Treatment agent for ready-mixed concrete, method for producing treatment agent for ready-mixed concrete, and method for treating ready-mixed concrete

A treatment agent using calcium carbonate, calcium hydroxide, silica, and talc addresses the hardening issues of residual ready-mixed concrete, enhancing recycling efficiency and strength through moisture absorption and hydration.

JP7560017B2Active Publication Date: 2024-10-02ASANO ARIAKE READY CONCRETE CO LTD +2
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022062776
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-04-05
Publication Date
2024-10-02
Estimated Expiration
2042-04-05

AI Technical Summary

Technical Problem

Existing methods for recycling residual ready-mixed concrete face challenges due to high water content leading to improper hardening, poor dispersibility, and economic inefficiencies with polymer flocculants, resulting in disposal as industrial waste.

Method used

A treatment agent composed of calcium carbonate, calcium hydroxide, silica, and talc is used to absorb moisture and restore separation resistance and formability in residual concrete, incorporating papermaking sludge ash to enhance hydration and strength.

Benefits of technology

The treatment agent effectively recycles residual concrete by improving hardening and formability while maintaining economic efficiency, achieving high water absorption and strength through a low-cost, simple process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560017000003
    Figure 0007560017000003
  • Figure 0007560017000004
    Figure 0007560017000004
  • Figure 0007560017000005
    Figure 0007560017000005
Patent Text Reader

Abstract

To provide a ready mixed concrete treatment agent capable of attaining the recycling of residual ready mixed concrete by a low cost and simple method, a ready mixed concrete treatment production method, and a ready mixed concrete treatment method.SOLUTION: A ready mixed concrete treatment agent is composed of a porous body essentially consisting of calcium carbonate, calcium hydroxide and silica and comprising talc as a minor component. Then by putting the treatment into residual ready mixed concrete, moisture added to the residual ready mixed concrete is absorbed to improve the properties of the residual ready mixed concrete.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a treatment agent for ready-mixed concrete, a manufacturing method for the treatment agent for ready-mixed concrete, and a method for treating ready-mixed concrete, and more particularly to a treatment agent for ready-mixed concrete that can recycle residual ready-mixed concrete at low cost and in a simple manner, a manufacturing method for the treatment agent for ready-mixed concrete, and a method for treating ready-mixed concrete. [Background technology]

[0002] Most of the concrete used at construction sites is transported as ready mixed concrete from concrete manufacturing plants to the construction site by agitator trucks (also called mixer trucks, ready mixed concrete trucks, truck mixers, etc.), and poured using equipment such as concrete pumps. However, for the convenience of the management of ready mixed concrete, construction sites generally order more than the required amount, so some of the ready mixed concrete transported to the construction site becomes surplus and is returned to the factory (remaining concrete). In addition, ready mixed concrete that does not meet quality standards or is an inappropriate mix due to an ordering error and fails the unloading inspection is also returned unused to the factory (returned concrete).

[0003] As described above, at construction sites where ready-mixed concrete is used, there is a constant production of surplus leftover concrete, or returned concrete, which is returned to the factory. Furthermore, some ready-mixed concrete produced at concrete manufacturing plants is not shipped and remains unused. This type of leftover ready-mixed concrete (residual ready-mixed concrete) is usually discharged from the drum of an agitator truck or the mixer at a concrete manufacturing plant before hardening, and is disposed of as industrial waste. For ready-mixed concrete providers, the cost of disposing of this leftover ready-mixed concrete is a significant burden.

[0004] Therefore, in recent years, from the viewpoint of effective use of resources, there has been a demand for technology to recycle this remaining ready-mix concrete into concrete blocks or recycled aggregate raw materials. On the other hand, since a large amount of water is added to the remaining concrete when it is discharged from the agitator truck, it becomes a highly fluid slurry-like material and there is a risk that it will not set normally as ready-mix concrete. In addition, when the cause of poor quality is an abnormal slump or an excessive unit water content, the returned concrete also has an excessive amount of water, which also causes a problem of it becoming a slurry-like material and being difficult to harden.

