and polymerizing a polycarbonate polyol component and a polyisocyanate component, and the mass ratio of the polycarbonate polyol component to the polyisocyanate component during the synthesis and polymerization (mass of the polycarbonate polyol component / mass of the polyisocyanate component) is 0.5 to 3.
4. 4. The metal-coated polyester film according to claim 1, wherein the content of the crosslinking agent is 5% by mass or more and 50% by mass or less when the total solid content of the polyester resin, the urethane resin having a polycarbonate structure, and the crosslinking agent is 100% by mass.
5. 5. The metal-coated polyester film according to claim 1, wherein the content of the urethane resin having a polycarbonate structure is 5% by mass or more and 50% by mass or less when the total solid content of the polyester resin, the urethane resin having a polycarbonate structure, and the crosslinking agent is 100% by mass.
6. 6. The metal-coated polyester film according to claim 1, wherein the polyester resin content is 10% by mass or more and 70% by mass or less when the total solid content of the polyester resin, the urethane resin having a polycarbonate structure, and the crosslinking agent is 100% by mass.
7. 7. The metal-coated polyester film according to claim 1, which is used for electromagnetic wave shielding, circuits, or mirrors.
Citation Information
Patent Citations
Manufacture of polyimide film with metallic gilt
JP1990149666A
Metal vapor-deposited polyester film capacitor
JP1995211584A
Electromagnetic wave shielding sheet
JP2007096164A
Transparent base with electromagnetic wave shielding film, and manufacturing method thereof
JP2008300724A
Method of manufacturing electromagnetic wave shield material
JP2009194071A