[0005] In order to address the above problems, for example, Patent Document 1 proposes a method for treating ready-mixed concrete in which a water-absorbent polymer is added to and mixed with a slurry-like ready-mixed concrete, and the slurry-like ready-mixed concrete is granulated by the water-absorbing action of the water-absorbent polymer. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2011-62943 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, when a polymer flocculant is used to treat ready-mix concrete as in the technology disclosed in Patent Document 1, the polymer flocculant has poor dispersibility in the ready-mix concrete, it takes a long time for the ready-mix concrete to harden, and a large amount of the polymer flocculant must be used, which poses problems in terms of economy.

[0008] On the other hand, the inventors of the present invention have found, through intensive research, that the reason why the remaining ready-mixed concrete does not harden normally is that the remaining ready-mixed concrete has a large unit water content, which reduces the separation resistance of the ready-mixed concrete, causing the aggregate and cement paste in the ready-mixed concrete to separate during hardening, and the aggregate to turn into sludge as only the cement paste hardens. Based on this knowledge, the inventors have developed a treatment agent mainly composed of paper sludge ash that can restore the separation resistance and moldability of the remaining ready-mixed concrete to a certain degree.

[0009] The present invention has been devised in view of the above points, and relates to a treatment agent for ready-mixed concrete that enables the recycling of remaining ready-mixed concrete in a low-cost and simple manner, a method for producing the treatment agent for ready-mixed concrete, and a method for treating ready-mixed concrete. [Means for solving the problem]

[0010] In order to achieve the above object, the treatment agent for ready-mixed concrete of the present invention is a porous material containing calcium carbonate, calcium hydroxide, and silica as main components and talc as a trace component.

[0011] Here, the components of the treatment agent for ready-mixed concrete are porous bodies containing calcium carbonate, calcium hydroxide, and silica as the main components, which enhances water absorption and absorbs water from the remaining ready-mixed concrete, such as the residual concrete that has had water added, or the returned concrete, thereby restoring the separation resistance and moldability of the ready-mixed concrete to a certain degree. Calcium carbonate and calcium hydroxide are substances that are contained in large amounts in cement reactants and limestone, which is the raw material for the reactants, and they actively react with the unreacted cement in the remaining ready-mixed concrete, thereby promoting the reaction.

[0012] Furthermore, by including talc as a trace component in the treatment agent for ready-mixed concrete, the talc can improve the smoothness and the tribological properties between aggregates, and therefore the properties of the ready-mixed concrete to which the treatment agent has been added can be improved, for example, in terms of self-leveling properties.

[0013] In addition, when the content of calcium (Ca), silicon (Si), and magnesium (Mg) in the paper sludge ash satisfies the numerical range of 65-85% by weight of Ca as CaO, 5-15% by weight of Si as SiO2, and 0.5% by weight or more of Mg as MgO, calculated as oxide equivalent with the total weight of the following oxides being 100%, the ash can absorb the moisture contained in the remaining ready-mixed concrete and recover the separation resistance and moldability of the ready-mixed concrete. In addition, since Ca and Mg each have a high affinity with cement, the presence of a certain amount of these components promotes the hydration reaction of cement and ensures the strength of the ready-mixed concrete.

[0014] Here, the treatment agent absorbs the water in the fresh concrete, thereby recovering the water-cement ratio of the fresh concrete and at the same time contributing as fine aggregate. The strength of concrete is affected by the water-cement ratio if the aggregate is the same, and depends on the strength of the aggregate used if the water-cement ratio is the same. Therefore, the treatment agent is required to have high water absorption and high strength as an aggregate.

[0015] The water absorbency in the treatment agent is generated during the manufacturing process of the agent by the combustion of cellulose at around 500°C and the thermal decomposition (decarbonation) of calcium carbonate contained in paper sludge at around 825°C. Also, at around 500°C, the cellulose, which accounts for around 40% of the volume fraction of the paper sludge, spontaneously combusts, causing the paper sludge aggregate particles to turn into a porous material. After that, at around 825°C, the calcium carbonate in the residue thermally decomposes, forming even finer pores in the porous material, improving water absorption performance due to capillary action, and the cellulose components are completely insulated, so the higher the calcium content, the higher the water absorbency tends to be.

[0016] However, calcium carbonate and calcium oxide (or calcium hydroxide that absorbs water at room temperature) are weak as aggregates, so considering the physical properties of hardened concrete, it is necessary to include an appropriate amount of silica (SiO2) (around 10%). The magnesium in the treatment agent is derived from talc. After the treatment agent is added, the ready-mix concrete becomes concrete with a very high fine aggregate ratio, which makes it highly thixotropic, but the fluidity between the aggregates can be maintained by including 0.5% or more talc in MgO equivalent.

[0017] In addition, the density of paper sludge ash is 1.9 to 2.3 g / cm 3 In the case where the water absorption rate is 45% or more, adding a treatment agent made from such paper sludge ash to ready-mix concrete to which water has been added effectively absorbs the water in the ready-mix concrete, improving the separation resistance and moldability of the ready-mix concrete.

[0018] In order to achieve the above-mentioned object, the manufacturing method of a treatment agent for ready-mix concrete of the present invention includes a step of adding a predetermined amount of coagulant to wastewater discharged during the waste paper recycling process to produce papermaking sludge, and a step of calcining the papermaking sludge under temperature conditions of 800°C to 900°C to produce papermaking sludge ash containing calcium carbonate, calcium hydroxide, and silica as main components, and talc as a trace component.

[0019] Here, by providing a process for generating papermaking sludge by adding a predetermined amount of coagulant to wastewater discharged during the wastepaper recycling process, it is possible to generate papermaking sludge by coagulating colloidal particles contained in the wastewater discharged during the wastepaper recycling process. More specifically, the coagulant generates papermaking sludge consisting of pulp (cellulose), talc, calcium hydroxide, and calcium carbonate contained in the wastepaper.

[0020] In addition, by providing a process of burning the paper sludge under a temperature condition of 800°C to 900°C to produce paper sludge ash made of porous bodies containing calcium carbonate, calcium hydroxide, and silica as main components, the cellulose in the paper sludge, which has a low melting point, is burned to form paper sludge ash made of porous bodies including calcium carbonate. In this way, the paper sludge ash made of porous bodies has high water absorption, and by adding it to residual concrete, which is water-added ready-mixed concrete, or residual ready-mixed concrete such as returned concrete, it can effectively absorb the water in the remaining ready-mixed concrete and restore the separation resistance and moldability of the ready-mixed concrete to a certain degree.

[0021] Furthermore, by calcining paper sludge, it is possible to incorporate talc as a minor component in addition to the main components described above. This talc has a high affinity with cement and can improve the properties of ready-mix concrete when water is added.

[0022] If the calcination temperature of the paper sludge is less than 500°C, the oxidation reaction does not proceed, so the cellulose contained in the paper sludge does not burn completely, and the treatment agent does not form a porous body, which may result in poor water absorption. On the other hand, the upper limit of the calcination temperature is not particularly limited, but when the calcination temperature exceeds approximately 825°C, calcium carbonate gradually changes to calcium oxide, and when it exceeds 850°C, it changes completely to calcium oxide, but during the cooling process of the paper sludge ash, some of the calcium oxide absorbs moisture in the air and changes to calcium hydroxide. Therefore, when the calcination temperature exceeds approximately 850°C, the content ratio of calcium carbonate and calcium hydroxide may change, but in either case, a treatment agent with high water absorption can be realized.

[0023] In order to achieve the above-mentioned object, the method for treating ready-mixed concrete of the present invention comprises adding a predetermined amount of a treatment agent made of a porous body containing calcium carbonate, calcium hydroxide, and silica as main components and containing talc as a trace component to the remaining ready-mixed concrete to which water has been added.

[0024] Here, the components of the treatment agent are porous bodies mainly composed of calcium carbonate, calcium hydroxide, and silica, and therefore have the property of being highly water absorbent. By adding a certain amount of this treatment agent to the remaining concrete with added water or the remaining ready-mixed concrete, which is the returned concrete, it is possible to absorb the moisture contained in the remaining ready-mixed concrete and restore the separation resistance and moldability of the remaining ready-mixed concrete to a certain degree.

[0025] In addition, the amount of treatment agent added (M PS ) is the mass of the remaining fresh concrete, M (kg), and the unit water content of the remaining fresh concrete before adding water, W0 (kg / m 3 ), the estimated unit water content of the remaining fresh concrete after adding water is W1 (kg / m 3 ), the unit volume mass of base concrete calculated from the specified mix ratio ρ (kg / m 3 ), and a proportionality constant α according to the type of cement. In this case, when the calculation is based on the formula shown in the following equation 1, the optimum treatment agent can be calculated based on various parameters such as the amount of water contained in the remaining fresh concrete, and therefore the separation resistance and moldability of the remaining fresh concrete can be more effectively restored.

number

[0026] Furthermore, when an amount of treatment agent corresponding to the amount calculated based on the formula shown in Mathematical Formula 1 is poured into the drum of an agitator vehicle in which the remaining fresh concrete remains, and the drum is agitated for a predetermined period of time, the treatment agent can be mixed uniformly throughout the remaining fresh concrete remaining in the drum, thereby maintaining a constant quality of the fresh concrete. Effect of the Invention

[0027] The treatment agent for ready-mixed concrete, the manufacturing method of the treatment agent for ready-mixed concrete, and the method for treating ready-mixed concrete according to the present invention make it possible to recycle remaining ready-mixed concrete in a low-cost and simple manner. [Brief description of the drawings]

[0028] [Figure 1] 1A to 1C are process diagrams illustrating a method for producing a treatment agent according to an embodiment of the present invention. [Diagram 2] 1 is a process diagram showing a method of using a treatment agent according to an embodiment of the present invention. [Diagram 3] FIG. 4 is a diagram showing the results of an analysis of components contained in a treatment agent according to an embodiment of the present invention. [Figure 4] FIG. 2 is a diagram showing the results of an X-ray analysis of ready-mix concrete before the addition of a treatment agent according to an embodiment of the present invention. [Diagram 5] FIG. 2 is a diagram showing the results of an X-ray analysis of ready-mix concrete after the addition of a treatment agent according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS A treatment agent for ready-mixed concrete, a manufacturing method for the treatment agent for ready-mixed concrete, and a method for treating ready-mixed concrete according to embodiments of the present invention will be described in detail below with reference to the drawings and the like for the purpose of understanding the present invention.

[0030] FIG. 1 shows a process diagram for manufacturing a treatment agent for ready-mix concrete according to an embodiment of the present invention. In the manufacturing method for a treatment agent for ready-mix concrete, waste paper to be recycled is first brought into a waste paper recycling processing plant, where the waste paper undergoes well-known recycling processes such as disintegration, dust removal, deinking, and bleaching (step 11). Then, a flocculant is added to the wastewater generated by the recycling process in step 11, and paper sludge is produced as a precipitate (step 12). Furthermore, the paper sludge is fired at a temperature condition of approximately 800°C to 900°C to produce paper sludge ash made of a porous body (step 13).

[0031] The paper sludge ash obtained by the above process is a treatment agent for ready-mixed concrete according to an embodiment of the present invention. The treatment agent is individually packaged, for example, in a water-soluble packaging material, and as described below, a required amount of the treatment agent can be added to the remaining ready-mixed concrete to restore the slump of the remaining ready-mixed concrete and improve the properties of the ready-mixed concrete to meet specified standards.

[0032] Here, the paper sludge ash does not necessarily have to be produced by burning paper sludge produced from wastewater discharged from the recycling process of waste paper. For example, the raw material can be paper sludge produced from wastewater generated in the process of making paper from new pulp (virgin pulp) made from wood.

[0033] However, when virgin pulp is used, substances such as calcium carbonate, silica, and talc, which are the main components of the treatment agent, are not contained in wood chips, and the amount of chemicals added for the purpose of strengthening the paper after the production of wood chips is unintentionally discharged as papermaking sludge. Therefore, the wastewater discharged from the papermaking process of virgin pulp may contain a small amount of the components that make up the treatment agent of the present invention, making it difficult to actively and consistently expect the separation resistance and moldability of the remaining ready-mixed concrete to be effectively restored.

[0034] More specifically, the elements contained in papermaking sludge ash resulting from wastewater discharged from virgin pulp are relatively high in elements such as silicon, aluminum, and iron, and low in calcium and magnesium components, so there is a risk that the specified performance of the treatment agent of the present invention will not be fully exhibited.

[0035] Inorganic flocculants mainly composed of polyaluminum chloride and polyiron chloride are used as the flocculants added to the wastewater to produce the paper sludge used in step 12. However, other inorganic flocculants or polymer flocculants can also be used.

[0036] Moreover, the conditions for burning the paper sludge in step 13 are not limited to the temperature conditions of about 800°C to 900°C. However, if the burning temperature is less than about 800°C, the calcium carbonate component contained in the paper sludge will not undergo a sufficient decarbonation reaction, and it may not be possible to generate a paper sludge ash made of a porous body, and it may not be possible to ensure a certain level of water absorption. However, if the burning temperature is less than 500°C, cellulose will not be decomposed, and the desired performance will not be obtained.

[0037] The upper limit of the burning temperature is not particularly limited, and can be set appropriately taking into consideration the burning cost, etc. If the burning temperature is within the range of approximately 800°C to 850°C, the paper sludge ash after burning will mainly contain calcium carbonate, calcium hydroxide, and silica as main components.

[0038] Furthermore, when paper sludge is burned at approximately 825°C or higher, the calcium carbonate contained in the paper sludge is converted to calcium oxide. Meanwhile, calcium oxide absorbs moisture in the air and converts to calcium hydroxide during the cooling process of the paper sludge ash. Therefore, when the burning temperature exceeds approximately 850°C, the content ratio of calcium carbonate and calcium hydroxide may change, but in either case, a treatment agent with high water absorption can be achieved. Furthermore, when the burning temperature exceeds 900°C, the talc component gradually begins to dehydrate and pyrolyze. Therefore, it is preferable to set the burning temperature to less than approximately 900°C.

[0039] Next, a method for using the treating agent (paper sludge ash) obtained by the above-mentioned manufacturing process will be described with reference to FIG.

[0040] First, the mass M (kg) of the remaining ready-mixed concrete remaining in the drum of the agitator truck that has returned to the concrete manufacturing plant is measured (step 21). The mass of the remaining ready-mixed concrete can be measured using a large weighing device such as a truck scale.

[0041] Next, a certain amount of the remaining fresh concrete (for example, 10 L) is taken from the drum, the mass of the sample is measured, the density is calculated, and the calculated density is input into the unit water meter to obtain the unit water content W0 (kg / m 3 ) is measured (step 22). The density may be measured by calculation or may be measured using a density measuring device.

[0042] The unit water content before water addition obtained in step 22 is divided by the correction coefficient set for each model of unit water meter used for measurement to obtain the estimated unit water content W1 (kg / m) of the remaining fresh concrete after water addition. 3 ) is calculated (step 23).

[0043] Furthermore, the unit volume mass ρ (kg / m) of the base concrete (basecon) calculated from the specified mix 3 ) is calculated (step 24).

[0044] Once the parameters are obtained in steps 21 to 24, the appropriate amount M of the treatment agent to be added to the drum of the agitator vehicle is calculated based on the formula shown in the above formula 1. PS (kg / m 3 ) is calculated (step 25). Here, α in the formula is a proportionality coefficient for each cement, and for example, for ordinary Portland cement (N cement), α is approximately 0.8.

[0045] In step 25, the appropriate amount of treatment agent to be added is M PS Once the amount of the treatment agent is obtained, the corresponding amount is measured with a scale and poured into the drum of the agitator car (step 26). At this time, if the treatment agent is prepared in small portions in water-soluble packages for each specified unit amount as described above, it is possible to pour the appropriate amount of treatment agent into the drum, thereby eliminating the need to measure the treatment agent with a scale.

[0046] After the treatment agent is poured into the drum, the drum is rotated to mix the treatment agent and the remaining fresh concrete until they are uniform. The time the drum is rotated depends on the rotation speed and the amount of remaining fresh concrete, but rotating the drum at high speed for about three minutes is sufficient.

[0047] <Example> Next, an example will be described. The remaining ready mixed concrete used in the example was ordinary Portland cement (N cement), and had a nominal strength, slump, and coarse aggregate size of "24-18-20N."

[0048] First, 500 L (0.5 m) of the remaining ready-mixed concrete in the drum was removed. 3 Based on the density of the sample, the unit water content (W0) of the remaining ready-mix concrete before adding water was calculated using a unit water meter (KEYTEC SONO-WZ) and was 184 kg / m 3 The estimated unit water volume (W1) after adding water was calculated by dividing the estimated unit water volume by the correction coefficient of the unit water volume meter used for the measurement (0.95 in the case of the unit water volume meter mentioned above), and the result was 251.6 kg / m 3 It was.

[0049] Based on the above parameters, the appropriate amount of treatment agent (M PS Based on this calculation result, 35 kg of the treatment agent was poured into the drum, and the drum was rotated at high speed until the treatment agent and the remaining ready-mixed concrete were uniformly mixed.

[0050] The ready-mixed concrete obtained in this way had an extremely good surface appearance and self-leveling properties due to the talc contained as a trace component in the treatment agent. Furthermore, when the slump of the ready-mixed concrete was measured before and after the addition of the treatment agent, it was confirmed that the slump of the ready-mixed concrete before the addition of the treatment agent was 65 cm, while the slump of the ready-mixed concrete after the addition of the treatment agent improved to 19 cm.

[0051] Furthermore, a strength test was conducted on the ready mixed concrete immediately after adding the treatment agent. The concrete specimens used in the strength test were cured by standard curing, and the strength after one week was 15.3 N / mm 2 , 2-week strength is 18.5N / mm 2 From these results, the estimated 4-week strength was about 21N, and while the ready-mixed concrete before the addition of the treatment agent was "24-18-20N," the ready-mixed concrete after the addition of the treatment agent was "18-18-20N," confirming that a certain level of strength was achieved.

[0052] Next, the results of a component analysis of the treatment agent using an X-ray diffraction device (Shimadzu Corporation) are shown in Figure 3. The measurement was performed three times, and the respective measurement results are displayed as PS1, PS2, and PS3. As shown in Figure 3, the main components of the treatment agent are calcium (Ca), silicon (Si), and magnesium (Mg), and the content of Ca as CaO is 65 to 85 weight %, Si as SiO2 is 5 to 15 weight %, and Mg as MgO is 0.5 weight % or more, calculated as oxides with the total weight of the oxides being 100 weight %.

[0053] The results of analyzing the composition of the ready-mixed concrete before and after the addition of the treatment agent using a wavelength dispersive X-ray fluorescence analyzer (ZSX Primus II, Rigaku Corporation) are shown in Figures 4 and 5. Figure 4 shows the results of the X-ray analysis of the ready-mixed concrete before the addition of the treatment agent, and Figure 5 shows the results of the X-ray analysis of the ready-mixed concrete after the addition of the treatment agent.

[0054] As shown in Figures 4 and 5, it can be confirmed that the magnesium (Mg), aluminum (Al), and calcium (Ca) contents in the fresh concrete after the addition of the treatment agent are increased compared to before the addition. Of these, magnesium is derived from talc contained as a trace component in the treatment agent. Meanwhile, aluminum is derived from polyaluminum chloride and polyferric chloride contained in the coagulant added to the paper sludge. Furthermore, calcium is derived from calcium carbonate, calcium hydroxide, or calcium oxide contained in the paper sludge.

[0055] Regarding silicon (Si) derived from the aggregate in the ready-mix concrete, the content after the addition of the treatment agent was lower than before it was added, but this is presumably due to a relative decrease in the content caused by an increase in the content of other elemental components.

[0056] INDUSTRIAL APPLICABILITY As described above, the treatment agent for ready-mixed concrete, the manufacturing method of the treatment agent for ready-mixed concrete, and the method for treating ready-mixed concrete according to the present invention enable the recycling of residual ready-mixed concrete in a low-cost and simple manner.

Claims

1. It is a porous material that mainly contains calcium carbonate, calcium hydroxide, and silica, and also contains talc as a minor component. A treatment agent for ready-mix concrete.

2. The contents of calcium (Ca), silicon (Si), and magnesium (Mg) in the porous body are expressed as oxide equivalents with the total weight of the following oxides being 100% by weight: 65 to 85% by weight of Ca as CaO, Si to SiO 2 5 to 15% by weight as Mg is 0.5% by weight or more as MgO. The treatment agent for ready mixed concrete according to claim 1.

3. The porous body has a density of 1.9 to 2.3 g / cm 3 , water absorption rate is 45% or more The treatment agent for ready mixed concrete according to claim 1 or 2.

4. A step of adding a predetermined amount of coagulant to wastewater discharged during a waste paper recycling process to generate papermaking sludge; and a step of burning the papermaking sludge under a temperature condition of 800°C to 900°C to produce papermaking sludge ash consisting of a porous body containing calcium carbonate, calcium hydroxide, and silica as main components and talc as a trace component. A manufacturing method for a treatment agent for ready-mix concrete.

5. A predetermined amount of a treatment agent consisting of a porous material containing calcium carbonate, calcium hydroxide, and silica as main components and talc as a trace component is added to the remaining fresh concrete to which water has been added. How to process ready mixed concrete.

6. The amount of the treatment agent added (M PS ) is the mass of the remaining fresh concrete M (kg), and the unit water content of the remaining fresh concrete before adding water W 0 (kg / m 3 ), the estimated unit water volume of the remaining fresh concrete after adding water is W 1 (kg / m 3 ), the unit volume data of base concrete calculated from the specified mix ratio ρ (kg / m 3 ), and a proportionality constant α according to the type of cement is used, and the formula is calculated based on the following formula: A method for treating ready mixed concrete according to claim 5. [0010]

7. The treatment agent is added in an amount equivalent to the amount calculated based on the formula into the drum of the agitator vehicle in which the remaining ready-mixed concrete remains, and the drum is agitated for a predetermined period of time. A method for treating ready mixed concrete according to claim 6.

Citation Information

Patent Citations

  • Lightweight mortar or concrete using granulated hydrothermal solid matter of paper sludge incineration ash

    JP2007015893A

  • Unused ready-mixed concrete treatment method, and recycled ready-mixed concrete

    JP2011062943A

  • Method for treating dredged sedimentary soil

    JP2012193223A

  • Treatment method of ready-mixed concrete residue

    JP2015093473A

  • Cement-free or low-cement low-dust hybrid flooring composition

    JP2016526058A